Continuous determination method for iron content in galvanizing flux

Through the titration method, the Fe2+ and Fe3+ content in the galvanized plating aid was calculated step by step by step, and the iron content in the galvanized plating aid was achieved, and the precision measurement in the prior art was solved. and the problem of low accuracy improves the quality and production efficiency of galvanizing.

CN119086686APending Publication Date: 2024-12-06HEBEI UNIV OF ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213876.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art has low precision and accuracy in detecting iron ions in galvanized plating aids, and the traditional method takes a long time and cannot provide real-time feedback on the changes in the iron in the plating aids, which affects the quality of galvanizing and production costs.

Method used

The saturated calomel electrode and platinum electrode were used for titration detection. The mixture was mixed with the acid mixing buffer and the plating agent solution and titrated in combination with the standard solution of cerium sulfate. The Fe2+ and Fe3+ content were calculated step by step to achieve continuous determination of the total iron content.

Benefits of technology

It improves the precision and accuracy of determining the iron content in galvanized plating aid, is easy to operate, can monitor iron changes in real time, and improves iron removal efficiency and galvanizing quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086686A_ABST
    Figure CN119086686A_ABST
Patent Text Reader

Abstract

The invention provides a continuous determination method for the iron content in a galvanizing assistant agent, and belongs to the technical field of galvanizing assistant agent solution analysis methods. According to the method, the content of Fe < 2 + > and total iron in the plating assistant solution is continuously measured through the automatic potentiometric titrator, an existing method for measuring the content of iron in the hot-dip galvanizing plating assistant is updated, and the method has the advantages of being good in precision, high in accuracy, convenient and rapid to operate and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of zinc plating auxiliary agent solution analysis methods, in particular to a method for continuously determining the iron content in a zinc plating auxiliary agent. Background Art

[0002] Hot-dip galvanizing has long been the most widely used process in steel galvanizing. The main process flow includes: pre-plating parts - alkaline washing and degreasing - water washing - pickling and rust removal - water washing - solvent-assisted plating - drying - hot-dip galvanizing - cooling - post-treatment, among which solvent-assisted plating plays a pivotal role in the galvanizing process. However, the presence of iron ions will have a negative impact on it, not only increasing the viscosity of the residual salt of the plating agent and the difficulty of removal, but also increasing the time required for the plating salt to crystallize on the surface of the workpiece. More importantly, the iron ions in the plating agent are brought into the zinc pot, where they react with zinc to form a zinc-iron alloy, namely zinc slag, resulting in ineffective zinc consumption, and eventually forming particles on the iron-based surface of the grid plate, namely quality defects. In order to effectively control the iron ions in the plating agent, it is necessary to adopt purification and iron removal technology, which mainly removes the divalent iron ions in the plating agent, oxidizes the divalent iron ions into trivalent iron ions, and hydrolyzes and precipitates them. When there is too much precipitated iron mud, it will affect the circulation of the plating agent solution. Therefore, it is removed by membrane filtration and left in the filter press, while the solution containing ammonium chloride and zinc chloride is returned to the plating agent pool, achieving limited separation of solid impurities and plating agent solution, and finally controlling the content of ferrous chloride and ferric hydroxide to be less than 0.4g / L. Therefore, it is particularly important to monitor the content of ferrous chloride and ferric hydroxide in the plating agent solution in real time and accurately. At present, most of the detection methods for the iron content of the plating solution in the domestic electroplating industry rely on the national standard method. Among them, the photometric method is suitable for micro-analysis, but not for constant detection, because the pH value of the solution increases when the electroplating solution sample to be tested is diluted exponentially, and the electroplating solution sample containing a variety of impurity ions will undergo different degrees of hydrolysis, which ultimately causes inaccurate test results, and is time-consuming and cumbersome. The titration method often uses high-chromium reagents, which pollutes the environment. In addition, the existing method is time-consuming and cannot timely feedback the changes in the iron in the electroplating tank, resulting in a decrease in the iron removal efficiency in the electroplating tank, which directly affects the quality of zinc plating and production costs. The national standard method for determining iron content is suitable for simple mixed systems with fewer interfering components, while the electroplating solution is a complex mixed system, so the pretreatment of the sample is particularly important. Therefore, it is of great significance to explore the sample pretreatment method for detecting the iron content in the electroplating tank and to establish an accurate and rapid method for detecting the iron content in the electroplating tank. Summary of the invention

