High-strength corrosion-resistant Al-Zn-Mg-Cu-Zr-Be alloy and application thereof
By adding Be and Zr elements to Al-Zn-Mg-Cu alloys, the microstructure structure and process processing are optimized, and the problem of insufficient corrosion resistance of traditional alloys in complex environments is solved, and high strength and corrosion resistance are achieved The improvement meets the high performance requirements of the aircraft.
Patent Information
- Application Number
- CN202411245002.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-06
AI Technical Summary
Traditional Al-Zn-Mg-Cu alloys have insufficient corrosion resistance in complex environments and cannot meet the high-strength corrosion resistance requirements for aircraft high-speed flight. The existing research methods still have insufficient performance problems in practical applications.
By adding an appropriate amount of Be and Zr elements to the Al-Zn-Mg-Cu alloy, the microstructure structure is controlled to form a second phase with a diffuse distribution, inhibiting the coarsification of the η phase, and combining with a single-stage homogenization treatment. , hot rolling and T74 dual-stage aging heat treatment, optimize the mechanical properties and corrosion resistance of aluminum alloys.
It significantly improves the strength and corrosion resistance of aluminum alloys, can maintain high strength and tensile properties in 3.5% NaCl corrosion environment, extend service life, and maintain high strength and corrosion resistance in long-term corrosion environments.
Smart Images

Figure CN119082564A_ABST
Abstract
Description
Technical Field
[0001] The invention provides a high-strength and corrosion-resistant aluminum alloy material, in particular to a high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy and application thereof, belonging to the field of aluminum alloys. Background Art
[0002] As a typical representative of age-hardenable aluminum alloys, 7xxx series (Al-Zn-Mg-Cu) alloys have excellent comprehensive mechanical properties and are generally considered to be the best series of high-strength and corrosion-resistant aluminum-based alloys. Aircraft often pass over the ocean during their flight paths, and the humid and electrolyte-rich environment will aggravate the corrosion of the fuselage materials. Under such environmental conditions, the mechanical properties of traditional aluminum alloys drop sharply due to the rapid degradation of the microstructure, and they cannot meet the high-strength and corrosion-resistant requirements of aircraft in complex environments at high speeds. Al-Zn-Mg-Cu alloys are widely used in the industrial field due to their very high strength and excellent corrosion resistance, especially in the aerospace field, and are important structural materials for aircraft.
[0003] The comprehensive corrosion resistance of Al-Zn-Mg-Cu alloys currently used in China still has a certain gap compared with the foreign level, and further optimization of composition and process is needed, mainly by controlling the evolution of microstructure, improving performance, and meeting the needs of aerospace. The main method of studying Al-Zn-Mg-Cu alloys is to improve the comprehensive performance of the material by adjusting the main element ratio and microalloying addition. Its microscopic mechanism is to inhibit the coarsening of the main strengthening phase η phase and increase the precipitation of the strengthening phase. Although the above composition and process optimization methods have improved the strength and corrosion resistance of aluminum alloys to a certain extent, the use environment of the material is changeable. In actual application scenarios, the problem of insufficient corrosion resistance often occurs, and stress corrosion cracking or severe corrosion occurs, which cannot cope with the complex working conditions faced by aviation aircraft. Therefore, the market urgently needs an aluminum alloy material with higher strength and better corrosion resistance. Summary of the invention
[0004] In view of the shortcomings of the prior art, the first object of the present invention is to provide a high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy. Based on the synergistic effect between the various elemental components, the alloy refines the microstructure grains by adding appropriate amounts of Be and Zr elements and performing microalloying, forms a dispersed second phase in the aluminum alloy, increases the precipitation of the η phase, improves the dispersed distribution of the η phase, and inhibits the coarsening of the η phase, so that the prepared aluminum alloy has higher strength, and the service life in a corrosive environment is improved by regulating the proportion of the grain structure; in the preparation process of the alloy, the mechanical properties of the aluminum alloy are controlled by controlling the key process parameters of each step, and substructure strengthening is achieved while avoiding excessive deformation energy storage through single-stage homogenization treatment, hot rolling and other treatment methods, combined with solid solution and two-stage T74 aging heat treatment, so as to achieve the purpose of maintaining high strength and high corrosion resistance of the aluminum alloy in a long-term corrosive environment.
[0005] The high-strength corrosion-resistant aluminum alloy provided by the present invention has excellent mechanical properties and corrosion resistance. After testing, the alloy material has not failed after being tested in a 3.5% NaCl corrosion environment C-ring stress corrosion 260MPa test for 30 days, and its yield strength is not less than 540MPa, and its tensile strength is not less than 580MPa; after a 48-hour standard aluminum alloy exfoliation corrosion test, the corrosion level is not less than EA, the maximum depth of the aluminum alloy intergranular corrosion test is not higher than 100um, and the intergranular corrosion level does not exceed level 3.
