Preparation method of carbon nanotube loaded bimetallic nano-catalyst
Through the preparation method of loading bimetallic nanocatalysts on carbon nanotubes, the problems of catalyst poisoning and small specific surface area in the selective oxidation reaction of ethylene glycol are solved, and efficient glycolic acid generation and hydrogen cogeneration are achieved, which improves the catalyst Activity and application performance.
Patent Information
- Application Number
- CN202310653729.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the catalyst is easily adsorbed by CO toxic intermediates in the selective oxidation reaction of ethylene glycol, and the small specific surface area of multi-walled carbon nanotubes affects its application performance, limiting the electrocatalytic alcohol oxidation reaction. efficiency and scalability in.
The preparation method of carbon nanotube-supported bimetallic nanocatalyst is adopted. Through ultrasonic dispersion, ball milling treatment and magnetic field guidance technology, the specific surface area of carbon nanotubes and the uniform distribution of metal nanoparticles are improved, forming a highly active PtAg catalyst for alkaline use. Selective oxidation of ethylene glycol was carried out under the conditions of nature.
The high selective oxidation of ethylene glycol into glycolic acid and the high-value hydrogen reaction is carried out in conjunction with hydrogen evolution, which improves the activity and application prospects of the catalyst and simplifies the separation process of the product and the catalyst.
Smart Images

Figure CN119082776A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrocatalysis and relates to a high-activity bimetallic nanocatalyst for selectively electrocatalyzing oxidation of ethylene glycol to glycolic acid under alkaline conditions and a preparation method thereof. Background Art
[0002] Electrocatalytic alcohol oxidation reaction (AOR) is one of the important electrocatalytic reactions, which can be coupled with other electrocatalytic reduction reactions to form reaction systems with different functions. For example, when AOR is combined with oxygen reduction reaction, direct alcohol fuel cells can produce high value-added organic acids and clean energy. When AOR is coupled with water reduction reaction (hydrogen evolution reaction), organic acids (or their salt form precursors) as biodegradable plastic monomers and hydrogen as clean energy carriers can also be obtained simultaneously, and the energy consumption is lower than that of water decomposition reaction. Glycolic acid, as a biodegradable plastic monomer and an important ingredient in cosmetics, can be produced by selectively oxidizing one end of the primary hydroxyl group of ethylene glycol. In the thermocatalytic process of selective oxidation of ethylene glycol, the main byproduct is water because oxygen is used as the oxidant. Since the catalyst is uniformly dispersed in the reaction solution in this process, additional processes are required to separate the products and recover the catalyst after the reaction. Platinum and platinum alloy materials have attracted widespread attention due to the rapid development of fuel cell technology. Platinum-based nanocatalysts also have important research value in the field of catalysis due to their unique physical and chemical properties, and are considered to be the best catalysts for alcohol oxidation reactions in acidic and alkaline media. However, there are several disadvantages of platinum metal that prevent it from being used commercially on a large scale: first, the reserves of platinum metal on Earth are low and its price is relatively expensive; second, during the catalytic oxidation of alcohols, platinum metal easily adsorbs toxic intermediates such as CO, which hinders the further adsorption and oxidation of small molecule alcohols on its surface, resulting in poisoning.
[0003] Carbon nanotubes (CNTs) are an important nanomaterial with good electrical, mechanical and structural properties. They not only have important application value in biomedicine, catalysts, sensors, etc., but also serve as carriers of precious metal nanoparticles to enhance their electrocatalytic activity. In addition, compared with traditional carbon materials, carbon nanotubes have a nanoscale microstructure, a small radial dimension, an adjustable lumen structure, a large specific surface area, unique electronic properties, excellent conductivity, the ability to promote electron transfer, good stability, active groups on the surface, strong chemical activity, and are conducive to surface functionalization. The main methods for preparing carbon nanotubes include arc method, chemical vapor deposition method, laser evaporation method, solar method, and low-temperature solid-state pyrolysis method. However, the common disadvantage of the carbon nanotubes prepared by the above methods is that the specific surface area is small, especially for multi-walled carbon nanotubes. If they are not specially treated, the specific surface area is generally not more than 200m 2 / g, which seriously affects the application performance of carbon nanotubes in adsorption separation, carrier, electrode, etc.
[0004] CN 107715874 B discloses a method for preparing a platinum-based catalyst co-modified with La and Al loaded on multi-walled carbon nanotubes, and the catalyst is applied to a glycerol hydrogenation reaction, and has a high glycerol conversion rate and 1,3-propylene glycol selectivity.
