Method for testing water vapor transmission capability of gas diffusion layer of fuel cell

By entering different gases and liquids into the fuel cell gas diffusion layer test fixture, using sensors to obtain data, calculate the oxygen diffusion rate and water vapor diffusion rate, the problem of difficult to measure the water vapor transmission capacity of the gas diffusion layer in the prior art is solved, and the problem of achieving the problem of achieving the difficulty in measuring the water vapor transmission capacity of the gas diffusion layer is achieved. Accurate assessment of water and gas transmission capabilities.

CN119086386AInactive Publication Date: 2024-12-06ANHUI RUIHE POWER TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410998207.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing test methods are difficult to accurately measure the water vapor transmission capacity of the fuel cell gas diffusion layer, especially the water transmission and gas transmission capacity of the gas diffusion layer, and the impact of humidification on breathability cannot be effectively evaluated.

Method used

A test method is adopted to provide a test fixture to encapsulate the sample to be tested, and then perform sealing tests, and humidified nitrogen and pure dry oxygen or liquid water and pure dry air are respectively obtained by using an oxygen sensor and humidity sensor. Data, calculate the oxygen diffusion rate, water vapor diffusion rate and liquid water permeability.

Benefits of technology

Accurate measurement of the water transmission capacity and gas transmission capacity of the gas diffusion layer is achieved, which meets the requirements of taking into account both water vapor transmission and gas transmission capacity, and improves the accuracy of the test results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086386A_ABST
    Figure CN119086386A_ABST
Patent Text Reader

Abstract

The invention discloses a method for testing the water vapor transmission capability of a gas diffusion layer of a fuel cell, and the method comprises the steps: S1, providing a test fixture, and packaging a to-be-tested sample; s2, after the packaging assembly is clamped by the test fixture, a sealing performance test is carried out; s3, introducing first gas or liquid water into the first inlet of the test fixture, introducing second gas or third gas into the second inlet of the test fixture, and testing; s4, acquiring related data; and S5, calculating the oxygen diffusivity, the water vapor diffusivity and the liquid water permeability. According to the method for testing the water vapor transmission capability of the gas diffusion layer of the fuel cell, the measurement requirements of the water transmission capability and the gas transmission capability of the gas diffusion layer can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of fuel cells, and in particular, relates to a method for testing the water vapor transmission capability of a fuel cell gas diffusion layer. Background Art

[0002] As one of the most promising and popular fuel cell technologies, proton exchange membrane fuel cell (PEMFC) has many advantages such as no pollution, high energy conversion rate, short charging time, low operating temperature and low noise. It can be widely used in transportation vehicles, cogeneration, fixed base stations, mobile portable devices, drones, military equipment and many other fields. The membrane electrode is the heart of the proton exchange membrane. It is a seven-in-one structure composed of carbon paper, proton exchange membrane, catalyst layer and frame layer. Its performance directly affects the performance of the proton exchange membrane.

[0003] During the operation of the fuel cell, water vapor transmission has a great impact on the battery performance and durability. Water management is one of the key issues for the efficient operation of PEM fuel cells. Improper water management and excessively low or high water content inside the battery will have a great impact. At low electrical density, less water is generated. Too low water content in the fuel cell will affect the proton conductivity of the membrane, which will directly affect the ohmic loss of the battery. At high electrical density, more water is generated, and the water content in the fuel cell is too high. Even excessive liquid water accumulation will cause flooding, affect the transmission of the reaction gas, and even cause the occurrence of reverse polarity, especially the huge damage to the battery caused by the reverse polarity of the anode, which will lead to serious performance and durability losses.

[0004] The gas diffusion layer is one of the important components for water vapor transport. It needs to transfer the excess water produced by the catalyst layer to the flow channel through capillary force and then discharge it from the battery; at the same time, it needs to transfer the reaction gas to the catalyst layer through molecular diffusion and Knudsen diffusion for reaction. The capillary force and the pore structure of the microporous layer are closely related to the hydrophilicity and hydrophobicity of the pores, but the pore structure is relatively complex and the hydrophilicity and hydrophobicity cannot be well measured, which leads to great difficulties in analyzing the water vapor transport of the gas diffusion layer. On the other hand, the support layer of the gas diffusion layer is composed of disordered stacking of carbon fibers, while the microporous layer is composed of carbon black particles and hydrophobic agent (PTFE). Its irregular pore structure also causes great difficulties in analyzing the gas transport of fuel cells.

