Environment-friendly waterproof and oil-proof film coating method for paper pulp molding

The construction of biomass-based coating agents through starch and nano-palm cellulose solves the problem of insufficient waterproof and oil-proof performance of pulp molding products, achieves efficient waterproof and oil-proof performance and mechanical properties improvement, and avoids the migration of additives. Extend service life.

CN119083235AActive Publication Date: 2024-12-06DONGGUAN DANGNA PRINTING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411215020.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Existing pulp molding products have shortcomings in waterproof and oil-proof performance. Due to environmental protection requirements, an environmentally friendly waterproof and oil-proofing film method is needed to replace traditional materials to avoid the impact of dissolution and migration of additives on personal health.

Method used

The biomass-based coating agent is constructed using starch and nanopalm cellulose. The coating agent is prepared by modifying the covalent bond crosslinking of nanopalm cellulose and starch and coated on the pulp molding surface, using nanostructures and wood. The ingredient components improve waterproof and oil-proof performance and prevent additive migration.

Benefits of technology

The superhydrophobic properties of the pulp molded surface are realized, the waterproof and oil-proof performance and mechanical properties are improved, the service life in the oil-water mixing system is extended, and the migration of additives is effectively avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083235A_ABST
    Figure CN119083235A_ABST
Patent Text Reader

Abstract

The invention discloses an environment-friendly waterproof and oil-proof filming method for paper pulp molding. The method specifically comprises the following steps: step 1, preparing nano brown cellulose; step 2, modifying the nano brown cellulose prepared in the step 1 to obtain modified nano brown cellulose; step 3, modifying starch to obtain modified starch; step 4, preparing an acrylic acid oligomer; 5, preparing a film coating agent according to products obtained in the steps 2-4; and step 6, laminating by using the laminating agent prepared in the step 5. According to the invention, the starch and the nano-brown cellulose are adopted to construct the biomass-based coating agent for the film coating of the paper pulp molding, so that the waterproof and oil-proof film coating is realized, and the dissolution and migration of auxiliaries in the paper pulp molding are effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waterproofing and oil-proofing, and relates to an environmentally friendly waterproofing and oil-proofing film-covering method for pulp molding. Background Art

[0002] Traditional pulp molding products are mostly used to manufacture paper tableware, fruit and egg trays, product packaging, paper containers, and industrial cushioning packaging. Pulp molding materials are used to replace plastics, and the fiber raw materials of pulp molding can be recycled for secondary use, which can effectively reduce the use of petroleum-based materials. However, the surface of existing pulp molding products is generally rough in appearance, which is far from petroleum-based materials. In addition, due to environmental protection requirements, many materials are strictly prohibited from using plastics, such as plastic straws, disposable tableware, plastic containers, difficult-to-foam materials, packaging pads, etc., and the most basic performance requirements of these products are waterproof and oil-proof, that is, they can prevent water and oil from corroding pulp molding during use. Therefore, waterproof and oil-proof pulp molding has broad application prospects in replacing these products. Waterproof and oil-proof coating treatment on the surface of pulp molding can not only improve the waterproof and oil-proof performance and improve the appearance, but also effectively prevent the dissolution and migration of various additives in the molding, avoiding adverse effects on human health. Summary of the invention

[0003] The purpose of the present invention is to provide an environmentally friendly waterproof and oil-proof film method for pulp molding. The method uses starch and nano-brown cellulose to construct a biomass-based coating agent for pulp molding, thereby achieving waterproof and oil-proof film and effectively avoiding the dissolution and migration of internal additives in pulp molding.

[0004] The technical solution adopted by the present invention is an environmentally friendly waterproof and oil-proof membrane method for pulp molding, which specifically includes the following steps:

[0005] Step 1, preparing nano brown cellulose;

[0006] Step 2, modifying the nano brown cellulose prepared in step 1 to obtain modified nano brown cellulose powder;

[0007] Step 3, modifying the starch to obtain modified starch;

[0008] Step 4, preparing acrylic acid oligomer;

[0009] Step 5, preparing a coating agent according to the products obtained in steps 2 to 4;

[0010] Step 6, coating using the coating agent prepared in step 5.

[0011] The present invention is also characterized in that:

[0012] The specific process of step 1 is:

[0013] Step 1.1, grinding 5000g-15000g of poplar wood by mechanical grinding, and sieving poplar wood powder of 50-100 mesh;

[0014] Step 1.2, weighing 300g of poplar wood powder and dispersing it in 1.5-3.0L of deionized water, then adding 6-12g of hydrogen peroxide, 12-24g of sodium hydroxide and 3-6g of sodium silicate in sequence, heating to 80-120°C for reaction for 60-90min, after the reaction is completed, lowering the temperature to room temperature, and refining with a pulping machine to obtain a pulp with a beating degree of 80-90°SR;

[0015] Step 1.3, add oxalic acid to the slurry obtained in step 1.2 to adjust the slurry pH to 6-8, filter, wash the filter cake with 3-6L deionized water, and repeat three times; weigh 10-30g of absolutely dry filter cake, put it in a 1000-2000mL beaker, add 500-1000mL deionized water; then use a mixer to shear at a rate of 1200-1500r / min for 5-10 minutes to form a 2-4wt% fiber suspension;

[0016] Step 1.4, pouring the fiber suspension obtained in step 1.3 into the feed port of a high-pressure homogenizer for high-pressure homogenization to obtain nano-brown cellulose.

[0017] In step 1.2, the clearance between the grinding discs of the refiner is 0.2-0.4 mm.

[0018] In step 1.4, the high-pressure homogenization process is divided into three times, namely: homogenization at a pressure of 10 MPa for 60-70 minutes, homogenization at a pressure of 40 MPa for 40-50 times, and homogenization at a pressure of 70 MPa for 20-30 times.

