Chip power inductor preparation method based on 3D printing
Through the 3D printing-based patch power inductor preparation method, magnetic slurry and micro-zone 3D printing technology, the problems of deformation, pressure and annealing temperature limitation in the process of small-volume inductor components are solved, and smaller volume, high precision and Low-loss inductor preparation improves magnetic permeability and production efficiency.
Patent Information
- Application Number
- CN202411252522.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing small-volume inductor component processes have problems such as coil deformation, short-circuit risk due to large pressure, limited annealing temperature of alloy powder, high losses, and difficult to improve magnetic permeability of magnetic materials, especially when preparing smaller volume and high-precision inductors.
Using a 3D printing-based patch power inductor preparation method, using magnetic slurry as the support medium, the coil and lead-out end are embedded through micro-zone 3D printing technology, and drying, isostatic pressure treatment, cleaning, end silver and annealing to form high Performance inductor.
It realizes a smaller volume of the inductor (wire diameter up to 10um), high precision and good yield rate, reduces losses, improves permeability and production efficiency, and simplifies the process flow.
Smart Images

Figure CN119092285A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a chip power inductor, in particular to a method for preparing a chip power inductor based on 3D printing, and belongs to the technical field of methods for preparing chip power inductors. Background Art
[0002] With the development of 5G electronics, the performance requirements for electronic components are getting higher and higher. On the one hand, they are required to have a smaller size, and on the other hand, the performance of electronic components is also required to be better than that of components of the same size. For smaller inductor components, the selected magnetic materials are required to have higher magnetic permeability, higher saturation magnetic induction intensity, and lower loss. Furthermore, smaller inductors have higher corresponding process accuracy requirements, which puts higher requirements on equipment accuracy.
[0003] Currently, small-volume inductor components are usually prefabricated with coils and then filled with powder and pressed. This method requires a relatively high molding pressure (500-800Mpa). Excessive pressure often causes the coil to deform, and even leads to risks such as short circuits and low Q. Therefore, this process also has certain disadvantages.
[0004] Secondly, the process method of pre-embedded enameled coils in one-piece molded inductors limits the annealing temperature of the alloy powder, which makes it difficult to eliminate the internal stress of the inductor caused by pressing, resulting in higher losses in the prepared inductor and difficulty in further improving the magnetic permeability of the magnetic material, which also restricts the improvement of the performance of metal power inductors.
[0005] In order to prepare smaller inductors, the LTCC process is also used to prepare stacked chip inductors. Although the stacked chip inductors prepared by the LTCC process can prepare smaller inductors, it is difficult to print coils with smaller wire diameters based on the printing process, as well as deviations caused by stacking alignment and magnetic phase deformation of the inductor. Therefore, a chip power inductor preparation method based on 3D printing is designed to solve the above problems. Summary of the invention
[0006] The main purpose of the present invention is to provide a method for preparing a chip power inductor based on 3D printing.
[0007] The purpose of the present invention can be achieved by adopting the following technical solutions:
[0008] A method for preparing a chip power inductor based on 3D printing comprises the following steps:
[0009] Step 1: Use magnetic slurry as the support medium for 3D printing;
[0010] Step 2: Using micro-area 3D printing technology to embed a printed coil and a lead end of the coil into the magnetic slurry to form an inductor blank;
[0011] Step 3: drying the supporting medium with the coil to form an inductor blank;
[0012] Step 4: performing isostatic pressing on the inductor blank;
[0013] Step 5: Clean the inductor and terminate it with silver;
[0014] Step 6: After the silver-terminated inductor is annealed, the inductor preparation is completed.
[0015] Preferably, between step 2 and step 3, the process further includes printing cutting lines after all coils are printed;
[0016] In step three, the drying temperature is 60-80°C and the drying time is 30-60min.
[0017] Preferably, the pressure of the isostatic pressure treatment in step 4 is 70-100 MPa;
[0018] Between step 4 and step 5, the process also includes cutting the inductor and performing medium-temperature debonding at a temperature of 290-320°C.
