Production process of directly-welded enameled wire
By pre-blocking the polyurethane resin liquid generated by the reaction of isocyanate and alcohols and transesterification reaction, and coating with felt method, the problem of insufficient self-adhesion effect of straight-welded enameled wire is solved, and the production of self-adhesive and easy-to-weld enameled wire is achieved, improving the improvement of self-adhesive and easy-to-weld enameled wire The use area and economic benefits of the product.
Patent Information
- Application Number
- CN202411205692.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The existing direct-welded enameled wire has insufficient self-adhesive effect, which limits its use area and economic benefits.
The polyurethane resin liquid is formed by pre-blocking isocyanate and alcohols, and the polyester resin liquid is formed by transesterification reaction between dimethyl terephthalate and zinc acetate, and the reaction is carried out by mixing and mixing solvents to control the temperature and time. A paint liquid with self-adhesion and easy soldering is formed, and is coated on the round copper wire by felt method.
It has achieved the self-adhesive effect of straight-welded enameled wire, and can be bonded by itself. There is no need to remove the patent leather during welding, which reduces the process and cost and improves the product quality.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of enameled wires, in particular to a production process of directly weldable enameled wires. Background Art
[0002] Direct-weldable enameled wire is a special enameled wire with direct-weldability; therefore, welding operation can be performed directly. The direct-weldable enameled wire has excellent electrical and mechanical properties and can be generally used as winding wire for electrical equipment such as motors, electrical appliances, instruments, and transformers.
[0003] Specifically, a single coating polyester, such as polyurethane; the enameled wire made of it has self-adhesiveness and easy solderability; at the same time, it also has the electrical properties, mechanical properties and chemical resistance of general electromagnetic wires, and can be coated at one time using existing enameling equipment. The coil wound by the enameled wire coated with this paint can be formed by baking for a short time without additional dipping. When welding the joint, it is not necessary to remove the paint and directly tin it. In this way, the working environment can be improved, costs can be reduced, processes can be shortened, and working hours can be reduced. The enameled wire coated with this paint can be widely used in micro motors, electrical appliances, instruments and communication equipment, etc.
[0004] Based on this, Chinese patent CN109096875A discloses a wire enamel production technology, specifically a modified polyurethane wire enamel suitable for low-temperature direct welding suitable for high-speed enamelling machines and a method for making the same. It includes 320-330g of glycerol, 170-180g of ethylene glycol, 280-300g of trimellitic anhydride, 170-180g of diphenylmethane, 420-440g of xylene, and 310-330g of m-p-cresol. After adopting the above formula and method, due to the reasonable selection of various component formulas and the limitation of the proportions of various component formulas, in addition, especially in the production process, by step-by-step addition and optimization and matching of the process, especially the temperature rise and fall control process, the prepared wire enamel can not only reduce the soldering temperature, after experimental verification, the soldering temperature is 310°C, and the product quality is effectively improved, and the effect is very outstanding.
[0005] However, the enameled wire produced by the above-disclosed wire enamel production technology still lacks the technical problem of self-adhesive effect. Specifically, at present, the commonly used materials for self-adhesive wire enamels disclosed in the prior art include polyvinyl butyral, polyvinyl acetate, epoxy resin and polyester resin. The materials used for easy-to-weld enameled wire enamels include polyurethane, polyacrylonitrile and polyamide. Since polyurethane enameled wire has good self-welding properties; if it can also have self-adhesive properties, a single-coating self-adhesive and easy-to-weld enameled wire can be obtained. This kind of straight-weld enameled wire with self-adhesive ability can have a wider range of uses, thereby improving its economic benefits. Summary of the invention
[0006] Based on this, it is necessary to provide a production process for direct-weld enameled wire to address the technical problem of insufficient self-adhesive effect of existing direct-weld enameled wire.
[0007] A production process for direct-weld enameled wire, comprising the following steps: S1: preparing diisocyanate, phenol, polyol, cyclohexanone, glycerol, cresol and xylene according to a preset ratio; and synthesizing a polyurethane resin liquid using the above raw materials; S2: preparing polyol, dimethyl terephthalate, glycerol, cresol, zinc acetate and methanol according to a preset ratio, and synthesizing a polyester resin liquid using the above raw materials; S3: preparing a mixed solvent with m-p-cresol, xylene and cyclohexanone according to a preset ratio; S4: Mixing the polyurethane resin liquid, the polyester resin liquid and the mixed modulation solvent; controlling the reaction temperature to 70 to 80° C., and continuing the reaction for 3 to 5 hours to obtain a finished paint liquid; S5: Use an enameling machine to coat the round copper wire with a finished lacquer liquid according to the felt method to obtain a straight-weld enameled wire product.
