High-strength anchor rod and preparation process thereof

High-strength anchors prepared through specific element composition and heat treatment processes solve the problem of insufficient strength of traditional anchors in complex geological environments, significantly improve the tensile strength and yield strength of anchors, and meet the high-performance needs of modern engineering construction. .

CN119082611APending Publication Date: 2024-12-06HANDAN SHENGXIANG MINING MACHINERY MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411271990.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional anchors are insufficient in complex geological environments, resulting in unstable tunnel support structures, affecting construction safety and long-term use performance.

Method used

High-strength anchor rods composed of specific components, including C, Ni, Cr, Si, Co, Mn, Al, Cu, Ce, Y, Re, Hf and other elements, are prepared through smelting, refining, continuous casting and heat treatment processes, and are limited The weight percentage and ratio of Y and Re, as well as the content of Hf, increase the strength of the anchor.

Benefits of technology

The tensile strength and yield strength of the anchor rod are significantly improved, meeting the high requirements for anchor rod performance in modern engineering construction, and ensuring construction safety and long-term use stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of metal materials, and provides a high-strength anchor rod and a preparation technology thereof.The high-strength anchor rod is prepared from, by weight, 0.35%-0.42% of C, 3.45%-4.20% of Ni, 2.3%-3.5% of Cr, 0.001%-0.01% of S, 0.001%-0.008% of P, 0.75%-0.95% of Si, 0.8%-1.2% of Co, 2.1%-2.8% of Mn, 0.05%-0.1% of Al, 0.45%-0.65% of Cu, 0.05%-0.1% of Ce, 0.01%-0.09% of Y, 0.001%-0.055% of Re, 0-0.01% of Hf and the balance Fe and inevitable impurities. By means of the technical scheme, the problem that in the related technology, the anchor rod is poor in strength is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal materials, and in particular to a high-strength anchor rod and a preparation process thereof. Background Art

[0002] In the field of modern engineering construction, especially in mining, tunnel construction, water conservancy and hydropower engineering, anchor rods, as an important support structure, play a vital role. With the continuous expansion of the scale of various projects and the increasing complexity of the engineering environment, the performance requirements for anchor rods are getting higher and higher. In many cases, traditional anchor rods can no longer meet the actual needs of current projects. For example, in tunnel construction projects, due to the complex and changeable geological environment of the tunnel and the uneven distribution of surrounding rock pressure, the insufficient strength of traditional anchor rods may lead to the instability of the tunnel support structure, thereby affecting the construction safety and long-term performance of the tunnel. Therefore, the research and development and application of high-strength anchor rods have become an important development direction in the current engineering construction field. Summary of the invention

[0003] The present invention provides a high-strength anchor rod and a preparation process thereof, which solves the problem of poor anchor rod strength in the related art.

[0004] The technical solution of the present invention is as follows: The invention provides a high-strength anchor rod, which is composed of the following components by weight percentage: C 0.35%-0.42%, Ni 3.45%-4.20%, Cr 2.3%-3.5%, S 0.001%-0.01%, P 0.001%-0.008%, Si 0.75%-0.95%, Co0.8%-1.2%, Mn 2.1%-2.8%, Al 0.05%-0.1%, Cu 0.45%-0.65%, Ce 0.05%-0.1%, Y 0.01%-0.09%, Re 0.001%-0.055%, Hf 0-0.01%, and the balance is Fe and inevitable impurities.

[0005] As a further technical solution, the sum of the weight percentages of Y and Re is 0.075%≤Y+Re≤0.12%.

[0006] In the present invention, the strength of the anchor rod is further improved by limiting the sum of the weight percentages of Y and Re in the anchor rod to 0.075% to 0.12%.

[0007] As a further technical solution, the ratio of Y to Re is 0.8≤Y / Re≤1.5.

[0008] In the present invention, when the sum of the weight percentages of Y and Re is 0.075% to 0.12%, the ratio of Y to Re in the anchor rod is further limited to 0.8 to 1.5, thereby further improving the strength of the anchor rod.

[0009] As a further technical solution, the weight percentage of Hf is 0.005%~0.008%.

[0010] In the present invention, the weight percentage of Hf is limited to 0.005% to 0.008%, and Hf is combined with Y and Re to further improve the strength of the anchor rod.

[0011] The present invention also provides a preparation process of a high-strength anchor rod, comprising the following steps: S1. After the ingredients are prepared, the anchor blank is obtained by smelting, refining and continuous casting; S2. The anchor rod blank is subjected to heat treatment to obtain a high-strength anchor rod.

[0012] As a further technical solution, the heat treatment includes normalizing, annealing, quenching and tempering.

[0013] As a further technical solution, the normalizing temperature is 850-870°C and the holding time is 4-5h.

[0014] As a further technical solution, the annealing temperature is 650-680° C., and the holding time is 7-8 hours.

[0015] As a further technical solution, the quenching temperature is 830-850°C and the holding time is 3-4h.

[0016] As a further technical solution, the tempering temperature is 290-310° C. and the holding time is 3-4 hours.

