Zn-Li-Mn-Y series degradable zinc alloy and preparation and application thereof

By adding Li, Mn and Y elements to the zinc alloy and adopting multi-pass thermal processing technology to form a Zn-Li-Mn-Y-based degradable zinc alloy, the problem of insufficient tensile strength of the zinc alloy is solved and high Strength and good biocompatibility, suitable for high-end medical devices such as thin-walled cardiovascular stents.

CN119082548APending Publication Date: 2024-12-06PEKING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411198078.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The tensile strength of existing zinc alloys is insufficient, making it difficult to meet the strength requirements of high-end medical devices such as thin-walled cardiovascular stents, especially in terms of the matching rate of in vivo degradation and tissue repair process.

Method used

By adding Li, Mn and Y elements to the zinc alloy, a multi-pass hot processing process is adopted, including smelting, hot rolling, forging and hot extrusion, to form a Zn-Li-Mn-Y-type degradable zinc alloy, and optimize its The grain structure and dislocation distribution significantly improve the tensile strength.

Benefits of technology

The tensile strength of zinc alloy is significantly improved to reach 779MPa, which meets the mechanical properties requirements of thin-walled scaffolds, and maintains good biocompatibility and degradation properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082548A_ABST
    Figure CN119082548A_ABST
Patent Text Reader

Abstract

The invention discloses a Zn-Li-Mn-Y series degradable zinc alloy as well as preparation and application of the Zn-Li-Mn-Y series degradable zinc alloy. In the zinc alloy, the mass percentage of Li is 0.8 + / -0.1%, the mass percentage of Mn is 0.1 + / -0.05%, and the mass percentage of Y is 0-3%, but not including 0; and the balance of zinc. The zinc alloy has excellent mechanical properties and biocompatibility, can provide long-term effective supporting force in vivo, and can be used as a degradable orthopedic implant and a degradable stent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of medical metal materials, and specifically relates to a Zn-Li-Mn-Y series degradable zinc alloy and a preparation method and application thereof. Background Art

[0002] Medical devices made of biomaterials interact with the body in vivo to promote diagnosis, treatment or tissue repair. According to the service life in the body, they are divided into permanent biomaterials and degradable biomaterials. In recent years, degradable biomaterials have become a research hotspot, including magnesium-based alloys, iron-based alloys and zinc-based alloys. These materials use the corrosion-prone properties of alloys in the human body environment to achieve the repair function of metal implants in a controllable manner, and completely degrade into harmless metal ions and other products after the reconstruction and functional repair of human tissues.

[0003] Compared with magnesium-based alloys and iron-based alloys, the core competitiveness of zinc-based alloys lies in their suitable degradation rate in vivo. The standard electrode potential of zinc (-0.76V) is between magnesium (-2.37V) and iron (-0.44V), and its degradation rate in vivo is more compatible with the tissue repair process. However, the strength of pure zinc is relatively low, the tensile strength of cast pure zinc is only about 18MPa (Materials & Design, 2015, 83: 95-102), and the tensile strength of extruded pure zinc is only about 110MPa (Journal of the Mechanical Behavior of Biomedical Materials, 2016, 60: 581-602). The tensile strength of zinc alloys reported so far is mostly below 600MPa, which is still a certain gap compared with traditional titanium alloys and Co-Cr alloys. Excellent strength is a necessary prerequisite for the development of high-end medical devices. For example, the current development trend of cardiovascular stents is to thin the wall (<80μm) to shorten the stent endothelialization time and reduce the risk of thrombosis; however, while reducing the wall thickness, the stent still needs to have a high radial support force to help blood vessel repair, which requires the strength of the stent material to be further improved. Therefore, it is urgent to develop high-strength biomedical degradable zinc alloys.

[0004] Researchers have carried out a lot of research work. For example, patent CN103736152B discloses a degradable strong and tough zinc alloy, which improves the performance of the alloy by adding four elements: Ce, Mg, Ca, and Cu; however, the plasticity of this alloy is still relatively low. Patent CN111334688A discloses a method for preparing a Zn-RE alloy, adding rare earth elements to the zinc alloy, and preparing alloy bars through a single hot extrusion process; however, the performance improvement is not obvious. Patent CN113005330A discloses a biodegradable ultrafine-grained Zn-Li alloy material, preparation method, and application, which improves its mechanical properties by adding Li elements and multiple deformation processes; but the yield strength is not high. Patent CN108315583A developed by the inventor in the early stage discloses a Zn-Li-Mn zinc alloy. By adding different contents of Li (strengthening) and Mn (plasticizing) elements to the zinc alloy matrix for synergistic optimization, the tensile strength of the Zn0.8Li0.1Mn alloy can reach 552MPa and the plasticity is 108%, which basically meets the mechanical performance requirements for preparing degradable stents (wall thickness 80μm; radial support force 120kPa), but there is still a certain distance from the latest developed DES stent or degradable iron-based stent (Iron Based Scaffold) (wall thickness <70μm; radial support force>140kPa). Therefore, the strength of the Zn-Li-Mn alloy needs to be further improved to achieve the requirements of thin-walled stents.

[0005] The comprehensive mechanical properties of the alloys involved in the above existing patents are summarized as follows:

[0006] Summary of the invention

[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a high tensile strength Zn-Li-Mn-Y series biodegradable zinc alloy and its preparation and application. The alloy material has excellent mechanical properties and biocompatibility and can provide long-term effective support in the body.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] A Zn-Li-Mn-Y series degradable zinc alloy, in which, by mass percentage, the mass percentage of Li is 0.8±0.1%, the mass percentage of Mn is 0.1±0.05%, the mass percentage of Y is 0-3% but not including 0; and the balance is zinc.

