Polyacrylonitrile pre-oxidized yarn and preparation method thereof

By optimizing the pretreatment and spinning process of polyacrylonitrile oxidized fibers, the problems of insufficient strength and high brittleness in textile processing are solved, and the polyacrylonitrile pre-oxidized yarn with high strength, uniformity and high production rate are achieved Line production.

CN119082966APending Publication Date: 2024-12-06NINGBO JINGZHEN TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411270864.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the textile processing process, polyacrylonitrile pre-oxidized fibers face problems such as insufficient strength, high brittleness, poor clinging force, low yarn count, uneven strips and many yarn defects and low production rate.

Method used

By pretreating polyacrylonitrile oxidized fibers before spinning, pretreating with a health solution to increase the adhesion and friction of the fibers, and by optimizing the process of cleaning, carding, stripping, roving and yarn, including Adjust the distance between the strike point and the grip point, the strike speed and twist coefficient, reduce fiber damage, and improve the strength and uniformity of the yarn.

Benefits of technology

It improves the strength, dry uniformity and production rate of polyacrylonitrile pre-oxidized yarn, reduces the brittleness and yarn defect rate of the yarn, meets the needs of different application scenarios, and improves the quality and processing efficiency of the product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a polyacrylonitrile pre-oxidized yarn and a preparation method thereof. The preparation method comprises the following steps: placing polyacrylonitrile oxidized fibers in a curing room, and uniformly spraying curing liquid for pretreatment to obtain treated polyacrylonitrile pre-oxidized short fibers; the polyacrylonitrile pre-oxidized short fibers are sequentially subjected to opening picking, cotton carding, cotton refining, drawing, roving and spinning treatment, and the polyacrylonitrile pre-oxidized yarn is obtained. The polyacrylonitrile pre-oxidized yarn obtained through the preparation method is high in linear density, even in evenness, few in defect, excellent in mechanical property and capable of meeting application requirements of different scenes. In addition, the preparation method is simple in process, high in feasibility and low in process cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of spinning, in particular to a polyacrylonitrile pre-oxidized yarn and a preparation method thereof. Background Art

[0002] As a high-performance fiber, carbon fiber is widely used in aerospace, sports equipment, automobile manufacturing and other fields. However, due to high production costs and limited production capacity, most of my country's carbon fiber products are in the initial operation stage and cannot meet market demand.

[0003] Polyacrylonitrile (PAN) fiber is a key precursor for the manufacture of carbon fiber. In the process of converting polyacrylonitrile fiber into carbon fiber, two important stages are required: pre-oxidation stabilization and carbonization. In the pre-oxidation stabilization stage, the polyacrylonitrile precursor is converted into a heat-resistant trapezoidal structure through a cyclization and cross-linking reaction to form a polyacrylonitrile pre-oxidized fiber, which exhibits excellent heat resistance and flame resistance, making it have huge market potential in applications such as thermal insulation, fire prevention and flame retardancy. However, as the degree of cyclization of the polyacrylonitrile precursor increases, the flexibility of its molecular chain decreases, resulting in a decrease in the strength of the polyacrylonitrile pre-oxidized fiber, an increase in brittleness, poor cohesion, and easy damage and breakage. This makes the polyacrylonitrile pre-oxidized fiber face many challenges in the textile processing process, such as the low count, insufficient strength, uneven yarn, many yarn defects and low production rate of the fiber yarn prepared by the traditional ring spinning system. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a polyacrylonitrile pre-oxidized yarn and a preparation method thereof, which solves the problems raised in the above-mentioned background technology.

[0006] (II) Technical solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] According to a first aspect of the present invention, there is provided a method for preparing polyacrylonitrile pre-oxidized yarn, comprising the following steps:

[0009] The polyacrylonitrile oxidized fiber is placed in a curing room and sprayed evenly with curing liquid for pretreatment to obtain polyacrylonitrile preoxidized short fiber;

[0010] The polyacrylonitrile preoxidized short fibers are then sequentially subjected to opening and cleaning, carding, refining, drawing, roving and spinning processes to obtain polyacrylonitrile preoxidized yarns.

