Preparation method and system of antifibrillating flame-retardant lyocell fiber
By forming a protective layer on the surface of the Lycel fiber and cross-linking treatment, the problem of the loss of flame retardant performance in the prior art after multiple washings is solved, and the flame retardant performance and antifibrillation effect of the fiber are improved.
Patent Information
- Application Number
- CN202411207581.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the flame retardant properties of the preparation of flame retardant Lycel fibers are easily lost during multiple washings, and the physical effect of alginate adhering to the fiber surface is not reliable, resulting in a reduced flame retardant performance.
By mixing the lyesel fibers with the sodium alginate solution, a protective layer is formed, and then mixed with the crosslinking agent solution is heated and cross-linked to enhance the chemical force between the protective layer and the fiber to ensure that the protective layer does not fall off.
The flame retardant performance and antifibrillation effect of Lycel fiber are improved, ensuring the stability of the flame retardant performance of the fiber during multiple washes.
Smart Images

Figure CN119083176A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lyocell fibers, and in particular relates to a preparation method and a system for anti-fibrillation flame-retardant lyocell fibers. Background Art
[0002] Lyocell fiber is a highly crystalline, highly oriented cellulose regenerated fiber, which is prepared by physical dissolution and regeneration using N-methylmorpholine-N-oxide (NMMO) as a solvent. Ordinary lyocell fiber has poor flame retardancy and is prone to cause fire. Therefore, how to improve the flame retardancy of lyocell fiber is very important for lyocell fiber.
[0003] In the prior art, in order to improve the flame retardancy of Lyocell fiber, alginate is usually added to the coagulation bath during the preparation of Lyocell fiber, and then metal cations are added during the washing process for curing, so that the Lyocell fiber finally has a certain flame retardancy. This preparation process can refer to the prior art, application number: CN 109162096 B A method for preparing flame-retardant Lyocell cellulose fiber based on post-treatment method.
[0004] However, the applicant has found in practice that the above method for preparing lyocell fiber has some shortcomings. The main shortcoming is that alginate is attached to the surface of lyocell fiber after being regenerated by metal cations. However, this physical effect is not reliable and is very easy to fall off during multiple washings of the fiber, which easily causes the fiber to lose its flame retardant properties. Summary of the invention
[0005] The invention provides a method for preparing anti-fibrillation flame-retardant lyocell fiber, aiming to solve the problem that the flame-retardant property of the lyocell fiber is lost during multiple washing processes in the prior art for preparing the flame-retardant lyocell fiber.
[0006] In order to achieve the above object, the present invention provides a method for preparing anti-fibrillation flame-retardant lyocell fiber, comprising S1: mixing lyocell fiber with sodium alginate solution;
[0007] S2: mixing the lyocell fiber adsorbed with the sodium alginate solution with a protective solution to form a protective layer on the surface of the lyocell fiber;
[0008] S3: Lyocell fiber is then mixed with the crosslinking agent solution;
[0009] S4: heating the lyocell fiber adsorbed with the crosslinking agent solution to crosslink the fiber.
[0010] In this solution, a protective layer is formed on the surface of the lyocell fiber, thereby improving the flame retardancy of the lyocell fiber. Then, the lyocell fiber is mixed with a cross-linking agent and heated for cross-linking, thereby strengthening the chemical interaction between the protective layer and the lyocell fiber. The protective layer on the surface of the lyocell fiber will not fall off during multiple washings, thereby solving the shortcomings of the lyocell fiber in the prior art.
[0011] Preferably, in order to remove the impurity solvent adsorbed on the surface of the lyocell fiber and avoid the impurity solvent affecting the treatment of the lyocell fiber, the scheme also includes S0, washing the lyocell fiber.
[0012] In this solution, the Lyocell fiber is washed with water to remove the impurity solvent adsorbed by the Lyocell fiber during the preparation process, thereby ensuring that the impurity solvent will not affect the subsequent treatment of the Lyocell fiber, and the treatment effect of the Lyocell fiber is better.
[0013] Preferably, after the lyocell fiber is washed, in order to remove excess liquid absorbed by the lyocell fiber, in S0 described in this solution, the lyocell fiber is dehydrated after washing.
[0014] In this solution, after the lyocell fiber is washed, the lyocell fiber is dehydrated, and the dehydration process can remove the clean water adsorbed on the lyocell fiber, ensuring that the clean water will not dilute the subsequent solution content. At the same time, the dehydration process also reduces the water content of the lyocell fiber.
[0015] In order to ensure that the processing of the lyocell fiber and the preparation of the lyocell fiber tow are performed asynchronously, in S0 described in this scheme, the lyocell fiber tow is washed with water, and after washing, the lyocell fiber tow is cut into lyocell staple fibers.
[0016] In this solution, the prepared lyocell fiber tow will be cut to form lyocell staple fibers. Therefore, the preparation speed of the lyocell fiber tow can be inconsistent with the processing speed of the lyocell staple fibers, so that the lyocell staple fibers can be processed at a more suitable speed without being affected by external factors, and the processing effect of the lyocell staple fibers is better.
[0017] Preferably, in order to ensure a better mixing effect of the lyocell fiber with the sodium alginate solution, the protective solution and the cross-linking agent solution, in S1, S2, S3 and S4 of this solution, the lyocell fiber is a lyocell staple fiber.
[0018] In this solution, the lyocell staple fibers can be laid so that the lyocell staple fibers can be in more complete contact with the sodium alginate solution, the protective solution and the cross-linking agent solution, thereby achieving a better mixing effect.
[0019] Preferably, in order to ensure that the protective solution can form a protective layer with the sodium alginate solution, the protective solution in this embodiment is a MgCl2 solution, a FeCl3 solution or a CaCl2 solution.
[0020] In this solution, the protective solution is set to MgCl2 solution, FeCl3 solution or CaCl2 solution. MgCl2 solution can form a magnesium alginate protective layer with sodium alginate solution to improve the flame retardancy of Lyocell staple fibers. FeCl3 solution can form an iron alginate protective layer with sodium alginate solution to improve the flame retardancy of Lyocell staple fibers. CaCl2 solution can form a calcium alginate protective layer with sodium alginate solution to improve the flame retardancy of Lyocell staple fibers.