[0019] Preferably, before step 1, the method further includes preparation of magnetic slurry, which specifically includes the following steps:
[0020] S11: annealing the Fe-based soft magnetic powder;
[0021] S12, passivating the annealed Fe-based soft magnetic powder;
[0022] S13, mixing the passivated Fe-based soft magnetic powder with a dispersant, a binder, a curing agent, a plasticizer and an organic solvent, stirring and ball milling until the Fe-based soft magnetic powder is evenly dispersed in the mixed solution;
[0023] S14, filtering the mixed solution to obtain magnetic slurry.
[0024] Preferably, the Fe-based soft magnetic powder is any one of FeSiCr powder, carbonyl iron powder, amorphous powder and nanocrystalline powder;
[0025] or
[0026] Mixed powder of FeSiCr powder, carbonyl iron powder, amorphous powder and nanocrystalline powder.
[0027] Preferably, the binder is any one of silicone resin, epoxy resin and water glass;
[0028] or
[0029] A mixture of silicone resin, epoxy resin and water glass;
[0030] The amount of binder added is 3-13wt%;
[0031] The plasticizer is phthalic acid, and the added amount is 1-6wt%;
[0032] The organic solvent is any one of ethanol, ethyl acetate and n-propyl acetate;
[0033] or
[0034] A mixture of ethanol, ethyl acetate and n-propyl acetate.
[0035] Preferably, the Fe-based soft magnetic powder is mixed with a phosphoric acid ethanol solution and dried at 80° C. to complete the passivation treatment of the Fe-based soft magnetic powder;
[0036] Wherein, the added amount of phosphoric acid ethanol solution is 0.5-2wt%.
[0037] Preferably, the magnetic slurry has a solid content of 65-85% and a viscosity of 2000-15000 Pa·S.
[0038] Preferably, the D50 of the Fe-based soft magnetic powder is 10-30 μm.
[0039] Beneficial technical effects of the present invention:
[0040] The present invention provides a method for preparing a chip power inductor based on 3D printing. The method uses a magnetic slurry as a supporting medium for 3D printing, and adopts a micro-area 3D printing technology to embed a printed coil and a lead-out end of the coil in the magnetic slurry to form an inductor blank. The supporting medium with the coil is dried to form an inductor blank. The inductor blank is subjected to isostatic pressing treatment, the inductor is cleaned and silver-terminated, and the silver-terminated inductor is annealed to complete the inductor preparation. The inductor prepared by the method of the present application has the advantage of a smaller volume, can reach a wire diameter of 10um, and has a good yield rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a flow chart of a preferred embodiment of a method for preparing a chip power inductor based on 3D printing according to the present invention;
[0042] Figure 2 The figure is a 3D printing schematic diagram of a preferred embodiment of a method for preparing a chip power inductor based on 3D printing according to the present invention. DETAILED DESCRIPTION
[0043] In order to make the technical solution of the present invention more clear and specific to those skilled in the art, the present invention is further described in detail below in conjunction with embodiments and drawings, but the implementation manner of the present invention is not limited thereto.
[0044] Embodiment 1
[0045] like Figure 1 As shown, the method for preparing a micro-chip power inductor based on 3D printing includes:
[0046] Annealing the Fe-based soft magnetic powder;
[0047] In this step, the Fe-based soft magnetic powder needs to be pre-annealed to reduce the internal stress of the Fe-based soft magnetic powder, wherein the Fe-based soft magnetic powder includes FeSiCr powder, carbonyl iron powder, amorphous powder, nanocrystalline powder or a mixed powder thereof. The D50 of the FeSiCr powder, amorphous powder or nanocrystalline powder is between 10-30 μm.
[0048] The annealing temperature of FeSiCr powder is 700-900°C for 2-4h, the annealing temperature of amorphous powder is 400-450°C for 1h, and the annealing temperature of nanocrystalline powder is 500-550°C for 1h. All the above annealing is carried out in nitrogen or vacuum.
[0049] Passivation treatment is performed on the annealed Fe-based soft magnetic powder;
[0050] In this step, the Fe-based soft magnetic powder is completely mixed with the phosphoric acid ethanol solution and dried at 80° C. to complete the passivation treatment of the Fe-based soft magnetic powder, wherein the amount of phosphoric acid added is 0.5-2wt% of the weight of the Fe-based soft magnetic powder.