[0010] In the Zn-Li-Mn-Y series degradable zinc alloy, the mass percentage of Y preferably ranges from 0 to 2%, but does not include 0; and more preferably ranges from 0 to 1%, but does not include 0.

[0011] Preferably, the Zn-Li-Mn-Y series degradable zinc alloy may be any one of the following, wherein the numbers represent mass percentages:

[0012] (1) Zn-0.8Li-0.1Mn-0.3Y

[0013] (2) Zn-0.8Li-0.1Mn-0.5Y

[0014] (3) Zn-0.8Li-0.1Mn-1.0Y

[0015] (4) Zn-0.8Li-0.1Mn-2.0Y.

[0016] The Zn-Li-Mn-Y series degradable zinc alloy is preferably Zn-0.8Li-0.1Mn-0.5Y.

[0017] The method for preparing the Zn-Li-Mn-Y series degradable zinc alloy comprises the following steps:

[0018] (1) high purity Zn and Y are mixed and smelted under the protection of CO2 and SF6 atmosphere, and then cast and cooled to obtain a master alloy Zn-10.0wt.%Y;

[0019] (2) Mixing and smelting high-purity Zn and Li under the protection of CO2 and SF6 atmosphere, and then casting and cooling to obtain an intermediate alloy Zn-5.0wt.%Li;

[0020] (3) Mixing and smelting high-purity Zn and Mn under the protection of CO2 and SF6 atmosphere, and then casting and cooling to obtain the intermediate alloy Zn-5.0wt.%Mn;

[0021] (4) The intermediate alloys Zn-10.0wt.%Y, Zn-5.0wt.%Li and Zn-5.0wt.%Mn and pure zinc are mixed and smelted in proportion under a protective atmosphere, and then cast and cooled to obtain the Zn-Li-Mn-Y series degradable zinc alloy.

[0022] In step (1), the smelting temperature is 650-900°C, preferably 700-800°C.

[0023] In step (2), the smelting temperature is 550-700°C, preferably 600-650°C.

[0024] In step (3), the smelting temperature is 420-800°C, preferably 550-650°C.

[0025] In steps (1), (2) and (3), a period of static treatment is required after smelting in order to separate impurities and purify the material.

[0026] In step (4), the smelting temperature is 620-850°C, preferably 660-750°C.

[0027] In step (4), the Zn-Li-Mn-Y series zinc alloy obtained after casting and cooling is mechanically processed, and the mechanical processing steps include three steps of hot rolling, forging and hot extrusion.

[0028] Before the mechanical processing, the zinc alloy is heat treated for homogenization: the heat treatment temperature is 250-350° C., the time is 12-25 hours, and oil quenching or water quenching is performed after the heat treatment.

[0029] The mechanical processing specifically comprises the following steps:

[0030] (1) Wire cutting: Cut the Zn-Li-Mn-Y zinc alloy ingot into cylinders with a diameter of 35-45 mm and a height of 35-45 mm, and heat and keep the cylinders warm for 6-8 hours at a temperature of 300-400°C.

[0031] (2) Forging: Forging the Zn-Li-Mn-Y zinc alloy cylinder with a forging machine to forge the cylinder into a disc with a thickness of 0.5-1 cm, and then heating it to 300-400° C. and keeping it warm for 30-60 min;

[0032] (3) Rolling: The rolling passes are 4-8, and the pressing amount each time is 0.5-1 mm; the material is rolled into a 1-6 mm rectangular thin plate, and the material is returned to the furnace and heated to 500-600 ° C and kept warm for 30-60 minutes;

[0033] (4) Lamination forging: Lamination of multiple thin plates, with adjacent sheets rolling in opposite directions, adding a layer of Zn-Li-Mn-Y zinc alloy raw metal powder between the two layers, with the number of laminated layers being 5-8 layers. After lamination, the plates are kept at 500-600°C for 30-60 minutes, then taken out for forging, and the layers of materials are forged into one body to eliminate internal residual stress, component segregation, pore inclusions and other defects, and forged into an approximate cylinder with a diameter between 15-30 mm;

[0034] (5) Hot extrusion: The cylinder is hot extruded at a temperature of 200-300°C to extrude a Zn-Li-Mn-Y biodegradable zinc alloy rod having a diameter of 10-15 mm.

[0035] The application of the Zn-Li-Mn-Y series degradable zinc alloy is as a degradable orthopedic implant, and the orthopedic implant includes: at least one of bone plates, bone nails, bone needles, bone rods, spinal fixation equipment, ligature wires, patellar collectors, bone wax, bone repair materials, bone tissue repair scaffolds, intramedullary nails and bone sleeves, and guided bone regeneration barrier (GBR) membranes.

[0036] The application of the Zn-Li-Mn-Y series degradable zinc alloy is as a degradable stent, and the stent includes at least one of: a cardiac stent, a ureteral stent, a prostate stent, an esophageal stent, a duodenal stent, a colon stent, a bile duct stent, a pancreatic stent, a tracheal stent, a bronchial stent, an airway stent, a nasolacrimal duct stent, and a peripheral vascular stent.

