Medium-entropy alloy bonded tungsten alloy and preparation method thereof

By using VCoNi medium-entropy alloy as the bonding phase and using high-energy ball milling and discharge plasma sintering technology, the problem of insufficient strength of tungsten alloy is solved, and a low-cost and high-performance medium-entropy alloy bonded tungsten alloy preparation is achieved, which significantly improves the Its mechanical properties and density.

CN119082578APending Publication Date: 2024-12-06HAINAN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411290289.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The lower strength of existing tungsten alloy materials limits its application in aerospace, medical and military fields. Although high entropy alloys have excellent mechanical properties, they are difficult to apply on a large scale due to their high cost.

Method used

VCoNi medium-entropy alloy is used as the bonding phase, and through high-energy ball milling and discharge plasma sintering technology, a medium-entropy alloy bonded tungsten alloy with high relative density, small tungsten grains and high strength is prepared, which reduces the preparation cost and improves the mechanical properties. .

Benefits of technology

The low-cost and high-performance preparation of tungsten alloys is achieved, which significantly improves its strength and hardness, reduces the sintering temperature and time, and improves the relative density and structure uniformity of the alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082578A_ABST
    Figure CN119082578A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of tungsten alloy materials, and discloses a medium-entropy alloy bonded tungsten alloy and a preparation method thereof. The preparation method comprises the following steps: firstly, carrying out high-energy ball milling on elementary substance powder of V, Co and Ni to obtain VCoNi medium-entropy alloy micro powder; then, the VCoNi medium-entropy alloy micro powder and W powder are subjected to ball milling and mixing, and composite powder is obtained; and finally, the composite powder is subjected to spark plasma sintering, and the medium-entropy alloy bonded tungsten alloy is obtained. Wherein the content of the entropy alloy micro powder in the VCoNi is 5 to 15 weight percent, and the content of the W powder is 85 to 95 weight percent. According to the preparation method, the VCoNi medium entropy alloy powder is adopted as a binding phase, and the spark plasma sintering technology is combined, so that the tungsten alloy of which the comprehensive mechanical property is remarkably improved is finally prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tungsten alloy materials, and in particular relates to a medium-entropy alloy-bonded tungsten alloy and a preparation method thereof. Background Art

[0002] Tungsten heavy alloy, also generally known as tungsten alloy, has a typical two-phase structure. It is a composite material with tungsten as the base metal (80-98wt%) and low melting point metals (such as Ni, Fe, Cu) as the bonding phase. Tungsten alloy has excellent comprehensive mechanical properties, and has been widely used in various fields such as aerospace, medical and military. Generally, the lower strength of tungsten alloy has an adverse effect on its application. Therefore, the pursuit of higher mechanical properties, especially higher strength, is one of the main research goals in the field of tungsten alloy. Material composition is the main factor that determines the mechanical properties of tungsten alloy. Among them, the use of new bonding phases and modification by alloying elements are important means to improve the mechanical properties of tungsten alloy.

[0003] In recent years, the research on multi-component alloys containing multiple elements has attracted much attention. Among them, the emergence of high entropy alloys and medium entropy alloys provides a new choice for the bonding phase of tungsten alloys. High entropy alloys or medium entropy alloys are generally composed of each element in an equiatomic ratio or a nearly equiatomic ratio. These alloys have attracted much attention due to their excellent strength, ductility, wear resistance and corrosion resistance. According to relevant reports, high entropy alloy bonded tungsten alloys show good strength and hardness, and the comprehensive mechanical properties of tungsten alloys are relatively high. For example, patent CN116024448A provides a preparation method for non-equiatomic ratio high entropy alloy bonded tungsten alloys, and the obtained tungsten alloy has the characteristics of fine tungsten grains and good comprehensive mechanical properties. For another example, patent CN111676408A provides a tungsten-energetic high entropy alloy composite material and its preparation method, and the obtained tungsten alloy has the characteristics of high strength, high fracture strain and high energy release characteristics. However, high entropy alloys are generally composed of five or more elements, which increases the cost of alloy raw materials and is not conducive to their large-scale application. However, medium-entropy alloys are generally alloys of three metal elements in equal or nearly equal atomic ratios, so their cost is relatively low. At the same time, the performance of medium-entropy alloys is similar to that of high-entropy alloys.

