High-strength and high-plasticity ultralight magnesium-lithium alloy based on zinc-silver synergistic effect and preparation method thereof

By adopting a high-strength plastic ultralight magnesium lithium alloy with zinc and silver synergistic effect in magnesium lithium alloy, combined with smelting, homogenization, deformation heat treatment and solid solution treatment, the problem of insufficient mechanical properties of magnesium lithium alloy is solved and high tensile strength is achieved and low-energy consumption magnesium lithium alloy preparation to meet the needs of lightweight structural materials.

CN119082570APending Publication Date: 2024-12-06NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411204083.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The comprehensive mechanical properties of magnesium lithium alloys are poor, and the existing strengthening methods are limited in effect, making it difficult to significantly improve their strength and corrosion resistance while maintaining lightweight properties.

Method used

High-strength plastic ultralight magnesium lithium alloy based on the synergistic effect of zinc and silver was adopted, and the specific alloy ratio was passed (Li: 11-18 wt.%, Zn: 3-12 wt.%, Ag: 0.5-7 wt.%, and the remainder was Mg) Perform vacuum induction smelting, homogenization treatment, deformation heat treatment and solid solution treatment to form efficient co-solvents and gap solid solutions to improve the tensile strength and thermal stability of the alloy.

Benefits of technology

The high tensile strength and Vickers hardness of magnesium lithium alloy are achieved, which reduces production costs, and is subjected to solid solution treatment at medium and low temperatures, which has low energy consumption and significantly improves the mechanical properties of the alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082570A_ABST
    Figure CN119082570A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of alloy materials, and provides a high-strength and high-plasticity ultralight magnesium-lithium alloy based on zinc-silver synergistic effect and a preparation method thereof.The method comprises the following specific processes of smelting and preparation, specifically, 11-18 wt% of Li, 3-12 wt% of Zn, 0.5-7 wt% of Ag and the balance Mg are mixed and then subjected to smelting casting through vacuum induction smelting, and the alloy is obtained; preliminarily preparing a magnesium-lithium alloy cast ingot; homogenization treatment: cutting the alloy ingot into a proper size, removing a surface oxide layer, and carrying out homogenization treatment at 300-350 DEG C for about 2-4 hours; thermomechanical treatment is conducted, specifically, the cast ingot is subjected to thermomechanical treatment at the temperature of 250-300 DEG C, the total pressing amount is 50%-60%, and the rolling speed is 5-15 m / min. And solution treatment: heating the sample in a muffle furnace at 350-430 DEG C for 5-15 minutes, then immediately quenching, and taking out the sample after the sample is cooled to room temperature. Based on the synergistic effect of zinc and silver, the magnesium-lithium alloy structure is regulated and controlled through a proper process, the strength and plasticity of the magnesium-lithium alloy are remarkably improved, and the high-strength and high-plasticity ultralight Mg-Li-Zn-Ag alloy is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnesium-lithium alloy processing, and in particular to a high-strength, plastic, ultra-light magnesium-lithium alloy based on the synergistic effect of zinc and silver and a preparation method thereof. Background Art

[0002] The density of magnesium-lithium alloy is generally 0.95g / cm 3 ~1.65g / cm 3 It is 1 / 4 to 1 / 3 lighter than ordinary magnesium alloys and 1 / 3 to 1 / 2 lighter than aluminum alloys. It is currently the lightest alloy structural material in the world, so it is also called an ultra-light alloy. Magnesium-lithium alloy has extremely high specific stiffness, specific strength, excellent seismic resistance and resistance to high-energy particle penetration. The alloy has been widely used in the automotive, electronics, medical equipment, weapons industry, aviation, aerospace and other fields. It has become a lightweight structural material with huge application potential, providing opportunities for my country to achieve its "dual carbon" goals.