[0005] The existing characterization methods for testing the water transmission capacity of gas diffusion layers often only test the contact angle, which is greatly affected by surface roughness and baseline selection, and cannot well characterize the hydrophilicity and hydrophobicity in the pores. In addition, the existing gas diffusion layer gas transmission tests are based on nitrogen vertical permeability and in-plane permeability, without considering the effect of humidification on permeability, and the vertical permeability and in-plane permeability are separated and not taken into account at the same time. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer, the purpose of which is to meet the measurement requirements of the water transmission capacity and gas transmission capacity of the gas diffusion layer.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer, comprising the steps of:

[0008] S1. Provide test fixture and package the sample to be tested;

[0009] S2. After the test fixture clamps the package assembly, a sealing test is performed;

[0010] S3, introducing a first gas or liquid water into a first inlet of the test fixture, and introducing a second gas or a third gas into a second inlet of the test fixture to perform a test;

[0011] S4. Obtain relevant data;

[0012] S5. Calculate the oxygen diffusivity, water vapor diffusivity, and liquid water permeability.

[0013] The test fixture includes a first end plate and a second end plate that cooperate to clamp the sample to be tested, the first end plate is provided with the first inlet and the first outlet, the second end plate is provided with the second inlet and the second outlet, a first flow channel is provided in the first end plate between the first inlet and the first outlet, the first flow channel is connected with the first inlet and the first outlet, a second flow channel is provided in the second end plate between the second inlet and the second outlet, the second flow channel is connected with the second inlet and the second outlet.

[0014] When testing the gas transmission capacity, a first gas is introduced into the first inlet of the test fixture, and a second gas is introduced into the second inlet of the test fixture. The first gas is humidified nitrogen, and the second gas is pure dry oxygen.

[0015] When testing the water transmission capacity, liquid water is introduced into the first inlet of the test fixture, and a third gas is introduced into the second inlet of the test fixture, wherein the third gas is pure dry air.

[0016] An oxygen sensor is arranged at the first outlet, and a humidity sensor is arranged at the second outlet.

[0017] In step S4, the acquired relevant data includes the oxygen concentration at the first outlet, the oxygen concentration at the second inlet, the humidity at the first inlet, and the humidity at the second outlet.

[0018] In step S5, according to the formula Calculate the oxygen diffusion rate DO2 , where S 测试活性面积 is the active area, C 入 is the oxygen concentration at the second inlet, C 出 is the oxygen concentration at the first outlet, μ is the gas flow rate, and h is the thickness of the sample to be tested.

[0019] In step S5, according to the formula Calculate the water vapor diffusion rate ξ O2 , where S 测试活性面积 is the active area, η 入 is the nitrogen humidity at the first inlet, η 出 is the humidity sensor reading at the second outlet, μ is the gas flow rate, and h is the thickness of the sample to be tested.

[0020] In step S5, according to the formula Calculate the liquid water permeability ψ O2 , where S 测试活性面积 is the active area, η liquid is the humidity sensor reading at the second outlet, μ is the gas flow rate, and h is the thickness of the sample to be tested.

[0021] The first end plate and the second end plate are made of transparent material.

[0022] The test method for the water vapor transmission capacity of the fuel cell gas diffusion layer of the present invention can meet the measurement requirements of the water transmission capacity and gas transmission capacity of the gas diffusion layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a flow chart of a method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer of the present invention;

[0024] Figure 2 It is a schematic diagram of the structure of the test fixture;

[0025] Figure 3 It is a structural diagram of the end plate;

[0026] Figure 4 It is a side schematic diagram of oxygen and water vapor diffusion rate test;

[0027] Figure 5 It is a schematic side view of the liquid water permeability of the GDL;

[0028] Figure 6 It is a border package diagram;

[0029] Figures 7 to 13 is a comparison diagram of calculation results of an embodiment;

[0030] The markings in the above figures are: 1. first end plate; 2. second end plate; 3. first inlet; 4. second outlet; 5. mounting hole; 6. fastening bolt; 7. sealing element; 8. sample to be tested. DETAILED DESCRIPTION

[0031] The specific implementation methods of the present invention are further explained in detail below by describing the embodiments with reference to the accompanying drawings, with the aim of helping those skilled in the art to have a more complete, accurate and in-depth understanding of the concept and technical solution of the present invention and facilitating its implementation.

[0032] It should be noted that when an element is referred to as being "fixed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower" and similar expressions used in this article are for illustrative purposes only.

[0033] It should be noted that, in the following embodiments, the “first”, “second” and “third” mentioned do not represent an absolute distinction in structure and / or function, nor do they represent a sequence of execution, but are merely for the convenience of description.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly connected by technicians in the technical field to which the present invention belongs. The terminology used in the specification of the present invention is for the purpose of describing specific embodiments and is not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0035] like Figure 1 As shown, the present invention provides a method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer, comprising the following steps:

[0036] S1. Provide test fixture and package the sample to be tested;

[0037] S2. After the test fixture clamps the package assembly, a sealing test is performed;

[0038] S3, introducing a first gas or liquid water into a first inlet of the test fixture, and introducing a second gas or a third gas into a second inlet of the test fixture to perform a test;

[0039] S4. Obtain relevant data;

[0040] S5. Calculate the oxygen diffusivity, water vapor diffusivity, and liquid water permeability.