[0004] Therefore, using medium-entropy alloy as the bonding phase and preparing high-density tungsten alloy with fine tungsten grains and high strength at a lower sintering temperature is very important for the development of low-cost, high-performance tungsten alloys. Summary of the invention

[0005] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide a medium entropy alloy bonded tungsten alloy. The medium entropy alloy bonded tungsten alloy of the present invention selects VCoNi medium entropy alloy with good mechanical properties and relatively low price as the bonding phase, which can reduce the preparation cost of conventional high entropy alloy bonded tungsten alloy and has the same effect as high entropy alloy bonded tungsten alloy.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned medium entropy alloy bonded tungsten alloy. The preparation method of the present invention adopts mechanical ball milling plus spark plasma sintering technology, which can further refine the tungsten grains of the tungsten alloy and significantly improve the relative density, structural uniformity and mechanical strength of the alloy.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] A medium entropy alloy-bonded tungsten alloy comprises a W matrix and a VCoNi medium entropy alloy bonding phase, wherein the content of the W matrix is ​​85-95wt%, the content of the VCoNi bonding phase is 5-15wt%, and the element molar ratio of V, Co and Ni in the VCoNi is 1:1:1.

[0009] Preferably, the relative density of the medium entropy alloy bonded tungsten alloy is greater than 95%, the macroscopic hardness is greater than 70HRA, and the bending strength is greater than or equal to 1400MPa.

[0010] Further preferably, the medium-entropy alloy bonded tungsten alloy comprises a W matrix and a VCoNi bonding phase, wherein the content of the W matrix is ​​90wt%, the content of the VCoNi bonding phase is 10wt%, and the element molar ratio of V, Co and Ni in VCoNi is 1:1:1; the relative density of the medium-entropy alloy bonded tungsten alloy is >96%, the macrohardness is >71HRA, and the bending strength is >1800MPa.

[0011] A method for preparing a medium entropy alloy bonded tungsten alloy comprises the following preparation steps:

[0012] (1) high-energy ball milling V, Co, and Ni single-element powders to obtain VCoNi medium-entropy alloy powder;

[0013] (2) ball milling the VCoNi medium entropy alloy powder and W powder to obtain a tungsten alloy composite powder;

[0014] (3) The composite powder is subjected to spark plasma sintering to obtain a medium entropy alloy bonded tungsten alloy.

[0015] Furthermore, the average particle size of the V, Co, and Ni single-substance powders is ≤20 μm; the average particle size of the VCoNi medium-entropy alloy powder is ≤30 μm; and the average particle size of the W powder is ≤5 μm.

[0016] Furthermore, the molar ratio of the V, Co and Ni single substance powders is 1:1:1.

[0017] Furthermore, the content of VCoNi entropy alloy powder in the composite powder is 5-15wt%, and the content of W powder is 85-95wt%.

[0018] Furthermore, the high-energy ball milling in step (1) is dry ball milling; the ball-to-material ratio of the ball milling is 10 to 20:1, the ball mill speed is 200 to 500 r / min, and the ball milling time is 20 to 30 h.

[0019] Further preferably, the high-energy ball milling in step (1) is an intermittent ball milling, wherein the running time of a single mixing is 30 to 60 minutes and the stopping time is 5 to 20 minutes.

[0020] Furthermore, the ball milling mixing in step (2) is carried out with or without adding grinding balls; the mixing method with adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder, W powder and grinding balls are placed in a ball mill, and the mixing is carried out for 10 to 30 hours at a ball-to-material ratio not exceeding 10:1 and a ball mill speed not exceeding 400 r / min; the mixing method without adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder and W powder are placed in a ball mill, and the mixing is carried out for 10 to 30 hours at a ball mill speed not exceeding 400 r / min.

[0021] Furthermore, the spark plasma sintering is a one-step sintering method; the air pressure in the furnace of the one-step sintering method is 10-50 Pa, the temperature is 1100-1300° C., the sintering pressure is 30-100 MPa, the heating rate is 100-400° C. / min, and the insulation time is 1-30 min.

[0022] The principle of the present invention is: first, vanadium powder, cobalt powder, and nickel powder are converted into VCoNi medium entropy alloy powder by high-energy ball milling technology, and then the VCoNi medium entropy alloy powder is evenly mixed with tungsten powder, and finally a high-performance fine-grained W-VCoNi alloy is obtained by spark plasma sintering. The present invention uses a specific VCoNi activated powder as a bonding phase, which has a low melting point, good fluidity in the molten state, and good compatibility with tungsten powder, can achieve low-temperature sintering, and can promote low-temperature densification of the alloy. The tungsten alloy prepared by the present invention has excellent mechanical properties, especially its strength is greatly improved.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) In the preparation method of the medium-entropy alloy bonded tungsten alloy provided by the present invention, the VCoNi powder content is relatively low, the sintering temperature is relatively low, and the sintering time is relatively short. Therefore, compared with the conventional method, the comprehensive preparation cost of the tungsten alloy is relatively low.

