Aluminum alloy cable for new energy automobile and production process
By controlling the composition ratio and process processing in aluminum alloy cables and combining with the PA12 insulation layer, the balance of conductivity and mechanical strength of new energy vehicles is solved, and an efficient and low-cost aluminum alloy cable design is achieved to meet the performance of new energy vehicles. Require.
Patent Information
- Application Number
- CN202411299372.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-06
AI Technical Summary
Existing aluminum alloy cables are difficult to balance between improving conductivity and mechanical strength, and cannot meet the requirements of new energy vehicles for conductivity exceeding 59.5% IACS and strength above 110MPa.
By controlling the Si, Mg, Ti, Fe and impurity content in the solid flat conductor of aluminum alloy, ensuring the content and ratio of Si and Mg, combining extrusion and aging treatment processes, the conductivity and mechanical strength are prepared to meet the requirements of new energy vehicles. Aluminum alloy cables and PA12 insulation layer are used to improve overall performance.
While the conductivity of aluminum alloy cable is greater than 59.5% IACS and the tensile strength is higher than 110MPa, the weight and cost of the cable are reduced, and the high temperature and aging resistance are improved.
Smart Images

Figure CN119092182A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of cable technology, and in particular to an aluminum alloy cable for new energy vehicles and a production process. Background Art
[0002] As an important development direction of the global automotive industry, new energy vehicles (NEVs) have an increasingly urgent need for lightweight materials. With the continued growth of the electric and hybrid vehicle markets, the requirements for reducing vehicle weight, improving energy efficiency, and extending driving range have become more prominent. At present, although copper cables are widely used in automotive electrical systems due to their excellent electrical conductivity, copper has a high density, which is not conducive to the overall lightweight design of new energy vehicles. Therefore, finding alternative materials has become one of the key research directions, among which aluminum alloys have attracted much attention due to their lower density and relatively good electrical conductivity.
[0003] Compared with pure aluminum cables, aluminum alloy cables show higher strength in mechanical properties and can better meet the cable strength requirements of new energy vehicles. Adding Mg2Si phase to aluminum alloy can significantly enhance its mechanical properties, but since Mg2Si is a non-conductive second phase particle, its presence will scatter electrons and increase resistance, resulting in a decrease in the conductivity of aluminum alloy. Therefore, how to ensure that aluminum alloy cables have sufficient conductive efficiency while maintaining good tensile strength to meet the requirements of new energy vehicle cables with a conductivity of more than 59.5% IACS and a strength of more than 110MPa has become a technical problem that needs to be solved urgently.
[0004] In order to solve the above problems, the present invention prepares an aluminum alloy cable for new energy vehicles. Summary of the invention
[0005] The purpose of the present invention is to provide a method to solve the technical problems mentioned in the above background technology.
[0006] The technical solution for achieving the purpose of the present invention is: an aluminum alloy cable for new energy vehicles, comprising an aluminum alloy solid flat conductor and an insulating layer coated on the outer peripheral surface of the aluminum alloy solid flat conductor; the components and percentages of the aluminum alloy solid flat conductor are: Si: 0.38-0.5wt%, Mg: 0.38-0.55wt%, Ti content is less than or equal to 0.1wt%, Fe content is less than or equal to 0.1wt%, and the balance is Al and unavoidable impurities, and the individual content of the unavoidable impurities is less than or equal to 0.01wt%.
[0007] The components and percentages of the aluminum alloy solid flat conductor of the present invention are Si: 0.38-0.5wt%, Mg: 0.38-0.55wt%, Ti content is less than or equal to 0.1wt%, Fe content is less than or equal to 0.1wt%, the balance is Al and inevitable impurities, and the individual content of the inevitable impurities is less than or equal to 0.01wt%. By controlling the contents of Si, Mg, Ti, Fe, Al and various impurities, the conductivity and mechanical strength of the aluminum alloy solid flat conductor can simultaneously meet the requirements that the conductivity of the cable for new energy vehicles is greater than 59.5% IACS and the strength is higher than 110MPa.
[0008] Furthermore, the sum of the contents of Si and Mg in the aluminum alloy solid flat conductor is 0.7-1.2 wt %, and the content ratio of Si to Mg is 0.7-0.9.