[0037] The present invention further adds alloying element Y to the Zn-Li-Mn zinc alloy, and the alloy is significantly strengthened. The specific principles are as follows: (1) Element Y can refine the alloy microstructure and significantly reduce the grain size. The finer the grains of the alloy, the more the number of internal grains and grain boundaries. According to the Hall-Petch relationship, the smaller the average diameter of the grains, the higher the yield strength of the material, which has the effect of fine grain strengthening. (2) Element Y will generate YZn in the zinc alloy matrix. 12 phase, evenly distributed in the matrix, hinders the movement of dislocations inside the alloy, and plays a role of dispersion strengthening. (3) The preparation method of the present invention includes alloy smelting, multiple rolling, forging and one extrusion. As the plastic deformation proceeds, the dislocation density increases continuously, resulting in enhanced interaction during dislocation movement, increased resistance to dislocation movement, and increased deformation resistance, which plays a role of deformation strengthening. Fig.13 The EBSD test results of the Zn-Li-Mn-Y alloy shown in the figure show that the grain size of the zinc matrix is ​​mostly below 10μm, and the YZn 12 The phase is uniformly and dispersedly distributed in the matrix, which verifies the strengthening principle of Y element in Zn-Li-Mn alloy.

[0038] Compared with the prior art, the present invention has the following advantages and effects:

[0039] (1) The present invention introduces the rare earth element Y into the ternary Zn-Li-Mn alloy, which can significantly improve the tensile strength of the alloy. The tensile strength of the Zn-Li-Mn-Y alloy reaches 779 MPa, which exceeds the reported strength of existing zinc alloys, and other rare earth elements cannot achieve the same strengthening effect;

[0040] (2) The alloy obtained by the present invention has very small grain size, uniform alloy structure, good biocompatibility and low hemolysis rate, and is an ideal biomedical implant material. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Schematic diagram of Zn-Li-Mn-Y zinc alloy ingot.

[0042] Figure 2 Schematic diagram of a small cast cylinder of Zn-Li-Mn-Y zinc alloy.

[0043] Figure 3 Schematic diagram of a rectangular thin sheet of Zn-Li-Mn-Y zinc alloy.

[0044] Figure 4 Schematic diagram of the forged cylinder of Zn-Li-Mn-Y zinc alloy.

[0045] Figure 5 Schematic diagram of the extruded round rod of Zn-Li-Mn-Y zinc alloy.

[0046] Figure 6 This is the microstructure of the extruded Zn-Li-Mn-Y zinc alloy.

[0047] Figure 7 This is the stress-strain curve of the Zn-Li-Mn-Y zinc alloy obtained in Example 3.

[0048] Figure 8 This is the Tafel curve of the Zn-Li-Mn-Y zinc alloy obtained in Example 4.

[0049] Fig. 9 This is the corrosion morphology of the Zn-Li-Mn-Y zinc alloy obtained in Example 5 after being immersed in simulated body fluid (SBF) for 28 days.

[0050] Fig.10 The relative survival rates of MC3T3 cells and HUVEC cells in the Zn-Li-Mn-Y zinc alloy extracts of different concentrations (concentrations of 50%, 25% and 12.5% ​​respectively) obtained in Example 6.

[0051] Fig.11 The spreading conditions of MC3T3 cells and HUVEC cells in the Zn-Li-Mn-Y zinc alloy extracts of different concentrations (concentrations of 50%, 25% and 12.5% ​​respectively) obtained in Example 6.

[0052] Fig.12 This is the hemolysis rate test result of the Zn-Li-Mn-Y series zinc alloy obtained in Example 7.

[0053] Fig.13 These are the EBSD test results of Zn-Li-Mn-Y alloys. DETAILED DESCRIPTION

[0054] In order to facilitate the understanding of the present invention, the present invention will be described in detail below in conjunction with specific embodiments. The following examples will help those skilled in the art to further understand the present invention, but do not limit the present invention in any form. It should be pointed out that, for those skilled in the art, without departing from the concept of the present invention, the present invention can also make some deformations and improvements, which all belong to the protection scope of the present invention. The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources. The percentages used in the following examples, unless otherwise specified, are all percentages by mass.

[0055] Example 1: Preparation of Zn-0.8Li-0.1Mn-0.3Y alloy

[0056] The intermediate frequency furnace is used for non-vacuum melting, and the graphite crucible is used for melting with rice husk covering. The Y mass percentage is 10.0wt.%, and the balance is zinc. The Y-10.0wt.% Y master alloy is prepared by weighing, melting, standing and casting. The Li mass percentage is 5.0wt.%, and the balance is zinc. The Zn-5.0wt.% Li master alloy is prepared by weighing, melting, standing and casting. The Mn mass percentage is 5.0wt.%, and the balance is zinc. The Zn-5.0wt.% Mn master alloy is prepared by weighing, melting, standing and casting. The calculated mass of Zn-10.0wt.%Y, Zn-5.0wt.%Li, Zn-5.0wt.%Mn intermediate alloys and pure zinc were mixed and melted in a medium frequency furnace for non-vacuum melting at a temperature of 620°C. After casting, Zn-0.8Li-0.1Mn-0.3Y ingots were obtained, which passed the inspection and were then cast.

[0057] The zinc alloy is heat treated for homogenization before machining: the heat treatment temperature is 250° C., the time is 12 h, and oil quenching is performed after the heat treatment.