[0019] The specific process of step 2 is:

[0020] Step 2.1, take 10-20g of nano-brown cellulose and disperse it in 1L of deionized water, add 0.1-0.2g of concentrated sulfuric acid, and stir and disperse it at room temperature for 2-4h; continue to mix it evenly with 1-2L of high sodium sulfate aqueous solution, ultrasonicate it at 85-125℃ for 1-2h, and then stir it for 1-2h; after the reaction is completed, add 0.2-0.4g of NaHCO3 to terminate the reaction to obtain a milky white suspension;

[0021] Step 2.2, dialyzing the milky white suspension obtained in step 2.1 using a 7000-10000Da dialysis bag to remove hydrolyzed cellulose, unreacted and newly generated inorganic salt impurities;

[0022] Step 2.3, centrifuging the suspension treated in step 2.2 at a speed of 10000-140000 r / min for 30-60 min, collecting the gel-like modified nano-brown cellulose, and freeze-drying it at -70°C to obtain modified nano-brown cellulose powder.

[0023] The specific process of step 3 is as follows: 10-20 g of corn starch is dispersed in 30-60 mL of deionized water, and the pH value is adjusted to 10-11 with a NaOH solution; then 2-4 g of citric acid and 0.05-0.1 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride are added, and the mixture is reacted at 45-90° C. for 1-2 h. After the reaction is completed, a sodium bicarbonate aqueous solution is used to adjust the pH of the reaction solution to 5-6 to obtain modified starch.

[0024] The specific process of step 4 is as follows: 10-20 g of diethylene glycol ethyl ether acrylate, 5-10 g of allyl isocyanate, 0.2-0.4 g of glycerol trihydroxypropyl ether triacrylate and 0.01-0.02 g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl are taken, stirred evenly, 0.02-0.04 g of initiator is added, heated to 60-90° C. under air conditions, reacted for 1-2 hours, cooled to room temperature after the reaction is completed, 0.03-0.06 g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl is added, stirred evenly, and an acrylic acid oligomer is obtained.

[0025] The specific process of step 5 is: take 5-10g of modified nano brown cellulose powder, 5-10g of modified starch, 3g of polylactic acid and 2-4g of acrylic acid oligomer, stir evenly, heat to 45-90°C under nitrogen atmosphere, and react for 1-2h; after the reaction, put the product into a drying oven for drying, the drying temperature is 45°C-90°C, and the drying time is 5-10h; put the dried product into a twin-screw extruder, melt blend at 150-200°C for 30-60min to obtain a coating agent.

[0026] The specific process of step 6 is: introduce the laminating agent prepared in step 5 into the laminating machine to laminat the paper, the working temperature of the laminating machine is 150-200°C, the laminating thickness is 30-40um, and the pulp molding lamination is completed.

[0027] The beneficial effect of the present invention is that the present invention uses green and environmentally friendly starch and nano brown cellulose to construct a film-forming agent, uses the nano-based structure in the nano brown cellulose structure to achieve super hydrophobicity on the surface, and cooperates with the lignin component in the nano structure to further improve the waterproof and oil-proof properties of the material. The covalent bond cross-linking between nano brown cellulose and starch effectively avoids the migration of additives in pulp molding and improves mechanical properties. The moisture curing group is retained in the film-forming agent, which greatly improves the service life of pulp molding in an oil-water mixed system. Nano brown cellulose can be used as a nucleating agent for film-forming crystallization. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a test diagram of the mechanical properties of the coating of Example 1 of the method for environmentally friendly waterproof and oil-proof coating for pulp molding of the present invention and Comparative Examples 1 to 4. DETAILED DESCRIPTION

[0029] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0030] The environmentally friendly waterproof and oil-proof film-forming method for pulp molding of the present invention specifically comprises the following steps:

[0031] Step 1, preparation of nano brown cellulose, the specific process is as follows:

[0032] 5000g-15000g of poplar wood is mechanically ground, and poplar wood powder of 50-100 mesh is sieved. 300g of poplar wood powder is weighed and dispersed in 1.5-3.0L of deionized water, and then 6-12g of hydrogen peroxide, 12-24g of sodium hydroxide and 3-6g of sodium silicate are added, and heated to 80-120℃ for reaction for 60-90min. After the reaction is completed, the temperature is lowered to room temperature. A pulping machine is used for pulping (the gap between the grinding discs is 0.2-0.4mm) to obtain a pulp with a beating degree of 80-90°SR. Then oxalic acid is added to adjust the pH of the pulp to 6-8. After suction filtration, the filter cake is washed with 3-6L of deionized water, and repeated three times. Weigh 10-30g of absolutely dry filter cake, place it in a 1000-2000mL beaker, and add 500-1000mL of deionized water. Then, a mixer is used to perform high-speed shearing (rate 1200-1500r / min) for 5-10 minutes to form a 2-4wt% fiber suspension, which is then poured into a high-pressure homogenizer feed port for high-pressure homogenization, homogenizing at a pressure of 10MPa for 60-70 minutes, at a pressure of 40MPa for 40-50 minutes, and then at 70MPa for 20-30 minutes to obtain nano-brown cellulose.

[0033] Step 2, modification of nano-brown cellulose, the specific process is as follows:

[0034] Take 10-20g of nano brown cellulose and disperse it in 1L of deionized water, add 0.1-0.2g of concentrated sulfuric acid (concentration is 98%), and stir and disperse it at room temperature for 2-4h. Continue to mix evenly with 1-2L (5mol / L) of high sodium sulfate aqueous solution, ultrasonicate for 1-2h at 85-125℃, and then stir for 1-2h. After the reaction is completed, add 0.2-0.4g of NaHCO3 to terminate the reaction and obtain a milky white suspension. Use a 7000-10000Da dialysis bag to remove hydrolyzed cellulose, unreacted and newly generated inorganic salt impurities. Finally, the suspension is centrifuged at a speed of 10000-140000r / min for 30-60min, collect the gel-like modified nano brown cellulose, and obtain modified nano brown cellulose powder (carboxylated nano brown cellulose) after -70℃ freeze drying to obtain modified nano brown cellulose powder.