[0003] The purpose of the present invention is to provide a method for continuously determining the iron content in a zinc plating auxiliary agent, so as to solve the technical problem that the detection precision and accuracy of divalent iron and trivalent iron ions in the current plating auxiliary agent solution are not high.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for continuously determining the iron content in a zinc plating auxiliary agent, comprising the following steps:

[0006] (1) Mixing a plating agent solution and a mixed acid buffer, stirring under heating until the solution is clear, and using the solution to be tested;

[0007] (2) Using a saturated calomel electrode as the reference electrode and a platinum electrode as the indicator electrode, the test solution was titrated with a cerium sulfate standard solution, the change in the system potential value was recorded, and a titration curve was drawn. Fe 2+ Content C1,

[0008]

[0009] Where C1 is the FeCl2 content in the plating agent solution, g / L; C2 is the concentration of the cerium sulfate standard solution, mol / L; V1 is the sampling volume of the plating agent solution, mL; V2 is the volume of the consumed cerium sulfate standard solution, mL; M1 is the relative molecular mass of FeCl2, g / mol;

[0010] (3) then adding hydrochloric acid solution to the test solution of step (2) and heating, adding stannous chloride solution until the solution is colorless, adding 2 to 3 drops of methyl orange solution to obtain a secondary titration solution;

[0011] (4) Using a saturated calomel electrode as the reference electrode and a platinum electrode as the indicator electrode, the secondary titration solution was titrated with a cerium sulfate standard solution, the change in the system potential value was recorded, and a titration curve was drawn. The Fe 3+ Content C3,

[0012]

[0013] Wherein: C3 is the Fe(OH)3 content in the plating agent, g / L; C2 is the concentration of the cerium sulfate standard solution, mol / L; V1 is the sampling volume of the plating agent solution, mL; V3 is the total volume of the cerium sulfate standard solution consumed, mL; M2 is the relative molecular mass of Fe(OH)3, g / mol;

[0014] The total iron content is C=C1+C3.

[0015] Furthermore, the mixed acid buffer contains disodium hydrogen phosphate, hydrochloric acid, citric acid, trichloroacetic acid and water, and the dosage ratio of the disodium hydrogen phosphate, hydrochloric acid, citric acid, trichloroacetic acid and water is 0.1-0.5g:10-50mL:0.03-0.05g:0.01-0.02g:50mL.

[0016] Furthermore, in step (1), the heating temperature is 50 to 90° C., and the stirring time is 1 to 30 min.

[0017] Furthermore, the volume ratio of the plating assistant solution to the mixed acid buffer is 25:10-15.

[0018] Furthermore, in step (3), the amount of hydrochloric acid solution added is 2 to 2.5 times the volume of the plating aid solution, the volume ratio of the stannous chloride solution to the hydrochloric acid solution is 1 to 3:50, and the concentration of the stannous chloride solution is 0.1 mol / L.

[0019] Furthermore, the preparation of the cerium sulfate standard solution refers to GB / T601-2002.

