Conductive ink and conductive glass fiber cloth based on same
Through the impregnation process of using conductive ink on glass fiber cloth, combined with the dispersion technology of carbon nanotubes, graphene and silver nanowires, the preparation period, high cost and insufficient uniformity of conductive glass fiber cloth preparation in the prior art is solved. The problem of low-cost and efficient conductivity and stability are achieved.
Patent Information
- Application Number
- CN202411210691.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The existing methods for preparing conductive glass fiber cloth have problems such as long preparation cycle, high process cost, high target resistance and insufficient uniformity of continuous sample preparation, and heavy metals are required for matrix activation treatment, resulting in environmental pollution and high process complexity.
Using a conductive ink, a conductive layer is formed by mixing and dispersing multi-walled carbon nanotubes, graphene and silver nanowires in a specific proportion, and combining modified aqueous polyurethane emulsion and crosslinking agent, the glass fiber cloth is formed by impregnation process. A uniform conductive and encapsulation layer is formed on it to ensure conductivity and adhesion.
It has achieved low-cost large-scale production of conductive glass fiber cloth, with uniform front and back sides, excellent coating adhesion fastness, excellent impact resistance, low square resistance value and high controllability, outstanding conductivity, and rapid heating and heating Characteristics of high stability of repeated heating.
Smart Images

Figure BDA0005020242760000021 
Figure BDA0005020242760000101 
Figure HDA0005020242780000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of glass fiber cloth preparation, and in particular relates to a conductive glass fiber cloth and a preparation method thereof. Background Art
[0002] Conductive glass fibers are widely used in blind holes, through holes, and connections between internal layers in the manufacturing process of printed circuit boards (PCBs) in the electronics field. By using conductive glass fibers, reliable electrical connections can be provided while maintaining good mechanical strength and heat resistance. In the field of communications, conductive glass fibers are used in fiber optic connectors and joints in fiber optic communications. Fiber connectors need to have good conductivity to ensure the transmission efficiency and stability of signals. In the aerospace field, conductive glass fibers are used to manufacture electromagnetic shielding and electrostatic protection equipment in aircraft and spacecraft. These devices can effectively shield electromagnetic interference and prevent static electricity accumulation, improving the safety and reliability of aircraft. Conductive glass fibers can also find applications in other fields such as medical, automotive, energy, etc. For example, in medical equipment, conductive glass fibers can be used to manufacture electrodes and sensors for monitoring biological signals and performing medical diagnosis.
[0003] Glass fiber cloth is woven from fiber bundles composed of fine glass fibers. The main ways to achieve its conductive properties include plating a metal conductive layer on the surface of the glass fiber, or in-situ polymerization on the fiber surface to form a conductive polymer, or blending and introducing conductive fiber materials during the weaving process of the glass fiber bundle, or coating the glass fiber cloth with a conductive slurry. However, the metal coating has defects such as heavy weight, poor corrosion resistance, poor oxidation resistance, and weak interface bonding with the glass fiber. At the same time, glass fiber is a poor conductor of electricity and does not have the catalytic activity of chemical metal plating. In order to ensure that the coating can be firmly attached to the glass fiber, the glass fiber matrix needs to be roughened and activated. Not only is the process complicated, but the heavy metals required for activation are expensive, and the heavy metal ions generated also pollute the environment. In addition, the prior art deposits a graphene conductive layer on the surface of the glass fiber cloth by chemical vapor deposition, and its electrical heating performance is excellent, but this method has problems such as long preparation cycle, high process cost, high target resistance, and insufficient uniformity of continuous sample preparation, which brings inconvenience to practical application.
[0004] The conductive functional structure is directly constructed on the surface of the formed fabric by coating, which has the advantages of simple process, easy control of conditions, multiple conductive phase selectivity, etc., and can maximize the original structure and performance of the fabric. The core of this method is the selection and dispersion of conductive materials in the coating. Patent CN106205862B discloses a method for preparing high-temperature conductive glass fiber cloth, which prepares a high-temperature polymer silver-coated copper powder conductive slurry by mixing an organic carrier and pure metal silver-coated copper powder, and then uses a wire rod coater to coat it on the glass fiber cloth and then dry it to obtain a high-temperature conductive glass fiber cloth. Patent CN114258167A discloses a method for preparing a carbon nanotube / glass fiber cloth flexible film heater, which uses a Meyer rod coating method to coat a single-layer carbon nanotube dispersion layer by layer on a glass fiber cloth substrate, and heats and anneals to weld the carbon nanotube nodes. There are significant differences in the conductive properties of the two sides of the conductive glass fiber cloth prepared by the above two methods, and it requires a long time of drying and curing conditions. Patent CN109233142A discloses a method for processing conductive glass fiber cloth, which comprises pre-roughening the surface of the glass fiber cloth, and then immersing the glass fibers in a conductive slurry for 2-3 hours, curing for 20-40 minutes, and drying. The preparation method requires a long impregnation and curing time, a long preparation cycle, and a high solid content of the conductive slurry used, and a large coating thickness, which easily leads to pore blockage in the glass fiber cloth. Summary of the invention
[0005] In view of the problems existing in the prior art, the first object of the present invention is to provide a conductive ink that is evenly dispersed, has no sedimentation during long-term storage, has good wettability to glass fiber cloth, and has high adhesion, so that it is suitable for the impregnation treatment of glass fiber cloth.