[0008] Specifically, in step S1, the step of synthesizing the polyurethane resin liquid includes: S11: putting all the pre-prepared 2,4-toluene diisocyanate and phenol into a reaction kettle, heating and raising the temperature, and controlling the temperature not to exceed 100° C.; S12: After the phenol is completely dissolved, stirring is started in the reactor, and the temperature is continued to rise to 130±3°C, and the temperature is maintained for 4 hours; S13: cooling the temperature in the reactor to less than 100° C., then adding a quarter of the pre-prepared cyclohexanone into the reactor; at the same time, mixing the pre-prepared glycerin, ethylene glycol and a quarter of the pre-prepared cyclohexanone to form a mixed liquid, and adding the mixed liquid into the reactor, controlling the reaction temperature not to exceed 110° C., and continuing for 30 minutes; S14: flush the header tank with one quarter of the cyclohexanone prepared in advance and put it into the reactor; S15: stopping heating the reactor, and sequentially adding m-p-cresol, xylene, and the remaining one-quarter of the pre-prepared cyclohexanone; starting stirring in the reactor, and controlling the stirring time to be no less than 30 minutes; S16: After the temperature of the reactor is lower than 60° C., the material is discharged and filtered to obtain a polyurethane resin liquid.
[0009] Furthermore, in step S11, the ratio of the input amount of 2,4-toluene diisocyanate to that of m-p-phenol is 5:1 in parts by mass.
[0010] Furthermore, in step S12, the ratio of the input amounts of glycerol to phenol is 1:1; the ratio of the input amounts of glycerol to ethylene glycol is 2:1.
[0011] Furthermore, in step S15, the input ratio of m-p-cresol to xylene is 2:1 in parts by mass.
[0012] Specifically, in step S2, the process for synthesizing the polyester resin liquid is as follows: S21: Take another reactor and add dimethyl terephthalate, glycerol and polyol into the reactor according to a preset ratio; S22: raising the temperature in the reactor to 140 to 150° C. to control the complete melting of dimethyl terephthalate; S23: After dimethyl terephthalate is completely melted, the prepared zinc acetate is added into the reaction kettle; and the temperature in the reaction kettle is slowly increased to not more than 180° C.; S24: using methanol to distill the reactants in the reactor, and gradually increasing the temperature in the reactor according to the distillation rate until the temperature in the reactor reaches 245±2° C.; S25: The temperature of the first reduced pressure polymerization is controlled at 245±2°C and the duration does not exceed 90 minutes. If distillate continues to appear in the reactor, the duration is extended by 60 minutes; S26: Control the temperature in the reactor at 245±2°C for 90 minutes. After the end of the insulation, raise the temperature to 250±1°C; at the same time, preheat the prepared cresol to 250°C, add the preheated cresol into the reactor, and stir for 5-0 minutes; S27: Continue to evacuate the reactor, maintain the temperature at 245±2°C, and make the vacuum degree in the reactor reach 600 mmHg within 5 minutes, until the sample is hard and brittle, and the process time is controlled within 30 minutes; S28: stopping the vacuuming, adding cresol preheated to 200° C. again, and maintaining the temperature in the reactor at 200° C. for 60 minutes; S29: After stopping heating the reactor, add cresol, cool down to no more than 150° C., and obtain a polyester resin liquid product after filtering.
[0013] Furthermore, the ratio of each raw material is: 20-30 parts of polyol, 40-50 parts of dimethyl terephthalate, 15-20 parts of glycerol, 20-40 parts of cresol, 1 part of zinc acetate and 10-12 parts of methanol, calculated by mass.
[0014] Furthermore, the polyol includes ethylene glycol and diethylene glycol, and the feed ratio of the two is 1:1 in parts by mass.