[0017] The working principle and beneficial effects of the present invention are: In the present invention, C, Ni, Cr, Si, Co, Mn, Al, Cu, and Ce elements cooperate with each other to make the anchor rod have a high tensile strength. Among them, the carbide formed by carbon and alloy elements can effectively hinder the dislocation movement and improve the strength of the anchor rod; at the same time, Y, Re, and Hf are added to be compatible with other components to further improve the strength of the anchor rod. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] In the following embodiments and comparative examples: Ferrochromium alloy, chromium content 60wt%; ferrosilicon alloy, silicon content 75wt%; ferrocobalt alloy, cobalt content 30wt%; ferrocerium alloy, cerium content 20wt%; ferroyttrium alloy, yttrium content 60wt%; nickel-rhenium alloy, rhenium content 20wt%.

[0020] Example 1 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.09%, Re 0.045%, the balance is Fe and unavoidable impurities; Y+Re=0.135%, Y / Re=2; The preparation process comprises the following steps: S1, mixing carbon powder, manganese powder, aluminum block, copper block, ferrochrome alloy, ferrosilicon alloy, cobalt-iron alloy, ferrocerium alloy, yttrium-iron alloy, nickel-rhenium alloy and iron block according to the above ingredients, and smelting, refining and continuously casting to obtain an anchor blank; S2. Normalize the anchor rod blank at 850°C for 5 hours, then anneal at 650°C for 8 hours, quench at 830°C for 4 hours, and temper at 290°C for 4 hours to obtain a high-strength anchor rod.

[0021] Example 2 The high-strength anchor is composed of the following components by weight percentage: C 0.39%, Ni 3.89%, Cr 2.9%, S0.006%, P 0.004%, Si 0.8%, Co 1.0%, Mn 2.5%, Al 0.08%, Cu 0.50%, Ce 0.08%, Y 0.01%, Re0.001%, the balance is Fe and unavoidable impurities; Y+Re=0.011%, Y / Re=10; The preparation process comprises the following steps: S1, mixing carbon powder, manganese powder, aluminum block, copper block, ferrochrome alloy, ferrosilicon alloy, cobalt-iron alloy, ferrocerium alloy, yttrium-iron alloy, nickel-rhenium alloy and iron block according to the above ingredients, and smelting, refining and continuously casting to obtain an anchor blank; S2. Normalize the anchor rod blank at 860°C for 5 hours, then anneal at 670°C for 8 hours, quench at 840°C for 4 hours, and temper at 300°C for 4 hours to obtain a high-strength anchor rod.

[0022] Example 3 The high-strength anchor is composed of the following components by weight percentage: C 0.42%, Ni 4.20%, Cr 3.5%, S0.01%, P 0.008%, Si 0.95%, Co 1.2%, Mn 2.8%, Al 0.1%, Cu 0.65%, Ce 0.1%, Y 0.015%, Re0.055%, the balance is Fe and unavoidable impurities; Y+Re=0.07%, Y / Re=0.27; The preparation process comprises the following steps: S1, mixing carbon powder, manganese powder, aluminum block, copper block, ferrochrome alloy, ferrosilicon alloy, cobalt-iron alloy, ferrocerium alloy, yttrium-iron alloy, nickel-rhenium alloy and iron block according to the above ingredients, and smelting, refining and continuously casting to obtain an anchor blank; S2. Normalize the anchor rod blank at 870°C for 4 hours, then anneal at 680°C for 7 hours, quench at 850°C for 3 hours, and temper at 310°C for 3 hours to obtain a high-strength anchor rod.

[0023] Example 4 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.034%, Re 0.017%, and the balance is Fe and unavoidable impurities; Y+Re=0.051%, Y / Re=2; The preparation process is the same as that of Example 1.

[0024] Example 5 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.08%, Re 0.04%, the balance is Fe and unavoidable impurities; Y+Re=0.12%, Y / Re=2; The preparation process is the same as that of Example 1.

[0025] Example 6 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.05%, Re 0.025%, the balance is Fe and unavoidable impurities; Y+Re=0.075%, Y / Re=2; The preparation process is the same as that of Example 1.

[0026] Example 7 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.06%, Re 0.03%, the balance is Fe and unavoidable impurities; Y+Re=0.09%, Y / Re=2; The preparation process is the same as that of Example 1.

[0027] Example 8 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.054%, Re 0.036%, the balance is Fe and unavoidable impurities; Y+Re=0.09%, Y / Re=1.5; The preparation process is the same as that of Example 1.

[0028] Example 9 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.04%, Re 0.05%, the balance is Fe and unavoidable impurities; Y+Re=0.09%, Y / Re=0.8; The preparation process is the same as that of Example 1.

[0029] Example 10 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.04%, Re 0.05%, Hf 0.001%, the balance is Fe and unavoidable impurities; Y+Re=0.09%, Y / Re=0.8; The preparation process is the same as that of Example 1.

[0030] Embodiment 11 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.04%, Re 0.05%, Hf 0.01%, the balance is Fe and unavoidable impurities; Y+Re=0.09%, Y / Re=0.8; The preparation process is the same as that of Example 1.