[0006] To achieve the above technical objectives, the present invention provides a high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy, comprising the following components by mass percentage: Cu 2.0-2.5%, Mg 2.0-2.8%, Zn 6.0-6.8%, Zr0.05-0.1%, Be0.05-0.1%, Fe≤0.05%, Si≤0.03%, and the balance is aluminum and non-removable impurities;
[0007] The high-strength corrosion-resistant Al-Zn-Mg-Cu alloy is prepared by the following process:
[0008] A. Melting: Use aluminum, magnesium, zinc, aluminum-copper master alloy, aluminum-zirconium master alloy, and aluminum-beryllium master alloy as raw materials; weigh the raw materials according to the composition ratio, load them into the smelting furnace, and heat and melt them;
[0009] B. Refining, impurity removal and degassing: After the metal melt is completely alloyed, add the impurity remover to the alloy melt to gather slag, and introduce argon gas at the same time for 10 to 20 minutes, add an appropriate amount of hexachlorohexane, let it stand, and remove the slag. Repeat the above operation 2 to 3 times, and then let the aluminum alloy melt stand for more than 20 minutes;
[0010] C. Pouring: After the aluminum alloy melt is refined, impurity-removed and degassed, the melt temperature is maintained at 730±5°C, poured into a mold, and cooled and solidified to obtain an ingot;
[0011] D. Single-stage homogenization heat treatment: heat the ingot obtained in step C to 465±5°C, keep it at this temperature for 12 to 36 hours, then take it out of the furnace and air cool it to room temperature;
[0012] E. Hot rolling: heating the homogenized ingot obtained in step D to 420±5°C and keeping the temperature for 60-120 minutes, and then performing multiple hot rolling to the set thickness of the alloy. During rolling, the pass reduction rate is controlled to be 5-20% and the total reduction rate is controlled to be 75-85%;
[0013] Annealing at 420±5℃ between rolling passes; after rolling, air cooling and / or water cooling to room temperature; isothermal deformation of the workpiece;
[0014] G. Heat treatment: firstly carry out solution treatment, heat the isothermally deformed parts to 465±5℃, keep them warm for 90-150min, and then quench them with water; then carry out T74 double-stage aging treatment; T74 double-stage aging treatment is as follows: heat the solution treated parts to 120-130℃ and keep them warm for 6-7h, then heat them to 175-185℃ and keep them warm for 7-8h, and then quench them with water to room temperature.
[0015] The homogenization treatment is a single-stage homogenization heat treatment, with a heating rate of 10 to 15° C. / min, a homogenization temperature of 465±5° C., and a heat preservation time of 20 to 28 hours.
[0016] The alloy material provided by the present invention is based on the synergistic effect between the various element components. Through the microalloying of appropriate amounts of Be and Zr, the microstructure grains are refined, a dispersed second phase is formed in the aluminum alloy, the concentrated distribution area of the substructure is controlled, and a mixed distribution structure of the subgrain structure and the recrystallized structure is formed. While the precipitation and dispersed distribution of the η phase are increased, the coarsening of the η phase is suppressed, so that the prepared aluminum alloy has higher strength and corrosion resistance under service conditions, and the service life and upper limit of use are improved.
[0017] The preparation process of the alloy provided by the present invention controls the mechanical properties of the aluminum alloy by controlling the key process parameters of each step, and achieves substructure strengthening while limiting deformation energy storage through single-stage homogenization treatment, hot rolling and other treatment methods, combined with solid solution and single-stage aging heat treatment, thereby achieving the purpose of improving the aluminum alloy to maintain high strength under the action of a long-term corrosive environment.
[0018] As a preferred solution, the present invention provides a high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy, comprising the following components in mass percentage: Cu 2.1-2.15%, Mg 2.4-2.5%, Zn 6.2-6.4%, Zr0.08-0.1%, Be0.08-0.1%, Fe≤0.05%, Si≤0.01%, and the balance is aluminum and non-removable impurities.
[0019] The proportions of the elements in the alloy material provided by the present invention should be strictly implemented in accordance with the above requirements. If the contents of Zn and Mg exceed the specified range, resulting in a corresponding change in the Zn / Mg ratio, the precipitation ratios and sizes of various strengthening phases (mainly η phases) in the structure of the alloy material will change accordingly, thereby reducing the alloy performance; if the proportions of alloying elements such as Be and Zr exceed the required proportions, the second phase in the alloy will become coarse, and a refractory coarse second phase will appear during smelting and casting, resulting in poor plasticity and reduced strength of the alloy.
[0020] As a preferred solution, the aluminum alloy raw materials include: high-purity aluminum, industrial pure magnesium, industrial pure zinc, aluminum-copper master alloy, aluminum-beryllium master alloy, and aluminum-zirconium master alloy.
[0021] As a preferred solution, the purity of the high-purity aluminum is ≥99.99%, the purity of the industrial-purity magnesium is ≥99.95%, and the purity of the industrial-purity zinc is ≥99.95%.
