Manufacturing method and application of lithium-lanthanum-zirconium-oxygen-based solid electrolyte film

By using nano-oxide powder after grinding and drying and high-temperature sintering in solid-state lithium-ion batteries, combined with dispersion and injection into wire technology, the lithium lanthanum zirconium oxy-based solid electrolyte film is formed, and the bonding of solid-state batteries is solved and Conductivity issues significantly improve battery performance.

CN119092801APending Publication Date: 2024-12-06江西中懋新能源材料技术有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410345223.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing solid-state lithium-ion batteries are difficult to fit effectively during processing, have large internal resistance and insufficient centrifugal conductivity, which affects the cycling performance of the magnification.

Method used

The nano-oxide powder is treated by grinding, drying and high-temperature sintering, and combined with dispersion, hydrolysis and spraying into wire processes, a lithium lanthanum zirconium oxy-based solid electrolyte film is formed on the substrate, reducing internal resistance and improving centrifugal conductivity.

Benefits of technology

It significantly reduces the internal resistance of the solid electrolyte, improves the centrifugal conductivity, improves the fit with the substrate, and makes the battery performance more stable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092801A_ABST
    Figure CN119092801A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium-lanthanum-zirconium-oxygen-based solid electrolyte film manufacturing method and application, and the method comprises the steps: S1, mixing a lithium source, a lanthanum source, a zirconium source and a doped metal, carrying out grinding drying and high-temperature sintering treatment to obtain oxide powder, then carrying out grinding drying on the oxide powder, and carrying out nanocrystallization to obtain oxide slurry; the method comprises the following steps: S1, mixing oxide slurry with a dispersing agent to form a precursor solution; s2, adding a catalyst and a regulator; s3, carrying out hydrolysis and condensation reaction; and S4, forming a solid electrolyte film on the substrate. Compared with the prior art, the preparation method has the beneficial effects that powder is firstly subjected to grinding, drying and high-temperature sintering treatment to be subjected to nanocrystallization, then the subsequent procedures of dispersion, hydrolysis and the like are carried out, and finally, a lithium lanthanum zirconium oxygen-based solid electrolyte film is formed on a base material by adopting a jet filamentation process, so that the internal resistance is reduced, the centrifugal conductivity is obviously improved, and the service life of the lithium lanthanum zirconium oxygen-based solid electrolyte film is prolonged. And the solid electrolyte and the base material are better in fitting property and are more stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing a lithium lanthanum zirconium oxide solid electrolyte film and application thereof, belonging to the technical field of solid-state batteries. Background Art

[0002] Lithium-ion batteries have the advantages of high energy density, long cycle life, and zero memory efficiency. As commercial energy storage devices, they are widely used in daily life and production. With the advancement of science and technology, people's demand for high-efficiency energy storage devices has gradually increased, and safety issues have become the main challenge facing lithium-ion batteries in new demands and new fields of application. The safety issues of lithium-ion batteries mainly come from the large amount of flammable organic solvents in liquid electrolytes. All-solid-state lithium-ion batteries use solid electrolytes instead of commercial liquid organic electrolytes, which can fundamentally solve the safety problems of lithium-ion batteries.

[0003] However, during the processing of existing solid-state batteries, solid-state batteries are difficult to effectively bond, have large internal resistance, are not conducive to rate cycling, and their centrifugal conductivity needs to be improved. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a lithium lanthanum zirconium oxide solid electrolyte film. The method comprises the following steps: firstly grinding and drying the powder and subjecting it to high-temperature sintering treatment to nano-crystallization, and then subjecting it to subsequent dispersion, hydrolysis and other procedures. Finally, a spray-filamentation process is adopted to form a lithium lanthanum zirconium oxide solid electrolyte film on a substrate, thereby reducing its internal resistance and significantly improving its centrifugal conductivity.

[0005] The present invention is achieved through the following scheme: a method for preparing a lithium lanthanum zirconium oxide solid electrolyte film and its application, which comprises the steps of:

[0006] S1, mixing a lithium source, a lanthanum source, a zirconium source and a doping metal, grinding and drying and high-temperature sintering to obtain an oxide powder, and then grinding and drying the oxide powder to nano-size it to obtain an oxide slurry;

[0007] S1, mixing the oxide slurry with the dispersant at a stirring rate of 500 to 1000 rpm for 8 hours to form a precursor solution;

[0008] S2, adding a catalyst and a regulator to the precursor solution to control the reaction rate and product morphology;

[0009] S3, controlling the temperature at 75-80°C to allow the raw materials in the precursor solution to undergo hydrolysis and condensation reactions, and the precursor is gradually converted into a sol;

[0010] S4. The sol is sprayed into filaments through a spraying device to form a solid electrolyte film on a substrate.

[0011] Preferably, the molar ratio of lithium source, lanthanum source and zirconium source is 7:3:2;

[0012] Preferably, the lithium source is at least one of lithium carbonate and lithium hydroxide;

[0013] Preferably, the lanthanum source is at least one of lanthanum oxide and lanthanum nitrate;

[0014] Preferably, the zirconium source is zirconium oxide or zirconium oxychloride;

[0015] Preferably, the doping metal is at least one of aluminum, zinc, titanium and magnesium.

