Preparation method of S-shaped steel wire with good corrosion resistance
By changing the contact surface of hot-dip galvanized steel wire to surface contact, and using hot-dip multi-alloy and multi-pass rolling process, a uniform thickness corrosion-resistant layer is formed, which solves the problem of S-shaped steel wire being easily corroded under stress, significantly improving the problem of S-shaped steel wire being easily corroded under stress. Corrosion resistance and service life.
Patent Information
- Application Number
- CN202411201203.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
Existing S-shaped hot-dip galvanized steel wires are prone to cracking under long-term stress working conditions, resulting in corrosion of the coating and short life, limiting its application.
By changing the contact surface of the hot-dip galvanized steel wire from linear to surface contact, a hot-dip multi-alloy is used, combined with annealing, multi-pass rolling, electrolytic pickling, auxiliary plating and finishing processes, a corrosion-resistant layer of uniform thickness is formed. Improve the coverage and stability of the coating.
The corrosion resistance of S-shaped steel wire is significantly improved, and the corrosion resistance rate of the coating is reduced from 30.376g/72h to 8.642g/72h, extending the service cycle and ensuring that the bridge is in normal working condition.
Smart Images

Figure CN119082651A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing an S-shaped steel wire, and in particular to a method for preparing an S-shaped steel wire with good corrosion resistance, which is more suitable for preparing a corrosion-resistant S-shaped steel wire with a cross-sectional size of 3 to 3.2×7 to 7.2 mm. Background Art
[0002] S-shaped steel wire is a special-shaped steel wire with an S-shaped axial cross-section. This shape has the advantages of uniform cross-section and high product quality. Compared with traditional round steel wire, S-shaped steel wire changes the contact mode between winding steel wires and between winding steel wires and main cable steel wires through the mutual bite between steel wires, that is, from point contact to line surface contact. Compared with the mutual contact between traditional round steel wires, this change in contact mode can prevent the invasion of moisture and atmospheric pollutants and the cracking of the outer coating film caused by changes in cable length due to temperature changes. Therefore, it is widely used in the fuselage winding of large forging equipment, the winding of main cable steel wires of suspension bridges, and the winding of aircraft cabins.
[0003] The production method of S-shaped hot-dip galvanized steel wire in the prior art, such as the Chinese patent application (publication number CN116371913A), although this technology improves the galvanizing pass rate of S-shaped steel wire, cannot overcome the problems that the coating of hot-dip galvanized steel wire is easy to crack under long-term stress working conditions, the steel wire is easy to be corroded, and the service life is short, which restricts the application of S-shaped steel wire. Summary of the invention
[0004] The purpose of the present invention is to address the problem of easy corrosion caused by linear contact on the contact surface of hot-dip galvanized S-shaped steel wire. Since the hot-dip galvanized intermediate alloy layer is a hard and brittle Fe-Zn phase layer, the hot-dip galvanized steel wire used for bridge cables is prone to cracks at the coating interface under stress working conditions for a long time, causing the steel wire to be frequently corroded. The present invention provides a method for preparing an S-shaped steel wire with good corrosion resistance, in which the contact surface of the hot-dip multi-alloy S-shaped steel wire is changed from linear to surface contact, that is, the contact surface is increased, and the corrosion-resistant layer caused by the contact surface is fully covered and has uniform thickness, so that the corrosion resistance rate of the S-shaped steel wire is increased from the existing 30.376g / 72h to 8.642g / 72h, thereby ensuring that the bridge is in normal working condition for a long time and prolonging the service life.
[0005] Technical measures to achieve the above objectives
[0006] A method for preparing an S-shaped steel wire with good corrosion resistance, comprising the following steps:
[0007] 1) Annealing a wire rod having a diameter of 4.5 to 5.5 mm and a carbon content not exceeding 0.13 wt %, and controlling:
[0008] The annealing temperature is 750-850°C and kept at this temperature for 60-300s;
[0009] 2) cooling to room temperature at a cooling rate of 20 to 30°C / s;
[0010] 3) Rolling is performed in seven to eight passes to the finished product specifications, and each pass is performed according to the following reduction rate distribution:
[0011] The first pass is rolled according to 10-15% of the wire rod diameter;
[0012] The second pass is rolled according to 8 to 10% of the cross-sectional size after the first pass;
[0013] The third pass is rolled according to 5-8% of the cross-sectional size after the second pass;
[0014] The fourth pass is rolled at 1 to 5% of the cross-sectional size after the third pass;
[0015] The fifth pass is rolled according to 0.8 to 1% of the cross-sectional size after the fourth pass;
[0016] The sixth pass is rolled at 0.6-0.8% of the cross-sectional size after the fifth pass;
[0017] The seventh pass is to roll the finished product according to 0.3-0.6% of the cross-sectional size after the sixth pass;
[0018] When the eighth rolling pass is required, the rolling is performed at a rolling rate of 0.1 to 0.3%.