[0022] The preparation process of the present invention strictly controls the purity of materials, reduces the content of Fe and Si elements, avoids the formation of coarse brittle phases, and affects the plasticity of the alloy; at the same time, the use of Be and Zr microalloying elements not only refines the grains and controls the substructure distribution, but also effectively inhibits the coarsening rate of the η phase at high temperature, thereby improving the tensile and corrosion resistance of the alloy.
[0023] As a preferred solution, the copper content in the aluminum-copper master alloy is ≥50.0%, the zirconium content in the aluminum-zirconium master alloy is ≥5.0%, and the beryllium content in the aluminum-beryllium master alloy is ≥10.0%. The content of each transition metal in the master alloy must be strictly in accordance with the above requirements. By controlling the content of the transition metal in the master alloy, the component valence of the second phase in the smelting and casting process can be controlled. If the proportion of the transition metal in the master alloy changes, the alloy will contain a second phase of aluminum-transition metals with different valences.
[0024] As a preferred solution, the smelting temperature is 750-780°C.
[0025] The process conditions of the single-stage homogenization heat treatment adopted by the present invention are determined according to the comprehensive performance improvement of the Al-Zn-Mg-Cu alloy. Keeping at 465±5°C for 12-36 hours is more conducive to the precipitation of dispersed phase particles and also promotes the precipitation of η phase in the subsequent aging treatment process, thereby achieving the purpose of improving the mechanical properties of the alloy through the synergistic effect of grain boundary strengthening and precipitation phase; according to the single-stage homogenization heat treatment method provided by the present invention, it can promote the full and uniform diffusion of each element component in the alloy and eliminate most of the dendrites.
[0026] As a preferred solution, the hot rolling is multi-stage hot rolling, and the process is: heating the ingot after homogenization treatment to 420±5°C and keeping it warm for 70 to 120 minutes; performing 8 to 12 rolling passes, with the alloy thickness changing by 2 to 4 mm in each rolling pass, and air cooling to room temperature after rolling.
[0027] The present invention uses multiple hot rolling passes to deform the alloy ingot, so that the ingot structure is homogenized, the small-angle grain boundary content is increased, and the high-strength, toughness and corrosion-resistant structure characteristics of the recrystallized structure and the substructure are mixed and distributed. At the same time, the coarse second phase is fully crushed and homogenized by rolling, the comprehensive properties of the alloy are improved, and a deformation structure with uniform deformation, small second phase size and uniform distribution is obtained, thereby improving the mechanical properties of the material.
[0028] As a preferred solution, the heat treatment includes solution treatment and unipolar aging treatment.
[0029] As an exploratory scheme, the present invention provides a high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy, the alloy composition is as follows: copper content is 2.07%, Mg content is 2.48%, Zr content is 0.09%, Zn content is 6.26%, Fe ≤ 0.05%, Si ≤ 0.01%, and the balance is aluminum and non-removable impurities, and the preparation method thereof is as follows:
[0030] A. Melting: Weigh the raw materials according to the composition ratio, put them into the resistance furnace, and heat and melt them;
[0031] B. Refining, impurity removal and degassing: After the metal melt is completely alloyed, add the impurity remover to the alloy melt to gather slag, and introduce argon gas at the same time for 10 to 20 minutes, add an appropriate amount of hexachlorohexane, let it stand, and remove the slag. Repeat the above operation 2 to 3 times, and then let the aluminum alloy melt stand for more than 20 minutes;
[0032] C. Pouring: After the aluminum alloy melt is refined, impurity-removed and degassed, the melt temperature is maintained at 730±5℃, poured into a mold, and cooled and solidified to obtain an ingot;
[0033] D. Single-stage homogenization heat treatment: heat the ingot obtained in step C to 465±5°C, keep it at this temperature for 24 hours, then take it out of the furnace and air cool it to room temperature;
[0034] E. Hot rolling: The homogenized ingot obtained in step D is heated to 420±5°C in a resistance furnace and kept warm for 90 min, and then hot rolled for multiple passes until the final thickness of the alloy is 4 mm, wherein the thickness of the alloy changes in each pass during the rolling process as follows: 20 mm→18.5 mm→17 mm→15.5 mm→14 mm→12.5 mm→11 mm→9.5 mm→8 mm→6.5 mm→5 mm→4 mm; annealing at 420°C between rolling passes; water cooling to room temperature after rolling; and an isothermal deformed workpiece is obtained.
[0035] F. Heat treatment: Firstly, carry out solution treatment, heat the isothermal deformed parts to 465±5℃, keep them warm for 2h, and then quench them with water; then carry out T74 double-stage aging treatment, heat the solution treated parts to 120℃ and keep them warm for 6h, then keep them warm at 175℃ for 7h, and then quench them with water to obtain the parts. With the above scheme, the mechanical properties of the products are extremely superior, but the corrosion resistance is average.