[0041] like Figure 2 and Figure 3 As shown, the test fixture includes a first end plate 1 and a second end plate 2 that cooperate to clamp the package assembly, a first inlet 3 and a first outlet are provided on the first end plate 1, a second inlet and a second outlet 4 are provided on the second end plate 2, a first flow channel is provided between the first inlet 3 and the first outlet in the first end plate 1, the first flow channel is communicated with the first inlet 3 and the first outlet, a second flow channel is provided between the second inlet and the second outlet 4 in the second end plate 2, the second flow channel is communicated with the second inlet and the second outlet 4. The first inlet 3 is provided for introducing a first gas or liquid water, and the second inlet is provided for introducing a second gas or a third gas.

[0042] Specifically, when testing the gas transmission capacity, a first gas is introduced into the first inlet of the test fixture, and a second gas is introduced into the second inlet of the test fixture, wherein the first gas is humidified nitrogen and the second gas is pure dry oxygen. When testing the water transmission capacity, liquid water is introduced into the first inlet of the test fixture, and a third gas is introduced into the second inlet of the test fixture, wherein the third gas is pure dry air.

[0043] An oxygen sensor is arranged at the first outlet, and a humidity sensor is arranged at the second outlet 4 .

[0044] The first end plate 1 and the second end plate 2 are provided with mounting holes 5 for mounting thermocouples.

[0045] The materials used for the first end plate 1 and the second end plate 2 are determined by specific tests. The first end plate 1 and the second end plate 2 can be made of high thermal conductivity materials such as graphite plates and aluminum alloys, and heating plates are installed on both sides of the first end plate 1 and the second end plate 2. The heating plates are used to heat the first end plate 1 and the second end plate 2 during the test. Thermocouples are installed on the first end plate 1 and the second end plate 2 to facilitate temperature control during heating.

[0046] The first end plate 1 and the second end plate 2 are made of transparent material. The first end plate 1 and the second end plate 2 are fixedly connected by fastening bolts 6, and a plurality of fastening bolts 6 are provided.

[0047] In step S4, the acquired relevant data include the oxygen concentration at the first outlet, the oxygen concentration at the second inlet, the humidity at the first inlet, and the humidity at the second outlet.

[0048] Embodiment 1

[0049] like Figures 2 to 4 As shown, the test fixture is used to clamp the packaging assembly when testing the gas transmission capability of the fuel cell gas diffusion layer.

[0050] When testing the oxygen and water vapor diffusion rates of the gas diffusion layer, in the above step S3, a first gas with a certain humidity is introduced into the first end plate 1 from the first inlet 3, the first gas flows to the gas diffusion layer through the first flow channel, and then flows into the second flow channel, and a second gas is introduced into the second end plate 2 from the second inlet, the second gas flows to the gas diffusion layer through the second flow channel, and then flows into the first flow channel.

[0051] In the above step S4 , an oxygen sensor is provided at the first outlet, and a humidity sensor is provided at the second outlet 4 . The oxygen sensor detects the oxygen concentration at the first outlet, and the humidity sensor detects the humidity at the second outlet 4 .

[0052] like Figure 2 As shown, mounting holes 5 for mounting thermocouples are provided on the first end plate 1 and the second end plate 2. Heating plates are installed on both sides of the first end plate 1 and the second end plate 2. In the above step S3, the heating plates are used to heat the first end plate 1 and the second end plate 2 respectively. Thermocouples are also installed on the first end plate 1 and the second end plate 2 to facilitate temperature control during heating.

[0053] In this embodiment, the first flow channel and the second flow channel are serpentine flow channels.

[0054] like Figure 2 As shown, the first end plate 1 and the second end plate 2 are fixedly connected by fastening bolts 6, a plurality of fastening bolts 6 are provided, and bolt holes for the fastening bolts 6 to pass through are provided on the first end plate 1 and the second end plate 2. By tightening the fastening bolts 6, the first end plate 1 and the second end plate 2 are fixedly connected together. In the above step S2, the first end plate 1 and the second end plate 2 clamp the sample to be tested in the middle.

[0055] like Figure 4 As shown, the edge of the packaging assembly is sealed with a sealing element 7 to ensure that the gas in the first end plate 1 below can only diffuse into the second end plate 2 through the gas diffusion layer. Similarly, the edge of the packaging assembly is sealed with a sealing element 7 to ensure that the gas in the second end plate 2 below can only diffuse into the first end plate 1 through the gas diffusion layer. A sealing element 7 is provided between the outer edge of the packaging assembly and the first end plate 1, and a sealing element 7 is also provided between the outer edge of the packaging assembly and the second end plate 2. In this way, during the test, the gas can only diffuse into the two end plates through the gas diffusion layer, and the gas cannot pass through the gap between the outer edge of the packaging assembly and the inner wall surface of the fixture, which helps to improve the accuracy of the test results.