[0035] Step 3, modification of starch, the specific process is as follows:

[0036] Take 10-20g corn starch, disperse it in 30-60mL deionized water, and adjust the pH value to 10-11 with (1-2%) NaOH solution. Then add 2-4g citric acid and 0.05-0.1g 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride. Raise the reaction temperature to 45-90℃ for 1-2h. After the reaction is completed, adjust the pH value of the reaction solution to 5-6 (carboxylated starch) with sodium bicarbonate aqueous solution (sodium bicarbonate aqueous solution concentration 10wt%) to obtain modified starch.

[0037] Step 4, preparation of acrylic acid oligomer, the specific process is as follows:

[0038] Take 10-20g of diethylene glycol ethyl ether acrylate, 5-10g of allyl isocyanate, 0.2-0.4g of glycerol trihydroxypropyl ether triacrylate and 0.01-0.02g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, then add 0.02-0.04g of initiator azobisisobutyronitrile. Heat to 60-90℃ in air for 1-2h, cool to room temperature after the reaction, continue to add 0.03-0.06g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, and obtain acrylic acid oligomer.

[0039] Step 5, preparation of the coating agent, the specific process is: take 5-10g of modified nano brown cellulose powder (step 2), 5-10g of modified starch (step 3), 3g of polylactic acid (1.5g each of left-handed and right-handed polylactic acid) and 2-4g of acrylic acid oligomer (step 4) and stir evenly, heat to 45-90°C under nitrogen atmosphere, and react for 1-2h. After the reaction is completed, the product is placed in a drying oven for drying, the drying temperature is 45°C-90°C, and the drying time is 5-10h; the dried product is placed in a twin-screw extruder, melt blended at 150-200°C for 30-60min, and a coating agent is obtained.

[0040] Step 6, introduce the laminating agent into the laminating machine to laminat the paper, the working temperature of the laminating machine is 150-200°C, the laminating thickness is 30-40um, and the pulp molding lamination is completed.

[0041] Example 1

[0042] Step 1, preparation of nano brown cellulose, the specific process is as follows:

[0043] 5000g of poplar wood was mechanically ground and sieved into 50-100 mesh poplar powder. 300g of poplar powder was weighed and dispersed in 1.5L of deionized water, and then 6g of hydrogen peroxide, 12g of sodium hydroxide and 3g of sodium silicate were added, and the mixture was heated to 80°C and reacted for 60min. After the reaction, the temperature was lowered to room temperature. The pulping disc gap of the pulping machine was 0.2mm, and a pulp with a beating degree of 80°SR was obtained. Then oxalic acid was added to adjust the pH of the pulp to 6. After filtration, the filter cake was washed with 3L of deionized water, and the process was repeated three times. 10g of absolutely dry filter cake was weighed, placed in a 1000mL beaker, and 500mL of deionized water was added. Then a mixer was used for high-speed shearing (rate 1200r / min) for 5 minutes to form a 2wt% fiber suspension. Then it was poured into the feed port of a high-pressure homogenizer for high-pressure homogenization, homogenizing at a pressure of 10 MPa for 60 times min, at a pressure of 40 MPa for 40 times, and then at a pressure of 70 MPa for 20 times to obtain nano-brown cellulose.

[0044] Step 2, modification of nano-brown cellulose, the specific process is as follows:

[0045] Take 10g of nano-brown cellulose and disperse it in 1L of deionized water, add 0.1g of concentrated sulfuric acid, and stir and disperse at room temperature for 2h. Continue to mix evenly with 1L (5mol / L) of sodium sulfate aqueous solution, ultrasonicate at 85℃ for 1h, and then stir for 1h. After the reaction is completed, add 0.2g of NaHCO3 to terminate the reaction to obtain a milky white suspension. Use a 7000Da dialysis bag to remove hydrolyzed cellulose, unreacted and newly generated inorganic salt impurities. Finally, centrifuge the suspension at 10000r / min for 30min, collect the gel-like modified nano-brown cellulose, and freeze-dry at -70℃ to obtain modified nano-brown cellulose powder (carboxylated nano-brown cellulose) to obtain modified nano-cellulose powder;

[0046] Step 3, modification of starch, the specific process is as follows:

[0047] Take 10g corn starch, disperse it in 30mL deionized water, and adjust the pH value of the medium to 10 with (1%) NaOH solution. Then add 2g citric acid and 0.05g 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride. Raise the reaction temperature to 45℃ for 1h. After the reaction is completed, adjust the pH value of the reaction solution to 6 (carboxylated starch) with sodium bicarbonate aqueous solution to obtain modified starch;

[0048] Step 4, preparation of acrylic acid oligomer, the specific process is as follows:

[0049] Take 10g of diethylene glycol ethyl ether acrylate, 5g of allyl isocyanate, 0.2g of glycerol trihydroxypropyl ether triacrylate and 0.01g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, add 0.02g of azobisisobutyronitrile, heat to 60°C in air conditions for reaction for 1h, cool to room temperature after the reaction, continue to add 0.03g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly to obtain an acrylic acid oligomer.

[0050] Step 5, preparation of the film-forming agent, the specific process is as follows:

[0051] Take 5g of modified nano-brown cellulose, 5g of modified starch, 3g of polylactic acid (1.5g each of left-handed and right-handed polylactic acid) and 2g of acrylic acid oligomer, stir evenly, heat to 45°C under nitrogen atmosphere, and react for 1h. After the reaction, put the product into a drying oven for drying at 45°C for 5h; put the dried raw materials into a twin-screw extruder, melt blend at 150°C for 30min, and obtain a coating agent.