[0015] In summary, the present invention provides a production process for direct solderable enameled wires. The isocyanate is sealed with phenol in advance, and then reacted with alcohols to polymerize into a polyurethane resin liquid with linear and stereoscopic structures; dimethyl terephthalate and excess ethylene glycol are then used to carry out an ester exchange reaction under the action of a catalyst, zinc acetate; when all the methanol is evaporated, the ester exchange is completed and the polycondensation reaction begins, and the temperature of the prepolymer is quickly increased to evaporate the excess ethylene glycol. When the temperature rises to a preset value, the prepolymer is polycondensed under reduced pressure, and the residual ethylene glycol is extracted to obtain a polyester resin liquid; then, the two resin liquids are mixed with a mixed modulation solvent and reacted to obtain a paint liquid, and then the paint liquid is applied to the surface of the round copper wire by a felt method to prepare the product. The wire coated by the above method can be self-bonded by baking after being wound into a coil, and its self-bonding temperature is 175°C and the bonding time interval is 60 minutes. Moreover, the joint welding part of the enameled wire prepared by this process can be directly tinned without removing the paint skin, and the tinning temperature is 375±5° C. Therefore, the direct soldering enameled wire production process of the present invention solves the technical problem of insufficient self-adhesive effect of the existing direct soldering enameled wire. DETAILED DESCRIPTION
[0016] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific implementation mode of the present invention is described in detail below in conjunction with embodiments. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0017] Specifically, since the structure of polyurethane resin contains strong polar groups, the polyurethane resin can be used as an adhesive material. The polar groups it possesses not only have a greater adhesion to metals, but also further enhance their ability to bond to each other due to the intermolecular effect. In addition, in the polyurethane enameled wire system, the chemical reaction between its active groups can also be used to combine with each other. From the preparation of polyurethane enameled wire paint, the coating of enameled wire to the molding of coil windings, the entire process can be divided into three stages: the first is the initial state after the polyester and polyurethane are prepared, and the product of this stage has a certain amount of active groups. The second is the self-adhesive and easy-to-weld coating formed under an appropriate wire coating process, at which time the aforementioned active groups have been partially cross-linked. The third is the state in which the remaining part reacts to bond the enameled wire under sufficient energy. Therefore, in order to ensure the basic electrical and mechanical properties of the materials, polyester and polyurethane can be made into a certain body structure so that they will not deform during the bonding molding process.
[0018] Specifically, the present invention provides a production process for a direct-weld enameled wire, which comprises the following steps, measured by weight: S1: preparing diisocyanate, phenol, polyol, cyclohexanone, glycerol, cresol and xylene according to a preset ratio; and synthesizing a polyurethane resin liquid using the above raw materials; S2: preparing polyol, dimethyl terephthalate, glycerol, cresol, zinc acetate and methanol according to a preset ratio, and synthesizing a polyester resin liquid using the above raw materials; S3: preparing a mixed solvent with m-p-cresol, xylene and cyclohexanone according to a preset ratio; S4: Mixing the polyurethane resin liquid, the polyester resin liquid and the mixed modulation solvent; controlling the reaction temperature to 70 to 80° C., and continuing the reaction for 3 to 5 hours to obtain a finished paint liquid; S5: Use an enameling machine to coat the round copper wire with a finished lacquer liquid according to the felt method to obtain a straight-weld enameled wire product.
[0019] Specifically, polyurethane resin liquid is mainly prepared by reacting polyisocyanate with polyols. In order to ensure quantitative cross-linking of polyurethane and polyester into film, in the actual production process, isocyanate can be pre-blocked with phenol, and then reacted with alcohols to polymerize into linear and certain volumetric polyurethane resins. Moreover, the unblocked part of the blocked isocyanate still retains its activity. This unblocked isocyanate group reacts with the hydroxyl group in glycerol and ethylene glycol, and finally, a carbamate group is generated. The polyurethane resin generated according to the preset ratio also has blocked isocyanate groups and hydroxyl groups; moreover, the gram molecular weight of glycerol is relatively small, and ethylene glycol with ether bonds is introduced, so the cross-linking degree is low and the flexibility is good.