[0021] Preferably, in order to ensure a higher processing efficiency of the lyocell fibers, in S1 of the present solution, the lyocell fibers are mixed with the sodium alginate solution by spraying.
[0022] In this solution, the lyocell fiber and the sodium alginate solution are mixed by spraying. Therefore, compared with the method of immersing the lyocell fiber into the sodium alginate solution, there are no steps of immersing and removing the lyocell fiber, which can obviously improve the processing efficiency of the lyocell fiber.
[0023] In order to ensure a higher processing efficiency of the lyocell fibers, in S2 of the present solution, the lyocell fibers are mixed with the protective solution by spraying.
[0024] In this solution, the lyocell fiber is mixed with the protective solution by spraying. Therefore, compared with the method of immersing the lyocell fiber into the protective solution, there are no steps of immersing and removing the lyocell fiber, which can obviously improve the processing efficiency of the lyocell fiber.
[0025] In order to ensure a higher processing efficiency of the lyocell fibers, in S3 of the present solution, the lyocell fibers are mixed with the crosslinking agent solution by spraying.
[0026] In this solution, the lyocell fiber and the crosslinking agent solution are mixed by spraying. Therefore, compared with the method of immersing the lyocell fiber into the crosslinking agent solution, there are no steps of immersing and removing the lyocell fiber, which can obviously improve the processing efficiency of the lyocell fiber.
[0027] Preferably, in order to ensure a higher utilization rate of the sodium alginate solution, in S1 of this solution, after the lyocell fiber is mixed with the sodium alginate solution, excess sodium alginate solution adsorbed by the lyocell fiber is removed.
[0028] In this solution, after the excess sodium alginate solution is removed, the sodium alginate solution can be reused, thereby improving the utilization rate of the sodium alginate solution. At the same time, after the excess sodium alginate solution is removed, the sodium alginate solution is prevented from affecting the subsequent treatment of the lyocell fiber, and the treatment effect of the lyocell fiber is higher.
[0029] In order to ensure a higher utilization rate of the protective solution, in S2 of this solution, after the lyocell fiber is mixed with the protective solution, the excess protective solution adsorbed by the lyocell fiber is removed.
[0030] In this solution, after the excess protective solution is removed, the protective solution can be reused, thereby improving the utilization rate of the protective solution. At the same time, after the excess protective solution is removed, the protective solution is prevented from affecting the subsequent treatment of the lyocell fiber, and the treatment effect of the lyocell fiber is higher.
[0031] In order to ensure a higher utilization rate of the sodium alginate solution, in S3 of this solution, after the lyocell fiber is mixed with the cross-linking agent solution, the excess cross-linking agent solution adsorbed by the lyocell fiber is removed.
[0032] In this solution, after the excess cross-linking agent solution is removed, the cross-linking agent solution can be reused, thereby improving the utilization rate of the cross-linking agent solution. At the same time, after the excess cross-linking agent solution is removed, the cross-linking agent solution is prevented from affecting the subsequent treatment of the lyocell fiber, and the treatment effect of the lyocell fiber is higher.
[0033] Preferably, in order to solve the problem of sodium alginate solution leakage, in S1 of this solution, the sodium alginate solution separated from the lyocell fiber is recovered.
[0034] In this scheme, the sprayed sodium alginate solution is recovered, and the removed excess sodium alginate solution is recovered, and the sodium alginate solution will not leak to the outside. At the same time, the sodium alginate solution is reused to improve the utilization rate of the sodium alginate solution.
[0035] In order to solve the problem of leakage of the protective solution, in S2 of this solution, the protective solution separated from the lyocell fiber is recovered.
[0036] In this solution, the sprayed protective solution is recovered, and the removed excess protective solution is recovered, and the protective solution will not leak to the outside. At the same time, the protective solution is reused to improve the utilization rate of the protective solution.
[0037] In order to solve the problem of leakage of the crosslinking agent solution, in S3 of this scheme, the protective solution separated from the lyocell fiber is recovered.
[0038] In this solution, the sprayed cross-linking agent solution is recovered, and the removed excess cross-linking agent solution is recovered, and the cross-linking agent solution will not leak to the outside. At the same time, the cross-linking agent solution is reused, thereby improving the utilization rate of the cross-linking agent solution.
[0039] Preferably, in this embodiment, the solubility of the sodium alginate solution is preferably 0.5wt% to 2.0wt%.
[0040] In order to solve the problem that the flame retardant properties of lyocell fibers are lost during multiple washing processes in the prior art, the second aspect of the present invention provides a preparation system for anti-fibrillation flame retardant lyocell fibers, comprising:
[0041] A conveying device, the conveying device is used to convey the lyocell fibers to move;
[0042] A sodium alginate solution spraying device, the sodium alginate solution spraying device is arranged corresponding to the conveying device, and the sodium alginate solution spraying device is used to spray the sodium alginate solution onto the lyocell fiber;
[0043] A protective solution spraying device, which is arranged corresponding to the conveying device and is located at the rear end of the sodium alginate solution spraying device, and is used to spray a protective solution onto the lyocell fiber;
[0044] A cross-linking agent spraying device, which is arranged corresponding to the conveying device and is located at the rear end of the protective solution spraying device, and is used to spray the cross-linking agent solution onto the lyocell fiber;
[0045] A heating cross-linking device is provided corresponding to the conveying device and is located at the rear end of the cross-linking agent spraying device. The heating cross-linking device is used to achieve heating cross-linking of the lyocell fiber.
[0046] The beneficial effects of the present invention are as follows: First, in this solution, a protective layer is formed on the surface of the lyocell fiber, thereby improving the flame retardancy of the lyocell fiber.
[0047] Secondly, by mixing the lyocell fiber with a crosslinking agent and heating and crosslinking, the crosslinking reaction strengthens the chemical interaction between the protective layer and the lyocell fiber, ensuring that the protective layer on the surface of the lyocell fiber will not fall off during multiple washings, thus solving the shortcomings of the lyocell fiber in the prior art.
[0048] Thirdly, this solution improves the flame retardant properties of Lyocell fiber and also improves the anti-fibrillation effect of Lyocell fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 This is a schematic diagram of the preparation method of the anti-fibrillation flame-retardant Lyocell fiber in Example 1.