[0025] (2) The formation of face-centered cubic (Ni, Co) solid solution during the high-energy ball milling process of the present invention and the solid solution strengthening caused by the further diffusion of W and V atoms into the solid solution during sintering are beneficial to improving the mechanical properties of the alloy.

[0026] (3) During the ball milling and sintering process of the present invention, the surface of the metal V powder is oxidized to form vanadium oxide, which can not only hinder the dissolution-precipitation process of tungsten, thereby inhibiting the growth of W grains and causing fine grain strengthening, but also hinder dislocation movement and cause dislocation accumulation, which is beneficial to improving the mechanical properties (especially strength) of the alloy.

[0027] (4) The medium-entropy alloy bonded tungsten alloy of the present invention has the characteristics of low sintering temperature, high relative density, fine tungsten grains, high strength and hardness, and the comprehensive mechanical properties are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The XRD pattern of the VCoNi medium entropy alloy powder prepared by high energy ball milling in Example 1;

[0029] Figure 2 The DSC graph of the VCoNi medium entropy alloy powder prepared by high energy ball milling in Example 1;

[0030] Figure 3 is the BSE diagram of the W-VCoNi alloy prepared in Example 1;

[0031] Figure 4 TEM image and EDS Mapping image of the W-VCoNi alloy prepared in Example 1. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0033] Example 1

[0034] 1. Raw materials:

[0035] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.

[0036] 2. Preparation:

[0037] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.

[0038] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 10wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.

[0039] (3) After the uniform tungsten alloy composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single power-on time of pulse voltage is 300ms, and single interruption time is 20ms. After the above sintering, a W-VCoNi alloy with uniform structure is obtained.

[0040] The W-VCoNi alloy prepared in this embodiment has an average tungsten grain size of less than 4 μm, a relative density of greater than 96%, a macroscopic hardness of 71.30 HRA, and a bending strength of 1883.00 MPa.

[0041] The phase analysis of the obtained VCoNi medium entropy alloy powder was carried out using an X-ray diffractometer (XRD, smartlab, RIGAKU, Japan). Figure 1 As shown in the figure, after 24 hours of high-energy ball milling, VCoNi medium-entropy alloy powder with face-centered cubic (fcc) (Ni, Co) solid solution and V-σ-rich phase was obtained. Differential scanning calorimetry (TGA / DSC3 + , Mettler Toledo Switzerland) analyzed the thermal effect of VCoNi medium entropy alloy powder during heating. The results are as follows Figure 2 As shown in the figure, the melting point of the medium entropy alloy powder is 1246℃, which is much lower than the melting points of single metals V, Co and Ni. The microstructure of the sintered tungsten alloy was characterized by scanning electron microscopy (FE-SEM, Verios G4 UC, Thermo Scientific, USA). The BSE image results are shown in Figure 3 .from Figure 3 It can be seen that the W-VCoNi alloy has a uniform structure, with a small number of nearly spherical tungsten grains interspersed with vanadium oxides (as shown in point 1), and the W grain growth is not obvious, indicating that the presence of vanadium oxides during sintering has the effect of hindering the growth of W grains, and the resulting fine grain strengthening is beneficial to improving the mechanical properties of tungsten alloys. The fine structure of tungsten alloys was analyzed using a transmission electron microscope (TEM, JEM2100F, Joel, Japan). The results are shown in Figure 2. Figure 4 As shown. It can be seen that the upper right corner and the lower left corner of the picture are W grains and (Ni, Co) bonding phases, respectively, and a "violin"-shaped vanadium oxide phase appears at the interface between the two. From the EDS Mapping diagram corresponding to each element in the alloy, it can be seen that a small amount of W and V atoms tend to diffuse into the bonding phase (Ni, Co). Therefore, to be precise, the bonding phase is a (Ni, Co) solid solution containing a small amount of W and V atoms. The resulting solid solution strengthening is also beneficial to improving the mechanical properties of the alloy.

[0042] Example 2

[0043] 1. Raw materials:

[0044] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.

[0045] 2. Preparation:

[0046] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.

[0047] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 10wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.

[0048] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1300℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, W-VCoNi alloy is obtained.

[0049] The W-VCoNi alloy obtained in this embodiment has an average tungsten grain size of less than 4 μm, a relative density of more than 95%, a macroscopic hardness of 70.20 HRA, and a bending strength of 1713.00 MPa.

[0050] Example 3

[0051] 1. Raw materials:

[0052] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.

[0053] 2. Preparation:

[0054] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.

[0055] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 10wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.

[0056] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1250℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, W-VCoNi alloy is obtained.