[0056] In this embodiment, the sealing element 7 is a rubber sealing ring.

[0057] The method for testing the water vapor transmission capacity of the fuel cell gas diffusion layer provided in this embodiment includes the following steps:

[0058] S1. Provide a test fixture, package the sample to be tested, and form a package assembly;

[0059] When packaging the sample to be tested, first cut two frames of pressure-sensitive or hot-melt PEN material into specific shapes to make a first frame and a second frame, and place them in the order of the first frame, the sample to be tested, and the second frame (where the sample to be tested is a gas diffusion layer), and then package them through a pressing or hot pressing process to ensure that there are no bubbles. The sample to be tested is sandwiched between the first frame and the second frame to assemble into a packaging component, such as Figure 6 As shown;

[0060] S2. After the test fixture clamps the package assembly, a sealing test is performed;

[0061] The packaging assembly is clamped by the first end plate 1 and the second end plate 2, and the edge of the packaging assembly is sealed with a sealing element 7. Pure dry nitrogen after drying is introduced into the first inlet and the second inlet of the test fixture to cause the air in the test fixture to be discharged to the outside, which helps to improve the accuracy of the test results. After the pressure in the test fixture reaches 50 kPa, the pressure is maintained for a period of time, and a pressure holding experiment is carried out to ensure that the test fixture is sealed.

[0062] S3, introducing a first gas into a first inlet of the test fixture, and introducing a second gas into a second inlet of the test fixture to perform a test;

[0063] S4. Obtain relevant data;

[0064] S5. Calculate the oxygen diffusivity, water vapor diffusivity, and liquid water permeability.

[0065] In the above step S3, the first gas is humidified nitrogen, the humidity of the first gas needs to reach the required value, and the second gas is pure dry oxygen. The flow rate of the first gas is 0.1-3 slpm, and the flow rate of the second gas is 0.1-3 slpm. The first end plate 1 and the second end plate 2 are heated to simulate the temperature during the operation of the fuel cell. Nitrogen with a specific humidity is introduced into the first inlet 3, and partial condensation simulates the real situation in the fuel cell.

[0066] In the above step S4, the acquired relevant data include the oxygen concentration at the first outlet, the oxygen concentration at the second inlet, the humidity at the first inlet and the humidity at the second outlet.

[0067] In the above step S4, part of the water vapor passes through the gas diffusion layer to the second end plate 2, and the water vapor humidity can be detected by the humidity sensor at the second outlet 4. The oxygen in the second end plate 2 passes through the gas diffusion layer to the first end plate 1, and the oxygen concentration can be detected at the first outlet. When obtaining relevant data, the duration of the first gas passing through the first inlet of the test fixture is at least 30 minutes, and the duration of the second gas passing through the second inlet of the test fixture is at least 30 minutes. Ensure that the readings of the oxygen sensor and the humidity sensor are stable. After it is considered that the overall steady state has been reached, read the corresponding value to obtain the oxygen concentration C O2 and humidity η O2 .

[0068] In the above step S5, the oxygen and water vapor diffusion rate test results are calculated according to the following formulas (1) and (2):

[0069]

[0070] Among them, D O2 is the oxygen diffusion rate, in m -2 ;

[0071] S 测试活性面积 is the active area, in m 2 ;

[0072] C 入 is the oxygen concentration at the second inlet;

[0073] C 出 is the oxygen concentration at the first outlet;

[0074] μ is the gas flow rate;

[0075] h is the thickness of the sample to be tested.

[0076]

[0077] Among them, ξ O2 is the water vapor diffusion rate, in m -2 ;

[0078] S 测试活性面积 is the active area, in m 2 ;

[0079] η 入 is the nitrogen humidity at the first inlet 3;

[0080] η 出 The humidity sensor reading at the second outlet 4;

[0081] μ is the gas flow rate;

[0082] h is the thickness of the sample to be tested.

[0083] Embodiment 2

[0084] like Figures 2 to 4 As shown, the test fixture is used to clamp the package assembly when testing the water transmission capacity of the gas diffusion layer of the fuel cell.

[0085] The first inlet 3 is configured to be used for introducing liquid water, which is deionized water, and the second inlet is configured to be used for introducing a third gas, which is pure dry air.