[0052] Step 6, introducing the laminating agent into the laminating machine to laminat the paper, the working temperature of the laminating machine is 150° C., the laminating thickness is 30 um, and the pulp molding lamination is completed.

[0053] Comparative Example 1 (modified nano-brown cellulose was not added to the film-forming agent, and the waterproof and oil-proof properties, mechanical properties and thermal stability were deteriorated)

[0054] Step 1: Take 10g corn starch, disperse it in 30mL deionized water, and adjust the pH value of the medium to 10 with (1%) NaOH solution. Then add 2g citric acid and 0.05g 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride. The reaction temperature is increased to 45°C for 1h. After the reaction is completed, the pH value of the reaction solution is adjusted to 6 (carboxylated starch) with sodium bicarbonate aqueous solution to obtain modified starch.

[0055] Step 2, take 10g of diethylene glycol ethyl ether acrylate, 5g of allyl isocyanate, 0.2g of glycerol trihydroxypropyl ether triacrylate and 0.01g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, add 0.02g of azobisisobutyronitrile initiator, heat to 60°C in air for 1h, cool to room temperature after the reaction, continue to add 0.03g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, and obtain acrylic acid oligomer.

[0056] Step 3, take 5g of modified starch, 3g of polylactic acid (1.5g each of left-handed and right-handed polylactic acid) and 2g of acrylic acid oligomer, stir evenly, heat to 45°C under nitrogen atmosphere, and react for 1h. After the reaction is completed, put the product into a drying oven for drying at a temperature of 45°C for 5h; put the dried product into a twin-screw extruder for melt blending, and melt blend at 150°C for 30min to obtain a coating agent.

[0057] Step 4, introducing the laminating agent into the laminating machine to laminat the paper, the working temperature of the laminating machine is between 150° C., the laminating thickness is 30 um, and a pulp molded lamination is obtained.

[0058] Comparative Example 2 (Nano-brown cellulose is not modified, and the mechanical properties are deteriorated)

[0059] Step 1, grind 5000g of poplar wood mechanically, sieve 50-100 mesh poplar powder, weigh 300g of poplar powder and disperse it in 1.5L of deionized water, then add 6g of hydrogen peroxide, 12g of sodium hydroxide and 3g of sodium silicate, heat to 80°C and react for 60min. After the reaction is completed, the temperature is reduced to room temperature. The pulping disc gap of the pulping machine is 0.2mm to obtain a pulp with a beating degree of 80°SR. Then oxalic acid is added to adjust the pH of the pulp to 6. After filtration, the filter cake is washed with 3L of deionized water, and repeated three times. Weigh 10g of the absolutely dry filter cake, place it in a 1000mL beaker, and add 500mL of deionized water. Then use a mixer to shear at high speed (rate 1200r / min) for 5 minutes to form a 2wt% fiber suspension. Then it was poured into the feed port of a high-pressure homogenizer for high-pressure homogenization, homogenizing at a pressure of 10 MPa for 60 times min, at a pressure of 40 MPa for 40 times, and then at a pressure of 70 MPa for 20 times to obtain nano-brown cellulose.

[0060] Step 2, take 10g corn starch, disperse it in 30mL deionized water, and adjust the pH value of the medium to 10 with (1%) NaOH solution. Then add 2g citric acid and 0.05g 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride. Raise the reaction temperature to 45°C for 1h. After the reaction is completed, adjust the pH value of the reaction solution to 6 (carboxylated starch) with sodium bicarbonate aqueous solution to obtain modified starch;

[0061] Step 3, take 10g of diethylene glycol ethyl ether acrylate, 5g of allyl isocyanate, 0.2g of glycerol trihydroxypropyl ether triacrylate and 0.01g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, add 0.02g of azobisisobutyronitrile initiator. Heat to 60°C under air conditions for reaction for 1h, cool to room temperature after the reaction, continue to add 0.03g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, and obtain acrylic acid oligomer.

[0062] Step 4, take 5g of nano brown cellulose, 5g of modified starch, 3g of polylactic acid (1.5g each of left-handed and right-handed polylactic acid) and 2g of acrylic acid oligomer, stir evenly, heat to 45°C under nitrogen atmosphere, and react for 1h. After the reaction is completed, the product is placed in a drying oven for drying at a temperature of 45°C for 5h. The dried raw materials are placed in a twin-screw extruder and melt blended at 150°C for 30min to obtain a coating agent.

[0063] Step 6, introducing the laminating agent into the laminating machine to laminat the paper, the working temperature of the laminating machine is 150° C., the laminating thickness is 30 um, and a pulp molded lamination is obtained.

[0064] Comparative Example 3 (Allyl isocyanate was not added to the modified resin, mechanical properties deteriorated, and additives leaked out)

[0065] Step 1, grind 5000g of poplar wood mechanically, sieve 50-100 mesh poplar powder, weigh 300g of poplar powder and disperse it in 1.5L of deionized water, then add 6g of hydrogen peroxide, 12g of sodium hydroxide and 3g of sodium silicate, heat to 80°C and react for 60min. After the reaction is completed, the temperature is reduced to room temperature. The pulping disc gap of the pulping machine is 0.2mm to obtain a pulp with a beating degree of 80°SR. Then oxalic acid is added to adjust the pH of the pulp to 6. After filtration, the filter cake is washed with 3L of deionized water, and repeated three times. Weigh 10g of the absolutely dry filter cake, place it in a 1000mL beaker, and add 500mL of deionized water. Then use a mixer to shear at high speed (rate 1200r / min) for 5 minutes to form a 2wt% fiber suspension. Then it was poured into the feed port of a high-pressure homogenizer for high-pressure homogenization, homogenizing at a pressure of 10 MPa for 60 times min, at a pressure of 40 MPa for 40 times, and then at a pressure of 70 MPa for 20 times to obtain nano-brown cellulose.