[0057] The W-VCoNi alloy obtained in this embodiment has an average tungsten grain size of less than 4 μm, a relative density of greater than 93%, a macroscopic hardness of 75.30 HRA, and a bending strength of 1285.31 MPa.

[0058] Example 4

[0059] 1. Raw materials:

[0060] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.

[0061] 2. Preparation:

[0062] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.

[0063] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 10wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.

[0064] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1200℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, W-VCoNi alloy is obtained.

[0065] The W-VCoNi alloy obtained in this embodiment has an average tungsten grain size of less than 4 μm, a relative density of greater than 93%, a macroscopic hardness of 75.50 HRA, and a bending strength of 931.36 MPa.

[0066] Example 5

[0067] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.

[0068] 2. Preparation:

[0069] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.

[0070] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 10wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.

[0071] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1150℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, W-VCoNi alloy is obtained.

[0072] The W-VCoNi alloy obtained in this embodiment has an average tungsten grain size of less than 4 μm, a relative density of greater than 93%, a macroscopic hardness of 76.40 HRA, and a bending strength of 894.90 MPa.

[0073] Example 6

[0074] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.

[0075] 2. Preparation:

[0076] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.

[0077] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 95wt%, VCoNi: 5wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.

[0078] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, W-VCoNi alloy is obtained.

[0079] The W-VCoNi alloy obtained in this embodiment has an average tungsten grain size of less than 4 μm, a relative density of greater than 95%, a macroscopic hardness of 73.14 HRA, and a bending strength of 1832.15 MPa.

[0080] Example 7

[0081] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.

[0082] 2. Preparation:

[0083] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.

[0084] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 85wt%, VCoNi: 15wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.

[0085] (3) After the composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step liquid phase sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, W-VCoNi alloy is obtained.

[0086] The W-VCoNi alloy obtained in this embodiment has an average tungsten grain size of less than 4 μm, a relative density of greater than 95%, a macroscopic hardness of 75.34 HRA, and a bending strength of 1672.85 MPa.

[0087] Comparative Example 1

[0088] Compared with Example 1, in this comparative example, V powder, Co powder and Ni powder were not pre-milled to prepare VCoNi medium entropy alloy powder, but were directly mixed with W powder to prepare tungsten alloy. The specific preparation steps are as follows:

[0089] 1. Raw materials:

[0090] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.

[0091] 2. Preparation:

[0092] (1) W powder, V powder, Co powder, and Ni powder (with corresponding mass fractions of 90 wt%, 3.02 wt%, 3.50 wt%, and 3.48 wt%, respectively) were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single operation time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, a uniform WV-Co-Ni composite powder was obtained.

[0093] (2) After the uniform WV-Co-Ni composite powder is loaded into a graphite mold, it is placed in a spark plasma sintering system heating chamber, and after vacuuming, spark plasma one-step sintering is performed; the sintering process conditions are: sintering vacuum degree <30Pa, sintering pressure is 40MPa, heating rate is 100℃ / min, sintering temperature is 1275℃, and holding time is 5min; pulse voltage is 4.5V, single pulse voltage power-on time is 300ms, and single interruption time is 20ms. After the above sintering, WV-Co-Ni alloy is obtained.

[0094] The WV-Co-Ni alloy obtained in this comparative example has an average tungsten grain size of less than 5 μm, a relative density of less than 92%, a macroscopic hardness of 72.10 HRA, and a bending strength of 1457.46 MPa. Compared with the W-VCoNi alloy prepared in Example 1, the hardness of the WV-Co-Ni alloy is similar, but its bending strength is reduced by 425.54 MPa.

[0095] Comparative Example 2

[0096] Compared with Example 1, this comparative example adopts conventional liquid phase sintering instead of spark plasma sintering, and the rest is the same. The specific steps are as follows:

[0097] 1. Raw materials:

[0098] The purity of W powder is greater than 99.9%, the purity of V powder is greater than 99.9%, the purity of Co powder is greater than 99.9%, and the purity of Ni powder is greater than 99.9%. The average particle size of W powder is 3μm. The average particle size of V powder, Co powder, and Ni powder is ≤20μm.

[0099] 2. Preparation:

[0100] (1) V powder, Co powder, and Ni powder (corresponding mass fractions of 30.22 wt%, 34.96 wt%, and 34.82 wt%, respectively) in a molar ratio of 1:1:1 were loaded into a ball mill and dry-milled on a high-energy ball mill with a ball-to-material ratio of 10:1, a single running time of 1 h, and an intermittent time of 10 min. After ball milling at a speed of 300 r / min for 24 h, VCoNi medium-entropy alloy powder was obtained.