[0058] The cast Zn-0.8Li-0.1Mn-0.3Y alloy ingot is cut into small cylinders by wire cutting method. The cylinder diameter is 35mm and the cylinder height is 35mm. The cylinder is heated and kept warm for 6 hours at a temperature of 300℃. After taking out, the cylinder is placed vertically (flat side facing down) and forged with a forging machine. The cylinder is forged into a disc with a thickness of 0.5cm. It is then returned to the furnace and heated to 300℃ again. It is kept warm for 30min and rolled. There are 4 rolling passes, and the pressing amount is 1mm each time. The material is rolled into a 1mm rectangular sheet. The material is returned to the furnace and heated to 500℃. It is kept warm for 30min. After taking out, multiple sheets are stacked. The rolling directions of the adjacent two sheets are opposite. A layer of Zn-0.8Li-0.1Mn-0.3Y zinc alloy raw metal powder is added between the two layers. The number of stacked layers is 5. After stacking, they are kept at 500℃ for 30 minutes, then taken out and forged. Several layers of materials are forged into one body to eliminate internal residual stress, component segregation, pore inclusions and other defects. They are forged into approximate cylinders with a diameter of 15mm. Radial hot extrusion is carried out at an extrusion process temperature of 200℃ to extrude Zn-0.8Li-0.1Mn-0.3Y rods with a diameter of 10mm.

[0059] Example 2: Preparation of Zn-0.8Li-0.1Mn-0.5Y alloy

[0060] The intermediate frequency furnace is used for non-vacuum melting, and the graphite crucible is used for melting with rice husk covering. The Y mass percentage is 10.0wt.%, and the balance is zinc. The Y-10.0wt.% Y master alloy is prepared by weighing, melting, standing and casting. The Li mass percentage is 5.0wt.%, and the balance is zinc. The Zn-5.0wt.% Li master alloy is prepared by weighing, melting, standing and casting. The Mn mass percentage is 5.0wt.%, and the balance is zinc. The Zn-5.0wt.% Mn master alloy is prepared by weighing, melting, standing and casting. The calculated mass of Zn-10.0wt.%Y, Zn-5.0wt.%Li, Zn-5.0wt.%Mn intermediate alloys and pure zinc were mixed and melted in a medium frequency furnace for non-vacuum melting at a temperature of 660°C. After casting, Zn-0.8Li-0.1Mn-0.5Y ingots were obtained, which passed the inspection and were then cast.

[0061] The zinc alloy is heat treated for homogenization before the mechanical processing: the heat treatment temperature is 300° C., the time is 15 hours, and oil quenching is performed after the heat treatment.

[0062] The cast Zn-0.8Li-0.1Mn-0.5Y alloy ingot is cut into small cylinders by wire cutting method. The cylinder diameter is 40mm and the cylinder height is 40mm. The cylinder is heated and kept warm for 7h at a temperature of 350℃. After taking out, the cylinder is placed vertically (flat side facing down) and forged with a forging machine. The cylinder is forged into a disc with a thickness of 0.6cm. It is then returned to the furnace and heated to 350℃ again, kept warm for 40min, and rolled. The rolling passes are 5, and the pressing amount is 1mm each time. The material is rolled into a 3mm rectangular sheet, the material is returned to the furnace and heated to 550℃, kept warm for 40min, and after taking out, multiple sheets are stacked. The rolling directions of the adjacent two sheets are opposite. A layer of Zn-0.8Li-0.1Mn-0.5Y zinc alloy raw metal powder is added between the two layers, and the number of stacked layers is 6. After stacking, they are kept at 550℃ for 40 minutes, then taken out for forging. Several layers of materials are forged into one body to eliminate internal residual stress, component segregation, pore inclusions and other defects. They are forged into an approximate cylinder with a diameter of 20mm. Radial hot extrusion is carried out at an extrusion process temperature of 250℃ to extrude Zn-0.8Li-0.1Mn-0.5Y rods with a diameter of 12mm.

[0063] Example 3: Preparation of Zn-0.8Li-0.1Mn-1.0Y alloy

[0064] The intermediate frequency furnace is used for non-vacuum melting, and the graphite crucible is used for melting with rice husk covering. The Y mass percentage is 10.0wt.%, and the balance is zinc. The Y-10.0wt.% Y master alloy is prepared by weighing, melting, standing and casting. The Li mass percentage is 5.0wt.%, and the balance is zinc. The Zn-5.0wt.% Li master alloy is prepared by weighing, melting, standing and casting. The Mn mass percentage is 5.0wt.%, and the balance is zinc. The Zn-5.0wt.% Mn master alloy is prepared by weighing, melting, standing and casting. The calculated mass of Zn-10.0wt.%Y, Zn-5.0wt.%Li, Zn-5.0wt.%Mn intermediate alloys and pure zinc are mixed and melted in a medium frequency furnace for non-vacuum melting at a temperature of 750°C. After casting, Zn-0.8Li-0.1Mn-1.0Y ingots are obtained, which pass the inspection and are available as car skins.

[0065] The zinc alloy is heat treated for homogenization before the mechanical processing: the heat treatment temperature is 350° C., the time is 25 hours, and water quenching is performed after the heat treatment.