[0066] Step 2, take 10g of nano brown cellulose and disperse it in 1L of deionized water, add 0.1g of concentrated sulfuric acid, and stir and disperse it at room temperature for 2h. Continue to mix evenly with 1L (5mol / L) of high sodium sulfate aqueous solution, ultrasonicate for 1h at 85℃, and then stir for 1h. After the reaction is completed, add 0.2g of NaHCO3 to terminate the reaction to obtain a milky white suspension. Use a 7000Da dialysis bag to remove impurities such as hydrolyzed cellulose, unreacted and newly generated inorganic salts. Finally, the suspension is centrifuged at 10000r / min for 30min, and the gel-like modified nano brown cellulose is collected, and the modified nano brown cellulose powder (carboxylated nano brown cellulose) is obtained by freeze drying at -70℃.

[0067] Step 3, take 10g corn starch, disperse it in 30mL deionized water, and adjust the pH value of the medium to 10 with (1%) NaOH solution. Then add 2g citric acid and 0.05g 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride. The reaction temperature is raised to 45°C for 1h. After the reaction is completed, the pH value of the reaction solution is adjusted to 6 (carboxylated starch) with sodium bicarbonate aqueous solution.

[0068] Step 4, take 10g of diethylene glycol ethyl ether acrylate, 0.2g of glycerol trihydroxypropyl ether triacrylate and 0.01g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, add 0.02g of azobisisobutyronitrile initiator, heat to 60°C in air for 1h, cool to room temperature after the reaction, continue to add 0.03g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, and obtain acrylic acid oligomer.

[0069] Step 5: Take 5g of modified nano-brown cellulose powder, 5g of modified starch, 3g of polylactic acid (1.5g each of left-handed and right-handed polylactic acid) and 2g of acrylic acid oligomer, stir evenly, heat to 45°C under nitrogen atmosphere, and react for 1h. After the reaction, put the product into a drying oven for drying at 45°C for 5h; put the dried raw materials into a twin-screw extruder, melt blend at 150°C for 30min, and obtain a coating agent.

[0070] Step 6, introduce the laminating agent into the laminating machine to laminat the paper, the working temperature of the laminating machine is between 150°C, the laminating thickness is 30um, and the pulp molding lamination is completed.

[0071] Comparative Example 4 (modified starch replaced with cationic starch, mechanical properties deteriorated, additive migration occurred)

[0072] Step 1, grind 5000g of poplar wood mechanically, sieve 50-100 mesh powder, weigh 300g of poplar wood powder and disperse it in 1.5L of deionized water, then add 6g of hydrogen peroxide, 12g of sodium hydroxide and 3g of sodium silicate, heat to 80°C and react for 60min. After the reaction is completed, the temperature is reduced to room temperature. The pulping disc gap of the pulping machine is 0.2mm to obtain a pulp with a beating degree of 80°SR. Then oxalic acid is added to adjust the pH of the pulp to 6. After filtration, the filter cake is washed with 3L of deionized water, and repeated three times. Weigh 10g of the absolutely dry filter cake, place it in a 1000mL beaker, and add 500mL of deionized water. Then use a mixer to shear at high speed (rate 1200r / min) for 5 minutes to form a 2wt% fiber suspension. Then it was poured into the feed port of a high-pressure homogenizer for high-pressure homogenization, homogenizing at a pressure of 10 MPa for 60 times min, at a pressure of 40 MPa for 40 times, and then at a pressure of 70 MPa for 20 times to obtain nano-brown cellulose.

[0073] Step 2, take 10g of nano brown cellulose and disperse it in 1L of deionized water, add 0.1g of concentrated sulfuric acid, and stir and disperse it at room temperature for 2h. Continue to mix evenly with 1L (5mol / L) of high sodium sulfate aqueous solution, ultrasonicate for 1h at 85℃, and then stir for 1h. After the reaction is completed, add 0.2g of NaHCO3 to terminate the reaction to obtain a milky white suspension. Use a 7000Da dialysis bag to remove impurities such as hydrolyzed cellulose, unreacted and newly generated inorganic salts. Finally, the suspension is centrifuged at 10000r / min for 30min, and the gel-like modified nano brown cellulose is collected, and the modified nano brown cellulose powder (carboxylated nano brown cellulose) is obtained by freeze drying at -70℃.

[0074] Step 3, take 10g of diethylene glycol ethyl ether acrylate, 5g of allyl isocyanate, 0.2g of glycerol trihydroxypropyl ether triacrylate and 0.01g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, add 0.02g of azobisisobutyronitrile initiator, heat to 60°C under air conditions for 1h, cool to room temperature after the reaction, continue to add 0.03g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, and obtain acrylic acid oligomer.

[0075] Step 4: Take 5g of modified nano-brown cellulose powder, 5g of cationic starch, 3g of polylactic acid (1.5g each of left-handed and right-handed polylactic acid) and 2g of acrylic acid oligomer, stir evenly, heat to 45°C under nitrogen atmosphere, and react for 1h. After the reaction is completed, put the product into a drying oven for drying at 45°C for 5h; put the dried raw materials into a twin-screw extruder, melt blend at 150°C for 30min, and obtain a coating agent.

[0076] Step 5, introduce the laminating agent into the laminating machine to laminat the paper, the working temperature of the laminating machine is between 150°C, the laminating thickness is 30um, and the pulp molding lamination is completed.