[0031] Example 12 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.04%, Re 0.05%, Hf 0.005%, the balance is Fe and unavoidable impurities; Y+Re=0.09%, Y / Re=0.8; The preparation process is the same as that of Example 1.

[0032] Example 13 The high-strength anchor is composed of the following components by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al 0.05%, Cu 0.45%, Ce 0.05%, Y 0.04%, Re 0.05%, Hf 0.008%, the balance is Fe and unavoidable impurities; Y+Re=0.09%, Y / Re=0.8; The preparation process is the same as that of Example 1.

[0033] Comparative Example 1 The only difference between this comparative example and Example 1 is that the high-strength anchor rod is composed of the following components, by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S 0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al0.05%, Cu 0.45%, Ce 0.05%, Re 0.135%, and the balance is Fe and unavoidable impurities.

[0034] Comparative Example 2 The only difference between this comparative example and Example 1 is that the high-strength anchor rod consists of the following components, by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S 0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al0.05%, Cu 0.45%, Ce 0.05%, Y 0.135%, and the balance is Fe and unavoidable impurities.

[0035] Comparative Example 3 The only difference between this comparative example and Example 1 is that the high-strength anchor rod is composed of the following components, by weight percentage: C 0.35%, Ni 3.45%, Cr 2.3%, S 0.001%, P 0.001%, Si 0.75%, Co 0.8%, Mn 2.1%, Al0.05%, Cu 0.45%, Ce 0.05%, and the balance is Fe and unavoidable impurities.

[0036] The yield strength and tensile strength of the anchor rods prepared in Examples 1 to 13 and Comparative Examples 1 to 3 were tested according to the standard in the implementation guide of GB / T 228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method", and the test results are shown in Table 1.

[0037] Table 1 Anchor performance test results

[0038] Compared with Example 1, Comparative Example 1 does not contain the Y element, Comparative Example 2 does not contain the Re element, and Comparative Example 3 does not contain the Y and Re elements. As a result, the tensile strength and yield strength of the anchor rods prepared in Comparative Examples 1 to 3 are both lower than those in Example 1, indicating that when Y and Re are contained at the same time, the mechanical strength of the anchor rod can be improved.

[0039] Compared with Example 1, the sum of the weight percentages of Y and Re was changed in Examples 4 to 7. As a result, the tensile strength and yield strength of the anchor rods prepared in Examples 5 to 7 were greater than those in Examples 1 and 4, indicating that when the sum of the weight percentages of Y and Re is 0.075%≤Y+Re≤0.12%, the mechanical strength of the anchor rod can be further improved.

[0040] Compared with Example 7, Examples 8~9 changed the ratio of Y and Re. As a result, the tensile strength and yield strength of the anchor rods prepared in Examples 8~9 were greater than those in Example 7, indicating that when the ratio of Y and Re is 0.8≤Y / Re≤1.5, the mechanical strength of the anchor rod can be further improved.

[0041] Compared with Example 8, the Hf content was changed in Examples 10 to 13. As a result, the tensile strength and yield strength of the anchors obtained in Examples 12 to 13 were greater than those in Examples 10 to 11, indicating that when the Hf content was 0.005% to 0.008%, the mechanical strength of the anchor was the highest.

[0042] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-strength anchor rod, characterized in that: Calculated by weight percentage, it is composed of the following components: C 0.35%~0.42%, Ni 3.45%~4.20%, Cr 2.3%~3.5%, S 0.001%~0.01%, P 0.001%~0.008%, Si 0.75%~0.95%, Co0.8%~1.2%, Mn 2.1%~2.8%, Al 0.05%~0.1%, Cu 0.45%~0.65%, Ce 0.05%~0.1%, Y 0.01%~0.09%, Re 0.001%~0.055%, Hf 0~0.01%, and the balance is Fe and inevitable impurities.

2. A high-strength anchor rod according to claim 1, characterized in that: The sum of the weight percentages of Y and Re is 0.075%≤Y+Re≤0.12%.

3. A high-strength anchor rod according to claim 2, characterized in that: The ratio of Y to Re is 0.8≤Y / Re≤1.

5.

4. A high-strength anchor rod according to claim 1, characterized in that: The weight percentage of Hf is 0.005% to 0.008%.

5. A process for preparing a high-strength anchor rod according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. After the ingredients are prepared, the anchor blank is obtained by smelting, refining and continuous casting; S2. The anchor rod blank is subjected to heat treatment to obtain a high-strength anchor rod.

6. The process for preparing a high-strength anchor rod according to claim 5, characterized in that: The heat treatment includes normalizing, annealing, quenching and tempering.

7. The process for preparing a high-strength anchor rod according to claim 6, characterized in that: The normalizing temperature is 850-870°C, and the holding time is 4-5h.

8. The process for preparing a high-strength anchor rod according to claim 6, characterized in that: The annealing temperature is 650-680° C., and the holding time is 7-8 hours.

9. The process for preparing a high-strength anchor rod according to claim 6, characterized in that: The quenching temperature is 830-850° C., and the holding time is 3-4 hours.

10. The process for preparing a high-strength anchor rod according to claim 6, characterized in that: The tempering temperature is 290-310° C., and the holding time is 3-4 hours.