[0019] 4) electrolytic pickling, the pickling solution is a pickling solution containing sulfuric acid at a concentration of 20 to 25 wt%, and the pickling temperature is 65 to 75° C.;
[0020] 5) Rinse with hot water at a temperature of 70-90°C;
[0021] 6) performing auxiliary plating in an auxiliary plating solution having an ammonium chloride concentration of 10 to 20%, and controlling the auxiliary plating temperature at 80 to 90° C.;
[0022] 7) Use alloy solution for hot-dip coating, the hot-dip coating temperature is controlled at 440-460℃, and the running speed of the steel wire is
[0023] At 10-13 m / min, the coating thickness is 0.08-0.1 mm;
[0024] 8) Cool naturally to room temperature;
[0025] 9) Perform finishing with a finishing rate of 0.1 to 0.3%.
[0026] Preferably, the pickling temperature is between 65 and 71°C.
[0027] Preferably, the plating assist temperature is between 83 and 87°C.
[0028] Preferably, the hot-dip temperature is controlled at 445-456°C.
[0029] Preferably: the composition of the alloy solution: pure Zn solution; or
[0030] A mixed solution of Zn and Al, wherein: Zn is 80-95wt% and Al is 5-20wt%; or
[0031] A mixed solution of Zn, Al, Mg and RE, wherein: Zn: 80-89wt%, Al: 9.5-20wt%, Mg:
[0032] 1~5wt%, RE; 0.01~0.5wt%.
[0033] Function and principle of the main process of the present invention
[0034] The reason why the present invention controls the annealing temperature of the wire rod to 750-850°C and keeps it at this temperature for 60-300s is to avoid excessive growth of austenite grains at high temperatures, while ensuring that the wire rod obtains good softening and uniform structure after annealing, eliminates internal stress, and improves mechanical properties.
[0035] The present invention adopts seven to eight passes to roll to the finished product specifications, and each pass is specifically performed according to the following reduction rate distribution:
[0036] The first pass is rolled according to 10-15% of the wire rod diameter;
[0037] The second pass is rolled according to 8 to 10% of the cross-sectional size after the first pass;
[0038] The third pass is rolled according to 5-8% of the cross-sectional size after the second pass;
[0039] The fourth pass is rolled at 1 to 5% of the cross-sectional size after the third pass;
[0040] The fifth pass is rolled according to 0.8 to 1% of the cross-sectional size after the fourth pass;
[0041] The sixth pass is rolled at 0.6-0.8% of the cross-sectional size after the fifth pass;
[0042] The seventh pass is to roll the finished product according to 0.3-0.6% of the cross-sectional size after the sixth pass;
[0043] When the eighth rolling pass is required, rolling is carried out at a rolling rate of 0.1-0.3%. This is because the stress and strain increase gradually in multiple rolling passes, which can reduce the possibility of cracks in the steel wire or breakage of the steel wire due to stress concentration. At the same time, the grains can be refined to improve the mechanical properties and toughness of the material.
[0044] The present invention adopts a pickling solution containing 20-25wt% sulfuric acid and a pickling temperature of 65-75°C because such a pickling solution and pickling temperature can remove surface impurities, improve surface quality, and make the surface of the steel wire uniform and clean white.
[0045] The reason why the present invention controls the plating to be carried out in a plating solution with an ammonium chloride concentration of 10-20% and controls the plating temperature to be 80-90° C. is to ensure that the plating solution has appropriate activity and stability to prevent excessive corrosion of the steel wire surface.
[0046] The reason why the hot-dip temperature is controlled at 440-460°C and the coating thickness is made 0.08-0.1mm when the running speed of the steel wire is 10-13m / min is that these process parameters help the zinc liquid to better penetrate into the concave part of the steel wire hook head to form a dense and uniform coating, thereby improving the corrosion resistance and service life of the steel wire.