[0077] Results and Discussion

[0078] Table 1 below shows the analysis and test results of the films after lamination of Example 1 and Comparative Examples 1-4:

[0079] Table 1

[0080]

[0081] Note: Tensile strength (MPa) and thermal decomposition temperature (℃) are the tests of the retained film layer after the pulp molding layer in the pulp molding film is removed. Water contact angle (°) is the water contact angle (°) of the film layer in the pulp molding film and the film layer after the pulp molding film is treated with oil and water (oil-water volume ratio is 1:1) for 48 hours. Since the additives in pulp molding contain a large number of cationic and anionic additives, the migration of additives can be achieved by the change in the conductivity of oil and water after the film is treated with oil and water for 48 hours.

[0082] Figure 1 The following are the mechanical properties test diagrams of the film after coating of Example 1 and Comparative Examples 1 to 4 of the environmentally friendly waterproof and oil-proof coating method for pulp molding of the present invention (the coating agent is cured on the surface of the pulp molding to complete the coating, and the coated film is peeled off to measure the mechanical properties). Figure 1 As shown in Table 1, Example 1 has the strongest breaking strength of 220 MPa, while Comparative Example 3 is the worst. The main reason is that no acrylic isocyanate is added to the resin of Comparative Example 3, resulting in the inability to form a network cross-linked structure in the prepared membrane, and the mechanical properties are poor. The breaking strength in Comparative Example 1 is also poor, mainly because of the lack of modified nano-brown cellulose and the lack of the reinforcing effect of nano-materials. Comparative Example 2 nano-brown cellulose is not modified, and the mechanical properties deteriorate, mainly because it fails to form a network structure with the resin.

[0083] Example 1 has a high water contact angle, which provides the possibility of waterproof and oil-proofing the membrane, and its waterproof and oil-proofing performance is the best. Comparative Example 1 has the lowest water contact angle, without modified nano-brown cellulose, lacking the membrane surface and lacking nano-microstructure. The water contact angle of Comparative Example 4 is also low, mainly because cationic starch is water-soluble and cationic starch does not react chemically with other components.

[0084] The change in contact angle of the membrane after oil-water treatment shows that the contact angle of the membrane in Example 1 hardly changes after 48 hours of treatment, indicating that it has a good service life. The contact angle of Comparative Example 3 changes the most before and after oil-water treatment. The reason is that no acrylic isocyanate is added, resulting in the inability to form a network cross-linked structure in the prepared membrane. After a long period of oil-water treatment, the membrane swells, resulting in a change in the contact angle.

[0085] The thermal decomposition temperature of Comparative Example 1 is the lowest, mainly due to the lack of modified nano-brown cellulose components with a high decomposition temperature (330°C), and the lack of nano-nucleating particles leads to poor crystallization performance of the membrane, and ultimately the worst thermal stability.

[0086] The membranes obtained in Comparative Examples 3 and 4 showed a significant increase in the conductivity of oil and water after 48 hours of treatment, which was due to the migration of conductive ions in the pulp molding film into the oil and water. The increase in conductivity in Comparative Example 3 was mainly due to the migration of additives in the pulp molding layer. The conductivity of Comparative Example 4 increased more significantly, mainly due to the migration of ions in the cationic starch in the film layer.

[0087] Example 2

[0088] Step 1, preparation of nano brown cellulose, the specific process is as follows:

[0089] 10000g of poplar wood was mechanically ground and sieved into 50-100 mesh poplar powder. 300g of poplar powder was weighed and dispersed in 2.5L of deionized water, and then 10g of hydrogen peroxide, 18g of sodium hydroxide and 5g of sodium silicate were added, and the mixture was heated to 100°C for reaction for 80min. After the reaction, the temperature was lowered to room temperature. The pulping disc gap of the pulping machine was 0.3mm, and a pulp with a beating degree of 85°SR was obtained. Then oxalic acid was added to adjust the pH of the pulp to 7. After filtration, the filter cake was washed with 5L of deionized water, and the process was repeated three times. 20g of absolutely dry filter cake was weighed, placed in a 1500mL beaker, and 800mL of deionized water was added. Then a mixer was used for high-speed shearing (rate 1400r / min) for 8 minutes to form a 3wt% fiber suspension. Subsequently, it was poured into the feed port of a high-pressure homogenizer for high-pressure homogenization, homogenizing at a pressure of 10 MPa for 65 times per minute, at a pressure of 40 MPa for 45 times, and then at a pressure of 70 MPa for 25 times to obtain nano-brown cellulose.

[0090] Step 2, modification of nano-brown cellulose, the specific process is as follows:

[0091] Take 15g of nano-brown cellulose and disperse it in 1L of deionized water, add 0.15g of concentrated sulfuric acid, and stir and disperse at room temperature for 3h. Continue to mix evenly with 1.5L (5mol / L) of sodium sulfate aqueous solution, ultrasonicate at 100℃ for 1.5h, and then stir for 1.5h. After the reaction is completed, add 0.3g of NaHCO3 to terminate the reaction to obtain a milky white suspension. Use an 8000Da dialysis bag to remove hydrolyzed cellulose, unreacted and newly generated inorganic salt impurities. Finally, centrifuge the suspension at 12000r / min for 50min, collect the gel-like modified nano-brown cellulose, and freeze-dry at -70℃ to obtain modified nano-brown cellulose powder (carboxylated nano-brown cellulose) to obtain modified nano-cellulose powder;

[0092] Step 3, modification of starch, the specific process is as follows:

[0093] Take 15g corn starch, disperse it in 50mL deionized water, and adjust the pH value of the medium to 10 with (1.5%) NaOH solution. Then add 3g citric acid and 0.08g 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride. Raise the reaction temperature to 80℃ and react for 1.5h. After the reaction is completed, adjust the pH value of the reaction solution to 6 (carboxylated starch) with sodium bicarbonate aqueous solution to obtain modified starch;

[0094] Step 4, preparation of acrylic acid oligomer, the specific process is as follows:

[0095] Take 15g of diethylene glycol ethyl ether acrylate, 8g of allyl isocyanate, 0.3g of glycerol trihydroxypropyl ether triacrylate and 0.015g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, add 0.03g of azobisisobutyronitrile, heat to 80°C in air conditions and react for 1.5h. After the reaction is completed, cool to room temperature, continue to add 0.04g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, and obtain an acrylic acid oligomer.