[0050] Figure 2 This is a schematic diagram of the preparation system of the anti-fibrillation flame-retardant Lyocell fiber in Example 4.
[0051] Figure 3 These are optical microscope images of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3.
[0052] The reference numerals include: a conveying device 1, a sodium alginate solution spraying device 2, a protective solution spraying device 3, a first water washing device 4, a cross-linking agent spraying device 5, a heating cross-linking device 6, a second water washing device 7, a first recovery tank 8, a first extrusion device 9, a second recovery tank 10, a second extrusion device 11, a third recovery tank 12, a third extrusion device 13, a fourth recovery tank 14, a fourth extrusion device 15, a fifth recovery tank 16, and a fifth extrusion device 17. DETAILED DESCRIPTION
[0053] In order to make the purpose, technical solutions and advantages of the embodiments more clear, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present disclosure. Instead, they are only examples of devices and methods consistent with some aspects of the present disclosure as detailed in the attached claims.
[0054] In the present disclosure, unless otherwise stated, the directional words used, such as "inside" and "outside", are defined according to the corresponding parts' own contours. The terms used in the present disclosure, such as "first" and "second", etc., are used to distinguish one element from another element and do not have order and importance.
[0055] Example 1
[0056] Basically as attached Figure 1 As shown, a method for preparing anti-fibrillation flame-retardant Lyocell fiber can make the Lyocell fiber have flame-retardant properties and ensure that the flame-retardant properties of the Lyocell fiber will not be significantly reduced during multiple washing processes.
[0057] The method for preparing the anti-fibrillation flame-retardant Lyocell fiber in the embodiment of the present disclosure specifically comprises the following steps:
[0058] S0, washing the lyocell fiber tow, and cutting the washed lyocell fiber tow to prepare lyocell staple fibers.
[0059] The Lyocell staple fibers are then dehydrated by squeezing, and the moisture content of the dehydrated Lyocell staple fibers is 45%, and the length of the staple fibers after cutting is 42 mm.
[0060] In the disclosed embodiment, the lyocell fiber tow can be purchased from outside or prepared by itself. At the same time, after the lyocell fiber tow undergoes the water washing process, the water washing can remove the impurity solvent remaining in the lyocell fiber tow, thereby preventing the impurity solvent from affecting the subsequent processing process. In the water washing process, in order to avoid liquid leakage and pollution of the environment, the bottom of the water washing spray device can be configured with a receiving container to realize the liquid receiving and recycling.
[0061] In the disclosed embodiment, by cutting the lyocell tow into lyocell staple fibers, the processing speed of the lyocell fiber tow can be ignored when the lyocell staple fibers are processed, and the preparation of the lyocell tow and the lyocell staple fibers can be processed asynchronously. That is, even if the processing speed of the lyocell fiber tow is fast, the lyocell staple fibers can still be processed at a slower speed, and the processing of the lyocell staple fibers will not be affected, so the processing of the lyocell staple fibers is more flexible.
[0062] In the embodiments of the present disclosure, if the lyocell staple fibers are prepared by themselves, the following method can be used:
[0063] The cellulose pulp is crushed and dissolved in an aqueous solution of N-methylmorpholine-N-oxide (NMMO) to form a cellulose solution, and then the solution is filtered and wet-spun by dry jet spinning to finally obtain a lyocell fiber tow, wherein the concentration of the cellulose solution is 12 wt%.
[0064] S1, mixing the lyocell staple fibers with the sodium alginate solution, and removing the excess sodium alginate solution through an extrusion process. At the same time, in order to ensure the recycling of the sodium alginate solution and avoid leakage of the sodium alginate solution, the extruded sodium alginate solution is recycled for secondary use.
[0065] The sodium alginate solution in the embodiment of the present disclosure can be purchased or prepared by itself. The concentration of sodium alginate in the sodium alginate solution is 1.0 wt %, and the temperature of the sodium alginate solution is 60°C.
[0066] In the embodiment of the present disclosure, a first recovery tank is provided below the squeezing device, and the first recovery tank can receive the squeezed sodium alginate solution to prevent leakage of the sodium alginate solution. The recovered sodium alginate solution can be reused, thereby improving the utilization rate of the sodium alginate solution.
[0067] In order to make lyocell staple fiber and sodium alginate solution fully mixed, the sodium alginate solution and lyocell staple fiber can be mixed by immersion or spraying in the disclosed embodiment. Meanwhile, it is more preferred to use spraying to mix sodium alginate solution and lyocell staple fiber. When the sodium alginate solution and lyocell staple fiber are mixed by spraying, the lyocell staple fiber does not need to be immersed in the inside of the sodium alginate solution and taken out from the lyocell staple fiber, so the processing efficiency is higher. Of course, when the sodium alginate solution and lyocell staple fiber are mixed by spraying, the first recovery tank can also receive the sodium alginate solution sprayed by the spraying device, thereby preventing the sodium alginate solution from leaking. Meanwhile, the sodium alginate solution recovered from the first recovery tank can be sprayed on the lyocell fiber again, thereby improving the utilization rate of the sodium alginate solution.
[0068] S2, mixing the lyocell staple fibers adsorbed with the sodium alginate solution with a protective solution, so that a protective layer is formed on the surface of the lyocell fibers. The protective solution may be a MgCl2 solution, a FeCl3 solution or a CaCl2 solution.
[0069] When the protective solution is MgCl2 solution, the sodium alginate solution reacts with the MgCl2 solution to form magnesium alginate on the surface of the Lyocell staple fiber, which protects the Lyocell staple fiber and improves the flame retardant properties of the Lyocell staple fiber; when the protective solution is FeCl3 solution, the sodium alginate solution reacts with the FeCl3 solution to form iron alginate on the surface of the Lyocell staple fiber, which protects the Lyocell staple fiber and improves the flame retardant properties of the Lyocell staple fiber; when the protective solution is CaCl2 solution, the sodium alginate solution reacts with the CaCl2 solution to form calcium alginate on the surface of the Lyocell staple fiber, which protects the Lyocell staple fiber and improves the flame retardant properties of the Lyocell staple fiber.
[0070] It should be noted that the MgCl2 solution, FeCl3 solution or CaCl2 solution in the embodiments of the present disclosure can be prepared by purchasing from outside or preparing by oneself.