[0006] The second object of the present invention is to provide a conductive glass fiber cloth based on the above-mentioned conductive ink, so that it can be produced on a large scale at low cost, and has the advantages of uniform front and back surfaces, excellent coating adhesion, excellent impact resistance, low square resistance and high controllability, and outstanding conductive performance.
[0007] In order to achieve the purpose, the present invention adopts the following technical scheme:
[0008] The present invention first provides a conductive ink for conductive glass fiber cloth, wherein the components thereof are composed of the following components in parts by weight:
[0009]
[0010] Preferably, the mass concentration of multi-walled carbon nanotubes in the multi-walled carbon nanotube aqueous dispersion is 8% to 10%, the diameter of the carbon nanotubes is 10-30nm, and the length is 2-20μm; the mass concentration of graphene in the graphene aqueous dispersion is 4% to 8%, the diameter of the graphene sheets is 1-6μm, and the number of layers is 6-10; the mass concentration of silver nanowires in the silver nanowire aqueous dispersion is 0.5% to 1%, the diameter of the silver nanowires is 10-30nm, and the aspect ratio is 800-2000. The solid content of the modified aqueous polyurethane emulsion is 35% to 45%.
[0011] Preferably, the wetting and dispersing agent is at least one of sodium dodecylbenzene sulfonate (SDBS) and sodium dodecyl sulfate (SDS); the crosslinking agent is a multifunctional aziridine crosslinking agent; and the 2% viscosity of the hydroxypropyl methylcellulose (HPMC) is 3-6 mPa·s.
[0012] The method for preparing the conductive ink of the present invention comprises the following steps:
[0013] S1. Preparation of carbon-based conductive component: adding a wetting dispersant to an appropriate amount of deionized water and an appropriate amount of ethanol and stirring until completely dissolved, continuing to add a multi-walled carbon nanotube aqueous dispersion and a graphene aqueous dispersion, grinding evenly, filtering, and obtaining a carbon-based conductive abrasive; placing an appropriate amount of deionized water and the remaining ethanol in a disperser and stirring evenly, adding the carbon-based conductive abrasive and the modified aqueous polyurethane emulsion in sequence under stirring, continuing to stir and disperse evenly, and obtaining a carbon-based conductive component;
[0014] S2. Preparation of silver nanowire component: Place an appropriate amount of deionized water in a disperser and stir, slowly add hydroxypropyl methylcellulose and stir until completely dissolved, continue to add silver nanowire aqueous dispersion and stir until uniformly dispersed, to obtain silver nanowire component;
[0015] S3. Preparation of conductive ink: After mixing the crosslinking agent and the remaining deionized water, add them to the carbon-based conductive component, stir and disperse at 500-800 rpm for 10-30 minutes, reduce the stirring speed to 200-300 rpm, add the silver nanowire component, mix well to obtain the conductive ink.
[0016] The present invention further discloses a conductive glass fiber cloth, which comprises a glass fiber cloth, a conductive layer formed on the glass fiber cloth, and a packaging layer formed on the conductive layer; the conductive layer is formed by impregnating the conductive ink, and the conductive ink forms a conductive layer on both the upper and lower surfaces of the glass fiber cloth. At the same time, the ink also adheres to the inner wall of the mesh of the fiber cloth to connect the upper and lower conductive layers.
[0017] Preferably, the encapsulation layer is formed by dipping encapsulation ink, and the components of the encapsulation ink are composed by weight of: 10-30 parts of modified waterborne polyurethane emulsion, 1-3 parts of multifunctional aziridine crosslinking agent, 20-40 parts of ethanol and 50-80 parts of deionized water.
[0018] The method for preparing the conductive glass fiber cloth of the present invention is characterized by comprising the following steps:
[0019] S1, washing the glass fiber cloth with acetone and deionized water in sequence, and drying the glass fiber cloth to obtain a clean glass fiber cloth;
[0020] S2, using an impregnation device to impregnate the conductive ink onto the clean glass fiber cloth, and then sequentially performing post-processing steps including squeezing, drying, calendering and cooling;
[0021] Repeat the dip coating and post-treatment 1-4 times to obtain a glass fiber cloth coated with a conductive layer;
[0022] S3, using an impregnation device to impregnate the encapsulation ink on the glass fiber cloth coated with the conductive layer, and then sequentially performing post-processing steps including squeezing, drying and cooling;
[0023] The dip coating and post-treatment are repeated 0-4 times to form a packaging layer and obtain a conductive glass fiber cloth.