[0011] The invention sequentially processes the pretreated polyacrylonitrile preoxidized short fibers into opening and cleaning, carding, refining, drawing, roving and spun yarn, and the obtained polyacrylonitrile preoxidized yarn has the characteristics of wide spinnable yarn count range, high strength, few cotton knots and good yarn evenness.

[0012] Preferably, the health care solution comprises an auxiliary agent and water, and the auxiliary agent is selected from a softening oil agent and a hydrophilic penetrating oil agent.

[0013] Specifically, the flexible oil agent is selected from at least one of silicone oil, glyceride, hexadecanol, stearyl alcohol or paraffin;

[0014] The hydrophilic penetrating oil agent is selected from at least one of acetone, dimethylformamide and polyvinyl pyrrolidone.

[0015] Preferably, the volume ratio of the auxiliary agent to water is 1:2-4;

[0016] The volume ratio of the softening oil agent to the hydrophilic penetrating oil agent is 1.5-3.5:1.

[0017] Preferably, the mass ratio of the health solution to the polyacrylonitrile oxidized fiber is 1:6-10;

[0018] The pretreatment temperature is 50-60° C., and the pretreatment time is 24-48 hours.

[0019] Since polyacrylonitrile oxidized fiber is easy to break, has problems such as low fiber cohesion, low strength, high brittleness, and poor spinnability, the present invention performs health treatment before spinning to improve the fiber cohesion and spinnability. The health solution selected by the present invention has good spreadability and permeability, can increase the fiber cohesion and friction, and can effectively improve the friction coefficient in the pre-oxidation spinning process, and can reduce the damage to the fiber caused by combing and striking during the spinning process.

[0020] Preferably, the process of cotton opening and cleaning is: the polyacrylonitrile pre-oxidized short fibers are sequentially passed through a cotton grabbing machine, a mixed cotton opening machine, a roller combing needle cotton opening machine, a vibrating cotton feeding box and a single-beater lap machine for cotton opening and cleaning to obtain polyacrylonitrile pre-oxidized short fibers with an impurity content of ≤1% and an unevenness rate of ≤1%.

[0021] Preferably, the roller combing needle cotton opener and the single beater lap machine both use a semi-holding striking interval to reduce the striking and damage of the fibers and enhance the opening degree of the fibers, and the distance between the striking point and the holding point is 25 to 45 mm;

[0022] The beating speed of the beater of the single-beater rolling machine is 300-500 r / min.

[0023] In the process of opening and cleaning cotton, the distance between the striking point and the holding point is increased by 40-60%, which can maximize the avoidance of damage to pre-oxidized fibers. By setting the striking speed of the single-beater lap machine to 300-500 r / min, the reduction range is 65-75% of the spinning cotton. If it is reduced too much, the pre-oxidized fibers will be damaged and a large amount of short fibers will be generated. If it is reduced too much, the fiber blocks will be opened and not transparent, which will affect the normal combing of the subsequent process.

[0024] Preferably, the carding process is: the polyacrylonitrile pre-oxidized short fibers after the cotton opening and cleaning process are carded by a carding machine;

[0025] The card clothing working angle of the carding machine is 75-80 degrees, the cotton feeding plate is raised by 10-15 mm, the licker-in speed is 700-750 rpm, the cylinder speed is 250-280 rpm, the doffer speed is 18-22 rpm, and the cover speed is 50-80 mm / min.

[0026] The working angle of the traditional carding machine card clothing is generally 60-80°C. Due to the characteristics of the polyacrylonitrile pre-oxidized fiber in the present invention being relatively slippery and having poor cohesion, it is not easy to transfer during the carding stage. Therefore, by optimizing the working angle of the card clothing of the carding machine, the gripping ability of the needle teeth on the fiber is significantly improved, which is beneficial to the fiber transfer. At the same time, the use of needle teeth with lower density can reduce the damage to the fiber. Since the cotton feeding plate is too low, the higher the short-pile rate, and the cotton board is too high, the worse the opening effect, so setting the cotton feeding plate to be raised by 10-15mm can reduce a large amount of short-pile caused by gripping and opening. In addition, if the speed of the combing piece is too fast, the short-pile rate will also increase, and if the combing piece is too slow, the opening effect will deteriorate. The present invention can reduce the impact strength of the pre-oxidized fiber, minimize the loss of the pre-oxidized fiber, and improve the yarn production rate of the pre-oxidized fiber by optimizing the process of the carding process.