[0071] After the lyocell staple fibers are mixed with the protective solution, the lyocell staple fibers can be squeezed by the squeezing device to remove the excess protective solution adsorbed on the lyocell staple fibers. Of course, in order to ensure that the squeezed protective solution does not leak, a second recovery tank is provided below the squeezing device in the disclosed embodiment, and the second recovery tank can receive the squeezed protective solution to avoid leakage of the protective solution. And the recovered protective solution can be sprayed onto the lyocell fibers again, and the protective solution is reused to improve the utilization rate of the protective solution.
[0072] In order to make the lyocell staple fiber and the protective solution fully mixed, the protective solution and the lyocell staple fiber can be mixed by immersion or spraying in the disclosed embodiment. At the same time, it is more preferred to use a spraying method to mix the protective solution and the lyocell staple fiber. When the protective solution and the lyocell staple fiber are mixed by spraying, the lyocell staple fiber does not need to be completely immersed in the protective solution, nor does it need to be taken out from the protective solution, so the processing efficiency is higher. Of course, when the protective solution and the lyocell staple fiber are mixed by spraying, the second recovery tank can also receive the protective solution leaked by the spraying device, thereby preventing the protective solution from leaking, thereby improving the utilization rate of the protective solution.
[0073] S2.5, lyocell staple fibers are washed.
[0074] In order to ensure that the protective solution on the lyocell staple fibers is removed more thoroughly in the disclosed embodiment, the squeezed lyocell staple fibers in the disclosed embodiment can also be subjected to a water washing process to remove the protective solution. The water washing temperature in the disclosed embodiment is 25°C.
[0075] S3, mixing the lyocell staple fibers with the crosslinking agent solution.
[0076] In the disclosed embodiment, the lyocell staple fibers are mixed with a crosslinking agent solution, and the lyocell staple fibers absorb the crosslinking agent.
[0077] The crosslinking agent solution in the embodiment of the present disclosure contains a crosslinking agent 1,3,5-triacryloylhexahydro-1,3,5-triazine (TAHT), Na2SO4 and Na2CO3. The concentration of the crosslinking agent 1,3,5-triacryloylhexahydro-1,3,5-triazine (TAHT) in the crosslinking agent solution is 0.5wt%, the concentration of Na2SO4 is 1.0wt%, and the concentration of Na2CO3 is 1.0wt%. The temperature of the crosslinking agent solution is 60°C.
[0078] After the lyocell staple fibers are mixed with the crosslinking agent solution, the lyocell staple fibers can be squeezed by the squeezing device to remove the excess crosslinking agent solution adsorbed on the lyocell staple fibers. Of course, in order to ensure that the squeezed crosslinking agent solution does not leak, a third recovery tank is provided below the squeezing device in the disclosed embodiment, and the third recovery tank can receive the squeezed crosslinking agent solution to avoid leakage of the crosslinking agent solution. And the recovered crosslinking agent solution can be sprayed onto the lyocell fibers again, thereby improving the utilization rate of the crosslinking agent solution.
[0079] In order to make the lyocell staple fiber and the crosslinking agent solution fully mixed, the crosslinking agent solution and the lyocell staple fiber can be mixed by immersion or spraying in the disclosed embodiment. At the same time, it is more preferred to use a spraying method to mix the crosslinking agent solution and the lyocell staple fiber. When the crosslinking agent solution and the lyocell staple fiber are mixed by spraying, the lyocell staple fiber does not need to be completely immersed in the crosslinking agent solution, so the processing efficiency is higher. Of course, when the crosslinking agent solution and the lyocell staple fiber are mixed by spraying, the third recovery tank can also receive the crosslinking agent solution leaked by the spraying device, thereby preventing the crosslinking agent solution from leaking, thereby improving the utilization rate of the crosslinking agent solution.
[0080] S4, cross-linking the lyocell fibers adsorbed with the cross-linking agent solution by steam heating.
[0081] The steam heating reaction temperature is 120°C and the heating reaction time is 20 min.
[0082] In the disclosed embodiment, the chemical interaction between the fiber surface protective layer and the cellulose fiber can be greatly enhanced by the cross-linking reaction. Therefore, during multiple washings, the protective layer of the lyocell staple fiber will not fall off in large quantities, and the flame retardant properties of the lyocell staple fiber will not be lost.
[0083] S5, washed cross-linked lyocell staple fibers.
[0084] When the water washing process is performed in the embodiment of the present disclosure, the water washing temperature is 25°C.
[0085] After the lyocell staple fibers are cross-linked in the disclosed embodiment, the cross-linking agent solution remaining in the lyocell staple fibers is removed by water washing. In order to receive the liquid after water washing and avoid leakage, a fourth recovery tank is provided below the water washing device in the disclosed embodiment, and the fourth recovery tank can receive and recover the liquid after water washing.
[0086] Example 2
[0087] Compared with Example 1, the concentration of the sodium alginate solution in this embodiment is 0.5 wt %.
[0088] The other process steps and the equipment used are the same as those in Example 1 and will not be described again. Finally, anti-fibrillation flame-retardant lyocell staple fibers are obtained.
[0089] Example 3
[0090] Compared with Example 1, the concentration of the sodium alginate solution in this embodiment is 2.0 wt %.
[0091] The other process steps and the equipment used are the same as those in Example 1 and will not be described again. Finally, anti-fibrillation flame-retardant lyocell staple fibers are obtained.
[0092] Comparative Example 1
[0093] Compared with Example 1, the concentration of the sodium alginate solution in the comparative example is 0.2 wt %.
[0094] The other process steps and the equipment used are the same as those in Example 1 and will not be described again. Finally, anti-fibrillation flame-retardant lyocell staple fibers are obtained.
[0095] Comparative Example 2
[0096] Compared with Example 1, the concentration of the sodium alginate solution in the comparative example is 5.0 wt %.
[0097] The other process steps and the equipment used are the same as those in Example 1 and will not be described again. Finally, anti-fibrillation flame-retardant lyocell staple fibers are obtained.
[0098] Comparative Example 3
[0099] Compared with Example 1, in this comparative example, the lyocell staple fibers are not mixed with the crosslinking agent, and the lyocell staple fibers mixed with the crosslinking agent are not placed in a steam heating device for crosslinking reaction.