[0101] (2) The obtained VCoNi medium entropy alloy powder and W powder are mixed in a ball mill according to a certain mass fraction (W powder: 90wt%, VCoNi: 10wt%), wherein the ball-to-material ratio is 10:1, the ball mill speed is 300r / min, and the ball milling time is 24h to obtain a uniform tungsten alloy composite powder.

[0102] (3) The composite powder is loaded into a mold, pressed and formed, and then the sample is placed in a heating chamber of a vacuum sintering furnace for conventional liquid phase sintering; the sintering process conditions are: heating rate of 5°C / min, sintering temperature of 1275°C, and holding time of 60min. After the above sintering, a W-VCoNi alloy is obtained.

[0103] The W-VCoNi alloy obtained in this comparative example has an average tungsten grain size of less than 5 μm, a relative density of less than 90%, a macroscopic hardness of 67.10 HRA, and a bending strength of 1158.00 MPa. Compared with the W-VCoNi alloy prepared in Example 1, the hardness and bending strength of the alloy have both dropped significantly.

[0104] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A medium entropy alloy bonded tungsten alloy, characterized in that: The invention comprises a W matrix and a VCoNi medium entropy alloy bonding phase, wherein the content of the W matrix is ​​85-95wt%, the content of the VCoNi bonding phase is 5-15wt%, and the molar ratio of V, Co and Ni in the VCoNi is 1:1:

1.

2. A medium entropy alloy bonded tungsten alloy according to claim 1, characterized in that: The medium entropy alloy bonded tungsten alloy has a relative density of more than 95%, a macroscopic hardness of more than 70HRA, and a bending strength of more than or equal to 1400MPa.

3. A medium entropy alloy bonded tungsten alloy according to claim 1, characterized in that: The medium-entropy alloy-bonded tungsten alloy comprises a W matrix and a VCoNi bonding phase, wherein the content of the W matrix is ​​90wt%, the content of the VCoNi bonding phase is 10wt%, and the element molar ratio of V, Co, and Ni in VCoNi is 1:1:1; the relative density of the medium-entropy alloy-bonded tungsten alloy is greater than 96%, the macroscopic hardness is greater than 71HRA, and the bending strength is greater than 1800MPa.

4. A method for preparing a medium entropy alloy bonded tungsten alloy, characterized in that: The method comprises the following preparation steps: (1) high-energy ball milling V, Co, and Ni single-element powders to obtain VCoNi medium-entropy alloy powder; (2) ball milling the VCoNi medium entropy alloy powder and W powder to obtain a tungsten alloy composite powder; (3) The composite powder is subjected to spark plasma sintering to obtain a medium entropy alloy bonded tungsten alloy.

5. The method for preparing a medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The average particle size of the V, Co, and Ni single-substance powders is ≤20 μm; the average particle size of the VCoNi medium-entropy alloy powder is ≤30 μm; the average particle size of the W powder is ≤5 μm; and the molar ratio of the V, Co, and Ni single-substance powders is 1:1:

1.

6. The method for preparing a medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The content of VCoNi entropy alloy powder in the composite powder is 5-15wt%, and the content of W powder is 85-95wt%.

7. The method for preparing a medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The high-energy ball milling in step (1) is dry ball milling; the ball-to-material ratio of the ball milling is 10 to 20:1, the ball mill speed is 200 to 500 r / min, and the ball milling time is 20 to 30 h.

8. The method for preparing a medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The high-energy ball milling in step (1) is an intermittent ball milling, wherein the running time of a single mixing is 30 to 60 minutes and the stopping time is 5 to 20 minutes.

9. The method for preparing a medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The ball milling mixing in step (2) is carried out with or without adding grinding balls; the mixing method with adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder, W powder and grinding balls are placed in a ball mill, and the mixing is carried out for 10 to 30 hours at a ball-to-material ratio not exceeding 10:1 and a ball mill speed not exceeding 400 r / min; the mixing method without adding grinding balls is specifically as follows: VCoNi medium entropy alloy powder and W powder are placed in a ball mill, and the mixing is carried out for 10 to 30 hours at a ball mill speed not exceeding 400 r / min.

10. The method for preparing a medium entropy alloy bonded tungsten alloy according to claim 4, characterized in that: The spark plasma sintering is a one-step sintering method; the air pressure in the furnace of the one-step sintering method is 10-50 Pa, the temperature is 1100-1300° C., the sintering pressure is 30-100 MPa, the heating rate is 100-400° C. / min, and the insulation time is 1-30 min.

Citation Information

Cited By

  • Preparation process of high-strength and high-toughness copper wire

    CN121331560A

  • Preparation process of high-strength and high-toughness copper wire

    CN121331560B