[0036] In order to improve the corrosion resistance of the product and ensure excellent mechanical properties, the following solutions can be adopted:
[0037] A high-strength, corrosion-resistant Al-Zn-Mg-Cu alloy, the alloy composition by weight percentage: copper content is 2.13%, Mg content is 2.46%, Zr content is 0.10%, Be content is 0.09%, Zn content is 6.39%, Fe: ≤0.05%, Si: ≤0.01%, and the balance is aluminum and non-removable impurities.
[0038] The specific preparation method and steps are as follows:
[0039] A. Smelting: High-purity aluminum, high-purity magnesium, high-purity zinc, aluminum-copper master alloy, aluminum-zirconium master alloy, and aluminum-beryllium master alloy are used as raw materials; among them, the purity of high-purity aluminum is ≥99.99%, the purity of industrial-purity magnesium is ≥99.95%, the purity of industrial-purity zinc is ≥99.95%, the copper content in the aluminum-copper master alloy is ≥50.0%, and the beryllium content in the aluminum-beryllium master alloy is ≥50.0%.
[0040] ≥10.0%, the zirconium content in the aluminum-zirconium master alloy is ≥4.0%; weigh the raw materials according to the composition ratio, put them into the resistance furnace, and heat and melt them;
[0041] B. Refining, impurity removal and degassing: After the metal melt is completely alloyed, add the impurity remover to the alloy melt to gather slag, and introduce argon gas at the same time for 10 to 20 minutes, add an appropriate amount of hexachlorohexane, let it stand, and remove the slag. Repeat the above operation 2 to 3 times, and then let the aluminum alloy melt stand for more than 20 minutes;
[0042] C. Pouring: After the aluminum alloy melt is refined, impurity-removed and degassed, the melt temperature is maintained at 730±5℃, poured into a mold, and cooled and solidified to obtain an ingot;
[0043] D. Single-stage homogenization heat treatment: heat the ingot obtained in step C to 465±5°C, keep it at this temperature for 24 hours, then take it out of the furnace and air cool it to room temperature;
[0044] E. Hot rolling: the homogenized ingot obtained in step D is heated to 420±5°C in a resistance furnace and kept warm for 90 min, and then hot rolled for multiple passes until the final thickness of the alloy is 4 mm, wherein the thickness of the alloy changes in each pass during the rolling process as follows: 20 mm→18.5 mm→17 mm→15.5 mm→14 mm→12.5 mm→11 mm→9.5 mm→8 mm→6.5 mm→5 mm→4 mm; annealing at 420°C between rolling passes; water cooling to room temperature after rolling; and isothermal deformation processing.
[0045] F. Heat treatment: Firstly, carry out solution treatment, heat the isothermally deformed parts to 465±5℃, keep them warm for 2h, and then quench them in water; then carry out T74 double-stage aging treatment, heat the solution treated parts to 120℃ and keep them warm for 6h, then keep them warm at 175℃ for 7h, then quench them in water to obtain the parts.
[0046] The present invention also provides an application of high-strength and corrosion-resistant Al-Zn-Mg-Cu for preparing aircraft skins. The high-strength and corrosion-resistant aluminum alloy provided by the present invention has excellent mechanical properties and corrosion resistance. After testing, the yield strength of the T74 state product of the alloy material at room temperature is not less than 540MPa, and the tensile strength is not less than 580MPa; it can meet the mechanical property requirements of aircraft skins for materials.
[0047] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0048] 1) The Al-Zn-Mg-Cu alloy provided by the present invention is based on the synergistic effect between the various element components, through the appropriate amount of Be and Zr microalloying, and under the cooperation of the preparation process, the organization grains are refined, the recrystallization structure is controlled, and a dispersed second phase is formed in the aluminum alloy, and the substructure and the recrystallization structure are mixed and distributed. The precipitation of the η phase is increased, which is conducive to the dispersed distribution of the η phase, and the coarsening of the η phase is suppressed, so that the prepared aluminum alloy maintains good corrosion resistance while maintaining a high mechanical strength.
[0049] 2) In the technical solution provided by the present invention, the mechanical properties of the aluminum alloy are controlled by controlling the key process parameters of each step in the preparation process. Through special single-stage homogenization treatment, hot rolling and other treatment methods, while controlling deformation energy storage, fine grain and substructure strengthening are achieved. Combined with solid solution and two-stage aging heat treatment, the aluminum alloy can maintain high mechanical strength while having good corrosion resistance.