[0100] The other process steps and the equipment used are the same as those in Example 1 and will not be described again. Finally, anti-fibrillation flame-retardant lyocell staple fibers are obtained.
[0101] Comparative Example 4
[0102] Compared with Example 1, in this comparative example, the lyocell staple fibers are not mixed with the sodium alginate solution, nor are the lyocell staple fibers mixed with the protective solution.
[0103] The other process steps and the equipment used are the same as those in Example 1 and will not be described again. Finally, anti-fibrillation flame-retardant lyocell staple fibers are obtained.
[0104] The lyocell staple fibers prepared in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 4 were tested using an ultrasonic cell disruptor (LICHEN, LC-JY92-IIN) and observed under a microscope. The fewer microfibrils peeled off from the fiber surface, the stronger the anti-fibrillation ability of the fiber.
[0105] The specific test method is as follows: the short fiber sample is immersed in deionized water to obtain a dispersion, and the bath ratio (fiber / deionized water) is 1 mg / mL. Then, the dispersion is placed in an ice water bath at 0°C and the dispersion is ultrasonically treated. Then the fiber is taken out and the surface moisture is removed. The distance between the ultrasonic probe and the bottom of the dispersion is 10 mm, the ultrasonic power is 500 W, and the ultrasonic treatment time is 20 min.
[0106] The specific operation method of microscopic observation is as follows: take multiple samples from the treated short fibers, place them on a clean glass slide, add glycerol to disperse the fiber samples, cover them with a glass slide, place them under a microscope with a digital camera attachment for observation, and take pictures after adjusting the magnification to a clear level.
[0107] Table 1 Lyocell staple fiber related performance indicators in different embodiments and comparative examples
[0108]
[0109]
[0110] The following conclusions can be drawn from the results in Table 1:
[0111] (1) By comparing Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2, it can be seen that the concentration of sodium alginate has a great influence on the preparation method of the present application.
[0112] As shown in Comparative Example 1, when the sodium alginate concentration is 0.2 wt%, the flame retardant properties of the lyocell staple fibers are significantly reduced, resulting in the fiber limiting oxygen index LOI (washed 50 times) being lower than 27%, which cannot reach the level of flame retardant materials.
[0113] As shown in Example 2, when the sodium alginate concentration is 0.5wt%, the flame retardant property of the lyocell staple fiber is good, and the fiber limiting oxygen index LOI (washed 50 times) is 27%, which has a good flame retardant effect.
[0114] As shown in Example 1, when the sodium alginate concentration is 1.0wt%, the flame retardant property of the lyocell staple fiber is good, and the fiber limiting oxygen index LOI (washed 50 times) is 28%, which has a good flame retardant effect.
[0115] As shown in Example 3, when the sodium alginate concentration is 2.0wt%, the flame retardant property of the lyocell staple fiber is good, and the fiber limiting oxygen index LOI (washed 50 times) is 30%, which has a good flame retardant effect.
[0116] As shown in Comparative Example 2, when the sodium alginate concentration is 5.0wt%, although the flame retardant properties of the fiber are improved (reaching 33%), the flame retardant properties are not improved much compared to when the sodium alginate concentration is 2.0wt%. On the contrary, the linear density of the lyocell staple fiber is significantly increased (reaching 1.63dtex), and the linear density deviation rate is significantly increased (reaching 22.3%), the thickness of the lyocell staple fiber is uneven, and at the same time, the dry breaking strength (3.93cN / dtex) and dry breaking elongation (8.21%) of the lyocell staple fiber are significantly reduced.
[0117] Therefore, only when the concentration of sodium alginate is within a certain range, i.e. 0.5-2.0wt%, the prepared lyocell staple fiber not only has good flame retardant properties (limiting oxygen index LOI>27%), but also does not cause an increase in the linear density of the lyocell staple fiber, nor does it lead to a significant decrease in the fiber's dry breaking strength and dry breaking elongation.
[0118] (2) By comparing Example 1 and Comparative Example 3, it can be seen that whether the lyocell staple fibers are cross-linked has a strong influence on whether they can maintain good flame retardant properties after washing.
[0119] As shown in Example 1, the flame retardant properties of the Lyocell staple fibers after the cross-linking reaction are good, and the fiber limiting oxygen index LOI (washed 50 times) is 28%, and the good flame retardant properties can still be maintained even after washing 50 times.
[0120] As shown in Comparative Example 3, the lyocell staple fibers prepared without cross-linking reaction have a fiber limiting oxygen index LOI (washed 50 times) lower than 27%, which cannot reach the level of flame retardant materials.
[0121] As can be seen from the above, after the cross-linking reaction, the cross-linking reaction can increase the chemical interaction between the inside and the surface of the Lyocell fiber, preventing the Lyocell fiber from fibrillating. At the same time, it can also enhance the adhesion of the protective layer on the fiber surface, thereby improving the water washing resistance of the Lyocell fiber and greatly reducing the effect of water washing on the flame retardant properties of the fiber.
[0122] (3) By comparing Example 1 with Comparative Example 4, it can be seen that the flame retardant properties of the Lyocell fibers can be improved by sequentially mixing the Lyocell staple fibers with the sodium alginate solution and the protective solution.
[0123] It can be concluded from Comparative Example 4 that when the lyocell staple fibers are not mixed with the sodium alginate solution and the protective solution, the fiber limiting oxygen index LOI (washed 50 times) is lower than 27%, which cannot reach the level of flame retardant materials.
[0124] It can be concluded from Example 1 that after the lyocell staple fibers are mixed with the sodium alginate solution and the protective solution, the fiber limiting oxygen index LOI (washed 50 times) is 28%, which has a good flame retardant effect.
[0125] As can be seen from the above, by introducing sodium alginate to coat the lyocell fiber, and then mixing the lyocell fiber with a protective solution, the sodium alginate reacts with the protective solution to form a protective layer, and then through a cross-linking reaction, the anti-fibrillation flame-retardant lyocell fiber can be finally obtained.
[0126] (4) It can be seen from Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 that the lyocell fibers prepared in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 not only have strong flame retardant properties, but also have strong anti-fibrillation properties.