[0086] When testing the water transmission capacity of the gas diffusion layer, in the above step S3, liquid water is introduced into the first end plate 1 from the first inlet 3, the liquid water flows to the gas diffusion layer through the first flow channel, and then flows into the second flow channel, the third gas is introduced into the second end plate 2 from the second inlet, the third gas flows to the gas diffusion layer through the second flow channel, and then flows into the first flow channel. A humidity sensor is provided at the second outlet 4, and the humidity sensor is used to detect the humidity at the second outlet 4. By detecting the humidity at the second outlet 4, the transmission capacity of the gas diffusion layer for liquid water can be obtained.

[0087] like Figure 2 As shown, mounting holes 5 for mounting thermocouples are provided on the first end plate 1 and the second end plate 2. Heating plates are installed on both sides of the first end plate 1 and the second end plate 2, and the heating plates are used to heat the first end plate 1 and the second end plate 2 respectively during the test process. Thermocouples are also installed on the first end plate 1 and the second end plate 2 to facilitate temperature control during heating.

[0088] In this embodiment, the first flow channel and the second flow channel are serpentine flow channels.

[0089] like Figure 2 As shown, the first end plate 1 and the second end plate 2 are fixedly connected by fastening bolts 6, a plurality of fastening bolts 6 are provided, and bolt holes for the fastening bolts 6 to pass through are provided on the first end plate 1 and the second end plate 2. By tightening the fastening bolts 6, the first end plate 1 and the second end plate 2 are fixedly connected together, and the first end plate 1 and the second end plate 2 clamp the packaging component in the middle.

[0090] like Figure 4 As shown, the edge of the packaging assembly is sealed with a sealing element 7 to ensure that the gas in the first end plate 1 below can only diffuse into the second end plate 2 through the gas diffusion layer. Similarly, the edge of the packaging assembly is sealed with a sealing element 7 to ensure that the gas in the second end plate 2 below can only diffuse into the first end plate 1 through the gas diffusion layer. A sealing element 7 is provided between the outer edge of the packaging assembly and the first end plate 1, and a sealing element 7 is also provided between the outer edge of the packaging assembly and the second end plate 2. In this way, during the test, the gas can only diffuse into the two end plates through the gas diffusion layer, and the gas cannot pass through the gap between the outer edge of the packaging assembly and the inner wall surface of the fixture, which helps to improve the accuracy of the test results.

[0091] In this embodiment, the sealing element 7 is a rubber sealing ring.

[0092] The method for testing the water vapor transmission capacity of the fuel cell gas diffusion layer provided in this embodiment includes the following steps:

[0093] S1. Provide a test fixture, package the sample to be tested, and form a package assembly;

[0094] When packaging the sample to be tested, first cut two frames of pressure-sensitive or hot-melt PEN material into specific shapes to make a first frame and a second frame, and place them in the order of the first frame, the sample to be tested, the proton exchange membrane, and the second frame (where the sample to be tested is a gas diffusion layer), and then package them through a pressing or hot pressing process to ensure that there are no bubbles. The sample to be tested and the proton exchange membrane are sandwiched between the first frame and the second frame to assemble into a packaging component, such as Figure 6 As shown;

[0095] S2. After the test fixture clamps the package assembly, a sealing test is performed;

[0096] The packaging assembly is clamped by the first end plate 1 and the second end plate 2, and the edge of the packaging assembly is sealed with a sealing element 7. Pure dry nitrogen after drying is introduced into the first inlet and the second inlet of the test fixture to promote the air in the test fixture to be discharged to the outside, which helps to improve the accuracy of the test results. After the pressure in the test fixture reaches 50kPa, the pressure is maintained for a period of time, and a pressure holding experiment is performed to ensure that the test fixture is sealed;

[0097] S3, introducing liquid water into the first inlet of the test fixture, and introducing a third gas into the second inlet of the test fixture to perform a test;

[0098] S4. Obtain relevant data;

[0099] S5. Calculate the oxygen diffusivity, water vapor diffusivity, and liquid water permeability.

[0100] In the above step S2, the first end plate 1 and the second end plate 2 are heated, the temperature of the first end plate 1 is set to Ta, and the temperature of the second end plate 2 is set to Tc, and Tc is higher than Ta.

[0101] In the above step S3, the flow rate of liquid water into the first inlet is 0.1-3 slpm, and the flow rate of the third gas into the second inlet is 0.1-3 slpm. The first end plate 1 and the second end plate 2 are heated to simulate the temperature during the operation of the fuel cell.

[0102] In the above step S4, the relevant data obtained includes the humidity at the second outlet.

[0103] In the above step S4, when obtaining relevant data, the duration of introducing liquid water into the first inlet of the test fixture is at least 30 minutes, and the duration of introducing the third gas into the second inlet of the test fixture is at least 30 minutes. Ensure that the humidity sensor reading is stable. After it is considered that the whole reaches a steady state, read the corresponding value to obtain the humidity η O2 .