[0066] The cast Zn-0.8Li-0.1Mn-1.0Y alloy ingot is cut into small cylinders by wire cutting method. The cylinder diameter is 45mm and the cylinder height is 45mm. The cylinder is heated and kept warm for 8 hours at a temperature of 400℃. After taking out, the cylinder is placed vertically (flat side facing down) and forged with a forging machine. The cylinder is forged into a disc with a thickness of 1cm. It is then returned to the furnace and heated to 400℃, kept warm for 60min, and rolled. There are 8 rolling passes, and the pressing amount is 0.5mm each time. The material is rolled into a 6mm rectangular sheet, and the material is returned to the furnace and heated to 600℃, kept warm for 60min. After taking out, multiple sheets are stacked, and the rolling directions of adjacent sheets are opposite. A layer of Zn-0.8Li-0.1Mn-1.0Y zinc alloy raw metal powder is added between the two layers, and the number of stacked layers is 8. After stacking, the material is kept at 600°C for 60 minutes, then taken out for forging. Several layers of material are forged into one body to eliminate internal residual stress, component segregation, pore inclusions and other defects. It is forged into an approximate cylinder with a diameter of 30 mm and subjected to radial hot extrusion. The extrusion process temperature is 300°C, and the extruded Zn-0.8Li-0.1Mn-1.0Y rod with a diameter of 15 mm is extruded.

[0067] Example 4: Preparation of Zn-0.8Li-0.1Mn-2.0Y alloy

[0068] The intermediate frequency furnace is used for non-vacuum melting, and the graphite crucible is used for melting with rice husk covering. The Y mass percentage is 10.0wt.%, and the balance is zinc. The Y-10.0wt.% Y master alloy is prepared by weighing, melting, standing and casting. The Li mass percentage is 5.0wt.%, and the balance is zinc. The Zn-5.0wt.% Li master alloy is prepared by weighing, melting, standing and casting. The Mn mass percentage is 5.0wt.%, and the balance is zinc. The Zn-5.0wt.% Mn master alloy is prepared by weighing, melting, standing and casting. The calculated mass of Zn-10.0wt.%Y, Zn-5.0wt.%Li, Zn-5.0wt.%Mn intermediate alloys and pure zinc are mixed and melted in a medium frequency furnace for non-vacuum melting at a temperature of 850°C. After casting, a Zn-0.8Li-0.1Mn-2.0Y ingot is obtained, which passes the inspection and is available as a car skin.

[0069] Before the mechanical processing, the zinc alloy is subjected to heat treatment for homogenization: the heat treatment temperature is 280° C., the time is 20 hours, and water quenching is performed after the heat treatment.

[0070] The cast Zn-0.8Li-0.1Mn-2.0Y alloy ingot is cut into small cylinders by wire cutting method. The cylinder diameter is 42mm and the cylinder height is 42mm. The cylinder is heated and kept warm for 7.5h at a temperature of 330℃. After taking out, the cylinder is placed vertically (flat side facing down) and forged with a forging machine. The cylinder is forged into a 1cm thick disc. It is then returned to the furnace and heated to 360℃ again. It is kept warm for 60min and rolled. The rolling passes are 7 times, and the pressing amount is 0.5mm each time. The material is rolled into a 6mm rectangular sheet. The material is returned to the furnace and heated to 600℃. It is kept warm for 60min. After taking out, multiple sheets are stacked. The rolling directions of the adjacent two sheets are opposite. A layer of Zn-0.8Li-0.1Mn-2.0Y zinc alloy raw metal powder is added between the two layers. The number of stacked layers is 6. After stacking, the material is kept at 520℃ for 50 minutes, then taken out for forging. Several layers of material are forged into one body to eliminate internal residual stress, component segregation, pore inclusions and other defects. It is forged into an approximate cylinder with a diameter of 22mm and subjected to radial hot extrusion. The extrusion process temperature is 250℃, and the extruded Zn-0.8Li-0.1Mn-2.0Y rod with a diameter of 10mm is extruded.

[0071] The morphology of the Zn-Li-Mn-Y series zinc alloy ingots prepared in Examples 1 to 4 is as follows: Figure 1 shown.

[0072] The morphology of the cast small cylinder of Zn-Li-Mn-Y series zinc alloy prepared by wire cutting in the above Examples 1 to 4 is as follows: Figure 2 shown.

[0073] The rectangular thin sheets of Zn-Li-Mn-Y zinc alloy prepared by rolling in the above-mentioned Examples 1 to 4 have the following shapes: Figure 3 shown.

[0074] The morphology of the Zn-Li-Mn-Y series zinc alloy cylinder prepared by forging in the above Examples 1 to 4 is as follows: Figure 4 shown.

[0075] The morphology of the Zn-Li-Mn-Y series zinc alloy rods prepared by extrusion in the above-mentioned Examples 1 to 4 is as follows: Figure 5 shown.

[0076] The microstructure of extruded Zn-Li-Mn-Y alloy is as follows Figure 6 As shown. It can be seen that there are large pieces of intermetallic compounds distributed in the Zn matrix, namely YZn 12 Particles.

[0077] Table 1 Elements and mass ratios of degradable zinc alloys in Zn-Li-Mn-Y system

[0078]

[0079] Test Example 1: Mechanical Properties Test of Zn-Li-Mn-Y Series Zinc Alloy

[0080] According to the ASTM-E8m-09 standard, the Zn-Li-Mn-Y series zinc alloy rod prepared in the embodiment is cut with an electric spark wire cutting machine. Then the samples are polished with 800#, 1000#, and 2000# sandpaper respectively to remove the oxide layer on the surface of the sample and polish it as smooth as possible. Then the outer surface of the sample is polished with a polishing cloth and polishing paste. Ultrasonicate in anhydrous ethanol for 5 minutes, the ultrasonic frequency is 100Hz, and then blow dry with cold air. A tensile test is performed at room temperature using a universal material mechanics testing machine, and the tensile rate is 4% / min. The results of the tensile test are shown in Table 2. As can be seen from Table 2, the tensile strength of the Zn-Li-Mn-Y series zinc alloy of the present invention is significantly improved, among which the tensile strength of Zn-0.8Li-0.1Mn-0.5Y reaches 779MPa, breaking through the reported strength of existing zinc alloys.