[0096] Step 5, preparation of the film-forming agent, the specific process is as follows:

[0097] Take 8g of modified nano-brown cellulose, 8g of modified starch, 3g of polylactic acid (1.5g each of left-handed and right-handed polylactic acid) and 3g of acrylic acid oligomer, stir evenly, heat to 80°C under nitrogen atmosphere, and react for 1.5h. After the reaction, put the product into a drying oven for drying at 80°C for 8h; put the dried raw materials into a twin-screw extruder, melt blend at 180°C for 40min, and obtain a coating agent.

[0098] Step 6, introducing the laminating agent into the laminating machine to laminat the paper, the working temperature of the laminating machine is 180° C., the laminating thickness is 35 um, and the pulp molding lamination is completed.

[0099] Example 3

[0100] Step 1, preparation of nano brown cellulose, the specific process is as follows:

[0101] 15000g of poplar wood was mechanically ground and sieved into 50-100 mesh poplar powder. 300g of poplar powder was weighed and dispersed in 3.0L of deionized water, and then 12g of hydrogen peroxide, 24g of sodium hydroxide and 6g of sodium silicate were added, and the mixture was heated to 120°C and reacted for 90min. After the reaction, the temperature was lowered to room temperature. The pulping disc gap of the pulping machine was 0.4mm, and a pulp with a beating degree of 90°SR was obtained. Then oxalic acid was added to adjust the pH of the pulp to 8. After filtration, the filter cake was washed with 6L of deionized water, and the process was repeated three times. 30g of the absolutely dry filter cake was weighed, placed in a 2000mL beaker, and 1000mL of deionized water was added. Then a mixer was used for high-speed shearing (rate 1500r / min) for 10 minutes to form a 4wt% fiber suspension. Subsequently, it was poured into the feed port of a high-pressure homogenizer for high-pressure homogenization, and homogenized at a pressure of 10 MPa for 70 times per minute, at a pressure of 40 MPa for 50 times, and then at 70 MPa for 30 times to obtain nano-brown cellulose.

[0102] Step 2, modification of nano-brown cellulose, the specific process is as follows:

[0103] Take 20g of nano-brown cellulose and disperse it in 1L of deionized water, add 0.2g of concentrated sulfuric acid, and stir and disperse at room temperature for 4h. Continue to mix evenly with 2L (5mol / L) of sodium sulfate aqueous solution, ultrasonicate at 125℃ for 2h, and then stir for 2h. After the reaction is completed, add 0.4g of NaHCO3 to terminate the reaction to obtain a milky white suspension. Use a 10000Da dialysis bag to remove hydrolyzed cellulose, unreacted and newly generated inorganic salt impurities. Finally, centrifuge the suspension at 14000r / min for 60min, collect the gel-like modified nano-brown cellulose, and freeze-dry at -70℃ to obtain modified nano-brown cellulose powder (carboxylated nano-brown cellulose) to obtain modified nano-cellulose powder;

[0104] Step 3, modification of starch, the specific process is as follows:

[0105] Take 20g corn starch, disperse it in 60mL deionized water, and adjust the pH value of the medium to 11 with (2%) NaOH solution. Then add 4g citric acid and 0.1g 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride. Raise the reaction temperature to 90℃ and react for 2h. After the reaction is completed, adjust the pH value of the reaction solution to 5 (carboxylated starch) with sodium bicarbonate aqueous solution to obtain modified starch;

[0106] Step 4, preparation of acrylic acid oligomer, the specific process is as follows:

[0107] Take 20g of diethylene glycol ethyl ether acrylate, 10g of allyl isocyanate, 0.4g of glycerol trihydroxypropyl ether triacrylate and 0.02g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly, add 0.04g of azobisisobutyronitrile, heat to 90°C in air conditions for reaction for 2h, cool to room temperature after the reaction, continue to add 0.06g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl, stir evenly to obtain an acrylic acid oligomer.

[0108] Step 5, preparation of the film-forming agent, the specific process is as follows:

[0109] Take 10g of modified nano-brown cellulose, 10g of modified starch, 3g of polylactic acid (1.5g each of left-handed and right-handed polylactic acid) and 4g of acrylic acid oligomer, stir evenly, heat to 90°C under nitrogen atmosphere, and react for 2h. After the reaction, put the product into a drying oven for drying at 90°C for 10h; put the dried raw materials into a twin-screw extruder, melt blend at 200°C for 60min, and obtain a coating agent.

[0110] Step 6, introduce the laminating agent into the laminating machine to laminat the paper, the working temperature of the laminating machine is 200° C., the laminating thickness is 40 um, and the pulp molding lamination is completed.

[0111] The present invention uses starch and nano brown cellulose to construct a biomass-based coating agent, which is used for pulp molding film. The film can be waterproof and oil-proof, has excellent mechanical properties, and a long service life, and can effectively avoid the dissolution and migration of the internal additives of the pulp molding. The nano brown cellulose can be used as a nucleating agent for film formation and crystallization of the film.

Claims

1. A method for making an environmentally friendly waterproof and oil-proof film for pulp molding, characterized in that: The specific steps include: Step 1, preparing nano brown cellulose; Step 2, modifying the nano brown cellulose prepared in step 1 to obtain modified nano brown cellulose powder; Step 3, modifying the starch to obtain modified starch; Step 4, preparing acrylic acid oligomer; Step 5, preparing a coating agent according to the products obtained in steps 2 to 4; Step 6, coating using the coating agent prepared in step 5.