[0020] Beneficial effects of the present invention:

[0021] The Fe in the plating aid of the present invention 2+ , Fe 3+ As well as a method for continuous determination of total iron content, the existing method for determining the iron content in hot-dip galvanizing flux is updated, and has the characteristics of good precision, high accuracy, and convenient and quick operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The titration curves are for different volumes of iron standard solution;

[0023] Figure 2 It is the continuous titration curve of total iron in different volumes of iron standard solution;

[0024] Figure 3 It is the standard curve for continuous titration of iron;

[0025] Figure 4 A separate standard curve was determined for total iron;

[0026] Figure 5 The Fe of the plating assistant solution in Example 1 of the present invention 2+ Assay curve;

[0027] Figure 6 This is the total iron content determination curve of the plating auxiliary agent solution in Inventive Example 1. DETAILED DESCRIPTION

[0028] The present invention provides a method for continuously determining the iron content in a zinc plating auxiliary agent, comprising the following steps:

[0029] (1) Mixing a plating agent solution and a mixed acid buffer, stirring under heating until the solution is clear, and using the solution to be tested;

[0030] (2) Using a saturated calomel electrode as the reference electrode and a platinum electrode as the indicator electrode, the test solution was titrated with a cerium sulfate standard solution, the change in the system potential value was recorded, and a titration curve was drawn. Fe 2+ Content C1,

[0031]

[0032] Where C1 is the FeCl2 content in the plating agent solution, g / L; C2 is the concentration of the cerium sulfate standard solution, mol / L; V1 is the sampling volume of the plating agent solution, mL; V2 is the volume of the consumed cerium sulfate standard solution, mL; M1 is the relative molecular mass of FeCl2, g / mol;

[0033] (3) then adding hydrochloric acid solution to the test solution of step (2) and heating, adding stannous chloride solution until the solution is colorless, adding 2 to 3 drops of methyl orange solution to obtain a secondary titration solution;

[0034] (4) Using a saturated calomel electrode as the reference electrode and a platinum electrode as the indicator electrode, the secondary titration solution was titrated with a cerium sulfate standard solution, the change in the system potential value was recorded, and a titration curve was drawn. The Fe 3+ Content C3,

[0035]

[0036] Wherein: C3 is the Fe(OH)3 content in the plating agent, g / L; C2 is the concentration of the cerium sulfate standard solution, mol / L; V1 is the sampling volume of the plating agent solution, mL; V3 is the total volume of the cerium sulfate standard solution consumed, mL; M2 is the relative molecular mass of Fe(OH)3, g / mol;

[0037] The total iron content is C=C1+C3.

[0038] In the present invention, the mixed acid buffer comprises disodium hydrogen phosphate, hydrochloric acid, citric acid, trichloroacetic acid and water, and the dosage ratio of the disodium hydrogen phosphate, hydrochloric acid, citric acid, trichloroacetic acid and water is 0.1-0.5g:10-50mL:0.03-0.05g:0.01-0.02g:50mL, preferably 0.2-0.4g:20-40mL:0.035-0.045g:0.01g:50mL, and more preferably 0.3g:30mL:0.04g:0.01g:50mL.

[0039] In the present invention, the heating temperature in step (1) is 50-90° C., preferably 90° C.; the stirring time is 1-30 min, preferably 1 min.

[0040] In the present invention, the volume ratio of the plating assistant solution to the mixed acid buffer is 25:10-15, preferably 25:15.

[0041] In the present invention, in step (3), the amount of hydrochloric acid solution added is 2 to 2.5 times the volume of the plating aid solution, preferably 2 times; the volume ratio of stannous chloride solution to hydrochloric acid solution is 1 to 3:50, preferably 2:50, and the concentration of stannous chloride solution is preferably 0.1 mol / L.

[0042] In the present invention, the preparation and calibration of the cerium sulfate standard solution refer to GB / T 601-2002.

[0043] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0044] Instruments and reagents

[0045] ZDJ-4B automatic potentiometric titrator, 213-01 platinum electrode, 232-01 reference electrode, T-818-B-6 temperature electrode (Shanghai Leici), electronic balance (Mettler).