[0050] 3) The high-strength corrosion-resistant aluminum alloy provided by the present invention has excellent mechanical properties and corrosion resistance. After optimization, the alloy material has not failed after being tested for 30 days in a 3.5% NaCl corrosion environment at a C-ring stress corrosion rate of 260 MPa, and its yield strength is not less than 540 MPa, and its tensile strength is not less than 580 MPa; after a 48-hour test on standard aluminum alloy exfoliation corrosion, the corrosion level is not less than EA, the maximum depth of the aluminum alloy intergranular corrosion test is not higher than 100 um, and the intergranular corrosion level does not exceed level 3. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] In order to make the technical solution and beneficial effects of the present invention clearer, the following drawings are provided for further explanation:
[0052] Figure 1 This is the exfoliation corrosion morphology of the T74 state product obtained in Example 1 after 48 hours of corrosion;
[0053] Figure 2 This is the exfoliation corrosion morphology of the T74 state product obtained in Example 2 after 48 hours of corrosion;
[0054] Figure 3 This is the exfoliation corrosion morphology of the T74 state product obtained in Comparative Example 1 after 48 hours of corrosion;
[0055] Figure 4 The grain boundary morphology distribution diagram of the T74 aged product obtained in Examples 1, 2 and Comparative Example 1; Figure 4 a is the grain boundary morphology distribution diagram of the T74 aged product obtained in Example 1, Figure 4 b is the grain boundary morphology distribution diagram of the T74 aged product obtained in Example 2, Figure 4 c is the grain boundary morphology distribution diagram of the T74 aged product obtained in comparative example 1.
[0056] from Figure 1 It can be seen that the metal surface is corroded and blackened, but there is no serious delamination and peeling, and the surface is relatively smooth, which is judged to be EA+ corrosion level;
[0057] from Figure 2 It can be seen that the metal surface is corroded, with slight peeling and flaking, but the surface still has metallic luster, which is determined to be EA grade flaking corrosion;
[0058] from Figure 3 It can be seen that the metal surface is severely corroded, with severe peeling and peeling phenomena, and is determined to be EC-level exfoliation corrosion.
[0059] Figure 4 It can be seen that the addition of an appropriate amount of Be effectively promotes grain refinement and the concentrated distribution of small-angle grain boundaries, has a fine-grain strengthening effect on the alloy, and also improves toughness to a certain extent. DETAILED DESCRIPTION
[0060] The following examples are intended to illustrate the present invention rather than to further limit the present invention.
[0061] Example 1
[0062] A high-strength, corrosion-resistant Al-Zn-Mg-Cu alloy, the alloy composition by weight percentage: copper content is 2.13%, Mg content is 2.46%, Zr content is 0.10%, Be content is 0.09%, Zn content is 6.39%, Fe: ≤0.05%, Si: ≤0.01%, and the balance is aluminum and non-removable impurities.
[0063] The specific preparation method and steps are as follows:
[0064] A. Smelting: High-purity aluminum, high-purity magnesium, high-purity zinc, aluminum-copper master alloy, aluminum-zirconium master alloy, and aluminum-beryllium master alloy are used as raw materials; among them, the purity of high-purity aluminum is ≥99.99%, the purity of industrial-purity magnesium is ≥99.95%, the purity of industrial-purity zinc is ≥99.95%, the copper content in the aluminum-copper master alloy is ≥50.0%, and the beryllium content in the aluminum-beryllium master alloy is ≥50.0%.
[0065] ≥10.0%, the zirconium content in the aluminum-zirconium master alloy is ≥4.0%; weigh the raw materials according to the composition ratio, put them into the resistance furnace, and heat and melt them;
[0066] B. Refining, impurity removal and degassing: After the metal melt is completely alloyed, add the impurity remover to the alloy melt to gather slag, and introduce argon gas at the same time for 10 to 20 minutes, add an appropriate amount of hexachlorohexane, let it stand, and remove the slag. Repeat the above operation 2 to 3 times, and then let the aluminum alloy melt stand for more than 20 minutes;
[0067] C. Pouring: After the aluminum alloy melt is refined, impurity-removed and degassed, the melt temperature is maintained at 730±5℃, poured into a mold, and cooled and solidified to obtain an ingot;
[0068] D. Single-stage homogenization heat treatment: heat the ingot obtained in step C to 465±5°C, keep it at this temperature for 24 hours, then take it out of the furnace and air cool it to room temperature;
[0069] E. Hot rolling: the homogenized ingot obtained in step D is heated to 420±5°C in a resistance furnace and kept warm for 90 min, and then hot rolled for multiple passes until the final thickness of the alloy is 4 mm, wherein the thickness of the alloy changes in each pass during the rolling process as follows: 20 mm→18.5 mm→17 mm→15.5 mm→14 mm→12.5 mm→11 mm→9.5 mm→8 mm→6.5 mm→5 mm→4 mm; annealing at 420°C between rolling passes; water cooling to room temperature after rolling; and isothermal deformation processing.
[0070] F. Heat treatment: Firstly, carry out solution treatment, heat the isothermally deformed parts to 465±5℃, keep them warm for 2h, and then quench them in water; then carry out T74 double-stage aging treatment, heat the solution treated parts to 120℃ and keep them warm for 6h, then keep them warm at 175℃ for 7h, then quench them in water to obtain the parts.
[0071] The alloy material has not failed after 30 days of C-ring stress corrosion test at 260MPa in 3.5% NaCl corrosion environment. Its yield strength is 542MPa and tensile strength is 585MPa. After 48 hours of standard aluminum alloy exfoliation corrosion test, the corrosion grade is EA+ (see Figure 1 ), the maximum depth of intergranular corrosion test of aluminum alloy is 6um, and the intergranular corrosion grade is level 1.