[0003] Magnesium-lithium alloys can be processed plastically, but their comprehensive mechanical properties are poor, so a variety of strengthening methods are used to improve their strength. Alloying, heat treatment and processing deformation are important means of strengthening magnesium-lithium alloys. Zn is one of the metal elements commonly added to magnesium-lithium alloys, with a melting point of 419.5°C. Zn and magnesium have the same HCP crystal structure, and their atomic radii are similar, so they can form a continuous eutectic solution; the solid solubility of Zn in magnesium is about 6.2wt.%. Zn will combine to form a metastable phase (MgLi2Zn) in magnesium-lithium alloys, and can be converted into a stable phase (MgLiZn) after aging treatment, so that the strength of the alloy is improved. At the same time, adding an appropriate amount of Zn can also improve the corrosion resistance of magnesium-lithium alloys. Under normal temperature conditions, Ag has a high solid solubility in magnesium (15%), dissolves in magnesium to form an interstitial solid solution, and can also react with Mg or Li to form MgAg and AgLi, improving the thermal stability and creep resistance of the alloy; at the same time, it has a significant effect in inhibiting the softening behavior of magnesium-lithium alloys over aging. Deformation heat treatment is a new metal heat treatment process that combines plastic deformation and heat treatment. It can effectively regulate the characteristics of the precipitated phase in magnesium-lithium alloys. Deformation heat treatment can optimize the alloy properties without changing the alloy composition. For magnesium-lithium alloys, solution treatment is one of the most effective processes to improve the mechanical properties of Mg-Li alloys. The alloy elements are dissolved in the matrix through solution treatment. At the same time, lattice distortion occurs due to the different atomic radii of the elements. The coherent stress field caused by the lattice distortion interacts with dislocations and hinders dislocation movement. The supersaturated solid solution obtained in the solution treatment can provide solute atoms for subsequent precipitation. In magnesium-lithium alloys, the solution atoms / precipitated precipitate phases effectively interact with dislocations, thereby improving the strength.

[0004] Therefore, we designed a high-strength, plastic, ultra-light magnesium-lithium alloy based on the synergistic effect of zinc and silver and its preparation method by combining the above processes. Summary of the invention

[0005] In view of the above shortcomings, the present invention proposes a high-strength, plastic, ultra-light magnesium-lithium alloy based on the synergistic effect of zinc and silver and a preparation method thereof. The alloy ratio used in the method is Li: 11-18wt.%, Zn: 3-12wt.%, Ag: 0.5-7wt.%, and the rest is Mg.

[0006] The specific preparation steps are as follows:

[0007] Step 1: smelting and preparation: mixing the raw materials according to the above ratio and then smelting and casting them through vacuum induction melting to initially produce magnesium-lithium alloy ingots.

[0008] Step 2: homogenization treatment: cut the alloy ingot into suitable sizes and remove the surface oxide layer, and perform homogenization treatment at 300-350° C. for about 2-4 hours to eliminate possible component segregation in the alloy.

[0009] Step three, thermomechanical treatment, thermomechanical treatment of the ingot at 250-300°C, with a total pressing amount of 50%-60% and a rolling speed of 5-15m / min.

[0010] Step 4: Solution treatment: heat the sample in a muffle furnace at 350-430°C for 5-15 minutes, then immediately quench it and take it out after it cools to room temperature.

[0011] Compared with the prior art, the present invention has the following significant advantages:

[0012] 1. The patented alloy does not contain rare earth elements, which is green and environmentally friendly while reducing production costs;

[0013] 2. The tensile strength of the magnesium-lithium alloy prepared by the present invention is above 350MPa, which is higher than the tensile strength of most bcc magnesium-lithium alloys reported so far;

[0014] 3. The patent of the present invention carries out solution treatment at medium and low temperatures, with low energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to better illustrate the practical application of the present invention, the following briefly introduces the drawings required for use in examples or prior art descriptions.

[0016] Figure 1 OM image of the metallographic microstructure of the magnesium-lithium alloy of Example 1.

[0017] Figure 2This is the EDS image of the Zn-Ag cluster of the magnesium-lithium alloy in Example 1.

[0018] Figure 3 OM image of the metallographic microstructure of the magnesium-lithium alloy of comparative example 1.

[0019] Figure 4 OM image of the metallographic microstructure of the magnesium-lithium alloy of comparative example 2.

[0020] Figure 5 The Vickers hardness diagram of magnesium-lithium alloys of Examples 1 and 2 of the present invention and Comparative Examples 1 and 2.

[0021] Figure 6 The stress-strain curves of magnesium-lithium alloys of Examples 1 and 2 of the present invention and Comparative Examples 1 and 2 are shown. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further illustrated below with specific implementation methods. The following implementations are all implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given, but the protection scope of the present invention is not limited to the following embodiments.