[0081] Table 2 Mechanical properties of Zn-Li-Mn-Y zinc alloy

[0082]

[0083] Figure 7 This is the tensile test curve of Zn-0.8Li-0.1Mn-0.5Y zinc alloy. The size of the alloy sample is processed according to the ASTM-E8m-09 standard and the tensile test is carried out using a universal material mechanical testing machine. Figure 7 It can be seen that the material undergoes elastic deformation at the initial stage of deformation, and when the stress reaches 694MPa, the material yields, and the shape is difficult to recover after unloading. The ultimate tensile strength of the material is 779MPa. After that, as the strain increases, the stress decreases, indicating that the material is unstable until it is broken, and the elongation at break is 7.3%. The mechanical tensile properties of the material can be obtained through the stress-strain curve of the material.

[0084] In order to further verify the strengthening effect of the Y element, other rare earth elements (Eu, Gd, Nd, Sm, Sc, La, Ce, Pr, Tb, Dy, Ho, Er, Tm, Yb and Lu, all added in an amount of 0.5wt%) were added to Zn-0.8Li-0.1Mn, and tensile samples were prepared according to the steps of the present invention. The tensile test was carried out at room temperature with a tensile rate of 4% / min. The tensile test results are shown in Table 3.

[0085] Table 3 Mechanical properties of Zn-0.8Li-0.1Mn-RE zinc alloy

[0086]

[0087]

[0088] Combining the published literature and Table 3, it can be seen that the present invention is a zinc alloy with the highest tensile strength reported so far. Its excellent strength can provide sufficient supporting force, laying a foundation for the subsequent development of orthopedic clinical medical devices.

[0089] Test Example 2: Electrochemical Performance Test of Zn-0.8Li-0.1Mn-0.5Y Zinc Alloy

[0090] The Zn-0.8Li-0.1Mn-0.5Y zinc alloy rod prepared in Example 2 was prepared into a metal sheet with a size of Φ10x1mm by wire cutting, and then the samples were polished with 800#, 1000#, and 2000# sandpapers respectively to remove the oxide layer on the surface of the sample and polish it as smooth as possible. The outer surface of the sample was then polished with a polishing cloth and polishing paste. Ultrasonication was performed in acetone and anhydrous ethanol for 10 minutes, respectively, at an ultrasonic frequency of 100Hz, and electrochemical testing was performed after drying with cold wind. The above-treated samples were electrochemically analyzed in simulated body fluid (SBF) using an Autolab electrochemical workstation.

[0091] Figure 8 This is the Tafel curve obtained after electrochemical testing of Zn-0.8Li-0.1Mn-0.5Y zinc alloy. From the Tafel curve, it can be calculated that the degradation rate of Zn-0.8Li-0.1Mn-0.5Y is 0.55mm / year, which is moderate and is an ideal medical degradable material.

[0092] Test Example 3: In vitro corrosion performance test of Zn-0.8Li-0.1Mn-0.5Y zinc alloy

[0093] The Zn-0.8Li-0.1Mn-0.5Y zinc alloy rod prepared in Example 2 was processed into a metal sheet with a size of φ10x1mm by wire cutting. The samples were carefully polished with 800#, 1000# and 2000# sandpaper in turn to remove the oxide layer and make the surface as smooth as possible. Then, the outer surface of the sample was finely polished with a polishing cloth and polishing paste. Finally, the samples were ultrasonically cleaned in acetone and anhydrous ethanol for 10 minutes (frequency of 100Hz), respectively, and then dried with cold air. The treated samples were immersed in simulated body fluid (SBF) for 28 days, during which the pH changes of the solution were measured. The morphology of the corrosion products of the immersed samples was photographed with SEM.

[0094] Fig. 9This is the corrosion morphology of Zn-0.8Li-0.1Mn-0.5Y zinc alloy after being immersed in simulated body fluid (SBF) for 28 days. It can be seen that the corrosion product is a loose white flocculent structure attached to the surface of the metal sheet. Grinding and polishing scratches can be vaguely seen on the metal surface, indicating that the corrosion is carried out on the surface of the metal and has not penetrated deep into the interior. At the same time, no obvious corrosion pits or pitting marks are seen, indicating that the corrosion is relatively uniform overall.

[0095] Test Example 4: Cytocompatibility test of Zn-0.8Li-0.1Mn-0.5Y zinc alloy

[0096] The Zn-0.8Li-0.1Mn-0.5Y zinc alloy rod prepared in Example 2 was processed into a metal sheet with a size of φ10x1mm by wire cutting. The samples were carefully polished with 800#, 1000# and 2000# sandpaper in turn to remove the oxide layer and make the surface as smooth as possible. Then, the outer surface of the sample was finely polished with a polishing cloth and polishing paste. Finally, the samples were ultrasonically cleaned in acetone and anhydrous ethanol for 10 minutes (frequency of 100Hz), respectively, and then blown dry with cold air. The sample was placed under ultraviolet light for sterilization for 2h, then turned over and sterilized again for 2h. After sterilization, the sample was placed in a 50ml centrifuge tube and the prepared culture medium (10% fetal bovine serum and 1% double antibody added to high-glucose DMEN) was added. The amount of culture medium added followed the ISO10993-5 standard, according to the volume of the extract: surface area = 1.25ml / cm 2 Then put it into an incubator at 37 degrees Celsius and 5% carbon dioxide concentration for 24 hours.