[0027] Preferably, the drawing process uses a FA306A drawing frame to perform a three-pass mixed drawing process, wherein the speed of the first pass is 150-200 m / min, 8 strands are combined, the total drafting multiple is 6-8 times, the drafting multiple in the rear zone is 1.5-2.0 times, and the roller spacing is 18×30 mm;

[0028] The speed of the second track is 150-200 m / min, 8 rollers are combined, the total drafting ratio is 6-8 times, the drafting ratio of the rear zone is 1.4-1.6 times, and the roller spacing is 18×30 mm;

[0029] The speed of the third track is 150-200 m / min, 8 rollers are combined, the total drafting multiple is 6-9 times, the drafting multiple in the rear zone is 1.3-1.5 times, and the roller spacing is 18×30 mm.

[0030] Preferably, the roving twist coefficient during the roving treatment process is 90 to 120;

[0031] The spun yarn process adopts a compact siro spinning method.

[0032] Since the cohesion of pre-oxidized fibers is small, a too small twist coefficient easily causes the roving to break when unwinding, while a too large twist coefficient easily produces a "hard end" and is difficult to draw. The present invention increases the twist coefficient during the roving treatment process and controls the twist coefficient to be 50-80% higher than the twist coefficient of conventional chemical fiber yarns, thereby avoiding the above-mentioned problems of unwinding breakage and difficulty in drawing.

[0033] Due to the brittleness of the fiber, the negative pressure mesh ring will block the yarn and deteriorate the yarn dryness, so mechanical compact spinning is used. Compared with ordinary ring spinning, the CV% of the yarn dryness is increased by 3 to 5 points by using compact siro spinning, the strength is increased by 20 to 30%, the kilometer fine section (-50%), the thick section (+50%), and the cotton knot (+200%) are reduced by 30 to 50%, and the hairiness is reduced by more than 50%, which effectively improves the cleanliness of the yarn, effectively improves the processing efficiency of the subsequent products, increases the product completion rate, reduces the production cost, and greatly improves the quality of the subsequent fabrics and products.

[0034] According to the second aspect of the present invention, there is provided a polyacrylonitrile pre-oxidized yarn obtained according to the above-mentioned preparation method, with a linear density of 15 to 60 tex*2, a yarn variation coefficient CVm (%): 6 to 10; a hairiness index: 2.5 to 4.0; fine knots (-50%, pieces / km): 0 to 10; coarse knots (+50%, pieces / km): 10 to 20; cotton knots (+200, pieces / km): 20 to 300; breaking strength (cN / tex): 8 to 12; and elongation at break (%): 8 to 14.

[0035] (III) Beneficial effects

[0036] The present invention provides a polyacrylonitrile pre-oxidized yarn and a preparation method thereof, which has the following beneficial effects:

[0037] (1) This scheme provides a method for preparing polyacrylonitrile pre-oxidized yarn, which optimizes the process for pre-spun fibers. The process is simple, highly feasible, and has low process costs.

[0038] (2) This scheme provides a method for preparing polyacrylonitrile pre-oxidized yarn, which overcomes the difficulty of spinning polyacrylonitrile pre-oxidized fibers and expands the count range of pre-oxidized staple yarn to 15tex, which can meet the application requirements of different scenarios.

[0039] (3) The present invention provides a method for preparing polyacrylonitrile pre-oxidized yarn. By optimizing the spinning process, the yarn can be smoothly produced. The 100% polyacrylonitrile pre-oxidized fiber short yarn produced has good mechanical properties, uniform yarn length, and few defects. DETAILED DESCRIPTION

[0040] In order to better illustrate the content of the present invention, a detailed description is given below in conjunction with specific embodiments.