[0024] Preferably, in step S2 and step S3, the dipping time of the dipping coating is 2-10 seconds and the dipping speed is 1-5 m / min.
[0025] Preferably, in step S2 and step S3, the drying method is infrared heating drying, the drying temperature is 80-140° C., and the drying time is 5-25 seconds.
[0026] As a preference: in step S2, the calendering pressure is 10-20 KgN / cm 2 .
[0027] As a preference: in the conductive glass fiber cloth, the weight per unit area of the glass fiber cloth is 40-200 g / m 2 The conductive ink has a dry coating weight of 0.5-10 g / m 2 The coating dry weight of the packaging ink is 0.2-5g / m 2 .
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The conductive ink provided by the present invention has a viscosity of 0.5-5mPa·s, is evenly dispersed, has no sedimentation during long-term storage, has good wettability to glass fiber cloth, has high adhesion, and is suitable for impregnation treatment of glass fiber cloth. Its advantages are specifically reflected in:
[0030] Firstly, the present invention mixes and disperses carbon nanotubes, graphene and silver nanowires in a specific ratio, utilizes the chemical and structural characteristics of shorter carbon nanotubes, flaky graphene and longer silver nanowires, and the carbon nanotubes isolate the physical entanglement between the silver nanowires in physical space, effectively avoiding the occurrence of cumulative precipitation, and at the same time forming an efficient electron transmission network that penetrates and overlaps each other, and combines the synergistic effect of the connecting resin material to improve the interface bonding force between the carbon nanotubes, graphene, silver nanowires and glass fiber bundles, so that the coating has good adhesion and conductivity on the glass fiber cloth, and realizes the preparation of conductive glass fiber cloth with a square resistance of 5 to 1000Ω / □.
[0031] Secondly, in the conductive ink of the present invention, carbon nanotubes, graphene and silver nanowires form a "line-line-surface" bridge structure on the glass fiber cloth bundles. When the glass fiber cloth is bent or folded by external force, although a certain degree of misalignment will occur between the glass fiber bundles, the silver nanowires have good flexibility and multiple overlapping contacts with the carbon nanotubes and graphene, the conductive glass fiber cloth still maintains good resistance stability after multiple bending.
[0032] Third, the carbon nanotube slurry will slightly agglomerate during storage. The present invention can effectively solve the problem of difficulty in uniform dispersion due to agglomeration by performing a short-term secondary grinding and dispersion treatment on the carbon nanotube slurry and graphene solution, thereby ensuring the storage stability and dispersion uniformity of the impregnated ink.
[0033] Fourth, the wetting dispersant, ethanol and aqueous emulsion in the conductive ink formula system all reduce the surface tension of the ink to a certain extent, so that the ink has sufficient wettability and adhesion to the glass fiber cloth. The addition of the crosslinking agent further increases the hardness and adhesion of the coating, and the formed coating has excellent temperature resistance and stability, which can significantly increase the stiffness of the glass fiber cloth and enhance its ability to resist deformation due to external forces. The impregnation ink provided by the present invention utilizes the synergistic effect between the components, that is, by adjusting the respective proportions, the stability and conductive properties of the impregnation ink are ensured.
[0034] Fifth, the conductive ink provided by the present invention has low viscosity and good fluidity, and can be evenly coated on the mesh-shaped glass fiber cloth through an impregnation process, so that the coating on the front and back sides is uniform.
[0035] 2. The square resistance of the conductive glass fiber cloth provided by the present invention can be adjusted in the range of 5 to 1000Ω / □, and has the characteristics of uniform front and back surfaces, excellent coating adhesion, excellent impact resistance, low square resistance and high controllability, outstanding conductivity, etc. It can heat up quickly, and has high stability in repeated heating, and can achieve low-cost large-scale production. Its advantages are specifically reflected in:
[0036] Firstly, the present invention effectively ensures that the glass fiber cloth has no pore blockage, the resistance value of each point on the front and back sides is uniform, and the surface conductive performance is consistent by impregnating and coating the glass fiber cloth with low-viscosity conductive ink.
[0037] Secondly, the present invention ensures that the carbon nanotubes, graphene and silver nanowires do not directly contact the outside by immersing and coating the encapsulation ink on the conductive layer, so that the adhesion is higher, and at the same time, the compactness of the silver nanowires is improved, so that they are attached to the surface of the fiber bundle, and the stability of the conductive layer structure is improved. In addition, the encapsulation layer also significantly improves the tensile strength and elastic modulus of the glass fiber cloth, making the electron transmission network composed of the carbon nanotubes, graphene and silver nanowires interwoven with each other more stable.