[0005] CN 113457672 A discloses a preparation method of a multi-walled carbon nanotube-supported platinum-based catalyst, and the multi-walled carbon nanotube-supported platinum-based catalyst can stabilize the conversion rate of furfural at 85% and the selectivity of furfuryl alcohol at 95% under the conditions of room temperature, hydrogen and normal pressure, wherein the number of carbon nanotube layers is about 15.
[0006] In the study of multi-walled carbon nanotube-loaded palladium (II) catalyst catalyzing the Suzuki-Miyaura reaction, short hydroxyl multi-walled carbon nanotubes with a purity of ≥95%, a diameter of 5-15nm, an inner diameter of 2-5nm, an outer diameter of less than 8nm, and a length of 0.5-2μm were used to load Pd. The number of carbon nanotube layers was about 8. It was found that the catalyst Pd-MWNTs can effectively catalyze the Suzuki-Miyaura coupling reaction of different substrates and obtain high yields.
[0007] Electrochimica Acta (2008, 53: 7807–7811) used a purity of ≥95% and a specific surface area of 40–300 m 2 / g, 10-20nm in diameter, 5-15μm in length multi-walled carbon nanotubes loaded with PtRu alloy, the number of carbon nanotube layers is about 6, the study found that Pt-Ru / CNTs catalyst exhibits better methanol oxidation activity than commercial Pt-Ru / C catalyst. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention provides a method for preparing a carbon nanotube-loaded bimetallic nanocatalyst. The catalyst prepared by the method of the present invention has high selectivity in the electrocatalytic selective oxidation of ethylene glycol to glycolic acid. At the same time, combined with the hydrogen evolution reaction, high-value hydrogen can be co-produced, and the catalyst has good prospects for promotion and application.
[0009] The preparation method of carbon nanotube-supported bimetallic nanocatalyst of the present invention comprises the following contents: (1) adding multi-walled carbon nanotubes into alkaline solution and mixing them by ultrasonic dispersion to obtain a black suspension; (2) subjecting the black suspension of step (1) to solid-liquid separation and drying to obtain adsorbed carbon nanotubes; (3) subjecting the carbon nanotubes obtained in step (2) to ball milling treatment, followed by washing, drying and roasting; (4) adding the roasted carbon nanotubes into water and subjecting them to ultrasonic dispersion treatment to obtain a black suspension; (5) adding a platinum-containing compound and a silver-containing compound into water to prepare a precursor solution, and adding a reducing agent thereto to reduce metal ions to simple substances; and (6) adding the suspension obtained in step (4) into the precursor solution of step (5) at room temperature, and mixing and reacting for a period of time under an external magnetic field, filtering, washing and drying to obtain the carbon nanotube-supported bimetallic nanocatalyst.
[0010] In the method of the present invention, the carbon nanotubes described in step (1) are commercially available multi-walled carbon nanotubes with a purity of >90%; the number of layers is 10 to 60, preferably 20 to 40; the inner diameter is 2 to 40 nm, preferably 5 to 20 nm; and the length is 2000 to 20000 nm, preferably 3000 to 10000 nm.
[0011] In the method of the present invention, the alkali solution in step (1) comprises an inorganic base, water, a low-carbon alcohol and an amide; the mass percentages of the components based on the mass of the alkali solution are: 10%-40% of the inorganic base, 40%-80% of water, 5%-20% of the low-carbon alcohol and 1%-10% of the amide.
[0012] Among them, the inorganic base is sodium hydroxide and / or potassium hydroxide; the low-carbon alcohol is a monohydric alcohol and a polyhydric alcohol with a carbon number not greater than 5, preferably one or more of methanol, ethanol or propanol; the amide is one or more of formamide, acetamide or dimethylformamide.
[0013] In the method of the present invention, the amount of the alkali solution in step (1) is sufficient to fully wet the carbon nanotube powder, and the final alkali loading is 10%-100% of the mass of the carbon nanotubes. It is further preferred that the impregnation solid-liquid mass ratio is determined according to the equal volume impregnation method, and the alkali loading is 30%-50%.
[0014] In the method of the present invention, the ultrasonic dispersion treatment conditions in step (1) are: ultrasonic treatment time is 5-60 minutes, ultrasonic power is 40-720W, ultrasonic frequency is 20-100kHz, and ultrasonic temperature is 5-90°C. The ultrasonic dispersion treatment conditions are preferably: time is 10-30 minutes, power is 40-100W, ultrasonic frequency is 20-60kHz, and ultrasonic temperature is 10-60°C.