[0051] Passivation refers to the use of phosphoric acid or nitric acid to form a passivation film on the surface of the powder to increase the resistivity of the powder particles.
[0052] The Fe-based soft magnetic powders of the present application are all gas-atomized spherical powders, and the prepared magnetic phase density distribution is uniform.
[0053] The Fe-based soft magnetic powder after passivation treatment is mixed with a dispersant, a binder, a curing agent, a plasticizer and an organic solvent, stirred and ball-milled until the Fe-based soft magnetic powder is uniformly dispersed in the mixed solution;
[0054] In this step, the ball milling time is 12 hours. In order to obtain a mixed solution in which the Fe-based soft magnetic powder is evenly dispersed, the mixed solution has formed a slurry at this time.
[0055] The binder comprises a mixture of one or more combinations of silicone resin, epoxy resin and water glass, and the added amount is 3-13wt% of the weight of the Fe-based soft magnetic powder; the plasticizer is phthalic acid, and the added amount is 1-6wt% of the weight of the Fe-based soft magnetic powder; the organic solvent is one of ethanol, ethyl acetate and n-propyl acetate or a mixture thereof; the solid content of the magnetic slurry is 65-85%, and the viscosity is 2000-15000 Pa·S.
[0056] The binder selected in the present application has the characteristic of high temperature resistance, so that the magnetic slurry can have good mechanical strength after curing.
[0057] The mixed solution is filtered to obtain magnetic slurry; in this step, the mixed solution is filtered with a 120-mesh screen to obtain the magnetic slurry, ensuring that fewer agglomerates appear in the mixed solution.
[0058] The magnetic slurry prepared in the above steps can first eliminate the internal stress of the Fe-based soft magnetic powder through annealing treatment, so that it can increase the resistivity as a magnetic phase, thereby reducing eddy current loss. The Fe-based soft magnetic powder can be passivated and mixed with various reagents to obtain a magnetic slurry. The magnetic slurry has excellent fluidity and low sintering shrinkage. It is an excellent supporting medium for 3D printed coils, can better match the printed coils, and reduce the risk of short circuit or open circuit of the inductor.
[0059] Using magnetic slurry as a supporting medium for 3D printing, wherein the magnetic slurry is prepared by mixing Fe-based soft magnetic powder as a magnetic phase with a binder, that is, prepared by the above steps;
[0060] Before this step, pour the prepared magnetic slurry into the printing mold, then scrape it flat with a scraper or other equipment, and place it in the printing area of the 3D printer after scraping.
[0061] The micro-area 3D printing technology is used to embed the printed coil and the lead-out end of the coil into the magnetic slurry to form an inductor blank;
[0062] In this step, adjust the printing parameters of the 3D printer, import the program corresponding to the coil model, start the 3D printer to start printing, and the print head of the 3D printer prints the coil and the coil lead-out terminal from bottom to top in the magnetic slurry according to the designed position. After printing, the inductor blank is formed, such as Figure 2 As shown, the magnetic support material in the figure is magnetic slurry.
[0063] Among them, the printing accuracy of the 3D printer of the present application is nanometer or micrometer level, and it adopts micro-area 3D printing technology, which can also be called micro-nano 3D printing technology. This equipment is an existing technology in the field of 3D printing, so its structure and principle will not be elaborated.
[0064] It is worth mentioning that in this embodiment, the metal material of the printing coil is conductive silver paste, which not only has good conductivity but also excellent fluidity. After curing, the resistivity can reach 2-4*10-6Ω*cm, and can be squeezed out of a 10um 3D printing head very stably.
[0065] After all coils are printed, print the cutting lines;
[0066] This step makes it easier to cut the coil blank from the entire magnetic slurry later, because multiple coils are usually printed at one time.
[0067] Dry the support medium and remove the inductor blank. The specific steps are as follows:
[0068] Drying the supporting medium with the coil to form an inductor blank at a temperature of 60-80° C. for 30-60 minutes;
[0069] This step is mainly to solidify the magnetic material and the coil, so that the magnetic material and the coil form a block. And remove other materials, such as organic solvents such as ethanol, etc. The block is the inductor blank, which is convenient for subsequent cutting operations to remove residual organic solvents such as ethanol. At this time, the supporting medium still has soft magnetic phases and organic resins, plasticizers and dispersants.