[0038] Third, when preparing the conductive layer on the glass fiber cloth, the present invention sets a calendering action after impregnation, squeezing, and drying, so that the glass fiber bundles are relatively flatter, and the uniformity of subsequent impregnation ink coating is improved. At the same time, the conductive glass fiber cloth will produce internal stress when subjected to external force, and then produce a post-shrinkage phenomenon of continuous deformation after processing, and the calendering action can make the intersection of the radial and weft fiber bundles smoother, and the subsequent changes under external force are small, which greatly reduces the occurrence of the post-shrinkage phenomenon, improves the ability of the conductive glass fiber cloth to resist external forces, and ensures the service life and conductive performance of the conductive glass fiber cloth.
[0039] Fourthly, the preparation method of the conductive glass fiber cloth of the present invention is simple to operate, low in cost, suitable for large-scale production, and has great application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is an optical magnifying glass photograph of the conductive glass fiber cloth in Example 1 of the present invention.
[0041] Figure 2 This is a scanning electron microscope photograph of the conductive layer of the conductive glass fiber cloth in Example 1 of the present invention.
[0042] Figure 3 This is a heating test diagram of the conductive glass fiber cloth in Example 1 of the present invention. DETAILED DESCRIPTION
[0043] The present invention is described in detail below in conjunction with embodiments. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0044] The mass concentration of multi-walled carbon nanotubes in the multi-walled carbon nanotube aqueous dispersion used in the following examples is 8.5%, and the diameter of the carbon nanotubes is 10-30 nm and the length is 2-20 μm.
[0045] The mass concentration of graphene in the graphene aqueous dispersion used in the following examples is 6.2%, the diameter of the graphene sheets is ≤6 μm, and the number of layers is 6-10.
[0046] The mass concentration of the silver nanowires in the silver nanowire aqueous dispersion used in the following examples is 0.8%, the diameter of the silver nanowires is 10-30 nm, and the aspect ratio is 800-2000.
[0047] The modified waterborne polyurethane emulsion used in the following examples was purchased from Yierfu Chemical (Shanghai) Co., Ltd., model PU-6155, with a solid content of 40%.
[0048] The cross-linking agent used in the following examples is a multifunctional aziridine cross-linking agent purchased from Sinopharm Chemical Reagent Co., Ltd., model ET 150.
[0049] The 2% viscosity of the hydroxypropyl methylcellulose HPMC used in the following examples is 3 mPa·s and it was purchased from Sinopharm Chemical Reagent Co., Ltd.
[0050] Example 1
[0051] This embodiment first provides a conductive ink, the components of which are composed by weight: 10 parts of multi-walled carbon nanotube aqueous dispersion, 2 parts of graphene aqueous dispersion, 20 parts of silver nanowire aqueous dispersion, 0.08 parts of sodium dodecylbenzene sulfonate, 2 parts of modified aqueous polyurethane emulsion, 0.04 parts of low-viscosity hydroxypropyl methylcellulose, 0.02 parts of multifunctional aziridine crosslinking agent, 10 parts of ethanol and 60 parts of deionized water. The preparation method thereof comprises the following steps:
[0052] S1. Preparation of carbon-based conductive components: Weigh 15 parts of deionized water and 5 parts of ethanol into a suitable container, add 0.08 parts of sodium dodecylbenzene sulfonate, a wetting and dispersing agent, stir until completely dissolved, continue to add 10 parts of multi-walled carbon nanotube aqueous dispersion and 2 parts of graphene aqueous dispersion, add grinding zirconium beads and place in an oscillator for grinding for 30 minutes, filter after grinding to obtain carbon-based conductive abrasives. Weigh 24 parts of deionized water and 5 parts of ethanol, place in a disperser and stir evenly, add the above-mentioned carbon-based conductive abrasives and 2 parts of modified aqueous polyurethane emulsion in sequence under 500rpm stirring, and continue to stir and disperse for 20 minutes to obtain carbon-based conductive components.
[0053] S2. Preparation of silver nanowire component: Weigh 20 parts of deionized water, place in a disperser and stir, slowly add 0.04 parts of low-viscosity hydroxypropyl methylcellulose, stir until completely dissolved, add 20 parts of silver nanowire aqueous dispersion under stirring at 200 rpm, continue stirring and dispersing for 10 minutes to obtain the silver nanowire component.
[0054] S3. Preparation of conductive ink: Mix 0.02 parts of multifunctional aziridine crosslinking agent and 1 part of deionized water, slowly add to the carbon-based conductive component, stir and disperse at 500 rpm for 10 minutes, reduce the stirring speed to 200 rpm, slowly continue to add the silver nanowire component, and mix well to obtain the conductive ink.
[0055] This embodiment further provides a conductive glass fiber cloth, which comprises a glass fiber cloth, a conductive layer coated on the glass fiber cloth, and a packaging layer coated on the conductive layer. The preparation method thereof is specifically as follows:
[0056] S1, glass fiber cloth (weight per unit area 40g / m 2 ) is washed with acetone and deionized water in turn and then dried to obtain a clean glass fiber cloth.