[0015] In the method of the present invention, the solid-liquid separation in step (2) is a conventional dry method, including but not limited to filtration, centrifugation, precipitation and the like; the drying conditions are: drying temperature 30-200°C, drying time 1-24 hours, preferably drying temperature 100-150°C, drying time 3-12 hours. More preferably, vacuum drying is performed, and the operating conditions are: pressure 0-100 Pa, temperature 20-200°C, time 3-24 hours, preferably pressure 0-40 Pa, temperature 100-150°C, time 6-12 hours.
[0016] In the method of the present invention, the ball milling treatment conditions in step (3) are: ball milling speed of 200-5000 r / min, ball to material mass ratio of 25-500:1, and ball milling time of 2-48 hours. Preferably, the ball milling speed is 200-3000 r / min, the ball to material mass ratio is 50-300:1, and the ball milling time is 6-12 hours.
[0017] In the method of the present invention, the washing in step (3) is a conventional process, preferably using water for washing until the washing liquid is neutral or nearly neutral. The drying conditions are: temperature 100-150°C, time 6-12 hours. The roasting conditions are: under the protection of an inert atmosphere, temperature 300-800°C, preferably 450-650°C, time 1-12 hours, preferably time 3-6 hours; wherein the inert atmosphere is an inert gas and / or nitrogen.
[0018] In the method of the present invention, the solid-liquid mass ratio of the carbon nanotube suspension in step (4) is 1:(3-10).
[0019] In the method of the present invention, the ultrasonic dispersion treatment conditions in step (4) are: ultrasonic treatment time is 5 to 10 minutes, ultrasonic power is 80 to 720 W, ultrasonic frequency is 30 to 50 KHz, and ultrasonic temperature is 20 to 25°C.
[0020] In the method of the present invention, the molar ratio of the platinum-containing compound, the silver-containing compound, the reducing agent and water in step (5) is (0.3-3):1:(0.3-15):(4.5-75), preferably (0.3-3):1:(0.6-10):(5-40).
[0021] In step (5) of the present invention, the platinum-containing compound is chloroplatinic acid, platinum chloride, platinum acetylacetonate, sodium chloroplatinite, sodium hexachloroplatinate, etc., preferably chloroplatinic acid; the silver-containing compound is silver nitrate, silver chloride, silver sulfate, silver oxide, etc., preferably silver nitrate.
[0022] In step (5) of the present invention, the reducing agent is potassium borohydride, sodium borohydride, lithium aluminum hydride, ascorbic acid, etc., preferably potassium borohydride.
[0023] In the method of the present invention, the amounts of the precursor solution and the carbon nanotube suspension in step (5) are prepared so that the theoretical total metal loading on the carbon nanotubes is 5 to 25.0 wt.%.
[0024] In the method of the present invention, step (5) is preferably performed by ultrasonic dispersion to accelerate dissolution.
[0025] In the method of the present invention, the strength of the external magnetic field in step (6) is 0.1 to 5 T, more preferably 2 to 4 T, and the ratio of the magnetic field strength to potassium borohydride in moles is 0.3 to 1.5:1. Under the combined action of the magnetic field and the reducing agent, the metal element can be better loaded on the carbon nanotubes.
[0026] In the method of the present invention, the mixing reaction described in step (6) can be carried out by mechanical stirring and ultrasonic dispersion, the mixing reaction time is 12 to 24 hours, and the mixing reaction temperature is 20 to 25°C. The conditions of mechanical stirring and ultrasonic dispersion are not particularly limited, the mechanical stirring is preferably 50 to 1000 rpm, and the ultrasonic dispersion conditions are preferably: ultrasonic power 240 to 480 W, ultrasonic frequency 30 to 50 KHz. In the method of the present invention, the bimetallic catalyst PtAg in step (6) has an alloy structure, and the size of the alloy nanoparticles is 3 to 6 nm.
[0027] The invention discloses an application of a carbon nanotube-loaded bimetallic nanocatalyst in the electrocatalytic selective oxidation of ethylene glycol to generate glycolic acid. The invention adopts a highly active bimetallic nanocatalyst as an anode catalyst, a mercury-mercury oxide electrode as a reference electrode, and nickel foam as a counter electrode. The reaction conditions are: a voltage of -0.33 to -0.48 V and a reaction time of 2 to 4 hours.