[0009] The sum of the Si and Mg contents of the aluminum alloy solid flat conductor of the present invention is 0.7-1.2wt%; the Si to Mg content ratio is 0.7-0.9, and the crystal structure, quantity and size of the Mg2Si strengthening phase are controlled by controlling the relationship between the silicon and magnesium contents, so that the conductivity and mechanical strength of the aluminum alloy solid flat conductor simultaneously meet the requirements of the conductivity of the cable for new energy vehicles being greater than 59.5% IACS and the strength being higher than 110MPa.
[0010] Furthermore, the material of the insulating layer is PA12.
[0011] The material of the insulating layer of the present invention is PA12, which has high strength and can reach 20MPa. PA12 has good temperature resistance and can withstand high temperatures of 125°C. PA12 has good aging resistance and its performance does not change much under thermal aging conditions for 3000h. The obtained aluminum alloy cable for new energy vehicles has good strength, high temperature resistance and aging resistance.
[0012] The present invention also provides a production process of aluminum alloy cables for new energy vehicles, comprising the following process steps:
[0013] S1. According to the aforementioned aluminum alloy solid flat conductor components and the percentage of each component ingredients, followed by smelting, boronization, continuous casting and rolling, annealing, to obtain an aluminum alloy rod;
[0014] S2. The aluminum alloy rod is put into an extruder and extruded, followed by aging treatment to obtain an aluminum alloy solid flat conductor;
[0015] S3. Extruding the insulating layer material onto the outer peripheral surface of the aluminum alloy solid flat conductor to obtain an aluminum alloy cable for new energy vehicles.
[0016] Furthermore, the outer diameter of the aluminum alloy rod is 14-16 mm.
[0017] Furthermore, the cross-sectional shape of the aluminum alloy solid flat conductor is rectangular or waist-shaped.
[0018] Furthermore, the aluminum alloy solid flat conductor has a width of 5 to 100 mm and a thickness of 0.5 to 10 mm.
[0019] The aluminum alloy solid flat conductor of the present invention has a rectangular or waist-shaped cross-sectional shape with a width of 5 to 100 mm and a thickness of 0.5 to 10 mm. Under the same current-carrying capacity, the laying of the aluminum alloy cable for new energy vehicles of the present application occupies less space, has lower weight and lower cost.
[0020] Furthermore, when the cross-sectional shape of the aluminum alloy solid flat conductor is a rectangle, the four corners of the aluminum alloy solid flat conductor are arc chamfered transitions.
[0021] Furthermore, the extrusion temperature of the extruder is 450-550°C.
[0022] Furthermore, the treatment temperature of the aging treatment is 220-280° C., and the treatment time is 6-12 hours.
[0023] The extrusion temperature of the extruder for preparing the aluminum alloy solid flat conductor of the present invention is controlled at 450-550°C, and the treatment temperature of the aging treatment is controlled at 220-280°C, which is combined with the control of the content of Si, Mg, Ti, Fe, Al and various impurities in the aforementioned aluminum alloy solid flat conductor to control the crystal structure, quantity and size of the Mg2Si strengthening phase to balance the conductivity and mechanical strength of the aluminum alloy solid flat conductor, so that the conductivity and mechanical strength of the aluminum alloy solid flat conductor simultaneously meet the requirements of the conductivity of the cable for new energy vehicles being greater than 59.5% IACS and the strength being higher than 110MPa.
[0024] By adopting the above technical solution, the present invention has the following beneficial effects:
[0025] (1) The components and percentages of the aluminum alloy solid flat conductor of the present invention are Si: 0.38-0.5wt%, Mg: 0.38-0.55wt%, Ti content is less than or equal to 0.1wt%, Fe content is less than or equal to 0.1wt%, and the balance is Al and inevitable impurities, and the individual content of the inevitable impurities is less than or equal to 0.01wt%. By controlling the contents of Si, Mg, Ti, Fe, Al and various impurities, the conductivity and mechanical strength of the aluminum alloy solid flat conductor can simultaneously meet the requirements of the conductivity of the cable for new energy vehicles being greater than 59.5% IACS and the tensile strength being higher than 110MPa.