[0057] S2. Use an impregnation device to dip-coat the above conductive ink on a clean glass fiber cloth, and then perform post-treatment steps including squeezing, drying, calendering and cooling in sequence. Repeat the dip-coating and post-treatment once to obtain a glass fiber cloth coated with a conductive layer. Calendering pressure 10KgN / cm 2 .
[0058] S3. Evenly mix 20 parts of modified waterborne polyurethane emulsion, 2 parts of multifunctional aziridine crosslinking agent, 30 parts of ethanol and 60 parts of deionized water to obtain encapsulation ink, and transfer it to a dipping tank.
[0059] The encapsulation ink is dip-coated on the glass fiber cloth coated with the conductive layer by using an impregnation device, and then the post-treatment steps including squeezing, drying and cooling are carried out in sequence. The dip-coating and post-treatment are repeated once to form an encapsulation layer, and the conductive glass fiber cloth is rolled up.
[0060] In step S2 and step S3: the dipping time of the dip coating is 5 seconds, and the dipping speed is 2 m / min; the drying method is infrared heating drying, the drying temperature is 120° C., and the drying time is 5 seconds.
[0061] Example 2
[0062] This embodiment first provides a conductive ink, the components of which are composed by weight: 5 parts of multi-walled carbon nanotube aqueous dispersion, 1 part of graphene aqueous dispersion, 30 parts of silver nanowire aqueous dispersion, 0.04 parts of sodium dodecyl sulfate, 1 part of modified aqueous polyurethane emulsion, 0.06 parts of low-viscosity hydroxypropyl methylcellulose, 0.01 parts of multifunctional aziridine crosslinking agent, 10 parts of ethanol and 40 parts of deionized water. The preparation method thereof comprises the following steps:
[0063] S1. Preparation of carbon-based conductive components: Weigh 10 parts of deionized water and 2 parts of ethanol into a suitable container, add 0.04 parts of wetting dispersant sodium dodecyl sulfate, stir until completely dissolved, continue to add 5 parts of multi-walled carbon nanotube aqueous dispersion and 1 part of graphene aqueous dispersion, add grinding zirconium beads and place in an oscillator for grinding for 30 minutes, filter after grinding to obtain carbon-based conductive abrasives. Weigh 14 parts of deionized water and 8 parts of ethanol, place in a disperser and stir evenly, add the above-mentioned carbon-based conductive abrasives and 1 part of modified aqueous polyurethane emulsion in sequence under stirring at 800rpm, and continue stirring and dispersing for 10 minutes to obtain carbon-based conductive components.
[0064] S2. Preparation of silver nanowire component: Weigh 15 parts of deionized water, place in a disperser and stir, slowly add 0.06 parts of low-viscosity hydroxypropyl methylcellulose, stir until completely dissolved, add 30 parts of silver nanowire aqueous dispersion under stirring at 200 rpm, continue stirring and dispersing for 10 minutes to obtain the silver nanowire component.
[0065] S3. Preparation of conductive ink: Mix 0.01 parts of multifunctional aziridine crosslinking agent and 1 part of deionized water, slowly add to the carbon-based conductive component, stir and disperse at 500 rpm for 10 minutes, reduce the stirring speed to 300 rpm, slowly continue to add the silver nanowire component, and mix well to obtain the conductive ink.
[0066] This embodiment further provides a conductive glass fiber cloth, which comprises a glass fiber cloth, a conductive layer coated on the glass fiber cloth, and a packaging layer coated on the conductive layer. The preparation method thereof is specifically as follows:
[0067] S1, glass fiber cloth (weight per unit area is 100g / m 2 ) is washed with acetone and deionized water in turn and then dried to obtain a clean glass fiber cloth.
[0068] S2. Use an impregnation device to dip-coat the above conductive ink on a clean glass fiber cloth, and then perform post-treatment steps including squeezing, drying, calendering and cooling in sequence. Repeat the dip-coating and post-treatment once to obtain a glass fiber cloth coated with a conductive layer. Calendering pressure 10KgN / cm 2 .
[0069] S3. Evenly mix 30 parts of modified waterborne polyurethane emulsion, 3 parts of multifunctional aziridine crosslinking agent, 20 parts of ethanol and 70 parts of deionized water to obtain encapsulation ink, and transfer it to a dipping tank.
[0070] The encapsulation ink is dip-coated on the glass fiber cloth coated with the conductive layer by using an impregnation device, and then post-processing steps including pressing, drying and cooling are carried out in sequence to form an encapsulation layer, which is then rolled up to obtain the conductive glass fiber cloth.
[0071] In step S2 and step S3: the dipping time of the dip coating is 10 seconds, and the dipping speed is 1 m / min; the drying method is infrared heating drying, the drying temperature is 80° C., and the drying time is 10 seconds.