2. The environmentally friendly waterproof and oil-proof film-forming method for pulp molding according to claim 1, characterized in that: The specific process of step 1 is as follows: Step 1.1, grinding 5000g-15000g of poplar wood by mechanical grinding, and sieving poplar wood powder of 50-100 mesh; Step 1.2, weighing 300g of poplar wood powder and dispersing it in 1.5-3.0L of deionized water, then adding 6-12g of hydrogen peroxide, 12-24g of sodium hydroxide and 3-6g of sodium silicate in sequence, heating to 80-120°C for reaction for 60-90min, after the reaction is completed, lowering the temperature to room temperature, and refining with a pulping machine to obtain a pulp with a beating degree of 80-90°SR; Step 1.3, add oxalic acid to the slurry obtained in step 1.2 to adjust the slurry pH to 6-8, filter, wash the filter cake with 3-6L deionized water, and repeat three times; weigh 10-30g of absolutely dry filter cake, put it in a 1000-2000mL beaker, add 500-1000mL deionized water; then use a mixer to shear at a rate of 1200-1500r / min for 5-10 minutes to form a 2-4wt% fiber suspension; Step 1.4, pouring the fiber suspension obtained in step 1.3 into the feed port of a high-pressure homogenizer for high-pressure homogenization to obtain nano-brown cellulose.

3. The environmentally friendly waterproof and oil-proof film-forming method for pulp molding according to claim 2, characterized in that: In the step 1.2, the clearance between the grinding discs of the refiner is 0.2-0.4 mm.

4. The environmentally friendly waterproof and oil-proof film-forming method for pulp molding according to claim 2, characterized in that: In the step 1.4, the high-pressure homogenization process is divided into three times, namely: homogenization at a pressure of 10 MPa for 60-70 minutes, homogenization at a pressure of 40 MPa for 40-50 times, and homogenization at a pressure of 70 MPa for 20-30 times.

5. The environmentally friendly waterproof and oil-proof film-forming method for pulp molding according to claim 2, characterized in that: The specific process of step 2 is: Step 2.1, take 10-20g of nano-brown cellulose and disperse it in 1L of deionized water, add 0.1-0.2g of concentrated sulfuric acid, and stir and disperse it at room temperature for 2-4h; continue to mix it evenly with 1-2L of high sodium sulfate aqueous solution, ultrasonicate it at 85-125℃ for 1-2h, and then stir it for 1-2h; after the reaction is completed, add 0.2-0.4g of NaHCO3 to terminate the reaction to obtain a milky white suspension; Step 2.2, dialyzing the milky white suspension obtained in step 2.1 using a 7000-10000Da dialysis bag to remove hydrolyzed cellulose, unreacted and newly generated inorganic salt impurities; Step 2.3, centrifuging the suspension treated in step 2.2 at a speed of 10000-140000 r / min for 30-60 min, collecting the gel-like modified nano-brown cellulose, and freeze-drying it at -70°C to obtain modified nano-brown cellulose powder.

6. The environmentally friendly waterproof and oil-proof film-forming method for pulp molding according to claim 5, characterized in that: The specific process of step 3 is as follows: 10-20 g of corn starch is dispersed in 30-60 mL of deionized water, and the pH value is adjusted to 10-11 with a NaOH solution; then 2-4 g of citric acid and 0.05-0.1 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride are added, and the mixture is reacted at 45-90° C. for 1-2 h. After the reaction is completed, a sodium bicarbonate aqueous solution is used to adjust the pH of the reaction solution to 5-6 to obtain modified starch.

7. The environmentally friendly waterproof and oil-proof film-forming method for pulp molding according to claim 6, characterized in that: The specific process of step 4 is as follows: 10-20 g of diethylene glycol ethyl ether acrylate, 5-10 g of allyl isocyanate, 0.2-0.4 g of glycerol trihydroxypropyl ether triacrylate and 0.01-0.02 g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl are taken, and after stirring evenly, 0.02-0.04 g of initiator is added, and the mixture is heated to 60-90° C. in air, and reacted for 1-2 h. After the reaction is completed, the mixture is cooled to room temperature, and 0.03-0.06 g of 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl is added, and after stirring evenly, an acrylic acid oligomer is obtained.

8. The environmentally friendly waterproof and oil-proof film-forming method for pulp molding according to claim 7, characterized in that: The specific process of step 5 is: take 5-10g of modified nano brown cellulose powder, 5-10g of modified starch, 3g of polylactic acid and 2-4g of acrylic acid oligomer, stir them evenly, heat them to 45-90°C under a nitrogen atmosphere, and react for 1-2h; after the reaction, put the product into a drying oven for drying, the drying temperature is 45°C-90°C, and the drying time is 5-10h; put the dried product into a twin-screw extruder, melt blend at 150-200°C for 30-60min, and obtain a coating agent.

9. The environmentally friendly waterproof and oil-proof film-forming method for pulp molding according to claim 8, characterized in that: The specific process of step 6 is: introducing the laminating agent prepared in step 5 into a laminating machine to laminat e the paper, the working temperature of the laminating machine is 150-200° C., the laminating thickness is 30-40 um, and the pulp molding laminating is completed.

Citation Information

Patent Citations

  • Polylactic acid degradable composite material and preparation method thereof

    CN104861600A

  • Nanocellulose-reinforced biomass coated oil-proof paper and production technology thereof

    CN108688285A

  • Ultrathin high-strength biodegradable film and preparation method thereof

    CN115926405A

  • Biodegradable control mulching film compound and biodegradable control mulching film prepared therefrom

    KR102669421B1