[0020] Specifically, in a direct solderable enameled wire production process of the present invention, a specific embodiment of a synthetic polyurethane resin liquid is as follows: S11: putting all the pre-prepared diisocyanate, for example, 2,4-toluene diisocyanate and phenol into a reaction kettle, heating and raising the temperature, and controlling the temperature not to exceed 100° C.; S12: After the phenol is completely dissolved, stirring is started in the reactor, and the temperature is continued to rise to 130±3°C, and the temperature is maintained for 4 hours; S13: cooling the temperature in the reactor to less than 100° C., then adding a quarter of the pre-prepared cyclohexanone into the reactor; at the same time, mixing the pre-prepared glycerin, polyols such as ethylene glycol and a quarter of the pre-prepared cyclohexanone to form a mixed solution; and adding the mixed solution into the reactor, controlling the reaction temperature not to exceed 110° C., and continuing for 30 minutes; S14: flush the header tank with one quarter of the cyclohexanone prepared in advance and put it into the reactor; S15: stopping heating the reactor, and sequentially adding m-p-cresol, xylene, and the remaining one-quarter of the pre-prepared cyclohexanone; starting stirring in the reactor, and controlling the stirring time to be no less than 30 minutes; S16: After the temperature of the reactor is lower than 60° C., the material is discharged and filtered to obtain a polyurethane resin liquid.
[0021] Furthermore, in step S11, the ratio of the amount of 2,4-toluene diisocyanate to that of m-phenol is 5:1 by mass. For example, the amount of phenol corresponding to 35 to 55 parts of 2,4-toluene diisocyanate is 7 to 11 parts.
[0022] Furthermore, in step S12, the input ratio of glycerol to phenol is 1:1, and the input ratio of glycerol to ethylene glycol is 2:1. For example, when the input amount of glycerol is 7 to 11 parts, the input amount of ethylene glycol is 3.5 to 5.5 parts.
[0023] Furthermore, in step S15, the input ratio of m-para-cresol to xylene is 2:1. When the input amount of m-para-cresol is 7 to 11 parts, the input amount of xylene is 3.5 to 5.5 parts.
[0024] Furthermore, in the aforementioned steps, the ratio of the input glycerol to the input cyclohexanone is 1:2; that is, when the input amount of glycerol is 7 to 11 parts, the input amount of cyclohexanone is 14 to 22 parts.
[0025] Furthermore, in a direct solderable enameled wire production process of the present invention, a specific embodiment of a synthetic polyester resin liquid is as follows: S21: Take another reactor and add dimethyl terephthalate, glycerol and polyol into the reactor according to a preset ratio; S22: raising the temperature in the reactor to 140 to 150° C. to control the complete melting of dimethyl terephthalate; S23: After the dimethyl terephthalate is completely melted, the prepared zinc acetate is added into the reaction kettle; and the temperature in the reaction kettle is slowly raised to not more than 180° C. to avoid the sublimation of the dimethyl terephthalate; S24: using methanol to distill the reactants in the reactor, and gradually increasing the temperature in the reactor according to the distillation rate until the temperature in the reactor reaches 245±2° C.; S25: The temperature of the first reduced pressure polymerization is controlled at 245±2°C and the duration does not exceed 90 minutes. If distillate continues to appear in the reactor, the duration is extended by 60 minutes; S26: Control the temperature in the reactor at 245±2°C for 90 minutes. After the end of the insulation, raise the temperature to 250±1°C; at the same time, preheat the prepared cresol to 250°C, add the preheated cresol into the reactor, and stir for 5-0 minutes; S27: Continue to evacuate the reactor, maintain the temperature at 245±2°C, and make the vacuum degree in the reactor reach 600 mmHg within 5 minutes, until the sample is hard and brittle, and the process time is controlled within 30 minutes; S28: stopping the vacuuming, adding cresol preheated to 200° C. again, and maintaining the temperature in the reactor at 200° C. for 60 minutes; S29: After stopping heating the reactor, add cresol, cool down to no more than 150° C., and obtain a polyester resin liquid product after filtering.
[0026] Specifically, in a specific embodiment, the ratio of the raw materials of the polyester resin liquid synthesis process: polyol, dimethyl terephthalate, glycerol, cresol, zinc acetate and methanol is: 20-30 parts of polyol, 40-50 parts of dimethyl terephthalate, 15-20 parts of glycerol, 20-40 parts of cresol, 1 part of zinc acetate and 10-12 parts of methanol.
[0027] The aforementioned polyols include ethylene glycol and diethylene glycol, and the feed ratio of the two is 1:1.