[0046] Ferric chloride (Tianjin Aopusheng Chemical Co., Ltd.), ferrous chloride (Xilong Scientific Co., Ltd.), ammonium cerium sulfate (Tianjin Komeiou Chemical Reagent Co., Ltd.), stannous chloride (Shanghai MacLean Biochemical Technology Co., Ltd.), tin particles (Tianjin Komeiou Chemical Reagent Co., Ltd.), disodium hydrogen phosphate, citric acid, trichloroacetic acid, and hydrochloric acid (Sinopharm Chemical Reagent Co., Ltd.). All reagents were of analytical grade.

[0047] The samples of the plating aid solution to be tested were taken from Handan Zhengda Pipe Manufacturing Co., Ltd. and Handan Hongda Pipe Manufacturing Group Co., Ltd., and were numbered 4, 5, 6, 10, and 12.

[0048] Take the above-mentioned No. 4 plating agent solution sample

[0049] Preparation of mixed acid buffer:

[0050] Accurately weigh 0.4g Na2HPO4 into a 100mL beaker, add 50mL deionized water and stir to dissolve, then add 30mL hydrochloric acid, 0.04g citric acid, and 0.01g trichloroacetic acid in sequence and mix well.

[0051] Preparation of iron standard solution:

[0052] Accurately weigh 0.3105 g of ferrous chloride and 0.3800 g of ferric chloride and place them in a 1-liter volumetric flask, add 20 mL of concentrated hydrochloric acid to dissolve, and add deionized water to dilute to the fixed volume.

[0053] Accurately pipette 25mL of the plating agent solution and add 5mL, 10mL, 15mL, and 20mL of the mixed acid buffer respectively, and stir in a water bath at room temperature (30℃), 50℃, 70℃, and 90℃ until clear, and record the corresponding time. The results are shown in Table 1 below:

[0054] Table 1 Different treatment conditions of flux samples

[0055]

[0056]

[0057] The plating agent sample is in a turbid colloidal state with a pH value of 4-5. When determining the iron content in the sample, it is necessary to first 2+ , Fe 3+ The content in the sample is fixed, so that Fe 2+ No longer oxidized, Fe 3+ No longer hydrolyzes. Therefore, it is necessary to add an appropriate amount of mixed acid buffer to make it clear. From the above table, it can be seen that adding different amounts of mixed acid buffer and heating in water baths at different temperatures will take different amounts of time to clarify. Generally speaking, the higher the acidity and the higher the temperature, the shorter the time required for the plating aid solution to be clear. Adding excessive mixed acid buffer will cause the silicon in the plating aid to precipitate. When 5mL of mixed acid buffer is added, the amount added is too small to reach the acidity required for the solution to be clear. Even if the water bath is heated to 90°C, the solution is still turbid. Therefore, we choose to add 15mL of mixed acid buffer to 25mL of plating aid solution and heat it in a 90°C water bath for 1min as the best condition.

[0058] Drawing of standard curve:

[0059] Accurately transfer 25mL, 50mL, 75mL, and 100mL of the iron standard solution to the titration cup, use the saturated calomel electrode as the reference electrode and the platinum electrode as the indicator electrode, perform step-by-step titration with the cerium sulfate standard solution, record the change in the system potential value, draw the titration curve, and calculate the FeCl2, FeCl3, and total iron content based on the titration curve. And draw the standard curve of different volumes of FeCl2, FeCl3, and total iron content.

[0060] from Figure 1 and Figure 2 It can be seen that the curves for continuous determination of ferrous iron and total iron are smooth, with obvious jumps, and the terminal electrode potential is around 800mv. Figure 3 The linear regression equations of FeCl2, FeCl3 and total iron in the solution are y=0.03698x+0.0265, R 2 =0.99977; y=0.056x+0.1595, R 2 =0.99539;

[0061] y=0.09298x+0.186,R 2 =0.99791, both showing a good linear correlation.