[0072] Example 3
[0073] This embodiment first provides a conductive ink, the components of which are composed by weight: 20 parts of multi-walled carbon nanotube aqueous dispersion, 5 parts of graphene aqueous dispersion, 10 parts of silver nanowire aqueous dispersion, 0.1 parts of sodium dodecylbenzene sulfonate, 5 parts of modified aqueous polyurethane emulsion, 0.02 parts of low-viscosity hydroxypropyl methylcellulose HPMC, 0.05 parts of multifunctional aziridine crosslinking agent ET150, 20 parts of ethanol and 80 parts of deionized water. The preparation method thereof comprises the following steps:
[0074] S1. Preparation of carbon-based conductive components: Weigh 30 parts of deionized water and 10 parts of ethanol into a suitable container, add 0.1 parts of sodium dodecylbenzene sulfonate, a wetting dispersant, stir until completely dissolved, continue to add 20 parts of multi-walled carbon nanotube aqueous dispersion and 5 parts of graphene aqueous dispersion, add grinding zirconium beads and place in an oscillator for grinding for 30 minutes, filter after grinding to obtain carbon-based conductive abrasives. Weigh 39 parts of deionized water and 10 parts of ethanol, place in a disperser and stir evenly, add the above-mentioned carbon-based conductive abrasives and 5 parts of modified aqueous polyurethane emulsion in sequence under 500rpm stirring, and continue to stir and disperse for 30 minutes to obtain carbon-based conductive components.
[0075] S2. Preparation of silver nanowire component: Weigh 10 parts of deionized water, place in a disperser and stir, slowly add 0.02 parts of low-viscosity hydroxypropyl methylcellulose HPMC, stir until completely dissolved, add 10 parts of silver nanowire aqueous dispersion under stirring at 200 rpm, continue stirring and dispersing for 10 minutes to obtain the silver nanowire component.
[0076] S3. Preparation of conductive ink: Mix 0.05 parts of multifunctional aziridine crosslinking agent and 1 part of deionized water, slowly add to the carbon-based conductive component, stir and disperse at 500 rpm for 10 minutes, reduce the stirring speed to 200 rpm, slowly continue to add the silver nanowire component, and mix well to obtain the conductive ink.
[0077] This embodiment further provides a conductive glass fiber cloth, which comprises a glass fiber cloth, a conductive layer coated on the glass fiber cloth, and a packaging layer coated on the conductive layer. The preparation method thereof is specifically as follows:
[0078] S1, glass fiber cloth (weight per unit area is 200g / m 2 ) is washed with acetone and deionized water in turn and then dried to obtain a clean glass fiber cloth.
[0079] S2. Use an impregnation device to dip-coat the above conductive ink on a clean glass fiber cloth, and then perform post-treatment steps including squeezing, drying, calendering and cooling in sequence. Repeat the dip-coating and post-treatment for 3 times to obtain a glass fiber cloth coated with a conductive layer. Calendering pressure 10KgN / cm 2 .
[0080] S3. Evenly mix 10 parts of modified waterborne polyurethane emulsion, 1 part of multifunctional aziridine crosslinking agent, 40 parts of ethanol and 50 parts of deionized water to obtain encapsulation ink, and transfer it to a dipping tank.
[0081] The encapsulation ink is dip-coated on the glass fiber cloth coated with the conductive layer by using an impregnation device, and then the post-treatment steps including squeezing, drying and cooling are carried out in sequence. The dip-coating and post-treatment are repeated three times to form an encapsulation layer, and the conductive glass fiber cloth is rolled up.
[0082] In step S2 and step S3: the dipping time of the dip coating is 2 seconds, and the dipping speed is 5 m / min; the drying method is infrared heating drying, the drying temperature is 140° C., and the drying time is 5 seconds.
[0083] Comparative Example 1
[0084] In this comparative example, conductive ink and conductive glass fiber cloth were prepared in the same manner as in Example 1, with the only difference being that the amount of silver nanowire aqueous dispersion and low-viscosity hydroxypropyl methylcellulose added to the conductive ink formula was 0, and correspondingly, step S2 was omitted when preparing the conductive ink, and the deionized water in step S2 was incorporated into step S1.
[0085] Comparative Example 2
[0086] In this comparative example, conductive ink and conductive glass fiber cloth were prepared in the same manner as in comparative example 1, except that when preparing the conductive glass fiber cloth, the total number of times the conductive ink was impregnated was 8 times.
[0087] Comparative Example 3
[0088] In this comparative example, conductive ink and conductive glass fiber cloth were prepared in the same manner as in Example 1, except that the amount of multi-walled carbon nanotube aqueous dispersion, graphene aqueous dispersion, sodium dodecylbenzene sulfonate, modified aqueous polyurethane emulsion and multifunctional aziridine crosslinking agent added in the formula of the conductive ink was 0. Correspondingly, the preparation steps of the conductive ink were as follows:
[0089] Weigh 60 parts of deionized water, place in a disperser and stir, slowly add 0.04 parts of low-viscosity hydroxypropyl methylcellulose HPMC, stir until completely dissolved, add 20 parts of silver nanowire aqueous dispersion under stirring at 200 rpm, continue stirring and dispersing for 10 minutes to obtain conductive ink.