[0104] In the above step S5, the liquid water permeability test result is calculated according to the following formula (3):

[0105]

[0106] Among them, ψ O2 is the liquid water permeability of the gas diffusion layer, in m -2 ;

[0107] S 测试活性面积 is the active area, in m 2 ;

[0108] η liquid The humidity sensor reading at the second outlet 4;

[0109] μ is the gas flow rate;

[0110] h is the thickness of the sample to be tested.

[0111] In this embodiment, the first end plate 1 and the second end plate 2 are made of a transparent material, which may be glass or transparent acrylic. During the test, the flow condition of liquid water in the flow channel can be observed through the transparent end plate, which facilitates the observation of the liquid water transmission process and the analysis of the flow channel and GDL water transmission conditions.

[0112] Embodiment 3

[0113] The method for testing the water vapor transmission capacity of the fuel cell gas diffusion layer provided in this embodiment includes the following steps:

[0114] S1. Provide a test fixture, package the sample to be tested, and form a package assembly;

[0115] When packaging the sample to be tested, first cut two frames of pressure-sensitive or hot-melt PEN material into specific shapes to make a first frame and a second frame, place them in the order of the first frame, the sample to be tested, and the second frame, and then package them by pressing or hot pressing to ensure that there are no bubbles. The sample to be tested is sandwiched between the first frame and the second frame, and the microporous layer of the sample to be tested faces the first frame, and is assembled into a packaging component, such as Figure 6 As shown;

[0116] S2. After the test fixture clamps the package assembly, a sealing test is performed;

[0117] A packaging assembly is clamped by the first end plate 1 and the second end plate 2, and the edge of the packaging assembly is sealed with a sealing element 7. Pure dry nitrogen after drying is introduced into the first inlet and the second inlet of the test fixture to cause the air in the test fixture to be discharged to the outside, which helps to improve the accuracy of the test results. After the pressure in the test fixture reaches 50kPa, the pressure is maintained for a period of time, and a pressure holding experiment is carried out to ensure that the test fixture is sealed.

[0118] S3, introducing a first gas into a first inlet of the test fixture, and introducing a second gas into a second inlet of the test fixture to perform a test;

[0119] The first gas is humidified nitrogen, and the humidity of the first gas needs to reach the required value. The second gas is pure dry oxygen. The flow rate of the first gas is 0.1-3slpm, and the flow rate of the second gas is 0.1-3slpm. Heat the first end plate 1 and the second end plate 2 to simulate the temperature during the operation of the fuel cell. Nitrogen with a specific humidity is introduced into the first inlet 3, and partial condensation simulates the real situation in the fuel cell.

[0120] S4. Obtain relevant data;

[0121] Part of the water vapor passes through the gas diffusion layer to the second end plate 2, and the water vapor humidity can be detected by the humidity sensor at the second outlet 4. The oxygen in the second end plate 2 passes through the gas diffusion layer to the first end plate 1, and the oxygen concentration can be detected at the first outlet. When obtaining relevant data, the first gas is introduced into the first inlet of the test fixture for at least 30 minutes, and the second gas is introduced into the second inlet of the test fixture for at least 30 minutes. Ensure that the readings of the oxygen sensor and the humidity sensor are stable. After the overall steady state is reached, read the corresponding value to obtain the oxygen concentration C O2 and humidity η O2 ;

[0122] S5. Calculate the oxygen diffusivity, water vapor diffusivity, and liquid water permeability.

[0123] In this embodiment, three gas diffusion layers are taken as samples to be tested, and the three gas diffusion layers are respectively made into three packaging components according to the process of step S1. Then, the three packaging components are tested in sequence according to the order of steps S2 to S5.

[0124] In the above step S4, corresponding data when the three package components are tested respectively are obtained.

[0125] In the above step S5, the oxygen and water vapor diffusion rate test results are calculated according to the following formulas (1) and (2):

[0126]

[0127] Among them, D O2is the oxygen diffusion rate, in m -2 ;

[0128] S 测试活性面积 is the active area, in m 2 ;

[0129] C 入 is the oxygen concentration at the second inlet;

[0130] C 出 is the oxygen concentration at the first outlet;

[0131] μ is the gas flow rate;

[0132] h is the thickness of the sample to be tested.

[0133]

[0134] Among them, ξ O2 is the water vapor diffusion rate, in m -2 ;

[0135] S 测试活性面积 is the active area, in m 2 ;

[0136] η 入 is the nitrogen humidity at the first inlet 3;

[0137] η 出 The humidity sensor reading at the second outlet 4;

[0138] μ is the gas flow rate;

[0139] h is the thickness of the sample to be tested.