[0026] (2) The sum of the Si and Mg contents of the aluminum alloy solid flat conductor of the present invention is 0.7 to 1.2 wt%, and the Si to Mg content ratio is 0.7 to 0.9. By simultaneously controlling the aforementioned proportional relationship between the silicon and magnesium contents to control the crystal structure, quantity and size of the Mg2Si strengthening phase, the electrical conductivity and mechanical strength of the aluminum alloy solid flat conductor can simultaneously meet the requirements of achieving a conductivity greater than 59.5% IACS and a tensile strength higher than 110 MPa for cables for new energy vehicles.
[0027] (3) The material of the insulating layer of the present invention is PA12, which has high strength and a tensile strength of up to 20 MPa. PA12 has good temperature resistance and can withstand a high temperature of 125°C. PA12 has good aging resistance and its performance does not change much after 3000 hours under thermal aging conditions. The obtained aluminum alloy cable for new energy vehicles has good strength, high temperature resistance and aging resistance.
[0028] (4) The aluminum alloy solid flat conductor of the present invention has a rectangular or waist-shaped cross-sectional shape with a width of 5 to 100 mm and a thickness of 0.5 to 10 mm. Under the same current carrying capacity, the laying of the aluminum alloy cable for new energy vehicles of the present application occupies less space, has lower weight and lower cost.
[0029] (5) The extrusion temperature of the extruder for preparing the aluminum alloy solid flat conductor of the present invention is controlled at 450-550°C, and the treatment temperature of the aging treatment is controlled at 220-280°C. Combined with the control of the contents of Si, Mg, Ti, Fe, Al and various impurities in the aforementioned aluminum alloy solid flat conductor, and the proportional relationship between the silicon and magnesium contents, the crystal structure, quantity and size of the Mg2Si strengthening phase are controlled to balance the conductivity and mechanical strength of the aluminum alloy solid flat conductor, so that the conductivity and mechanical strength of the aluminum alloy solid flat conductor simultaneously meet the requirements of the electrical conductivity of the cable for new energy vehicles being greater than 59.5% IACS and the tensile strength being higher than 110 MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments and in conjunction with the accompanying drawings, wherein
[0031] Figure 1 It is a schematic structural diagram of the aluminum alloy cable for new energy vehicles of the present invention.
[0032] The reference numerals in the accompanying drawings are: aluminum alloy solid flat conductor 1, insulating layer 2. DETAILED DESCRIPTION
[0033] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0034] The following embodiments are only used to more clearly illustrate the technical solutions of the present invention, and are not intended to limit the protection scope of the present invention.
[0035] (Overall Embodiment)
[0036] See Figure 1 , an aluminum alloy cable for new energy vehicles, comprising an aluminum alloy solid flat conductor 1, and an insulating layer 2 coated on the outer peripheral surface of the aluminum alloy solid flat conductor; the components and percentages of the components of the aluminum alloy solid flat conductor are:
[0037] Si: 0.38-0.5wt%, Mg: 0.38-0.55wt%, Ti content is less than or equal to 0.1wt%, Fe content is less than or equal to 0.1wt%, and the balance is Al and inevitable impurities, and the content of each inevitable impurity is less than or equal to 0.01wt%.
[0038] The sum of the contents of Si and Mg in the aluminum alloy solid flat conductor is 0.7 to 1.2 wt %, and the content ratio of Si to Mg is 0.7 to 0.9.
[0039] The material of the insulating layer is PA12.
[0040] The present invention also provides a production process of aluminum alloy cables for new energy vehicles, comprising the following process steps:
[0041] S1. According to the aforementioned aluminum alloy solid flat conductor components and the percentage of each component ingredients, followed by smelting, boronization, continuous casting and rolling, annealing, to obtain an aluminum alloy rod;
[0042] S2. The aluminum alloy rod is put into an extruder and extruded, followed by aging treatment to obtain an aluminum alloy solid flat conductor;
[0043] S3. Extruding the insulating layer material onto the outer peripheral surface of the aluminum alloy solid flat conductor to obtain an aluminum alloy cable for new energy vehicles.