[0041] Example 1

[0042] Prepare health solution: evenly mix 1.5L silicone oil, 1L dimethylformamide and 3L water to obtain health solution;

[0043] Pretreatment: 10 kg of polyacrylonitrile oxidized fiber was placed in a curing solution containing 1 kg of nitrile and pretreated at 60°C for 48 hours to obtain polyacrylonitrile preoxidized short fibers;

[0044] Opening and cleaning cotton: the polyacrylonitrile pre-oxidized short fibers are sequentially passed through a cotton plucker, a mixed cotton opener, a roller combing needle cotton opener, a vibrating cotton feeding box and a single-beater lap machine for opening and cleaning cotton. Among them, all the beaters of the roller combing needle cotton opener and the single-beater lap machine are exposed at the bottom, and a half-grip striking distance is adopted. The distance between the striking point and the gripping point is 25mm, and the distance between the striking point and the gripping point is increased by 40%. The beating speed of the beater of the single-beater lap machine is 480r / min, and the polyacrylonitrile pre-oxidized short fiber lap with a trash content of ≤1% and an unevenness of ≤1% is obtained;

[0045] Carding: The polyacrylonitrile pre-oxidized short fibers after the cotton opening and cleaning treatment are carded by a carding machine, wherein the card clothing working angle of the carding machine is 75°, the cotton feeding plate is raised by 10mm, the licker-in speed is 700rpm, the cylinder speed is 250rpm, the doffer speed is 18rpm, and the flat plate speed is 50mm / min;

[0046] Drawing: The carded polyacrylonitrile pre-oxidized short fibers are subjected to three-pass mixed drawing process by FA306A drawing frame, wherein the speed of the first pass is 150m / min, 8 fibers are combined, the total drafting multiple is 6 times, the drafting multiple in the back zone is 1.5 times, and the roller spacing is 18×30mm; the speed of the second pass is 150m / min, 8 fibers are combined, the total drafting multiple is 8 times, the drafting multiple in the back zone is 1.4 times, and the roller spacing is 18×30mm; the speed of the third pass is 150m / min, 8 fibers are combined, the total drafting multiple is 8 times, the drafting multiple in the back zone is 1.3 times, and the roller spacing is 18×30mm;

[0047] Roving: The polyacrylonitrile pre-oxidized short fibers after drawing treatment are treated with a roving twist coefficient of 90, and then spun by a compact siro spinning method to obtain polyacrylonitrile pre-oxidized yarn.

[0048] Example 2

[0049] Prepare health solution: mix 2L silicone oil, 1L dimethylformamide and 4L water evenly to obtain health solution;

[0050] Pretreatment: 10 kg of polyacrylonitrile oxidized fiber was placed in a curing solution containing 1 kg of nitrile and pretreated at 60°C for 48 hours to obtain polyacrylonitrile preoxidized short fibers;

[0051] Opening and cleaning cotton: the polyacrylonitrile pre-oxidized short fibers are sequentially passed through a cotton plucker, a mixed cotton opener, a roller combing needle cotton opener, a vibrating cotton feeding box and a single-beater lap machine for opening and cleaning cotton. All the beaters of the roller combing needle cotton opener and the single-beater lap machine are exposed at the bottom, and a half-grip striking distance is adopted. The distance between the striking point and the gripping point is 30mm, and the distance between the striking point and the gripping point is increased by 45%. The beating speed of the beater of the single-beater lap machine is 500r / min, and the polyacrylonitrile pre-oxidized short fiber lap with a trash content of ≤1% and an unevenness of ≤1% is obtained;

[0052] Carding: The polyacrylonitrile pre-oxidized short fibers after the cotton opening and cleaning treatment are carded by a carding machine, wherein the card clothing working angle of the carding machine is 80°, the cotton feeding plate is raised by 15mm, the licker-in speed is 750rpm, the cylinder speed is 280rpm, the doffer speed is 22rpm, and the flat plate speed is 80mm / min;

[0053] Drawing: The carded polyacrylonitrile pre-oxidized short fibers are subjected to three-pass mixed drawing process by FA306A drawing frame, wherein the speed of the first pass is 200m / min, 8 fibers are combined, the total drafting multiple is 8 times, the drafting multiple in the rear zone is 2 times, and the roller spacing is 18×30mm; the speed of the second pass is 200m / min, 8 fibers are combined, the total drafting multiple is 8 times, the drafting multiple in the rear zone is 1.6 times, and the roller spacing is 18×30mm; the speed of the third pass is 150m / min, 8 fibers are combined, the total drafting multiple is 8 times, the drafting multiple in the rear zone is 1.5 times, and the roller spacing is 18×30mm;

[0054] Roving: The polyacrylonitrile pre-oxidized short fibers after drawing treatment are treated with a roving twist coefficient of 120, and then spun by a compact siro spinning method to obtain polyacrylonitrile pre-oxidized yarn.