[0140] The oxygen permeabilities of GDL1 (the gas diffusion layer of the first package component), GDL2 (the gas diffusion layer of the second package component), and GDL3 (the gas diffusion layer of the third package component) are measured as follows: O2,GDL1 =0.432m -2 , D O2,GDL2 =0.682m -2 , D O2,GDL3 =1.121m -2 The water vapor permeabilities of GDL1 (the gas diffusion layer of the first package component), GDL2 (the gas diffusion layer of the second package component), and GDL3 (the gas diffusion layer of the third package component) are: ξ O2,GDL1 =0.323m -2 , O2,GDL2 =0.421m -2 , O2,GDL3 =0.432m -2In addition, the porosity and contact angle of GDL1, GDL2 and GDL3 were tested. The specific test results are as follows: Figure 7 , Figure 8 and Fig.11 shown.

[0141] The above three GDLs were assembled with standard CCM (membrane electrode assembly) to form MEA (fuel cell), and the battery was assembled for testing. Test condition 1 (high humidity) was a cathode air stoichiometric ratio of 2.5, cathode humidification of 100% RH; anode hydrogen stoichiometric ratio of 1.8, anode humidification of 100% RH; battery temperature of 85°C. Test condition 2 (low humidity) was a cathode air stoichiometric ratio of 2.5, cathode no humidification, humidity of 0; anode hydrogen stoichiometric ratio of 1.8, cathode no humidification, humidity of 0; battery temperature of 85°C.

[0142] Embodiment 4

[0143] The method for testing the water vapor transmission capacity of the fuel cell gas diffusion layer provided in this embodiment includes the following steps:

[0144] S1. Provide a test fixture, package the sample to be tested, and form a package assembly;

[0145] When packaging the sample to be tested, first cut two frames of pressure-sensitive or hot-melt PEN material into specific shapes to make a first frame and a second frame, place them in the order of the first frame, the sample to be tested, the proton exchange membrane, and the second frame, and then package them through a pressing or hot pressing process to ensure that there are no bubbles. The sample to be tested and the proton exchange membrane are sandwiched between the first frame and the second frame to assemble into a packaging component, such as Figure 6 As shown;

[0146] S2. After the test fixture clamps the package assembly, a sealing test is performed;

[0147] The packaging assembly is clamped by the first end plate 1 and the second end plate 2, and the edge of the packaging assembly is sealed with a sealing element 7. Pure dry nitrogen after drying is introduced into the first inlet and the second inlet of the test fixture to promote the air in the test fixture to be discharged to the outside, which helps to improve the accuracy of the test results. After the pressure in the test fixture reaches 50kPa, the pressure is maintained for a period of time, and a pressure holding experiment is performed to ensure that the test fixture is sealed;

[0148] S3, introducing liquid water into the first inlet of the test fixture, and introducing a third gas into the second inlet of the test fixture to perform a test;

[0149] The flow rate of liquid water introduced into the first inlet is 0.1 to 3 slpm, and the flow rate of the third gas introduced into the second inlet is 0.1 to 3 slpm. The first end plate 1 and the second end plate 2 are heated to simulate the temperature during the operation of the fuel cell;

[0150] S4. Obtain relevant data;

[0151] When obtaining relevant data, liquid water is introduced into the first inlet of the test fixture for at least 30 minutes, and the third gas is introduced into the second inlet of the test fixture for at least 30 minutes. Ensure that the humidity sensor reading is stable. After the overall steady state is reached, read the corresponding value to obtain the humidity η O2 ;

[0152] S5. Calculate the oxygen diffusivity, water vapor diffusivity, and liquid water permeability.

[0153] In this embodiment, three gas diffusion layers are taken as samples to be tested, and the three gas diffusion layers are respectively made into three packaging components according to the process of step S1. Then, the three packaging components are tested in sequence according to the order of steps S2 to S5.

[0154] In the above step S4, corresponding data when the three package components are tested respectively are obtained.

[0155] In the above step S5, the liquid water permeability test result is calculated according to the following formula (3):

[0156]

[0157] Among them, ψ O2 is the liquid water permeability of the gas diffusion layer, in m -2 ;

[0158] S 测试活性面积 is the active area, in m 2 ;

[0159] η liquid The humidity sensor reading at the second outlet 4;

[0160] μ is the gas flow rate;

[0161] h is the thickness of the sample to be tested.

[0162] The liquid water permeability ψ of GDL1 (the gas diffusion layer of the first package component), GDL2 (the gas diffusion layer of the second package component), and GDL3 (the gas diffusion layer of the third package component) was measured. O2,GDL1 =0.421m -2 , O2,GDL2 =0.552m -2 , O2,GDL3 =0.684m -2 , the specific test results are as follows Fig. 9 shown.

[0163] Example description:

[0164] Example 3 mainly tests the oxygen permeability D of GDL1, GDL2, and GDL3 O2 and the water vapor permeability ξ O2 ; Example 4 mainly tests the liquid water permeability ψ of GDL1, GDL2, and GDL3 O2 . The same samples were used in Examples 3 and 4, and the porosity and contact angle of these GDLs were tested, mainly to mutually verify the results of water vapor permeability with the pore contact angle; the battery performance of these GDLs under high and low humidity conditions was tested, mainly to verify the influence of different water vapor permeabilities on battery performance.