[0062] Standard curve for total iron determination:

[0063] Accurately transfer 25mL, 50mL, 75mL, and 100mL of the standard iron solution to the titration cup, add 5mL of hydrochloric acid to each titration cup, heat to 70°C, add 0.1M stannous chloride solution until the solution is colorless, add 2-3 drops of methyl orange solution, cool to room temperature, use a saturated calomel electrode as the reference electrode and a platinum electrode as the indicator electrode, and titrate with a ceric sulfate standard solution. Plot the titration results of different volumes into a standard curve.

[0064] from Figure 4 It can be seen that the linear regression equations for total iron determination are y=0.09325x+0.134, R 2 =0.99883. It can be seen that the continuous determination of total iron shows a good linear correlation.

[0065] Table 2 Comparison of the results of continuous and separate determination of total iron

[0066]

[0067] As can be seen from Table 2, the relative deviation between the continuous determination of total iron and the single determination of total iron is between 0.000% and 0.8729%, which is relatively small. Therefore, there is no difference between the two determination methods.

[0068] Example 1

[0069] Accurately transfer 50 mL of the treated No. 4 plating aid sample to the titration cup, add 30 mL of mixed acid buffer, heat in a 90°C water bath for 1 min until the solution is clear, use a saturated calomel electrode as the reference electrode and a platinum electrode as the indicator electrode, perform distribution titration with a cerium sulfate standard solution, record the change in the system potential value, draw a titration curve, and calculate the FeCl2 content C1.

[0070]

[0071] Where C1 is the FeCl2 content in the plating agent solution, g / L; C2 is the concentration of the cerium sulfate standard solution, mol / L; V1 is the sampling volume of the plating agent solution, mL; V2 is the volume of the consumed cerium sulfate standard solution, mL; M1 is the relative molecular mass of FeCl2, g / mol;

[0072] Then, 100 mL of hydrochloric acid solution was added to the solution to be tested in step (2) and heated to 90° C., 6 mL of 0.1 M stannous chloride solution was added until the solution became colorless, and 2 to 3 drops of methyl orange solution were added to obtain a secondary titration solution; the secondary titration solution was titrated with a saturated calomel electrode as a reference electrode and a platinum electrode as an indicator electrode using a cerium sulfate standard solution, the change in the system potential value was recorded, a titration curve was drawn, and Fe was calculated according to the titration curve. 3+ Content C3,

[0073]

[0074] Wherein: C3 is the Fe(OH)3 content in the plating agent, g / L; C2 is the concentration of the cerium sulfate standard solution, mol / L; V1 is the sampling volume of the plating agent solution, mL; V3 is the total volume of the cerium sulfate standard solution consumed, mL; M2 is the relative molecular mass of Fe(OH)3, g / mol;

[0075] The total iron content is C=C1+C3.

[0076] The titration results are as follows Figure 5 and Figure 6 It can be seen from the figure that the amount of titrant consumed when determining FeCl2 is 0.645mL, and the amount of titrant consumed when determining total iron is 1.364mL. Therefore, the amount of titrant required to determine Fe(OH)3 is 0.719mL.

[0077] Verification of method accuracy:

[0078] Accurately pipette 25mL of No. 4, No. 5, No. 6, No. 10, and No. 12 plating agent solutions, take 25mL of iron standard solution for spike addition, treat the solution according to the above method, and use an automatic potentiometric titrator for determination. Repeat the determination 6 times for each sample. As can be seen from the table, the sample spike recovery rate ranges from 100.1% to 100.8%, and the recovery rate determination results show that the accuracy of this method is very high. The sample spike experiment results are shown in Table 3.

[0079] Table 3 Recovery rate of samples in different batches of plating tanks

[0080]

[0081]

[0082] Example 2

[0083] Precision Analysis of Continuous Determination of FeCl2, FCl3 and Total Iron

[0084] Accurately transfer 50 mL of the standard iron solution to 6 titration cups respectively, use a saturated calomel electrode as the reference electrode and a platinum electrode as the indicator electrode, perform step-by-step titration with the ceric sulfate standard solution, record the change in the system potential value, draw a titration curve, and calculate the FeCl2, FeCl3 and total iron contents based on the titration curve.