[0028] Compared with the prior art, the method of the present invention has the following advantages: the alkaline solution containing low-carbon alcohol and amide can reduce the surface tension of the solution, so that the alkali can be evenly dispersed on the inner and outer surfaces of the carbon nanotubes, which is conducive to improving the uniformity of ball milling modification; the local high temperature generated by ball milling extrusion is used to make the alkali etch the carbon nanotubes to produce defects, thereby increasing the specific surface area of the carbon tubes. By adjusting the magnetic field intensity and the reducing agent concentration to control the growth process of metal nanoparticles on multi-walled carbon nanotubes, the carbon-carbon cracking caused by the dissociative adsorption of C2 substances on adjacent active sites can be more effectively reduced, and the conversion of aldehyde-containing intermediates to carboxylates can be promoted, further achieving high catalytic performance of electrocatalytic selective oxidation of ethylene glycol to glycolic acid under alkaline conditions.
[0029] The method of the present invention is simple to operate and has a mild reaction. The prepared catalyst is not easy to agglomerate. In addition, the electrocatalytic material participates in the reaction process in the form of an electrode (similar to a fixed catalyst bed), which simplifies the separation of the reaction products and the catalyst, and opens up a new path for the electrocatalytic cogeneration of high-value chemicals and H2. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 TEM image of PtAg / high specific surface area carbon nanotubes. DETAILED DESCRIPTION
[0031] The present invention will be described in more detail through examples, but the protection scope of the present invention is not limited to these examples. The successful synthesis of the PtAg alloy phase was confirmed by X-ray diffraction (XRD) test, the metal loading on the carbon nanotubes was tested by ICP, and the PtAg / high specific surface area carbon nanotubes were characterized by transmission electron microscopy. Example 1
[0032] Prepare alkali solution, weigh a certain amount of potassium hydroxide, water, ethanol, and formamide, and the proportion of each component by mass is: 40% potassium hydroxide, 60% water, 10% ethanol, and 5% formamide. Immerse the carbon nanotubes in the alkali solution and use an ultrasonic disperser (100W, 40kHz) to disperse them at room temperature (20°C) for 10 minutes. The amount of alkali solution must ensure that the carbon nanotube powder can be fully wetted. The carbon nanotubes used are commercially available products with an average length of 10.2μm, an inner diameter of 8nm, a wall thickness of 4.8nm, an aspect ratio of 607, and a specific surface area of 39 m 2 / g. After the carbon nanotubes fully absorb the alkali solution, they are filtered and then dried at 150°C for 6 hours. Calculated based on the dried carbon nanotubes, the final alkali loading is 45% of the mass of the carbon nanotubes. The dried carbon nanotube powder is put into a ball mill for grinding, with a ball-to-material mass ratio of 200:1, a rotation speed of 2000r / min, and a ball milling time of 8 hours. After grinding, it is thoroughly washed with distilled water, filtered, dried at 120°C for 12 hours, and then calcined at 600°C for 3 hours under nitrogen protection. After natural cooling, the high specific surface carbon nanotubes are obtained. After testing, the average length is 8.3μm, the inner diameter of the tube is 7.3nm, the wall thickness is 4.4nm, the aspect ratio of the nanotube is 531, and the specific surface area is 1093m 2 / g.
[0033] Weigh a certain amount of high specific surface carbon nanotubes and mix them with water (solid-liquid mass ratio is 1:5) under ultrasonic dispersion conditions (ultrasonic power 240W, ultrasonic frequency 40KHz) at room temperature. A uniformly dispersed black suspension is obtained in 10 minutes. Chloroplatinic acid and silver nitrate are completely dissolved in water under ultrasound to obtain a precursor solution, and potassium borohydride is added thereto to obtain a mixed solution. In terms of molar amount, the ratio of each material is 1:1:2:20. The carbon nanotube suspension is added to the mixed solution under stirring, and the beaker is placed in a magnetic field with an intensity of 3T set by a superconducting coil and reacted for 24 hours. The final suspension is filtered and washed with ultrapure water several times to ensure that there are no impurities. The obtained black solid particles are dried at 40°C for 12 hours to finally obtain a PtAg / high specific surface area carbon nanotube catalyst with a total metal loading of 15.0wt.%. From Figure 1 It can be observed that the PtAg nanoparticles are dispersed relatively evenly in the carbon nanotubes, and the size of the alloy particles is 4.2 nm.