[0165] The test results show that: D O2,GDL1 < D O2,GDL2 < D O2,GDL3 ; ξ O2,GDL1 < ξ O2,GDL2 < ξ O2,GDL3 , which shows that; the oxygen permeability of GDL1 is the smallest, followed by GDL2, and the largest is GDL3, which is consistent with the porosity test results, that is, the porosity size order is GDL1 < GDL2 < GDL3, while the contact angles of GDL1, GDL2, and GDL3 are not much different, then there is a great correlation between its water vapor permeability, liquid water permeability and pore size, and the laws of its water vapor permeability and liquid water permeability also conform to GDL1 < GDL2 < GDL3. Finally, the battery performance test shows that the battery performance is higher under high humidity, but there are high requirements for the drainage ability, so GDL1 < GDL2 < GDL3. Under low humidity, the battery performance is slightly worse, and there are certain requirements for the water retention ability of GDL, so GDL1 > GDL2 > GDL3.

[0166] In summary, the present invention provides two test methods, namely Method 1 for simultaneously testing oxygen permeability and water vapor permeability, and Method 2 for testing liquid water permeability. Its test results are mutually verified with the porosity and high and low humidity battery performance results. This test method provides a good method for characterizing the water and gas characteristics of GDL.

[0167] The present invention has been described exemplarily above in conjunction with the accompanying drawings. Obviously, the specific implementation of the present invention is not limited by the above-mentioned manner. As long as various non-substantive improvements are made by adopting the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer, characterized in that: Includes steps: S1. Provide test fixture and package the sample to be tested; S2. After the test fixture clamps the package assembly, a sealing test is performed; S3, introducing a first gas or liquid water into a first inlet of the test fixture, and introducing a second gas or a third gas into a second inlet of the test fixture to perform a test; S4. Obtain relevant data; S5. Calculate the oxygen diffusivity, water vapor diffusivity, and liquid water permeability.

2. The method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer according to claim 1, characterized in that: The test fixture includes a first end plate and a second end plate that cooperate to clamp the sample to be tested, the first end plate is provided with the first inlet and the first outlet, the second end plate is provided with the second inlet and the second outlet, a first flow channel is provided in the first end plate between the first inlet and the first outlet, the first flow channel is connected with the first inlet and the first outlet, a second flow channel is provided in the second end plate between the second inlet and the second outlet, the second flow channel is connected with the second inlet and the second outlet.

3. The method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer according to claim 1, characterized in that: When testing the gas transmission capacity, a first gas is introduced into the first inlet of the test fixture, and a second gas is introduced into the second inlet of the test fixture. The first gas is humidified nitrogen, and the second gas is pure dry oxygen.

4. The method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer according to claim 1, characterized in that: When testing the water transmission capacity, liquid water is introduced into the first inlet of the test fixture, and a third gas is introduced into the second inlet of the test fixture, wherein the third gas is pure dry air.

5. The method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer according to claim 2, characterized in that: An oxygen sensor is arranged at the first outlet, and a humidity sensor is arranged at the second outlet.

6. The method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer according to any one of claims 1 to 5, characterized in that: In step S4, the acquired relevant data includes the oxygen concentration at the first outlet, the oxygen concentration at the second inlet, the humidity at the first inlet, and the humidity at the second outlet.

7. The method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer according to claim 6, characterized in that: In step S5, according to the formula Calculate the oxygen diffusion rate D O2 , where S 测试活性面积 is the active area, C 入 is the oxygen concentration at the second inlet, C 出 is the oxygen concentration at the first outlet, μ is the gas flow rate, and h is the thickness of the sample to be tested.

8. The method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer according to claim 6, characterized in that: In step S5, according to the formula Calculate the water vapor diffusion rate ξ O2 , where S 测试活性面积 is the active area, η 入 is the nitrogen humidity at the first inlet, η 出 is the humidity sensor reading at the second outlet, μ is the gas flow rate, and h is the thickness of the sample to be tested.

9. The method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer according to claim 6, characterized in that: In step S5, according to the formula Calculate the liquid water permeability ψ O2 , where S 测试活性面积 is the active area, η liquid is the humidity sensor reading at the second outlet, μ is the gas flow rate, and h is the thickness of the sample to be tested.

10. The method for testing the water vapor transmission capacity of a fuel cell gas diffusion layer according to any one of claims 2 to 9, characterized in that: The first end plate and the second end plate are made of transparent material.

Citation Information

Cited By

  • PEM electrolytic cell GDL performance test method and system based on multi-dimensional parameters

    CN120445325A