[0016] Preferably, the high temperature sintering temperature is 1000-1200°C.

[0017] Preferably, the dispersant is at least one of ethanol and isopropanol.

[0018] Preferably, the catalyst is a metal ion catalyst, specifically at least one of aluminum ions and titanium ions.

[0019] Preferably, the regulator is a polymer compound, specifically at least one of polyethylene glycol and polyvinyl pyrrolidone.

[0020] Preferably, the lithium lanthanum zirconium oxide solid electrolyte film is applied to solid-state batteries or lithium-ion batteries.

[0021] Preferably, the positive and negative electrodes of the solid-state battery or lithium-ion battery adopt a porous diaphragm material substrate, and a solid electrolyte film is formed by coating the porous diaphragm material.

[0022] Preferably, the positive and negative electrodes of the solid-state battery or lithium-ion battery are substrate-free structures, and are coated on the carrier release profile to form a solid electrolyte film.

[0023] The beneficial effects of the present invention are:

[0024] The present invention discloses a method for preparing a lithium lanthanum zirconium-based solid electrolyte film. The method comprises the following steps: firstly grinding and drying the powder and subjecting it to high-temperature sintering treatment to nano-crystallization, and then subjecting it to subsequent dispersion, hydrolysis and other procedures. Finally, a spray-filament forming process is adopted to form a lithium lanthanum zirconium-based solid electrolyte film on a substrate, so that the internal resistance is reduced, the centrifugal conductivity is significantly improved, and the solid electrolyte has better adhesion to the substrate and is more stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a structural diagram of an oxide slurry of a lithium lanthanum zirconium-based solid electrolyte film of the present invention.

[0026] Figure 2 This is a SEM image of a lithium lanthanum zirconium-based solid electrolyte film of the present invention.

[0027] Figure 3 Ionic conductivity test results DETAILED DESCRIPTION

[0028] Combine the following Figure 1-3 The present invention is further described, but the protection scope of the present invention is not limited to the described contents.

[0029] Example 1

[0030] A method for preparing a lithium lanthanum zirconium oxide solid electrolyte film, comprising the steps of:

[0031] S1. Mix lithium carbonate, lanthanum oxide, zirconium oxide and aluminum, wherein the molar ratio of lithium carbonate, lanthanum oxide and zirconium oxide is 7:3:2, grind and dry the mixture and perform high-temperature sintering treatment, wherein the high-temperature sintering temperature is 1000-1200° C. to obtain oxide powder, and then grind and dry the oxide powder to make it nano-sized to obtain oxide slurry;

[0032] S1, mixing the oxide slurry with ethanol at a stirring rate of 500 to 1000 rpm for 8 hours to form a precursor solution;

[0033] S2, adding aluminum ions and polyethylene glycol to the precursor solution to control the reaction rate and product morphology;

[0034] S3, controlling the temperature at 75-80°C to allow the raw materials in the precursor solution to undergo hydrolysis and condensation reactions, and the precursor is gradually converted into a sol;

[0035] S4. The sol is sprayed into filaments through a spraying device to form a solid electrolyte film on a substrate.

[0036] Example 2

[0037] A method for preparing a lithium lanthanum zirconium oxide solid electrolyte film, comprising the steps of:

[0038] S1. Mix lithium hydroxide, lanthanum nitrate, zirconyl chloride and zinc, wherein the molar ratio of lithium hydroxide, lanthanum nitrate and zirconyl chloride is 7:3:2, grind and dry the mixture and perform high-temperature sintering treatment, wherein the high-temperature sintering temperature is 1000-1200° C. to obtain oxide powder, grind and dry the oxide powder to make it nano-sized, and obtain oxide slurry;

[0039] S1, mixing the oxide slurry with isopropanol at a stirring rate of 500 to 1000 rpm for 8 hours to form a precursor solution;

[0040] S2, adding titanium ions and polyvinyl pyrrolidone to the precursor solution to control the reaction rate and product morphology;

[0041] S3, controlling the temperature at 75-80°C to allow the raw materials in the precursor solution to undergo hydrolysis and condensation reactions, and the precursor is gradually converted into a sol;

[0042] S4. The sol is sprayed into filaments through a spraying device to form a solid electrolyte film on a substrate.

[0043] Example 3

[0044] The only difference from Example 1 is that the reference metal is titanium.

[0045] Example 4

[0046] The only difference from Example 1 is that the reference metal is magnesium.

[0047] Example 5

[0048] The only difference from Example 1 is that the reference metal is a mixture of aluminum, zinc, titanium and magnesium, and the molar ratio of aluminum, zinc, titanium and magnesium is 1:1:1:1.

[0049] Example 6

[0050] The only difference from Example 1 is that the lithium source is a mixture of lithium carbonate and lithium hydroxide, and the molar ratio of lithium carbonate to lithium hydroxide is 1:1.