[0090] Comparative Example 4
[0091] In this comparative example, conductive ink and conductive glass fiber cloth were prepared in the same manner as in Example 1, except that step S3 was not performed when preparing the conductive glass fiber cloth, thereby obtaining a conductive glass fiber cloth without an encapsulation layer.
[0092] Comparative Example 5
[0093] In this comparative example, conductive ink and conductive glass fiber cloth were prepared in the same manner as in Example 1, except that no calendering process was performed in step S2 when preparing the conductive glass fiber cloth.
[0094] The properties of the conductive glass fiber cloths obtained in the above-mentioned embodiments and comparative examples were tested and compared according to the following testing methods. The results are shown in Table 1.
[0095] (1) Square resistance and coefficient of variation: The obtained conductive glass fiber cloth was cut into test samples with a length of 250 mm and a width of 200 mm. The A side and the B side were marked, and each side was divided into 20 test areas. The square resistance of each area was tested using a four-probe tester, and the arithmetic mean and coefficient of variation were calculated.
[0096] (2) Adhesion fastness: The obtained conductive glass fiber cloth was subjected to the 3M tape test method to evaluate the coating adhesion fastness.
[0097] (3) Dry weight of coating: The obtained conductive glass fiber cloth was cut into three square specimens of 100 mm × 100 mm and weighed on an electronic balance with an accuracy of 0.0001 g. The arithmetic mean of the dry weight of coating was calculated compared with that of the blank control group.
[0098] (4) Tensile strength / elastic modulus: The obtained conductive glass fiber cloth was cut into three specimens of 250 mm in length and 25 mm in width, and the specimens were placed in a tensile testing machine for testing at a tensile speed of 50 mm / min. The arithmetic mean value was calculated.
[0099] (5) Heating temperature: Cut the obtained conductive glass fiber cloth into three 100 mm × 100 mm square samples, select the opposite sides in the length direction to coat with conductive silver paste, dry and cool, connect to an AC voltage regulating power supply, slowly increase the output working voltage after power-on, and use an infrared imager to detect the heating temperature of the conductive glass fiber cloth, and adjust the heating target temperature to 120°C.
[0100] (6) Heating time: The rated working voltage is applied to the sample to be tested, and the heating temperature of the conductive glass fiber cloth is detected by an infrared imager. The heating curve from room temperature to the stable state of the target temperature is recorded. The time required to rise from room temperature to 90% (108°C) of the target temperature is taken as the heating time.
[0101] (7) Resistance change rate after repeated heating: Apply the rated working voltage to the sample to be tested, power it on continuously for 16 hours, then turn it off and cool it down for 8 hours. After repeatedly powering it on and off 25 times, use a multimeter to measure the resistance at both ends of the electrode and calculate the resistance change rate.
[0102] The test results of the above embodiments and comparative examples are shown in Table 1.
[0103] Table 1
[0104]
[0105] It can be seen from Table 1 that:
[0106] (1) The results of Examples 1-3 show that the conductive glass fiber cloth of the present invention has the characteristics of uniform front and back surfaces, excellent coating adhesion, excellent impact resistance, low square resistance and high controllability, outstanding conductive performance, etc., can heat up quickly, and has high repeated heating stability.
[0107] (2) The results of Comparative Examples 1 and 2 show that when carbon nanotube and graphene slurries are impregnated separately, their conductivity has an upper limit due to the influence of wetting dispersants, film-forming resins and other substances. Even if the glass fiber cloth is impregnated with thick coatings for multiple times, it is still difficult to achieve a square resistance data below 1000Ω / □, and the glass fiber cloth grids are prone to clogging problems after thick coating.
[0108] (3) In Comparative Example 3, when silver nanowires were impregnated alone, the square resistance of the glass fiber cloth surface was measured. Although the square resistance data could be reduced to the ten-digit level, its stability was poor. The silver nanowires broke after being compressed, resulting in the failure of the conductive network. At the same time, during the test, it was found that there was a cumulative precipitation phenomenon on the laminating rubber roller. This may be because the individual silver nanowires are easily physically entangled, which is very easy to transfer to the glass fiber cloth and cause contamination of the glass fiber cloth.
[0109] (4) The sample in Comparative Example 4 was not impregnated with encapsulation ink, and the adhesion strength of the conductive ink coating met the requirements. However, when it was prepared into a heating element and powered on for heating, its resistance increased greatly, and stable heating of 120°C could not be achieved.
[0110] (5) The results of comparative example 5 show that calendering treatment of the conductive coated glass fiber cloth can effectively improve the repeated heating resistance stability of the conductive glass fiber cloth.