[0055] Example 3

[0056] Prepare the health solution: mix 3.5L glyceride, 1.2L acetone and 4L water evenly to obtain the health solution;

[0057] Pretreatment: 6 kg of polyacrylonitrile oxidized fiber was placed in a curing solution containing 1 kg of polyacrylonitrile and pretreated at 60°C for 48 hours to obtain polyacrylonitrile preoxidized short fibers;

[0058] Opening and cleaning cotton: the polyacrylonitrile pre-oxidized short fibers are sequentially passed through a cotton plucker, a mixed cotton opener, a roller combing needle cotton opener, a vibrating cotton feeding box and a single-beater lap machine for opening and cleaning cotton. All the beaters of the roller combing needle cotton opener and the single-beater lap machine are exposed at the bottom, and a half-grip striking distance is adopted. The distance between the striking point and the gripping point is 30mm, and the distance between the striking point and the gripping point is increased by 45%. The beating speed of the beater of the single-beater lap machine is 500r / min, and the polyacrylonitrile pre-oxidized short fiber lap with a trash content of ≤1% and an unevenness of ≤1% is obtained;

[0059] Carding: The polyacrylonitrile pre-oxidized short fibers after the cotton opening and cleaning treatment are carded by a carding machine, wherein the card clothing working angle of the carding machine is 80°, the cotton plate is raised by 15mm, the licker-in speed is 750rpm, the cylinder speed is 280rpm, the doffer speed is 22rpm, and the flat plate speed is 80mm / min;

[0060] Drawing: The carded polyacrylonitrile pre-oxidized short fibers are subjected to three-pass mixed drawing process by FA306A drawing frame, wherein the speed of the first pass is 200m / min, 8 fibers are combined, the total drafting multiple is 8 times, the drafting multiple in the rear zone is 2 times, and the roller spacing is 18×30mm; the speed of the second pass is 200m / min, 8 fibers are combined, the total drafting multiple is 8 times, the drafting multiple in the rear zone is 1.6 times, and the roller spacing is 18×30mm; the speed of the third pass is 150m / min, 8 fibers are combined, the total drafting multiple is 8 times, the drafting multiple in the rear zone is 1.5 times, and the roller spacing is 18×30mm;

[0061] Roving: The polyacrylonitrile pre-oxidized short fibers after drawing treatment are treated with a roving twist coefficient of 120, and then spun by a compact siro spinning method to obtain polyacrylonitrile pre-oxidized yarn.

[0062] The polyacrylonitrile pre-oxidized yarns prepared in Examples 1 to 3 were subjected to performance tests, and the results are shown in Table 1;

[0063] Table 1

[0064] Example Example 1 Example 2 Example 3 Linear density (tex) 59*2 43*2 58*2 Coefficient of variation of stripe XVm (%) 9.32 9.25 9.57 Hairiness index 4 3.5 4 Details (-50%, pcs / km) 0 0 0 Thick places (+50%, pieces / km) 15.8 14.3 13.3 Cotton neps (+200, pcs / km) 20 22 21 Breaking strength (cN / tex) 8.1 8.7 9.4 Elongation at break (%) 13 12 14

[0065] According to the data in Table 1, the preparation method of the polyacrylonitrile pre-oxidized yarn provided by the present invention is first pretreated with a health solution and then combined with the optimized spinning work. The prepared polyacrylonitrile pre-oxidized yarn has good mechanical properties, uniform yarn length and few defects.

[0066] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing polyacrylonitrile pre-oxidized yarn, Features: The following steps are involved: The polyacrylonitrile oxidized fiber is placed in a curing room and sprayed evenly with curing liquid for pretreatment to obtain polyacrylonitrile preoxidized short fiber; The polyacrylonitrile preoxidized short fibers are then sequentially subjected to opening and cleaning, carding, refining, drawing, roving and spinning processes to obtain polyacrylonitrile preoxidized yarns.