[0047] The reason why the present invention controls the finishing rate to be 0.1-0.3% to finish the S-shaped steel wire after hot-dip galvanizing is to further remove tiny flaws, oxides or other impurities on the surface of the steel wire after hot-dip galvanizing, so as to make the surface of the steel wire smoother and more uniform, thereby improving the appearance quality and anti-corrosion performance of the product.
[0048] Compared with the prior art, the contact surface of the hot-dip multi-alloy S-shaped steel wire of the present invention is changed from linear to surface contact, and the contact surface is increased. The corrosion-resistant layer caused by this has comprehensive coverage and uniform thickness, so that the corrosion resistance rate of the S-shaped steel wire is increased from the existing 30.376g / 72h to 8.642g / 72h, thereby ensuring that the bridge is in normal working condition for a long time and improving the service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 The state diagram of the deformation of each pass in the S-shaped steel wire rolling process of the present invention using a total of seven passes;
[0050] Figure 2 This is a state diagram of the deformation of each pass in which the S-shaped steel wire is rolled in eight passes in the present invention. DETAILED DESCRIPTION
[0051] The present invention is further described in detail below
[0052] Table 1 is a list of parameter values of the main processes of various embodiments and comparative examples of the present invention using seven or eight passes;
[0053] Table 2 is a list of the effects obtained by the components and contents of the lotions used in the embodiments of the present invention and the comparative examples;
[0054] Table 3 is a table of the effects of various embodiments and comparative examples of the present invention.
[0055] Each embodiment of the present invention is prepared according to the following steps:
[0056] 1) Annealing a wire rod having a diameter of 4.5 to 5.5 mm and a carbon content not exceeding 0.13 wt %, and controlling:
[0057] The annealing temperature is 750-850°C and kept at this temperature for 60-300s;
[0058] 2) cooling to room temperature at a cooling rate of 20 to 30°C / s;
[0059] 3) Rolling is performed in seven to eight passes to the finished product specifications, and each pass is performed according to the following reduction rate distribution:
[0060] The first pass is rolled according to 10-15% of the wire rod diameter;
[0061] The second pass is rolled according to 8 to 10% of the cross-sectional size after the first pass;
[0062] The third pass is rolled according to 5-8% of the cross-sectional size after the second pass;
[0063] The fourth pass is rolled at 1 to 5% of the cross-sectional size after the third pass;
[0064] The fifth pass is rolled according to 0.8 to 1% of the cross-sectional size after the fourth pass;
[0065] The sixth pass is rolled at 0.6-0.8% of the cross-sectional size after the fifth pass;
[0066] The seventh pass is to roll the finished product according to 0.3-0.6% of the cross-sectional size after the sixth pass;
[0067] When the eighth rolling pass is required, the rolling is performed at a rolling rate of 0.1 to 0.3%.
[0068] 4) electrolytic pickling, the pickling solution is a pickling solution containing sulfuric acid at a concentration of 20 to 25 wt%, and the pickling temperature is 65 to 75° C.;
[0069] 5) Rinse with hot water at a temperature of 70-90°C;
[0070] 6) performing auxiliary plating in an auxiliary plating solution having an ammonium chloride concentration of 10 to 20%, and controlling the auxiliary plating temperature at 80 to 90° C.;
[0071] 7) Use alloy solution for hot-dip coating, the hot-dip coating temperature is controlled at 440-460℃, and the running speed of the steel wire is
[0072] At 10-13 m / min, the coating thickness is 0.08-0.1 mm;
[0073] 8) Cool naturally to room temperature;
[0074] 9) Perform finishing with a finishing rate of 0.1 to 0.3%.