[0051] The lanthanum source is a mixture of lanthanum oxide and lanthanum nitrate, and the molar ratio of lanthanum oxide to lanthanum nitrate is 2:1;

[0052] The zirconium source is a mixture of zirconium oxide and zirconium oxychloride, and the molar ratio of zirconium oxide to zirconium oxychloride is 1:1.

[0053] Example 7

[0054] Application of lithium lanthanum zirconium oxide solid electrolyte film: Apply lithium lanthanum zirconium oxide solid electrolyte film to solid-state batteries, specifically:

[0055] S1, positive electrode film formation, receiving the sprayed lithium lanthanum zirconium oxide solid electrolyte film on the aluminum porous diaphragm material to form the battery positive electrode material;

[0056] S2, negative electrode film formation, receiving the sprayed lithium lanthanum zirconium oxide solid electrolyte film on the copper porous diaphragm material to form the battery negative electrode material.

[0057] The battery energy of the finished product is increased by 5%-15%.

[0058] Example 8

[0059] Application of lithium lanthanum zirconium oxide solid electrolyte film: Apply lithium lanthanum zirconium oxide solid electrolyte film to solid-state batteries, specifically:

[0060] S1, positive electrode film formation, receiving the sprayed lithium lanthanum zirconium oxide solid electrolyte film on the aluminum carrier profile to form a battery positive electrode material;

[0061] S2, negative electrode film formation, receiving the sprayed lithium lanthanum zirconium oxide solid electrolyte film on the copper carrier release material to form the battery negative electrode material.

[0062] Comparative Example 1

[0063] The only difference from Example 1 is that the colloid is sprayed directly onto the substrate.

[0064] Comparative Example 2

[0065] The only difference from Example 1 is that in S1, lithium hydroxide, lanthanum nitrate, zirconyl chloride and zinc are only mixed and ground into micron-sized powder before entering into subsequent operations.

[0066] The ionic conductivity of the solid electrolytes in Example 1, Comparative Example 1 and Comparative Example 2 was tested, and the test results are shown in Figure 3 .

[0067] Although the technical solutions of the present invention have been described and listed in detail, it should be understood that it is obvious to those skilled in the art to make modifications to the above embodiments or adopt equivalent alternatives. These modifications or improvements made without departing from the spirit of the present invention are within the scope of protection required by the present invention.

Claims

1. A method for preparing a lithium lanthanum zirconium oxide solid electrolyte film, It is characterized in that It includes the steps of: S1, mixing a lithium source, a lanthanum source, a zirconium source and a doping metal, grinding and drying and high-temperature sintering to obtain an oxide powder, and then grinding and drying the oxide powder to nano-size it to obtain an oxide slurry; S1, mixing the oxide slurry with the dispersant at a stirring rate of 500 to 1000 rpm for 8 hours to form a precursor solution; S2, adding a catalyst and a regulator to the precursor solution to control the reaction rate and product morphology; S3, controlling the temperature at 75-80°C to allow the raw materials in the precursor solution to undergo hydrolysis and condensation reactions, and the precursor is gradually converted into a sol; S4. The sol is sprayed into filaments through a spraying device to form a solid electrolyte film on a substrate.

2. A method for preparing a lithium lanthanum zirconium oxide solid electrolyte film according to claim 1, It is characterized in that The molar ratio of the lithium source, the lanthanum source and the zirconium source is 7:3:

2.

3. A method for preparing a lithium lanthanum zirconium-based solid electrolyte film according to claim 1, It is characterized in that The lithium source is at least one of lithium carbonate and lithium hydroxide; The lanthanum source is at least one of lanthanum oxide and lanthanum nitrate; The zirconium source zirconium oxide, zirconyl chloride; The doping metal is at least one of aluminum, zinc, titanium and magnesium.

4. A method for preparing a lithium lanthanum zirconium-based solid electrolyte film according to claim 1, It is characterized in that The high temperature sintering temperature is 1000-1200℃.

5. The method for preparing a lithium lanthanum zirconium-based solid electrolyte film according to claim 1, It is characterized in that The dispersant is at least one of ethanol and isopropanol.

6. A method for preparing a lithium lanthanum zirconium-based solid electrolyte film according to claim 1, It is characterized in that The catalyst is a metal ion catalyst, specifically at least one of aluminum ions and titanium ions.

7. A method for preparing a lithium lanthanum zirconium-based solid electrolyte film according to claim 1, It is characterized in that The regulator is a polymer compound, specifically at least one of polyethylene glycol and polyvinyl pyrrolidone.

8. Application of a lithium lanthanum zirconium oxide solid electrolyte film, It is characterized in that The lithium lanthanum zirconium oxide solid electrolyte film is applied to solid-state batteries or lithium-ion batteries.

9. Use of a lithium lanthanum zirconium-based solid electrolyte film according to claim 8, It is characterized in that The positive and negative electrodes of the solid-state battery or lithium-ion battery adopt a porous diaphragm material substrate, and a solid electrolyte film is formed by coating the porous diaphragm material.

10. Use of a lithium lanthanum zirconium-based solid electrolyte film according to claim 8, It is characterized in that The positive and negative electrodes of the solid-state battery or lithium-ion battery are substrate-free structures, and are coated on a carrier release material to form a solid electrolyte film.