[0127] The lyocell staple fibers prepared in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 were crushed by an ultrasonic cell crusher and observed under a microscope. The surface of the lyocell staple fibers had few microfibers peeled off (see also Figure 3 ), and has strong anti-fibrillation performance.
[0128] The lyocell staple fibers prepared in Comparative Example 3 were crushed by an ultrasonic cell crusher and observed under a microscope. It was found that a large number of microfibers were peeled off from the surface of the lyocell staple fibers (see also Figure 3 ), and its anti-fibrillation performance is poor.
[0129] Example 4
[0130] The present embodiment discloses a preparation system of anti-fibrillation flame-retardant lyocell fiber, which specifically includes a conveying device 1, a sodium alginate solution spraying device 2, a protective solution spraying device 3, a first water washing device 4, a cross-linking agent spraying device 5, a heating cross-linking device 6 and a second water washing device 7.
[0131] In the disclosed embodiment, the conveying device 1 is mainly used for laying the lyocell staple fibers flatly and conveying the lyocell staple fibers to move, thereby ensuring that the lyocell staple fibers can be processed in different ways.
[0132] The conveying device 1 is preferably a mesh conveyor belt, which mainly includes a mesh belt, a transmission roller, a support roller, a drive motor and a frame. The transmission roller, the support roller and the drive motor are all installed on the frame, and the transmission roller and the support roller are respectively arranged at both ends, and a mesh belt is arranged between the transmission roller and the support roller as a transmission power. The transmission roller is connected to the output shaft of the drive motor in a transmission manner. In other words, when the drive motor is working, the drive motor drives the transmission roller to rotate. Since the mesh belt is installed on the transmission roller, when the transmission roller rotates, the mesh belt rotates accordingly. The upper surface of the mesh belt is used for evenly laying and placing the lyocell staple fibers. The specific structure of the mesh conveyor belt can also refer to the conventional mesh conveyor belt in the prior art.
[0133] It should be noted that, since the conveying device 1 in the embodiment of the present invention adopts a mesh conveyor belt, when the sodium alginate solution, the protective solution and the cross-linking agent solution are sprayed onto the lyocell staple fibers, the sodium alginate solution, the protective solution and the cross-linking agent solution can drip downward from the gaps in the mesh belt, and the sodium alginate solution, the protective solution and the cross-linking agent solution will not be blocked. The sodium alginate solution, the protective solution and the cross-linking agent solution can be recovered, thereby increasing the recovery amount of the sodium alginate solution, the protective solution and the cross-linking agent solution.
[0134] The sodium alginate solution spraying device 2 in the disclosed embodiment may be a spraying device with a spraying function in the prior art, and the spraying device may spray the sodium alginate solution downward.
[0135] The sodium alginate solution spraying device 2 is specifically installed above the conveying device 1. The sodium alginate solution spraying device 2 is used to spray the sodium alginate solution on the top of the conveying device 1 so that the sodium alginate solution is fully in contact with the lyocell staple fibers. In order to ensure that the sodium alginate solution spraying device 2 can be stably installed above the conveying device 1, during implementation, the sodium alginate solution spraying device 2 can be installed on a bracket or a ceiling, etc., to achieve stable installation of the sodium alginate solution spraying device 2, and to be located above the conveying device 1.
[0136] It should be noted that: since the lyocell staple fibers are laid on the mesh belt, the lyocell staple fibers can fully contact with the sodium alginate solution after the sodium alginate solution spraying device 2 sprays the sodium alginate solution. At the same time, the conveying device 1 drives the lyocell staple fibers to move, which has a higher production efficiency than using an immersion method to make the sodium alginate solution contact with the lyocell staple fibers.
[0137] After the sodium alginate solution is sprayed onto the lyocell staple fibers, in order to solve the problem of waste of the sodium alginate solution, it is necessary to involve the recovery of the sodium alginate solution. Therefore, in the disclosed embodiment, the first recovery tank 8 is arranged below the conveying device 1. After the sodium alginate solution is sprayed onto the lyocell staple fibers, the sodium alginate solution drips downward, and the sodium alginate solution passes through the conveying device 1 and drips into the first recovery tank 8, thereby realizing the recovery of the sodium alginate solution. At the same time, in order to realize the reuse of the sodium alginate solution, the first recovery tank 8 can be connected to the sodium alginate solution spraying device 2. The sodium alginate solution recovered by the first recovery tank 8 can be continued to be sprayed and used by the sodium alginate solution spraying device 2.
[0138] At the same time, in order to remove the excess sodium alginate solution adhering to the lyocell staple fibers, a first squeezing device 9 is provided in the embodiment of the present disclosure. The first squeezing device 9 includes a squeezing roller, and two squeezing rollers are provided, one above and one below. The squeezing roller can be installed on a frame. The gap between the upper and lower squeezing rollers is for the mesh belt in the conveying device 1 to pass through. Each squeezing roller is connected to a driving motor in a transmission manner. The driving motor drives the squeezing roller to rotate.
[0139] Take an application scenario as an example: when the lyocell staple fibers are on the surface of the mesh belt, the lyocell staple fibers pass through the gap between the upper and lower pressing rollers. The pressing rollers separate the lyocell staple fibers from the adhered sodium alginate solution. The separated sodium alginate solution enters the first recovery tank 8 to prevent leakage of the sodium alginate solution.
[0140] In the embodiment of the present disclosure, the protective solution spraying device 3 may be a spraying device with a spraying function in the prior art, and the spraying device may spray the protective solution downwards. The protective solution may be a MgCl2 solution, a FeCl3 solution or a CaCl2 solution.
[0141] The protective solution spraying device 3 is specifically installed above the conveying device 1 and is located at the rear end of the sodium alginate solution spraying device 2, so that the lyocell staple fibers adsorbed with the sodium alginate solution can contact with the protective solution.
[0142] In the disclosed embodiment, the protective solution spraying device 3 is used to spray the protective solution onto the top of the conveying device 1, so that the protective solution is in full contact with the lyocell staple fibers. In order to ensure that the protective solution spraying device 3 can be stably installed above the conveying device 1, during implementation, the protective solution spraying device 3 can be installed on a bracket or a ceiling, etc., to achieve a stable installation of the protective solution spraying device 3, and to be located above the conveying device 1.