[0044] The outer diameter of the aluminum alloy rod is 14-16 mm.
[0045] The aluminum alloy solid flat conductor has a rectangular or waist-shaped cross section.
[0046] The aluminum alloy solid flat conductor has a width of 5 to 100 mm and a thickness of 0.5 to 10 mm.
[0047] When the cross-sectional shape of the aluminum alloy solid flat conductor is a rectangle, the four corners of the aluminum alloy solid flat conductor are arc chamfered transitions.
[0048] The smelting temperature is 800-900°C.
[0049] The extrusion temperature of the extruder is 450-550°C.
[0050] The treatment temperature of the aging treatment is 220-280° C., and the treatment time is 6-12 hours.
[0051] (Effect Example)
[0052] The following Table 1 is a table of the performance effects of the sum of Si and Mg contents and the content ratio of Si to Mg of the aluminum alloy solid flat conductors prepared in Examples 1 to 15 and Comparative Examples 1 to 4, wherein the process steps and the contents of other components of Examples 1 to 15 and Comparative Examples 1 to 4 are the same as those of the general example.
[0053] Table 1
[0054]
[0055] It can be seen from the above table that, compared with Examples 1 to 15 and Comparative Examples 1 to 6, the sum of the contents of Si and Mg is controlled at 0.7 to 1.2 wt%; the content ratio of Si to Mg is controlled at 0.7 to 0.9, and the conductivity and mechanical strength of the obtained aluminum alloy solid flat conductor simultaneously meet the requirements of the conductivity of the cable for new energy vehicles being greater than 59.5% IACS and the strength being higher than 110 MPa.
[0056] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An aluminum alloy cable for new energy vehicles, comprising an aluminum alloy solid flat conductor (1), and an insulating layer (2) coated on the outer peripheral surface of the aluminum alloy solid flat conductor (1); It is characterized in that The components and percentages of the aluminum alloy solid flat conductor (1) are as follows: Si: 0.38-0.5wt%, Mg: 0.38-0.55wt%, Ti content is less than or equal to 0.1wt%, Fe content is less than or equal to 0.1wt%, and the remainder is Al and inevitable impurities, wherein the content of each inevitable impurity is less than or equal to 0.01wt%.
2. The aluminum alloy cable for new energy vehicles according to claim 1, It is characterized in that The sum of the contents of Si and Mg in the aluminum alloy solid flat conductor is 0.7 to 1.2 wt %, and the content ratio of Si to Mg is 0.7 to 0.
9.
3. The aluminum alloy cable for new energy vehicles according to claim 1, It is characterized in that The material of the insulating layer (2) is PA12.
4. A production process of aluminum alloy cables for new energy vehicles, It is characterized in that The process steps include: S1. The aluminum alloy solid flat conductor (1) according to any one of claims 1 to 2 is prepared according to the components and percentages of the components, and then smelted, borided, continuously cast and rolled, and annealed to obtain an aluminum alloy rod; S2. The aluminum alloy rod is put into an extruder and extruded, followed by aging treatment to obtain an aluminum alloy solid flat conductor; S3. Extruding the insulating layer (2) material onto the outer peripheral surface of the aluminum alloy solid flat conductor to obtain an aluminum alloy cable for new energy vehicles.
5. The production process of aluminum alloy cable for new energy vehicles according to claim 4, It is characterized in that The outer diameter of the aluminum alloy rod is 14-16 mm.
6. The production process of aluminum alloy cable for new energy vehicles according to claim 4, It is characterized in that The aluminum alloy solid flat conductor has a rectangular or waist-shaped cross section.
7. The production process of aluminum alloy cable for new energy vehicles according to claim 4, It is characterized in that The aluminum alloy solid flat conductor has a width of 5 to 100 mm and a thickness of 0.5 to 10 mm.
8. The production process of aluminum alloy cable for new energy vehicles according to claim 6, It is characterized in that When the cross-sectional shape of the aluminum alloy solid flat conductor is a rectangle, the four corners of the aluminum alloy solid flat conductor are arc chamfered transitions.
9. The production process of aluminum alloy cable for new energy vehicles according to claim 4, It is characterized in that The extrusion temperature of the extruder is 450-550°C.