2. The method for preparing a polyacrylonitrile pre-oxidized yarn according to claim 1, Features: The health care liquid comprises an auxiliary agent and water, wherein the auxiliary agent is selected from a softening oil agent and a hydrophilic penetrating oil agent.

3. The method for preparing a polyacrylonitrile pre-oxidized yarn according to claim 2, Features: The volume ratio of the auxiliary agent to water is 1:2-4; The volume ratio of the softening oil agent to the hydrophilic penetrating oil agent is 1.5-3.5:

1.

4. The method for preparing a polyacrylonitrile pre-oxidized yarn according to claim 1, Features: The mass ratio of the health solution to the polyacrylonitrile oxidized fiber is 1:6-10; The pretreatment temperature is 50-60° C., and the pretreatment time is 24-48 hours.

5. The method for preparing a polyacrylonitrile pre-oxidized yarn according to claim 1, Features: The process of cotton opening and cleaning is as follows: the polyacrylonitrile pre-oxidized short fibers are sequentially subjected to cotton opening and cleaning treatment by a cotton plucker, a mixed cotton opener, a roller combing needle cotton opener, a vibrating cotton feeding box and a single-beater lap forming machine to obtain a polyacrylonitrile pre-oxidized fiber cotton roll with a trash content of ≤1% and an unevenness of ≤1%.

6. The method for preparing a polyacrylonitrile pre-oxidized yarn according to claim 5, Features: The roller combing needle cotton opener and the single beater lap machine both use a semi-holding striking interval to reduce the striking and damage of the fibers and enhance the opening degree of the fibers. The distance between the striking point and the holding point is 25 to 45 mm. The beating speed of the beater of the single-beater rolling machine is 300-500 r / min.

7. The method for preparing a polyacrylonitrile pre-oxidized yarn according to claim 1, Features: The carding process is as follows: the polyacrylonitrile pre-oxidized short fibers after the cotton opening and cleaning process are carded by a carding machine; The card clothing working angle of the carding machine is 75-80 degrees, the cotton feeding plate is raised by 10-15 mm, the licker-in speed is 700-750 rpm, the cylinder speed is 250-280 rpm, the doffer speed is 18-22 rpm, and the cover speed is 50-80 mm / min.

8. The method for preparing a polyacrylonitrile pre-oxidized yarn according to claim 1, Features: The drawing process uses a FA306A drawing frame to perform a three-pass mixed drawing process, wherein the speed of the first pass is 150-200 m / min, 8 strands are combined, the total drafting multiple is 6-8 times, the drafting multiple in the rear zone is 1.5-2.0 times, and the roller spacing is 18×30 mm; The speed of the second track is 150-200 m / min, 8 rollers are combined, the total drafting ratio is 6-8 times, the drafting ratio of the rear zone is 1.4-1.6 times, and the roller spacing is 18×30 mm; The speed of the third track is 150-200 m / min, 8 rollers are combined, the total drafting multiple is 6-9 times, the drafting multiple in the rear zone is 1.3-1.5 times, and the roller spacing is 18×30 mm.

9. The method for preparing a polyacrylonitrile pre-oxidized yarn according to claim 1, Features: The roving twist coefficient in the roving treatment process is 90 to 120; The spun yarn process adopts a compact Siro spinning method.

10. A polyacrylonitrile pre-oxidized yarn obtained according to the preparation method according to any one of claims 1 to 9, Features: Linear density 15~60tex*2, yarn variation coefficient CVm (%): 6~10; hairiness index: 2.5~4.0; fine knots (-50%, pieces / km): 0~10; coarse knots (+50%, pieces / km): 10~20; cotton knots (+200, pieces / km): 20~300; breaking strength (cN / tex): 8~12; elongation at break (%): 8~14.

Citation Information

Patent Citations

  • Fireproof yarn high in limit oxygen index, preparation method of fireproof yarn and fabric of fireproof yarn

    CN105040222A

  • Processing method of cotton and copper alginate blended yarn

    CN106884239A

  • Production process of cotton / wool / acrylic / Modal fiber blended yarn

    CN110644089A

  • Polyacrylonitrile pre-oxidized fiber fabric and production process thereof

    CN116240727A