[0072] Example 2
[0073] A high-strength, corrosion-resistant Al-Zn-Mg-Cu alloy comprises the following alloy compositions by weight: 2.07% copper, 2.48% Mg, 0.09% Zr, 6.26% Zn, ≤0.05% Fe, ≤0.01% Si, and the remainder aluminum and non-removable impurities.
[0074] A. Melting: Use high-purity aluminum, high-purity magnesium, high-purity zinc, aluminum-copper master alloy, aluminum-zirconium master alloy, and aluminum-beryllium master alloy as raw materials; among which, the purity of high-purity aluminum is ≥99.99%, the purity of industrial-purity magnesium is ≥99.95%, the purity of industrial-purity zinc is ≥99.95%, the copper content in the aluminum-copper master alloy is ≥50.0%, the beryllium content in the aluminum-beryllium master alloy is ≥10.0%, and the zirconium content in the aluminum-zirconium master alloy is ≥4.0%; weigh the raw materials according to the composition ratio, load them into a resistance furnace, and heat and melt them;
[0075] B. Refining, impurity removal and degassing: After the metal melt is completely alloyed, add the impurity remover to the alloy melt to gather slag, and introduce argon gas at the same time for 10 to 20 minutes, add an appropriate amount of hexachlorohexane, let it stand, and remove the slag. Repeat the above operation 2 to 3 times, and then let the aluminum alloy melt stand for more than 20 minutes;
[0076] C. Pouring: After the aluminum alloy melt is refined, impurity-removed and degassed, the melt temperature is maintained at 730±5℃, poured into a mold, and cooled and solidified to obtain an ingot;
[0077] D. Single-stage homogenization heat treatment: heat the ingot obtained in step C to 465±5°C, keep it at this temperature for 24 hours, then take it out of the furnace and air cool it to room temperature;
[0078] E. Hot rolling: The homogenized ingot obtained in step D is heated to 420±5°C in a resistance furnace and kept warm for 90 min, and then hot rolled for multiple passes until the final thickness of the alloy is 4 mm, wherein the thickness of the alloy changes in each pass during the rolling process as follows: 20 mm→18.5 mm→17 mm→15.5 mm→14 mm→12.5 mm→11 mm→9.5 mm→8 mm→6.5 mm→5 mm→4 mm; annealing at 420°C between rolling passes; water cooling to room temperature after rolling; and an isothermal deformed workpiece is obtained.
[0079] F. Heat treatment: Firstly, carry out solution treatment, heat the isothermally deformed parts to 465±5℃, keep them warm for 2h, and then quench them in water; then carry out T74 double-stage aging treatment, heat the solution treated parts to 120℃ and keep them warm for 6h, then keep them warm at 175℃ for 7h, then quench them in water to obtain the parts.
[0080] The alloy material did not fail after 30 days of C-ring stress corrosion test at 260MPa in a 3.5% NaCl corrosion environment. Its yield strength is 582MPa and its tensile strength is 604MPa. After 48 hours of standard aluminum alloy exfoliation corrosion test, the corrosion level is EA. The maximum depth of the aluminum alloy intergranular corrosion test is 310um, and the intergranular corrosion level is level 5.
[0081] Comparative Example 1
[0082] A high-strength, corrosion-resistant Al-Zn-Mg-Cu alloy comprises the following alloy compositions by weight: 2.08% copper, 2.44% Mg, 0.10% Zr, 0.18% Be, 6.31% Zn, ≤0.05% Fe, ≤0.01% Si, and the remainder aluminum and non-removable impurities.
[0083] A. Melting: Use high-purity aluminum, high-purity magnesium, high-purity zinc, aluminum-copper master alloy, aluminum-zirconium master alloy, and aluminum-beryllium master alloy as raw materials; among which, the purity of high-purity aluminum is ≥99.99%, the purity of industrial-purity magnesium is ≥99.95%, the purity of industrial-purity zinc is ≥99.95%, the copper content in the aluminum-copper master alloy is ≥50.0%, the beryllium content in the aluminum-beryllium master alloy is ≥10.0%, and the zirconium content in the aluminum-zirconium master alloy is ≥4.0%; weigh the raw materials according to the composition ratio, load them into a resistance furnace, and heat and melt them;
[0084] B. Refining, impurity removal and degassing: After the metal melt is completely alloyed, add the impurity remover to the alloy melt to gather slag, and introduce argon gas at the same time for 10 to 20 minutes, add an appropriate amount of hexachlorohexane, let it stand, and remove the slag. Repeat the above operation 2 to 3 times, and then let the aluminum alloy melt stand for more than 20 minutes;
[0085] C. Pouring: After the aluminum alloy melt is refined, impurity-removed and degassed, the melt temperature is maintained at 730±5°C, poured into a mold, and cooled and solidified to obtain an ingot;
[0086] D. Single-stage homogenization heat treatment: heat the ingot obtained in step C to 465±5°C, keep it at this temperature for 24 hours, then take it out of the furnace and air cool it to room temperature;
[0087] E. Hot rolling: The homogenized ingot obtained in step D is heated to 420±5°C in a resistance furnace and kept warm for 90 min, and then hot rolled for multiple passes until the alloy has a final thickness of 4 mm, wherein the alloy thickness changes in each pass during the rolling process as follows: 20 mm→18.5 mm→17 mm→15.5 mm→14 mm→12.5 mm→11 mm→9.5 mm→8 mm→6.5 mm→5 mm→4 mm; annealing is performed at 420°C between rolling passes; and water-cooling is performed to room temperature after rolling.