[0070] The inductor blank is subjected to isostatic pressing at a pressure of 70-100 MPa;
[0071] The purpose of this step is to increase the density of the bar.
[0072] Cut off the inductor and perform medium temperature debonding at a temperature of 290-320℃;
[0073] This step is to remove the glue wrapped around the inductor.
[0074] Clean the inductor and terminate it with silver;
[0075] In this step, there is also a step S301, in which the inductor is chamfered and then silver-terminated. The silver-terminated process is also called silvering. The widely used silver-terminated process is: silver spraying, that is, using high pressure to make the silver paste atomized and sprayed on the parts to be electroplated. The silver-terminated process can change the surface properties or size of the substrate, improve the corrosion resistance of metal parts in the use environment, improve the working performance of the parts, hardness, wear resistance, conductivity, electromagnetic properties, heat resistance, etc., and thus improve the performance of the inductor.
[0076] The silver-terminated inductor is annealed to complete the inductor preparation. This step is mainly to remove the stress generated by the magnetic material in step S202 so that the magnetic material has good performance again.
[0077] The inductor generally includes a coil, an end electrode and a magnet part. Therefore, the end electrode and the coil are directly printed during the printing process, and the magnet part is formed by solidifying the magnetic material in the magnet slurry and wrapping it around the coil.
[0078] Annealing treatment is carried out in a vacuum or nitrogen environment to ensure that the inductor has a high magnetic permeability. Its magnetic permeability is 1.5-3 times that before annealing. The magnetic loss of the inductor decreases significantly after annealing.
[0079] In summary, the method of the present invention has a simple process, can greatly improve the production efficiency of the inductor, and is conducive to reducing the production cost. The power inductor prepared by this process can be annealed at high temperature, which can improve the magnetic permeability of the alloy powder and reduce the loss of the inductor. The wire diameter of the printed coil can be between 10-200um, that is, the minimum printed wire diameter can reach 10um, and the printing accuracy is controllable.
[0080] Example 2
[0081] A micro-chip power inductor based on 3D printing is prepared using the above-mentioned method for preparing a micro-chip power inductor based on 3D printing.
[0082] The inductor prepared by the method of the present application has the advantage of being smaller in size, can reach a wire diameter of 10um, and has a good yield rate. Compared with the LTCC process, this process is simple and has high precision; on the other hand, the minimum size of the prepared power inductor can be less than 1mm, and the height is about 0.5mm. The inductor can be widely used in mobile phones, notebooks, tablet computers, wearable electronics and other products.
[0083] Example 3
[0084] The inductor prepared by the method of the present application is prepared in the following steps: first, annealed amorphous powder (powder particle size D50 = 10μm, magnetic permeability 22, saturation magnetic induction intensity Bs value 1.6T) is used as raw material, and phosphating treatment is performed on it to prepare slurry, and the printed 3D coil is embedded in the slurry, and the wire is made of low-temperature silver paste. After the processes of debinding, cutting, and silver termination, the magnetic core blank is annealed, and the annealing atmosphere is a nitrogen protective atmosphere, the annealing temperature is 450℃, and the time is 1h. The size of the prepared inductor is L*W*H2.0*1.2*1.0mm, the DCR design requirement is a maximum of 95mΩ, and the inductance is 1.0uH.