[0143] It should be noted that: since the lyocell staple fibers are laid on the mesh belt, after the protective solution spraying device 3 sprays the protective solution, the lyocell staple fibers can fully contact with the protective solution, and a protective layer is formed on the surface of the lyocell staple fibers.
[0144] After the protective solution is sprayed onto the lyocell staple fibers, in order to solve the problem of waste of the protective solution, it is necessary to recycle the protective solution. Therefore, in the embodiment of the present disclosure, the second recovery tank 10 is arranged below the conveying device 1. After the protective solution is sprayed onto the lyocell staple fibers, the protective solution drips downward, passes through the conveying device 1 and drips into the second recovery tank 10, so as to realize the recovery of the protective solution. At the same time, in order to realize the reuse of the protective solution, the second recovery tank 10 can be connected to the protective solution spraying device 3. The protective solution recovered by the second recovery tank 10 can be sprayed and used by the protective solution spraying device 3.
[0145] At the same time, in order to remove the excess protective solution adhering to the lyocell staple fibers, a second squeezing device 11 is provided in the embodiment of the present disclosure. The second squeezing device 11 includes a squeezing roller, and two squeezing rollers are provided, one above and one below. The squeezing roller can be installed on a frame. The gap between the upper and lower squeezing rollers is for the mesh belt in the conveying device 1 to pass through. Each squeezing roller is connected to a driving motor. The driving motor drives the squeezing roller to rotate.
[0146] Take an application scenario as an example: when the lyocell staple fibers are on the surface of the mesh belt, the lyocell staple fibers pass through the gap between the upper and lower pressing rollers. The pressing rollers separate the lyocell staple fibers from the adhered protective solution. The separated protective solution enters the second recovery tank 10 to prevent leakage of the protective solution.
[0147] In the disclosed embodiment, the first washing device 4 is also a spraying device, which mainly sprays the cleaning liquid downward to wash the lyocell fibers.
[0148] The first water washing device 4 is specifically installed above the conveying device 1 and is located at the rear end of the protective solution spraying device 3. The first water washing device 4 can remove the excess protective solution adsorbed on the lyocell staple fibers.
[0149] In the disclosed embodiment, the first washing device 4 is used to spray cleaning liquid onto the top of the conveying device 1, so that the cleaning liquid is in full contact with the lyocell staple fibers. In order to ensure that the cleaning liquid spraying device can be stably installed above the conveying device 1, during implementation, the cleaning liquid spraying device can be installed on a bracket or a ceiling, etc., to achieve stable installation of the cleaning liquid spraying device, and to be located above the conveying device 1.
[0150] When the cleaning liquid is sprayed onto the lyocell staple fibers, in order to solve the problem of waste of the cleaning liquid, it is necessary to recover the cleaning liquid. Therefore, in the embodiment of the present disclosure, the third recovery tank 12 is arranged below the conveying device 1. When the cleaning liquid is sprayed onto the lyocell staple fibers, the cleaning liquid drips downward, passes through the conveying device 1 and drips into the third recovery tank 12, thereby recovering the cleaning liquid and preventing leakage of the cleaning liquid.
[0151] At the same time, in order to remove the excess cleaning liquid adhering to the lyocell staple fibers, a third squeezing device 13 is provided in the embodiment of the present disclosure. The third squeezing device 13 includes a squeezing roller, and two squeezing rollers are provided, one above and one below. The squeezing roller can be installed on a frame. The gap between the upper and lower squeezing rollers is for the mesh belt in the conveying device 1 to pass through. Each squeezing roller is connected to a driving motor in a transmission manner. The driving motor drives the squeezing roller to rotate.
[0152] Take an application scenario as an example: when the lyocell staple fibers are on the surface of the mesh belt, the lyocell staple fibers pass through the gap between the upper and lower pressing rollers. The pressing rollers separate the lyocell staple fibers from the adhered cleaning liquid. The separated cleaning liquid enters the third recovery tank 12 to prevent leakage of the cleaning liquid.
[0153] In the embodiment of the present disclosure, the cross-linking agent spraying device 5 may be a spraying device with a spraying function in the prior art, and the spraying device may spray the cross-linking agent solution downward.
[0154] The crosslinking agent spraying device 5 is specifically installed above the conveying device 1. The crosslinking agent spraying device 5 is used to spray the crosslinking agent to the top of the conveying device 1 so that the crosslinking agent is fully in contact with the lyocell staple fibers. In order to ensure that the crosslinking agent spraying device 5 can be stably installed above the conveying device 1, during implementation, the crosslinking agent spraying device 5 can be installed on a bracket or a ceiling, etc., to achieve stable installation of the crosslinking agent spraying device 5, and to be located above the conveying device 1.
[0155] It should be noted that: since the lyocell staple fibers are laid on the mesh belt, the lyocell staple fibers can fully contact with the crosslinking agent after the crosslinking agent spraying device 5 sprays the crosslinking agent. At the same time, the conveying device 1 drives the lyocell staple fibers to move, which is more efficient than using an immersion method to allow the crosslinking agent to contact with the lyocell staple fibers.
[0156] When the cross-linking agent is sprayed onto the lyocell staple fibers, in order to solve the problem of cross-linking agent waste, it is necessary to recycle the cross-linking agent. Therefore, in the disclosed embodiment, the fourth recovery tank 14 is arranged below the conveying device 1. When the cross-linking agent is sprayed onto the lyocell staple fibers, the cross-linking agent drips downward, passes through the conveying device 1 and drips into the fourth recovery tank 14, so that the cross-linking agent is recycled. At the same time, in order to realize the reuse of the cross-linking agent, the fourth recovery tank 14 can be connected to the cross-linking agent spraying device 5, and the cross-linking agent recovered by the fourth recovery tank 14 can be sprayed and used by the cross-linking agent spraying device 5.
[0157] At the same time, in order to remove the excess crosslinking agent adhered to the lyocell staple fibers, a fourth squeezing device 15 is provided in the embodiment of the present disclosure. The fourth squeezing device 15 includes a squeezing roller, and two squeezing rollers are provided, one above and one below. The squeezing roller can be installed on a frame. The gap between the upper and lower squeezing rollers is for the mesh belt in the conveying device 1 to pass through. Each squeezing roller is connected to a driving motor. The driving motor drives the squeezing roller to rotate.