[0034] The PtAg / high specific surface area carbon nanotube catalyst prepared as above was used as the working electrode to test the catalytic performance of selective oxidation of ethylene glycol to glycolic acid under alkaline conditions. The PtAg / high specific surface area carbon nanotube catalyst was made into a working electrode. The specific method of the electrocatalytic selective oxidation of ethylene glycol to glycolic acid reaction is: using a highly active bimetallic nanocatalyst as an anode catalyst, a mercury-mercury oxide electrode as a reference electrode, and nickel foam as a counter electrode, and the reaction conditions are: at a voltage of -0.33 to -0.48 V, the reaction is 2 to 4 hours.
[0035] The catalytic test results show that PtAg / high specific surface area carbon nanotubes have high catalytic activity for the electrocatalytic oxidation of ethylene glycol to produce glycolic acid: the ethylene glycol conversion rate can reach 60.2%, and the selectivity of glycolic acid can reach 90.5%. Example 2
[0036] The preparation method of high specific surface carbon nanotubes and metal precursor solution is the same as that of Example 1, except that the ultrasonic power is 150 W, the solid-liquid mass ratio of high specific surface carbon nanotubes to water is 1:3, the molar ratio of platinum-containing compound, silver-containing compound, reducing agent and water is 0.5:1:2:10, and other conditions remain unchanged. The ethylene glycol conversion rate is 53.6%, and the selectivity of glycolic acid is 73.4%. Example 3
[0037] The preparation method of high specific surface carbon nanotubes and metal precursor solution is the same as that of Example 1, except that the ultrasonic power is 360 W, the solid-liquid mass ratio of high specific surface carbon nanotubes to water is 1:10, the molar ratio of platinum-containing compound, silver-containing compound, reducing agent and water is 2:1:6:15, and other conditions remain unchanged. The ethylene glycol conversion rate is 55.3%, and the selectivity of glycolic acid is 81.2%.
[0038] Comparative Example 1 The same as Example 1, except that no amide was added during the treatment of multi-walled carbon nanotubes, and other conditions remained unchanged. The ethylene glycol conversion rate was 51.7%, and the selectivity of glycolic acid was 78.4%.
[0039] Comparative Example 2 The same as Example 1, except that commercially available multi-walled carbon nanotubes that have not been treated with alkali solution are directly used as carriers, and other conditions remain unchanged. The ethylene glycol conversion rate is 48.4%, and the selectivity of glycolic acid is 67.8%.
[0040] Comparative Example 3 The same as Example 1, except that the ratio of magnetic field strength to potassium borohydride in moles is 3:1, and other conditions remain unchanged. The ethylene glycol conversion rate is 50.5%, and the selectivity of glycolic acid is 72.1%.
[0041] Comparative Example 4 The same as Example 1, except that the magnetic field strength was set to 0 T by the superconducting coil, and other conditions remained unchanged. The ethylene glycol conversion rate was 49.9%, and the selectivity of glycolic acid was 70.6%.
[0042] Comparative Example 5 CN 109713323 B uses an impregnation and thermal reduction method to prepare a supported alloy catalyst, and the reaction conditions are high temperature; the article International Journal of Hydrogen Energy (2022, 47: 30147-30159.) uses a sonochemical method to prepare a platinum-silver catalyst supported on carbon nanotubes. The operating conditions are simple, but all solvents need to be evaporated to recover the solids, which results in a small loading amount and uneven dispersion.
Claims
1. A method for preparing a carbon nanotube-supported bimetallic nanocatalyst, characterized in that The method comprises the following steps: (1) adding multi-walled carbon nanotubes to an alkaline solution and mixing them by ultrasonic dispersion to obtain a black suspension; (2) subjecting the black suspension of step (1) to solid-liquid separation and drying to obtain adsorbed carbon nanotubes; (3) subjecting the carbon nanotubes obtained in step (2) to ball milling treatment, followed by washing, drying and roasting; (4) adding the roasted carbon nanotubes to water and subjecting them to ultrasonic dispersion treatment to obtain a black suspension; (5) adding a platinum-containing compound and a silver-containing compound to water to prepare a precursor solution, and adding a reducing agent thereto to reduce metal ions to simple substances; and (6) adding the suspension obtained in step (4) to the precursor solution of step (5) at room temperature, mixing and reacting for a period of time under an external magnetic field, filtering, washing and drying to obtain a carbon nanotube-loaded bimetallic nanocatalyst.
2. The method according to claim 1, characterized in that: The carbon nanotubes described in step (1) are commercially available multi-walled carbon nanotubes with a purity of >90%; the number of layers is 10 to 60, preferably 20 to 40; the inner diameter is 2 to 40 nm, preferably 5 to 20 nm; and the length is 2000 to 20000 nm, preferably 3000 to 10000 nm.