[0075] Table 1 List of parameter values of main processes of various embodiments and comparative examples of the present invention
[0076]
[0077] Table 2 List of effects obtained by various embodiments of the present invention and comparative examples
[0078]
[0079] Table 3 Effect list of various embodiments of the present invention and comparative examples
[0080]
[0081] Corrosion test description: Take 3 samples of each of the above steel wires and place them in a salt spray test box at a temperature of 35℃±2℃, a pH value of 6.5-7.2, and a sodium chloride solution concentration of 50g / L±5g / L for a 72-hour corrosion resistance test. After the test time reaches the specified cycle time, soak in a 20% (mass fraction) analytical grade diammonium citrate aqueous solution at 23℃ for 10 minutes. After soaking, wash the sample with water at room temperature, then wash with ethanol, and dry. Weigh each steel wire after the salt spray test and record the data as the weight after the test, and then dissolve the coating on the steel wire. Dissolve 3.5g of chemically pure hexamethylenetetramine in 500ml of concentrated hydrochloric acid, dilute to 1000ml with deionized water, and record the mass of the bare steel wire after the coating is dissolved as the weight after the coating is dissolved.
[0082] From the results in Table 3, it can be clearly seen that compared with the pure zinc coating, the multi-element alloy coating has better corrosion resistance, and with the reduction of Zn content in the alloy coating and the increase of elements such as Al, Mg, and RE, the corrosion resistance of the coating gradually increases, and the corrosion resistance can be increased by about 71.5% at most. In addition, it can be seen from the comparison between the embodiments that increasing the rolling pass can also appropriately increase the corrosion resistance of the S-shaped steel wire.
[0083] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A method for preparing an S-shaped steel wire with good corrosion resistance, comprising the following steps: 1) annealing a wire rod having a diameter of 4.5 to 5.5 mm and a carbon content not exceeding 0.13 wt %, and controlling the annealing temperature to be 750 to 850° C. and keeping the temperature at this temperature for 60 to 300 seconds; 2) cooling to room temperature at a cooling rate of 20 to 30°C / s; 3) Rolling is performed in seven to eight passes to the finished product specifications, and each pass is performed according to the following reduction rate distribution: The first pass is rolled according to 10-15% of the wire rod diameter; The second pass is rolled according to 8 to 10% of the cross-sectional size after the first pass; The third pass is rolled according to 5-8% of the cross-sectional size after the second pass; The fourth pass is rolled at 1 to 5% of the cross-sectional size after the third pass; The fifth pass is rolled according to 0.8 to 1% of the cross-sectional size after the fourth pass; The sixth pass is rolled at 0.6-0.8% of the cross-sectional size after the fifth pass; The seventh pass is to roll the finished product according to 0.3-0.6% of the cross-sectional size after the sixth pass; When the eighth rolling pass is required, the rolling is performed at a rolling rate of 0.1 to 0.3%. 4) electrolytic pickling, the pickling solution is a pickling solution containing sulfuric acid at a concentration of 20 to 25 wt%, and the pickling temperature is 65 to 75° C.; 5) Rinse with hot water at a temperature of 70-90°C; 6) performing auxiliary plating in an auxiliary plating solution having an ammonium chloride concentration of 10 to 20%, and controlling the auxiliary plating temperature at 80 to 90° C.; 7) hot-dip coating is performed using alloy solution, the hot-dip coating temperature is controlled at 440-460°C, and the coating thickness is 0.08-0.1 mm at a running speed of 10-13 m / min for the steel wire; 8) Cool naturally to room temperature; 9) Perform finishing with a finishing rate of 0.1 to 0.3%.
2. The method for preparing an S-shaped steel wire with good corrosion resistance as claimed in claim 1, characterized in that: The pickling temperature is between 65 and 71°C.
3. The method for preparing an S-shaped steel wire with good corrosion resistance according to claim 1, characterized in that: The auxiliary plating temperature is between 83 and 87°C.
4. The method for preparing an S-shaped steel wire with good corrosion resistance according to claim 1, characterized in that: The hot-dip temperature is controlled at 445-456°C.
5. The method for preparing an S-shaped steel wire with good corrosion resistance as claimed in claim 1, characterized in that: Composition of the alloy solution: pure Zn solution; or A mixed solution of Zn and Al, wherein: Zn is 80-95wt% and Al is 5-20wt%; or A mixed solution of Zn, Al, Mg and RE, wherein: Zn: 80-89wt%, Al: 9.5-20wt%, Mg: 1-5wt%, RE; 0.01-0.5wt%.
Citation Information
Patent Citations
Method for manufacturing explosion-proof cage for blindage made of zinc-aluminum-magnesium coated steel wires
CN115401079A
Technological process for manufacturing S-shaped hot-dip galvanized steel wire
CN116371913A