[0097] Cell proliferation activity detection: MC3T3 osteoblasts, HUVEC endothelial cells and HASMC smooth muscle cells were taken out of the liquid nitrogen tank, and they were shaken back and forth in a 37-degree Celsius water bath. After some of the cells were dissolved, they were held with tweezers and continued to shake until the cells dissolved to a point where only a little ice nucleus remained. Then, they were sprayed with alcohol immediately, taken to the clean bench, the sealing film was removed, and the cells were sucked into a 15ml centrifuge tube. The culture medium was added at a ratio of freezing solution: culture medium = 1:5, and then the culture medium was blown evenly, and then placed in a centrifuge for centrifugation. The centrifugation speed was 1000rpm, and the time was 5min. After the centrifugation was completed, the cells were deposited at the bottom of the centrifuge tube, the upper waste liquid was poured out, the culture medium was added, and after blowing evenly, the cells were planted into a 96-well plate at a density of 50,000 / ml, 100ul was added to each well, and cultured in an incubator for 24h. Then the original culture medium was aspirated, and different concentrations of extracts (50%, 25% and 12.5% ​​respectively) were added to the experimental group, new culture medium was added to the negative group, and culture medium containing 10% DMSO (dimethyl sulfoxide) was added to the positive group. Then it was placed in an incubator at 37 degrees Celsius and 5% carbon dioxide concentration for 24 hours. Then the 96-well plate was taken out, and 10ul of cck-8 (Cell Counting Kit-8) reagent was added to each well for cell proliferation and toxicity tests.

[0098] Fig.10 It is the relative survival rate of MC3T3 cells and HUVEC cells in different concentrations of leaching solutions (concentrations are 50%, 25% and 12.5% ​​respectively). It can be seen that for two different cells, the relative survival rate in the material leaching solution is more than 75%. According to the GB / T16886.5 standard, the material is non-toxic. This shows that the Zn-0.8Li-0.1Mn-0.5Y zinc alloy provided by the present invention has good biocompatibility.

[0099] Cell adhesion morphology detection: The revived MC3T3 osteoblasts and HUVEC endothelial cells were subcultured in culture dishes, and the second-generation cells were used for cell adhesion morphology detection. First, 2 ml of trypsin was added to the culture dish, and the culture dish was placed in an incubator at 37 ° C and 5% carbon dioxide concentration for digestion for 60 s. Take out the culture dish, add 4 ml of complete culture medium, stop digestion, and blow with a pipette to make the cells that grow on the wall completely fall off and become a cell suspension. Then centrifuge the suspension at a speed of 1000 rpm for 5 min. After centrifugation, the cells are deposited at the bottom of the centrifuge tube, the upper waste liquid is poured out, the culture medium is added, and after blowing evenly, the cells are planted in a 24-well plate at a density of 20,000 / ml, 100ul is added to each well, and different concentration gradients of material extracts (concentrations are 50%, 25% and 12.5%) are added respectively, and then placed in an incubator for 24 hours. After 24 hours, the plate was removed, the culture medium was aspirated, and the cells were stained using a live / dead cell staining kit (Calcein AM, EthD-I method). At the same time, DAPI and FITC fluorescent dyes were used to stain the cell nucleus and cytoskeleton, respectively.

[0100] Fig.11 The figure shows the spreading of MC3T3 cells and HUVEC cells in extracts of different concentrations (50%, 25% and 12.5% ​​respectively). The nucleus is colored blue and the cytoskeleton is colored green. It can be seen that the cells have good spreading morphology in extracts of different concentrations, indicating that the material has good biocompatibility and is an ideal biomedical material.

[0101] Test Example 5: Blood compatibility test of Zn-0.8Li-0.1Mn-0.5Y zinc alloy

[0102] The Zn-0.8Li-0.1Mn-0.5Y zinc alloy rod prepared in Example 2 was processed into a metal sheet with a size of φ10x1mm by wire cutting. The samples were carefully polished with 800#, 1000# and 2000# sandpaper in turn to remove the oxide layer and make the surface as smooth as possible. Next, the outer surface of the sample was finely polished with a polishing cloth and polishing paste. Finally, the samples were ultrasonically cleaned in acetone and anhydrous ethanol for 10 minutes (frequency was 100Hz), respectively, and then blown dry with cold air. The sample was placed under ultraviolet light for irradiation and sterilization for 2h, then turned over and sterilized again for 2h. 8ml of venous whole blood was collected from a healthy adult (female, 26 years old), placed in an anticoagulant tube, and then 10ml of normal saline was added for dilution, and then placed in a 37°C environment for preheating. The sample metal sheet was placed in a 50ml centrifuge tube, 12ml of normal saline was added to the centrifuge tube, and soaked in a 37°C environment for half an hour. After half an hour, add 200ul of diluted blood and continue soaking for one hour. After one hour, take out the sample slices and put the soaking liquid into a centrifuge for centrifugation at a speed of 1200rpm for 5 minutes. The supernatant after centrifugation is aspirated into a 96-well plate with a pipette, and the absorbance of the supernatant is tested using a Multiskan FC microplate reader, with a wavelength of 545nm.

[0103] Fig.12 The hemolysis rate test results are shown. According to the national standard, the hemolysis rate of biomedical materials should be less than 5%. The hemolysis rate of the material provided by the present invention is only 4%, which meets the national standard requirements.