[0111] The above are merely exemplary embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A conductive ink for conductive glass fiber cloth, characterized in that: The components of the conductive ink are composed of the following by weight: 5-20 parts of multi-walled carbon nanotube aqueous dispersion 1-5 parts of graphene aqueous dispersion 10-30 parts of silver nanowire aqueous dispersion Wetting and dispersing agent 0.04-0.1 parts 1-5 parts of modified waterborne polyurethane emulsion Hydroxypropyl methylcellulose 0.02-0.06 parts Crosslinking agent 0.01~0.05 parts 10-20 parts of ethanol 40-80 parts of deionized water.
2. The conductive ink according to claim 1, characterized in that: The mass concentration of multi-walled carbon nanotubes in the multi-walled carbon nanotube aqueous dispersion is 8% to 10%; the mass concentration of graphene in the graphene aqueous dispersion is 4% to 8%; and the mass concentration of silver nanowires in the silver nanowire aqueous dispersion is 0.5% to 1%.
3. The conductive ink according to claim 1, characterized in that: The solid content of the modified waterborne polyurethane emulsion is 35% to 45%.
4. The conductive ink according to claim 1, characterized in that: The wetting and dispersing agent is at least one of sodium dodecylbenzene sulfonate and sodium dodecyl sulfate; and the crosslinking agent is a multifunctional aziridine crosslinking agent.
5. The conductive ink according to claim 1, characterized in that: The 2% viscosity of the hydroxypropyl methylcellulose is 3-6 mPa·s.
6. A method for preparing the conductive ink according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Preparation of carbon-based conductive component: adding a wetting dispersant to an appropriate amount of deionized water and an appropriate amount of ethanol and stirring until completely dissolved, continuing to add a multi-walled carbon nanotube aqueous dispersion and a graphene aqueous dispersion, grinding evenly, filtering, and obtaining a carbon-based conductive abrasive; placing an appropriate amount of deionized water and the remaining ethanol in a disperser and stirring evenly, adding the carbon-based conductive abrasive and the modified aqueous polyurethane emulsion in sequence under stirring, continuing to stir and disperse evenly, and obtaining a carbon-based conductive component; S2. Preparation of silver nanowire component: Place an appropriate amount of deionized water in a disperser and stir, slowly add hydroxypropyl methylcellulose and stir until completely dissolved, continue to add silver nanowire aqueous dispersion and stir until uniformly dispersed, to obtain silver nanowire component; S3. Preparation of conductive ink: After mixing the crosslinking agent and the remaining deionized water, add them to the carbon-based conductive component, stir and disperse at 500-800 rpm for 10-30 minutes, reduce the stirring speed to 200-300 rpm, add the silver nanowire component, mix well to obtain the conductive ink.
7. A conductive glass fiber cloth, characterized in that: The invention comprises a glass fiber cloth, a conductive layer formed on the glass fiber cloth, and a packaging layer formed on the conductive layer; the conductive layer is formed by impregnating the conductive ink according to any one of claims 1 to 5.
8. The conductive glass fiber cloth according to claim 7, characterized in that: The encapsulation layer is formed by dipping the encapsulation ink, and the components of the encapsulation ink are composed of 10-30 parts of modified waterborne polyurethane emulsion, 1-3 parts of multifunctional aziridine crosslinking agent, 20-40 parts of ethanol and 50-80 parts of deionized water in parts by weight.
9. A method for preparing the conductive glass fiber cloth according to claim 7 or 8, characterized in that: The steps include: S1, cleaning and drying the glass fiber cloth to obtain a clean glass fiber cloth; S2, using an impregnation device to impregnate the conductive ink onto the clean glass fiber cloth, and then sequentially performing post-processing steps including squeezing, drying, calendering and cooling; Repeat the dip coating and post-treatment 1-4 times to obtain a glass fiber cloth coated with a conductive layer; S3, using an impregnation device to impregnate the encapsulation ink on the glass fiber cloth coated with the conductive layer, and then sequentially performing post-processing steps including squeezing, drying and cooling; The dip coating and post-treatment are repeated 0-4 times to form a packaging layer and obtain a conductive glass fiber cloth.
10. The preparation method according to claim 9, characterized in that: In step S2 and step S3, the immersion coating has an immersion time of 2-10 seconds and an immersion speed of 1-5 m / min.
11. The preparation method according to claim 9, characterized in that: In step S2 and step S3, the drying method is infrared heating drying, the drying temperature is 80-140° C., and the drying time is 5-25 seconds.
12. The preparation method according to claim 9, characterized in that: In step S2, the calendering pressure is 10-20 KgN / cm 2 .
13. The preparation method according to claim 9, characterized in that: In the conductive glass fiber cloth, the weight per unit area of the glass fiber cloth is 40-200 g / m 2 The conductive ink has a dry coating weight of 0.5-10 g / m 2 The coating dry weight of the packaging ink is 0.2-5g / m 2 .