[0158] Take an application scenario as an example: when the lyocell staple fibers are on the surface of the mesh belt, the lyocell staple fibers pass through the gap between the upper and lower pressing rollers. The pressing rollers separate the lyocell staple fibers from the adhered crosslinking agent. The separated crosslinking agent enters the fourth recovery tank 14 to prevent the crosslinking agent from leaking.
[0159] In the embodiment of the present disclosure, the heating cross-linking device 6 is preferably a steam heating device, which is used to heat and cross-link the lyocell fibers, and the conveying device 1 passes through the heating cross-linking device 6. When the lyocell staple fibers enter the heating cross-linking device 6, the heating cross-linking device 6 heats and cross-links the lyocell staple fibers.
[0160] When the Lyocell staple fibers are heated by the heating and cross-linking device 6 and the cross-linking reaction is completed, the Lyocell staple fibers are output from the outlet of the heating and cross-linking device 6 .
[0161] The second washing device 7 in the disclosed embodiment is also a spraying device, which mainly sprays the cleaning liquid downwards to wash the lyocell fibers and clean the cross-linking agent remaining on the lyocell staple fibers.
[0162] In order to recycle the separated cleaning water and crosslinking agent mixed liquid, the fifth recovery tank 16 is arranged below the conveying device 1 in the embodiment of the present disclosure. The second washing device 7 sprays the cleaning liquid onto the lyocell staple fibers, and the cleaning liquid drips downward, passes through the conveying device 1 and drips into the fifth recovery tank 16, so as to recycle the cleaning liquid.
[0163] At the same time, in order to remove the excess cleaning liquid adhering to the lyocell staple fibers, a fifth squeezing device 17 is provided in the embodiment of the present disclosure. The fifth squeezing device 17 includes a squeezing roller, and two squeezing rollers are provided, one above and one below. The squeezing roller can be installed on a frame. The gap between the upper and lower squeezing rollers is for the mesh belt in the conveying device 1 to pass through. Each squeezing roller is connected to a driving motor in a transmission manner. The driving motor drives the squeezing roller to rotate.
[0164] Take an application scenario as an example: when the lyocell staple fibers are on the surface of the mesh belt, the lyocell staple fibers pass through the gap between the upper and lower pressing rollers. The pressing rollers separate the lyocell staple fibers from the adhered cleaning liquid. The separated cleaning liquid enters the fifth recovery tank 16 to prevent leakage of the cleaning liquid.
[0165] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A method for preparing anti-fibrillation flame-retardant lyocell fiber, characterized in that: include S1: mixing lyocell fiber with sodium alginate solution; S2: mixing the lyocell fiber adsorbed with the sodium alginate solution with a protective solution to form a protective layer on the surface of the lyocell fiber; S3: Lyocell fiber is then mixed with the crosslinking agent solution; S4: heating the lyocell fiber adsorbed with the crosslinking agent solution to crosslink the fiber.
2. The method for preparing the anti-fibrillation flame-retardant lyocell fiber according to claim 1, characterized in that: Also included is S0, which is water washing of lyocell fibers.
3. The method for preparing the anti-fibrillation flame-retardant lyocell fiber according to claim 2, characterized in that: In S0, the lyocell fiber is washed and then dehydrated; and / or; In the step S0, the lyocell fiber tow is washed with water, and after washing, the lyocell fiber tow is cut into lyocell staple fibers.
4. The method for preparing the anti-fibrillation flame-retardant lyocell fiber according to claim 1, characterized in that: In S1, S2, S3 and S4, the lyocell fiber is lyocell staple fiber.
5. The method for preparing the fibrillation-resistant flame-retardant lyocell fiber according to claim 1, characterized in that: The protective solution is MgCl2 solution, FeCl3 solution or CaCl2 solution.
6. The method for preparing the anti-fibrillation flame-retardant lyocell fiber according to claim 1, characterized in that: In S1, the lyocell fiber and the sodium alginate solution are mixed by spraying; and / or; In S2, the lyocell fiber and the protective solution are mixed by spraying; and / or; In S3, the lyocell fiber and the crosslinking agent solution are mixed by spraying.
7. The method for preparing the anti-fibrillation flame-retardant lyocell fiber according to claim 1, characterized in that: In S1, after the lyocell fiber is mixed with the sodium alginate solution, excess sodium alginate solution adsorbed by the lyocell fiber is removed; and / or; In S2, after the lyocell fiber is mixed with the protective solution, the excess protective solution adsorbed by the lyocell fiber is removed; and / or; In S3, after the lyocell fiber is mixed with the cross-linking agent solution, the excess cross-linking agent solution adsorbed by the lyocell fiber is removed.
8. The method for preparing the anti-fibrillation flame-retardant lyocell fiber according to claim 6 or 7, characterized in that: In S1, the sodium alginate solution separated from the lyocell fiber is recovered; and / or; In S2, the protective solution separated from the lyocell fiber is recovered; and / or; In S3, the cross-linking agent solution separated from the lyocell fiber is recovered.
9. The method for preparing the fibrillation-resistant flame-retardant lyocell fiber according to claim 1, characterized in that: The solubility of the sodium alginate solution is 0.5wt% to 2.0wt%.
10. A system for preparing anti-fibrillation flame-retardant lyocell fiber, characterized in that: include A conveying device, the conveying device is used to convey the lyocell fibers to move; A sodium alginate solution spraying device, the sodium alginate solution spraying device is arranged corresponding to the conveying device, and the sodium alginate solution spraying device is used to spray the sodium alginate solution onto the lyocell fiber; A protective solution spraying device, which is arranged corresponding to the conveying device and is located at the rear end of the sodium alginate solution spraying device, and is used to spray a protective solution onto the lyocell fiber; A cross-linking agent spraying device, which is arranged corresponding to the conveying device and is located at the rear end of the protective solution spraying device, and is used to spray the cross-linking agent solution onto the lyocell fiber; A heating cross-linking device is provided corresponding to the conveying device and is located at the rear end of the cross-linking agent spraying device. The heating cross-linking device is used to achieve heating cross-linking of the lyocell fiber.
Citation Information
Cited By
Blending modified antifibrillated lyocell fiber and preparation method thereof
CN120575359A