[0028] Specifically, the polycondensation product of polyacid and polyol is polyester resin. Due to the different number of functional groups of acid and alcohol, a polyester resin with linear or further stereoscopic structure can be obtained. Determined by the nature of the viscosity required to be added to the direct soldering enameled wire, a linear thermosetting polyester resin is required. Therefore, a saturated dibasic acid and diol polycondensation can be used. In order to meet the basic and special properties of the self-adhesive easy-to-weld coating, it is required that there are appropriate cross-linking groups in the molecule, and it is best to have flexible links in the molecular chain, so diethylene glycol and glycerol are introduced. Among the properties of direct soldering enameled wire, the bonding strength after molding is particularly important. Its size depends on the reaction degree of the polyester resin, that is, the size of the degree of polymerization. When other conditions are the same, the greater the degree of polymerization, the lower the bonding strength. The degree of polymerization is measured by the number of hydroxyl groups contained in the resin. Practice has shown that the -OH value is preferably 3.5-5.5%. The -OH value should not be too high, because too high a value will cause the tinning time to be extended or the temperature to be increased, which is not conducive to solderability.
[0029] Specifically, the steps of coating enameled wire using the felt method include: S51: Use a felt clamp to clamp the felt flatly on both sides of the round copper wire, ensuring that the felt is in close contact with the wire to form a uniform die hole; S52: Taking advantage of the loose, soft, elastic and porous characteristics of felt, mold holes are formed; these mold holes help control the flow and distribution of the paint liquid; S52: Scrape off the excess paint on the wire to ensure that only the right amount of paint is applied to the wire surface to avoid waste and excessive paint layer; S53: The paint liquid is absorbed, stored, transported and replenished through capillary action, and the surface of the conductor is evenly coated with the paint liquid. The capillary action of the felt helps to evenly coat the paint liquid on the surface of the conductor.
[0030] Specifically, when using the felt painting method, you need to pay attention to the distance between the felt and the oven inlet. Considering the combined force of leveling and gravity after painting, as well as the sag and paint gravity of the line, the distance between the felt and the paint tank should be 50 to 80 mm, and the distance between the felt and the oven mouth should be 200 to 250 mm.
[0031] In addition, it is also necessary to select the appropriate felt according to the specifications and requirements of the enameled wire. For example, when coating coarse specifications, the felt is required to be wide, thick, soft, elastic, and have many pores; while when coating fine wires, it is required to be narrow, thin, dense, and have small pores. Cotton wool or sweater cloth can be used to wrap the felt to form a dense and soft surface, so that the amount of paint applied is small and even.
[0032] In summary, the present invention provides a production process for direct solderable enameled wires. The isocyanate is sealed with phenol in advance, and then reacted with alcohols to polymerize into a polyurethane resin liquid with linear and stereoscopic structures; dimethyl terephthalate and excess ethylene glycol are then used to carry out an ester exchange reaction under the action of a catalyst, zinc acetate; when all the methanol is evaporated, the ester exchange is completed and the polycondensation reaction begins, and the temperature of the prepolymer is quickly increased to evaporate the excess ethylene glycol. When the temperature rises to a preset value, the prepolymer is polycondensed under reduced pressure, and the residual ethylene glycol is extracted to obtain a polyester resin liquid; then, the two resin liquids are mixed with a mixed modulation solvent and reacted to obtain a paint liquid, and then the paint liquid is applied to the surface of the round copper wire by a felt method to prepare the product. The wire coated by the above method can be self-bonded by baking after being wound into a coil, and its self-bonding temperature is 175°C and the bonding time interval is 60 minutes. Moreover, the joint welding part of the enameled wire prepared by this process can be directly tinned without removing the paint skin, and the tinning temperature is 375±5° C. Therefore, the direct soldering enameled wire production process of the present invention solves the technical problem of insufficient self-adhesive effect of the existing direct soldering enameled wire.
[0033] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0034] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A process for producing direct-weld enameled wire, characterized in that: It includes the following steps: S1: preparing diisocyanate, phenol, polyol, cyclohexanone, glycerol, cresol and xylene according to a preset ratio; and synthesizing a polyurethane resin liquid using the above raw materials; S2: preparing polyol, dimethyl terephthalate, glycerol, cresol, zinc acetate and methanol according to a preset ratio, and synthesizing a polyester resin liquid using the above raw materials; S3: preparing a mixed solvent with m-p-cresol, xylene and cyclohexanone according to a preset ratio; S4: Mixing the polyurethane resin liquid, the polyester resin liquid and the mixed modulation solvent; controlling the reaction temperature to 70 to 80° C., and continuing the reaction for 3 to 5 hours to obtain a finished paint liquid; S5: Use an enameling machine to coat the round copper wire with a finished lacquer liquid according to the felt method to obtain a straight-weld enameled wire product.