[0023] Example 1

[0024] An ingot with the composition of Mg-15Li-9Zn-2Ag was selected, the alloy ingot was cut into suitable sizes and the surface oxide layer was removed. The ingot was homogenized at 350°C for about 4 hours, and the ingot was subjected to deformation heat treatment at 300°C, with a total pressing amount of 60% and a rolling speed of 10m / min. The subsequent solution treatment first placed the sample in a 400°C muffle furnace for heating for 10 minutes, and then immediately quenched. After the sample was cooled to room temperature, it was taken out, and its tensile strength was 350MPa and Vickers hardness was 100HV.

[0025] Example 2

[0026] The steps are the same as those of Example 1, except that the composition of Example 2 is Mg-15Li-9Zn, the tensile strength is 300 MPa, and the Vickers hardness is 82 HV.

[0027] Comparative Example 1

[0028] The alloy composition is the same as that of Example 1, except that the alloy is a Mg-15Li-9Zn-2Ag ingot without any heat treatment, and has a tensile strength of 295 MPa and a Vickers hardness of 89 HV.

[0029] Comparative Example 2

[0030] The alloy composition is the same as that of Example 2, except that the alloy is a Mg-15Li-9Zn ingot without any heat treatment, and has a tensile strength of 250 MPa and a Vickers hardness of 70 HV.

[0031] Figure 2 The EDS image of the magnesium-lithium alloy of Example 1 shows nanoscale Zn-Ag co-segregated nanoclusters, which are rich in zinc and silver atoms. The tensile strength and hardness of Example 1 are higher than those of other alloys, which is closely related to the synergistic effect of zinc and silver. At the same time, the comparison between Example 1 and Example 2 shows that the addition of Ag element can further improve the strength of the alloy. Figure 3 and Figure 4 The comparison shows that adding an appropriate amount of silver atoms to the Mg-Li-Zn alloy can further refine the grains, thereby improving the performance of the alloy.

[0032] The above embodiments of the present invention are merely examples for explaining the present invention, and are not intended to limit the implementation methods of the present invention. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.

[0033] Matters not covered by the present invention are known technologies.

Claims

1. A high-strength, plastic, ultra-light magnesium-lithium alloy based on the synergistic effect of zinc and silver, characterized in that: The mass percentages of the components in the magnesium-lithium alloy include: Li: 11-18 wt.%, Zn: 3-12 wt.%, Ag: 0.5-7 wt.%, and the rest is Mg.

2. The method for preparing a high-strength, plastic, ultra-light magnesium-lithium alloy based on the synergistic effect of zinc and silver according to claim 1, characterized in that: The following steps are involved: (1) Melting and preparation, mixing the raw materials according to the above ratio and then melting and casting them by vacuum induction melting to initially produce a magnesium-lithium alloy ingot; (2) Homogenization treatment: cutting the alloy ingot into appropriate sizes and removing the surface oxide layer, followed by homogenization treatment to eliminate possible component segregation in the alloy; (3) Deformation heat treatment: performing deformation heat treatment on the ingot; (4) Solution treatment: Place the sample in a muffle furnace for heating, then immediately perform quenching treatment, and take it out after the sample cools to room temperature.

3. The high-strength, plastic, ultra-light magnesium-lithium alloy based on the synergistic effect of zinc and silver according to claim 1, characterized in that: The mass percentage of components in the magnesium-lithium alloy: Zn: 3-12wt.%, Ag: 0.5-7wt.%.

4. The method for preparing a high-strength, plastic, ultra-light magnesium-lithium alloy based on the synergistic effect of zinc and silver according to claim 2, characterized in that: In step (2), the homogenization treatment temperature is between 300 and 350° C., and the treatment time is between 2 and 4 hours.

5. The method for preparing a high-strength, plastic, ultra-light magnesium-lithium alloy based on the synergistic effect of zinc and silver according to claim 2, characterized in that: In step (3), the deformation heat treatment temperature is 250-300° C., the total pressing amount is 50%-60%, and the rolling speed is 5-15 m / min.

6. The method for preparing a high-strength, plastic, ultra-light magnesium-lithium alloy based on the synergistic effect of zinc and silver according to claim 2, characterized in that: In step (3), the solution treatment temperature is 350-430° C. and the treatment time is 5-15 min.