[0088] F. Heat treatment: Firstly, solution treatment is carried out, the isothermal deformed workpiece is heated to 465±5℃, kept at this temperature for 2h, and then water quenched after being taken out of the furnace; then T74 double-stage aging treatment is carried out, the solution treated workpiece is heated to 120℃ and kept at this temperature for 6h, then kept at 175℃ for 7h, and then water quenched after being taken out of the furnace to obtain the workpiece;
[0089] The alloy product did not fail after 30 days of C-ring stress corrosion test at 260MPa in 3.5% NaCl corrosion environment. The yield strength of the alloy product is 541MPa and the tensile strength is 575MPa. After 48 hours of standard aluminum alloy exfoliation corrosion test, the corrosion level is EC, and the maximum depth of aluminum alloy intergranular corrosion test is 169um, and the intergranular corrosion level is 4.
[0090] Performance Testing:
[0091] The aluminum alloy products of the above-mentioned implementation examples and comparative examples were tested, and the tensile test specimens were processed according to GB / T228.1-2010, and the results were averaged. The test results are shown in Table 1.
[0092] Table 1
[0093]
[0094] The above are only preferred implementation examples of the present invention and are not intended to limit the present invention. Any modifications, substitutions, etc. made within the principles of the present invention are included in the protection scope of the present invention.
Claims
1. A high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy, characterized in that: The invention comprises the following components in mass percentage: Cu 2.0-2.5%, Mg 2.0-2.8%, Zn 6.0-6.8%, Zr0.05-0.1%, Be0.05-0.1%, Fe≤0.05%, Si≤0.03%, and the balance is aluminum and non-removable impurities; The high-strength corrosion-resistant Al-Zn-Mg-Cu alloy is prepared by the following process: A. Melting: Use aluminum, magnesium, zinc, aluminum-copper master alloy, aluminum-zirconium master alloy, and aluminum-beryllium master alloy as raw materials; weigh the raw materials according to the composition ratio, load them into the smelting furnace, and heat and melt them; B. Refining, impurity removal and degassing: After the metal melt is completely alloyed, add the impurity remover to the alloy melt to gather slag, and introduce argon gas at the same time for 10 to 20 minutes, add an appropriate amount of hexachlorohexane, let it stand, and remove the slag. Repeat the above operation 2 to 3 times, and then let the aluminum alloy melt stand for more than 20 minutes; C. Pouring: After the aluminum alloy melt is refined, impurity-removed and degassed, the melt temperature is maintained at 730±5°C, poured into a mold, and cooled and solidified to obtain an ingot; D. Single-stage homogenization heat treatment: heat the ingot obtained in step C to 465±5°C, keep it at this temperature for 12 to 36 hours, then take it out of the furnace and air cool it to room temperature; E. Hot rolling: heating the homogenized ingot obtained in step D to 420±5°C and keeping the temperature for 60-120 minutes, and then performing multiple hot rolling to the set thickness of the alloy. During rolling, the pass reduction rate is controlled to be 5-20% and the total reduction rate is controlled to be 75-85%; Annealing at 420±5℃ between rolling passes; air cooling and / or water cooling to room temperature after rolling; isothermal deformation of parts; F. Heat treatment: Firstly, carry out solution treatment, heat the isothermally deformed parts to 465±5℃, keep them warm for 90-150min, and then quench them with water; then carry out T74 two-stage aging treatment; T74 two-stage aging treatment is as follows: heat the solution treated parts to 120-130℃ and keep them warm for 6-7h, then heat them to 175-185℃ and keep them warm for 7-8h, then quench them with water to room temperature. The homogenization treatment is a single-stage homogenization heat treatment, with a heating rate of 10 to 15° C. / min, a homogenization temperature of 465±5° C., and a heat preservation time of 20 to 28 hours.
2. The high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy according to claim 1, characterized in that: The high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy comprises the following components in mass percentage: Cu 2.1-2.15%, Mg 2.4-2.5%, Zn 6.2-6.4%, Zr0.08-0.1%, Be0.08-0.1%, Fe≤0.05%, Si≤0.01%, and the balance is aluminum and non-removable impurities.