2. A process for producing a direct solderable enameled wire according to claim 1, characterized in that: In step S1, the step of synthesizing the polyurethane resin liquid includes: S11: putting all the pre-prepared 2,4-toluene diisocyanate and phenol into a reaction kettle, heating and raising the temperature, and controlling the temperature not to exceed 100° C.; S12: After the phenol is completely dissolved, stirring is started in the reactor, and the temperature is continued to rise to 130±3°C, and the temperature is maintained for 4 hours; S13: cooling the temperature in the reactor to less than 100° C., then adding a quarter of the pre-prepared cyclohexanone into the reactor; at the same time, mixing the pre-prepared glycerin, ethylene glycol and a quarter of the pre-prepared cyclohexanone to form a mixed liquid, and adding the mixed liquid into the reactor, controlling the reaction temperature not to exceed 110° C., and continuing for 30 minutes; S14: flush the header tank with one quarter of the cyclohexanone prepared in advance and put it into the reactor; S15: stopping heating the reactor, and sequentially adding m-p-cresol, xylene, and the remaining one-quarter of the pre-prepared cyclohexanone; starting stirring in the reactor, and controlling the stirring time to be no less than 30 minutes; S16: After the temperature of the reactor is lower than 60° C., the material is discharged and filtered to obtain a polyurethane resin liquid.
3. A process for producing a direct-weldable enameled wire according to claim 2, characterized in that: In step S11, the ratio of the input amount of 2,4-toluene diisocyanate to that of m-p-phenol is 5:1 by mass.
4. A process for producing a direct solderable enameled wire according to claim 3, characterized in that: In step S12, the ratio of the input amounts of glycerol to phenol is 1:1; the ratio of the input amounts of glycerol to ethylene glycol is 2:
1.
5. A process for producing a direct solderable enameled wire according to claim 4, characterized in that: In step S15, the input ratio of m-p-cresol to xylene is 2:1 in parts by mass.
6. A process for producing a direct solderable enameled wire according to claim 2, characterized in that: In step S2, the process of synthesizing polyester resin liquid is as follows: S21: Take another reactor and add dimethyl terephthalate, glycerol and polyol into the reactor according to a preset ratio; S22: raising the temperature in the reactor to 140 to 150° C. to control the complete melting of dimethyl terephthalate; S23: After dimethyl terephthalate is completely melted, the prepared zinc acetate is added into the reaction kettle; and the temperature in the reaction kettle is slowly raised to not more than 180° C.; S24: using methanol to distill the reactants in the reactor, and gradually increasing the temperature in the reactor according to the distillation rate until the temperature in the reactor reaches 245±2° C.; S25: The temperature of the first reduced pressure polymerization is controlled at 245±2°C and the duration does not exceed 90 minutes. If distillate continues to appear in the reactor, the duration is extended by 60 minutes; S26: Control the temperature in the reactor at 245±2°C for 90 minutes. After the end of the insulation, raise the temperature to 250±1°C; at the same time, preheat the prepared cresol to 250°C, add the preheated cresol into the reactor, and stir for 5-0 minutes; S27: Continue to evacuate the reactor, maintain the temperature at 245±2°C, and make the vacuum degree in the reactor reach 600 mmHg within 5 minutes, until the sample is hard and brittle, and the process time is controlled within 30 minutes; S28: stopping the vacuuming, adding cresol preheated to 200° C. again, and maintaining the temperature in the reactor at 200° C. for 60 minutes; S29: After stopping heating the reactor, add cresol, cool down to no more than 150° C., and obtain a polyester resin liquid product after filtering.
7. A process for producing a direct solderable enameled wire according to claim 6, characterized in that: The proportions of the raw materials are as follows, by mass: 20-30 parts of polyol, 40-50 parts of dimethyl terephthalate, 15-20 parts of glycerol, 20-40 parts of cresol, 1 part of zinc acetate and 10-12 parts of methanol.
8. A process for producing a direct solderable enameled wire according to claim 7, characterized in that: The polyol includes ethylene glycol and diethylene glycol, and the feed ratio of the two is 1:1 by weight.