[0085] Table 4 Precision analysis of FeCl2 in continuous determination

[0086]

[0087] Table 5 Precision analysis of FeCl3 in continuous determination

[0088]

[0089]

[0090] Table 6 Analysis of total iron precision in continuous determination

[0091]

[0092] The test results show that in 5 measurements, the RSD values ​​(n=5) of FeCl2, FeCl3 and total iron content were 1.59%, 2.62% and 1.37% respectively. The experimental results meet the national standard requirements (RSD<5%) and the detection method has good reproducibility.

[0093] It can be seen from the above embodiments that the present invention provides a method for continuously determining the iron content in a galvanizing auxiliary agent, which updates the existing method for determining the iron content in a hot-dip galvanizing auxiliary agent and has the characteristics of good precision, high accuracy, and convenient and quick operation.

[0094] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for continuously determining the iron content in a zinc plating aid, characterized in that: The following steps are involved: (1) Mixing a plating flux solution and a mixed acid buffer, stirring under heating until the solution is clear, and using the solution to be tested; (2) Using a saturated calomel electrode as the reference electrode and a platinum electrode as the indicator electrode, the test solution was titrated with a cerium sulfate standard solution, the change in the system potential value was recorded, and a titration curve was drawn. Fe 2+ Content C1, Where C1 is the FeCl2 content in the plating agent solution, g / L; C2 is the concentration of the cerium sulfate standard solution, mol / L; V1 is the sampling volume of the plating agent solution, mL; V2 is the volume of the consumed cerium sulfate standard solution, mL; M1 is the relative molecular mass of FeCl2, g / mol; (3) then adding hydrochloric acid solution to the test solution of step (2) and heating, adding stannous chloride solution until the solution is colorless, adding 2 to 3 drops of methyl orange solution to obtain a secondary titration solution; (4) Using a saturated calomel electrode as the reference electrode and a platinum electrode as the indicator electrode, the secondary titration solution was titrated with a cerium sulfate standard solution, the change in the system potential value was recorded, and a titration curve was drawn. The Fe 3+ Content C3, Wherein: C3 is the Fe(OH)3 content in the plating agent, g / L; C2 is the concentration of the cerium sulfate standard solution, mol / L; V1 is the sampling volume of the plating agent solution, mL; V3 is the total volume of the cerium sulfate standard solution consumed, mL; M2 is the relative molecular mass of Fe(OH)3, g / mol; The total iron content is C=C1+C3.

2. The method for continuously determining the iron content in the zinc plating auxiliary agent according to claim 1, characterized in that: The mixed acid buffer comprises disodium hydrogen phosphate, hydrochloric acid, citric acid, trichloroacetic acid and water, and the dosage ratio of the disodium hydrogen phosphate, hydrochloric acid, citric acid, trichloroacetic acid and water is 0.1-0.5 g: 10-50 mL: 0.03-0.05 g: 0.01-0.02 g: 50 mL.

3. The method for continuously determining the iron content in the zinc plating auxiliary agent according to claim 1 or 2, characterized in that: In the step (1), the heating temperature is 50 to 90° C., and the stirring time is 1 to 30 minutes.

4. The method for continuously determining the iron content in the zinc plating auxiliary agent according to claim 3, characterized in that: The volume ratio of the plating assistant solution to the mixed acid buffer is 25:10-15.

5. The method for continuously determining the iron content in the zinc plating auxiliary agent according to claim 1, 2 or 4, characterized in that: In the step (3), the amount of hydrochloric acid solution added is 2 to 2.5 times the volume of the plating agent solution, the volume ratio of the stannous chloride solution to the hydrochloric acid solution is 1 to 3:50, and the concentration of the stannous chloride solution is 0.1 mol / L.

6. The method for continuously determining the iron content in the zinc plating auxiliary agent according to claim 5, characterized in that: The preparation of the cerium sulfate standard solution refers to GB / T601-2002.