[0085] The following is a performance comparison example of an inductor made by the method of the present application and a power inductor of Murata Electronics, the comparative example is DFE201210U-1R0M, the magnetic phase material is made of metal alloy magnetic powder, the conductor is copper wire, and it is a product made by a traditional method. The comparative structure is shown in Table 1:
[0086] project L value / uH(1.0±20%) Saturation current / A DCR / mΩ Temperature rise current / A This product 0.84 3.5 83 3.2 Comparative Example 0.97 3.6 88 2.4
[0087] It can be seen that Table 1 lists the performance of this product and the comparative example. It can be seen from Table 1 that the power inductor prepared by the present invention can meet the basic requirements of the same series of products. It can be seen that the DCR value of the inductor prepared by this method can be lower, and the temperature rise current of the inductor is higher than that of the inductor of Murata Electronics 201210U-1R0 model, which shows that the inductor prepared by this method has lower loss. The inductor prepared by the present invention can meet the requirements of miniaturization and high current of power inductors. Compared with molded inductors, this method will have the defect of low density of the magnetic phase of the inductor. In terms of design, the inductor wire needs to consider using silver paste with a smaller DCR, and the number of turns is increased appropriately to meet the requirements on the inductance. However, in general, the present invention provides a new process method, which can prepare a smaller inductor, and has extremely high controllable accuracy, and can realize the printing of wires with a wire diameter of micrometer level, which is of great significance to the development of the prepared inductor in a more miniaturized direction.
[0088] The above description is only a further embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and concepts of the present invention within the scope disclosed by the present invention, which belong to the protection scope of the present invention.
Claims
1. A method for preparing a chip power inductor based on 3D printing, characterized in that: The steps include: Step 1: Use magnetic slurry as the support medium for 3D printing; Step 2: Using micro-area 3D printing technology to embed a printed coil and a lead end of the coil into the magnetic slurry to form an inductor blank; Step 3: drying the supporting medium with the coil to form an inductor blank; Step 4: performing isostatic pressing on the inductor blank; Step 5: Clean the inductor and terminate it with silver; Step 6: After the silver-terminated inductor is annealed, the inductor preparation is completed.
2. The method for preparing a chip power inductor based on 3D printing according to claim 1, characterized in that: Between step 2 and step 3, it also includes printing cutting lines after all coils are printed; In step three, the drying temperature is 60-80°C and the drying time is 30-60min.
3. The method for preparing a chip power inductor based on 3D printing according to claim 1, characterized in that: The pressure of the isostatic treatment in step 4 is 70-100 MPa; Between step 4 and step 5, the process also includes cutting the inductor and performing medium-temperature debonding at a temperature of 290-320°C.
4. The method for preparing a chip power inductor based on 3D printing according to claim 1, characterized in that: Before step 1, the preparation of magnetic slurry is also included, which specifically includes the following steps: S11: annealing the Fe-based soft magnetic powder; S12, passivating the annealed Fe-based soft magnetic powder; S13, mixing the passivated Fe-based soft magnetic powder with a dispersant, a binder, a curing agent, a plasticizer and an organic solvent, stirring and ball milling until the Fe-based soft magnetic powder is evenly dispersed in the mixed solution; S14, filtering the mixed solution to obtain magnetic slurry.
5. The method for preparing a chip power inductor based on 3D printing according to claim 4, characterized in that: The Fe-based soft magnetic powder is any one of FeSiCr powder, carbonyl iron powder, amorphous powder and nanocrystalline powder; or Mixed powder of FeSiCr powder, carbonyl iron powder, amorphous powder and nanocrystalline powder.
6. The method for preparing a chip power inductor based on 3D printing according to claim 5, characterized in that: The adhesive is any one of silicone resin, epoxy resin and water glass; or A mixture of silicone resin, epoxy resin and water glass; The amount of binder added is 3-13wt%; The plasticizer is phthalic acid, and the added amount is 1-6wt%; The organic solvent is any one of ethanol, ethyl acetate and n-propyl acetate; or A mixture of ethanol, ethyl acetate and n-propyl acetate.
7. The method for preparing a chip power inductor based on 3D printing according to claim 6, characterized in that: The Fe-based soft magnetic powder is mixed with a phosphoric acid ethanol solution and dried at 80° C. to complete the passivation treatment of the Fe-based soft magnetic powder; Wherein, the added amount of phosphoric acid ethanol solution is 0.5-2wt%.
8. The method for preparing a chip power inductor based on 3D printing according to claim 7, characterized in that: The solid content of the magnetic slurry is 65-85%, and the viscosity is 2000-15000 Pa·S.
9. The method for preparing a chip power inductor based on 3D printing according to claim 8, characterized in that: The D50 of Fe-based soft magnetic powder is 10-30μm.