3. The high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy according to claim 1, characterized in that: The aluminum alloy raw materials include: high-purity aluminum, industrial pure magnesium, industrial pure zinc, aluminum-copper master alloy, aluminum-beryllium master alloy, and aluminum-zirconium master alloy; The purity of the high-purity aluminum is ≥99.99%, the purity of the industrial-purity magnesium is ≥99.95%, and the purity of the industrial-purity zinc is ≥99.95%; The copper content in the aluminum-copper master alloy is ≥50.0%, the zirconium content in the aluminum-zirconium master alloy is ≥5.0%, and the beryllium content in the aluminum-beryllium master alloy is ≥10.0%.
4. The high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy according to claim 1, characterized in that: The smelting temperature is 750-780°C.
5. The high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy according to claim 1, characterized in that: The hot rolling is a multi-stage hot rolling, and the process is: heating the homogenized ingot to 420±5°C and keeping it warm for 70-120 minutes; performing 8-12 rolling passes, and the alloy thickness change in each rolling pass is 2-4 mm.
6. The high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy according to claim 2, characterized in that: The alloy material did not fail after being subjected to a C-ring stress corrosion test at 260MPa in a 3.5% NaCl corrosion environment for 30 days.
7. The high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy according to claim 2, characterized in that: The yield strength of the alloy material in the T74 state is not less than 540 MPa, and the tensile strength is not less than 580 MPa.
8. The high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy according to claim 2, characterized in that: The corrosion level of the alloy material after 48 hours of standard aluminum alloy exfoliation corrosion test is not less than EA, the maximum depth of aluminum alloy intergranular corrosion test is not higher than 100um, and the intergranular corrosion level does not exceed level 3.
9. The high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy according to claim 2, characterized in that: It includes the following components in mass percentage: copper content is 2.13%, Mg content is 2.46%, Zr content is 0.10%, Be content is 0.09%, Zn content is 6.39%, Fe: ≤0.05%, Si: ≤0.01%, and the balance is aluminum and non-removable impurities; The specific preparation method and steps are as follows: A. Smelting: High-purity aluminum, high-purity magnesium, high-purity zinc, aluminum-copper master alloy, aluminum-zirconium master alloy, and aluminum-beryllium master alloy are used as raw materials; among them, the purity of high-purity aluminum is ≥99.99%, the purity of industrial-purity magnesium is ≥99.95%, the purity of industrial-purity zinc is ≥99.95%, the copper content in the aluminum-copper master alloy is ≥50.0%, and the beryllium content in the aluminum-beryllium master alloy is ≥50.0%. ≥10.0%, the zirconium content in the aluminum-zirconium master alloy is ≥4.0%; weigh the raw materials according to the composition ratio, put them into the resistance furnace, and heat and melt them; B. Refining, impurity removal and degassing: After the metal melt is completely alloyed, add the impurity remover to the alloy melt to gather slag, and introduce argon gas at the same time for 10 to 20 minutes, add an appropriate amount of hexachlorohexane, let it stand, and remove the slag. Repeat the above operation 2 to 3 times, and then let the aluminum alloy melt stand for more than 20 minutes; C. Pouring: After the aluminum alloy melt is refined, impurity-removed and degassed, the melt temperature is maintained at 730±5℃, poured into a mold, and cooled and solidified to obtain an ingot; D. Single-stage homogenization heat treatment: heat the ingot obtained in step C to 465±5°C, keep it at this temperature for 24 hours, then take it out of the furnace and air cool it to room temperature; E. Hot rolling: the homogenized ingot obtained in step D is heated to 420±5°C in a resistance furnace and kept warm for 90 min, and then hot rolled for multiple passes until the final thickness of the alloy is 4 mm, wherein the thickness of the alloy changes in each pass during the rolling process as follows: 20 mm→18.5 mm→17 mm→15.5 mm→14 mm→12.5 mm→11 mm→9.5 mm→8 mm→6.5 mm→5 mm→4 mm; annealing at 420°C between rolling passes; water cooling to room temperature after rolling; and isothermal deformation processing.
10. The use of a high-strength and corrosion-resistant Al-Zn-Mg-Cu alloy according to any one of claims 1 to 9, characterized in that: Used for aircraft skins or other rolled sheet parts.
Citation Information
Patent Citations
Al-Zn-Mg-Cu high-strength aluminum alloy material and preparation method thereof
CN104711465A
High-strength Al-Zn-Mg-Cu aluminum alloy and preparation method thereof
CN111996425A
Heat-resistant low-vanadium Al-Cu-Mg-Ag alloy and application thereof
CN115558828A
High-strength corrosion-resistant Al-Zn-Mg aluminum alloy and preparation method thereof
CN116065067A
Ultrahigh-strength, high-toughness and stress-corrosion-resistant aluminum alloy and preparation method thereof
CN117144212A
Cited By
Corrosion-resistant aluminum alloy with anti-exfoliation corrosion grade of N grade
CN119753457A
An etch-resistant aluminum alloy having an exfoliation corrosion rating of N
CN119753457B