3. The method according to claim 1, characterized in that: The alkali solution in step (1) comprises an inorganic base, water, a low-carbon alcohol and an amide; the mass percentage of each component based on the mass of the alkali solution is: 10%-40% of the inorganic base, 40%-80% of water, 5%-20% of the low-carbon alcohol and 1%-10% of the amide.
4. The method according to claim 3, characterized in that: The inorganic base is sodium hydroxide and / or potassium hydroxide; the low-carbon alcohol is a monohydric alcohol or a polyhydric alcohol with a carbon number not greater than 5, preferably one or more of methanol, ethanol or propanol; the amide is one or more of formamide, acetamide or dimethylformamide.
5. The method according to claim 1, characterized in that: The amount of alkali solution used in step (1) must be sufficient to fully wet the carbon nanotube powder, and the final alkali loading is 10%-100% of the mass of the carbon nanotubes. It is further preferred that the impregnation solid-liquid mass ratio is determined according to the equal volume impregnation method, and the alkali loading is 30%-50%.
6. The method according to claim 1, characterized in that: The ultrasonic dispersion treatment conditions in step (1) are as follows: ultrasonic treatment time is 5-60 minutes, ultrasonic power is 40-720W, ultrasonic frequency is 20-100kHz, and ultrasonic temperature is 5-90°C.
7. The method according to claim 1, characterized in that: The drying conditions in step (2) are: drying temperature 30-200° C., drying time 1-24 hours, preferably drying temperature 100-150° C., drying time 3-12 hours.
8. The method according to claim 1, characterized in that: The ball milling conditions in step (3) are as follows: the ball milling speed is 200-5000 r / min, the ball-to-material mass ratio is 25-500:1, and the ball milling time is 2-48 hours.
9. The method according to claim 1, characterized in that: The drying conditions in step (3) are: temperature 100-150°C, time 6-12 hours; the calcination conditions are: under the protection of an inert atmosphere, temperature 300-800°C, time 1-12 hours; wherein the inert atmosphere is an inert gas and / or nitrogen.
10. The method according to claim 1, characterized in that: The solid-liquid mass ratio of the carbon nanotube suspension in step (4) is 1:3-10.
11. The method according to claim 1, characterized in that: The ultrasonic dispersion treatment conditions in step (4) are as follows: ultrasonic treatment time is 5 to 10 minutes, ultrasonic power is 80 to 720 W, ultrasonic frequency is 30 to 50 KHz, and ultrasonic temperature is 20 to 25°C.
12. The method according to claim 1, characterized in that: The molar ratio of the platinum-containing compound, the silver-containing compound, the reducing agent and the water in step (5) is 0.3-3:1:0.3-15:4.5-75.
13. The method according to claim 1, characterized in that: The platinum-containing compound is one or more of chloroplatinic acid, platinum chloride, platinum acetylacetonate, sodium chloroplatinite or sodium hexachloroplatinate; the silver-containing compound is one or more of silver nitrate, silver chloride, silver sulfate or silver oxide.
14. The method according to claim 1, characterized in that: The reducing agent is one or more of potassium borohydride, sodium borohydride, lithium aluminum hydride or ascorbic acid.
15. The method according to claim 1, characterized in that: The amounts of the precursor solution and the carbon nanotube suspension in step (5) are prepared according to the theoretical total metal loading on the carbon nanotubes being 5 to 25.0 wt.%.
16. The method according to claim 1, characterized in that: The strength of the external magnetic field in step (6) is 0.1 to 5 T, more preferably 2 to 4 T, and the ratio of the magnetic field strength to potassium borohydride in moles is 0.3 to 1.5:
1.
17. The method according to claim 1, characterized in that: The bimetallic nanocatalyst PtAg in step (6) has an alloy structure, and the size of the alloy nanoparticles is 3 to 6 nm.
18. Use of a carbon nanotube-supported bimetallic nanocatalyst prepared by the method of any one of claims 1 to 17 in the electrocatalytic selective oxidation of ethylene glycol to produce glycolic acid.
19. The use according to claim 18, characterized in that: The carbon nanotube-loaded bimetallic nanocatalyst is the anode catalyst, the mercury-mercury oxide electrode is the reference electrode, the nickel foam is the counter electrode, and the reaction conditions are: at a voltage of -0.33~-0.48V, the reaction lasts for 2~4 hours.