[0104] It can be understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solution described in the implementation of the present invention. Ordinary technicians in the field should understand that the present invention can still be partially modified or replaced by equivalents to achieve the same technical effect; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A Zn-Li-Mn-Y series degradable zinc alloy, characterized in that: In terms of mass percentage, the mass percentage of Li is 0.8±0.1%, the mass percentage of Mn is 0.1±0.05%, the mass percentage of Y is 0 to 3%, but excluding 0; and the balance is zinc.

2. The Zn-Li-Mn-Y based degradable zinc alloy according to claim 1, characterized in that: The mass percentage of Y ranges from 0 to 2%, but does not include zero.

3. The Zn-Li-Mn-Y based degradable zinc alloy according to claim 1, characterized in that: The zinc alloy is any one of the following, wherein the numbers represent mass percentages: (1) Zn-0.8Li-0.1Mn-0.3Y (2) Zn-0.8Li-0.1Mn-0.5Y (3) Zn-0.8Li-0.1Mn-1.0Y (4) Zn-0.8Li-0.1Mn-2.0Y.

4. A method for preparing a Zn-Li-Mn-Y based degradable zinc alloy according to any one of claims 1 to 3, characterized in that The steps include: (1) high-purity Zn and Y are mixed and smelted under the protection of CO2 and SF6 atmosphere, and then cast and cooled to obtain a master alloy Zn-10.0wt.%Y; (2) Mixing and smelting high-purity Zn and Li under the protection of CO2 and SF6 atmosphere, and then casting and cooling to obtain an intermediate alloy Zn-5.0wt.%Li; (3) Mixing and smelting high-purity Zn and Mn under the protection of CO2 and SF6 atmosphere, and then casting and cooling to obtain the intermediate alloy Zn-5.0wt.%Mn; (4) The intermediate alloys Zn-10.0wt.%Y, Zn-5.0wt.%Li and Zn-5.0wt.%Mn and pure zinc are mixed and smelted in proportion under a protective atmosphere, and then cast and cooled to obtain the Zn-Li-Mn-Y series degradable zinc alloy.

5. The method for preparing the Zn-Li-Mn-Y series degradable zinc alloy according to claim 4, characterized in that: In step (1), the smelting temperature is 650-900°C; in step (2), the smelting temperature is 550-700°C; in step (3), the smelting temperature is 420-800°C; in step (4), the smelting temperature is 620-850°C.

6. The method for preparing the Zn-Li-Mn-Y series degradable zinc alloy according to claim 4, characterized in that: In step (4), the Zn-Li-Mn-Y series zinc alloy obtained after casting and cooling is mechanically processed, and the mechanical processing steps include three steps of hot rolling, forging and hot extrusion.

7. The method for preparing the Zn-Li-Mn-Y series degradable zinc alloy according to claim 6, characterized in that: Before the mechanical processing, the zinc alloy is heat treated for homogenization: the heat treatment temperature is 250-350° C., the time is 12-25 hours, and oil quenching or water quenching is performed after the heat treatment.

8. The method for preparing the Zn-Li-Mn-Y based degradable zinc alloy according to claim 6, characterized in that: The mechanical processing comprises the following steps: (1) Wire cutting: Cut the Zn-Li-Mn-Y zinc alloy ingot into cylinders, heat and keep them warm for 6-8 hours at a temperature of 300-400°C; (2) Forging: Forging the Zn-Li-Mn-Y zinc alloy cylinder with a forging machine to forge the cylinder into a disc with a thickness of 0.5-1 cm, and then heating it to 300-400° C. and keeping it warm for 30-60 min; (3) Rolling: The rolling passes are 4-8, and the pressing amount each time is 0.5-1 mm; the material is rolled into a 1-6 mm rectangular thin plate, and the material is returned to the furnace and heated to 500-600 ° C and kept warm for 30-60 minutes; (4) Lamination forging: Lamination of multiple thin plates, with adjacent sheets rolling in opposite directions, adding a layer of Zn-Li-Mn-Y zinc alloy raw metal powder between the two layers, with the number of laminated layers being 5-8 layers. After lamination, the plates are kept at 500-600°C for 30-60 minutes, then taken out for forging, and the layers of materials are forged into one body to eliminate internal residual stress, component segregation, pore inclusions and other defects, and forged into an approximate cylinder with a diameter between 15-30 mm; (5) Hot extrusion: The cylinder is hot extruded at a temperature of 200-300°C to extrude a Zn-Li-Mn-Y biodegradable zinc alloy rod having a diameter of 10-15 mm.

9. An application of the Zn-Li-Mn-Y degradable zinc alloy according to any one of claims 1 to 3, characterized in that: The invention is a degradable orthopedic implant, which includes at least one of bone plates, bone nails, bone needles, bone rods, spinal internal fixation equipment, ligature wires, patellar collectors, bone wax, bone repair materials, bone tissue repair scaffolds, intramedullary nails and bone sleeves, and guided bone regeneration barrier membranes.

10. An application of the Zn-Li-Mn-Y degradable zinc alloy according to any one of claims 1 to 3, characterized in that: The biodegradable stent includes at least one of a cardiac stent, a ureteral stent, a prostate stent, an esophageal stent, a duodenal stent, a colon stent, a bile duct stent, a pancreatic stent, a tracheal stent, a bronchial stent, an airway stent, a nasolacrimal duct stent, and a peripheral vascular stent.