Method for preparing all-solid-state lithium metal battery composite electrolyte by PVB (Polyvinyl Butyral) additive

By using PVB as an additive in all-solid lithium-ion batteries and preparing MOF and organometallic lithium-zirconium precursors in combination with hydrothermal method, the problem of poor contact between the solid electrolyte membrane and the electrode interface is solved, and the conductivity and discharge ratio of the battery are significantly improved. Capacity improves electrochemical performance.

CN119092807AInactive Publication Date: 2024-12-06ZHEJIANG SHANGAO NEW ENERGY CO LTD

Patent Information

Application Number
CN202411178474.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In all-solid lithium-ion batteries, the interface contact between the solid electrolyte membrane and the solid electrode is poor, resulting in a low discharge capacity, and the interface compatibility is needed to improve the electrochemical performance.

Method used

Using PVB as an additive, MOF (UIO-67) and organometallic lithium zirconium precursors were prepared by hydrothermal method, combining LiTFSI, PVB and PVDF-HFP to enhance adhesion between the electrolyte and the electrode, reduce interface resistance, and improve interface phase Capacity.

Benefits of technology

It effectively improves the conductivity and discharge specific capacity of all solid-state batteries and improves electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011410470000061
    Figure BDA0005011410470000061
Patent Text Reader

Abstract

The invention discloses a method for preparing an all-solid-state lithium metal battery composite electrolyte from a PVB (Polyvinyl Butyral) additive. Comprising the following steps: A, preparing MOF (UIO-67) by adopting a hydrothermal method; the preparation method comprises the following steps: A, preparing an organic metal lithium zirconium precursor UiO-67, B, preparing a 2 '-amino-[1, 1': 4 ', 1' '-terphenyl]-4, 4' '-dicarboxylic acid / zirconium complex, C, preparing an electrolyte membrane from LiTFSI, the organic metal lithium zirconium precursor UiO-67, PVB and PVDF-HFP, and D, assembling into a solid-state battery, and testing the conductivity and specific discharge capacity of the solid-state battery. According to the method, the adhesive force between the electrolyte and the electrode is enhanced, so that the interface resistance is effectively reduced, the interface compatibility between the electrolyte and the electrode is improved, and the electrochemical performance of the all-solid-state battery is finally improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium battery solid electrolytes, and in particular relates to a method for preparing an all-solid-state lithium metal battery composite electrolyte by using a PVB additive. Background Art

[0002] Traditional lithium-ion batteries have many disadvantages in practical applications due to the use of liquid electrolytes. In addition, the leakage and flammability of liquid electrolytes have caused many safety problems in actual life and production. Compared with traditional liquid electrolytes, solid electrolytes in all-solid-state lithium-ion batteries have the advantages of low flammability, wide electrochemical stability window, good thermal stability, no leakage, and high safety.

[0003] Patent CN116053568A discloses a polymer composite electrolyte and a preparation method thereof. The technical problem solved by the present invention is to provide a low-cost lithium ion solid electrolyte with high lithium ion conductivity. The solid electrolyte comprises a polymer substrate, a lithium salt and an additive, wherein the additive is eucryptite-type LiAlSiO4. A new inorganic solid electrolyte additive is used.

[0004] Patent CN115020818A discloses a polymer solid electrolyte containing 2,3,4,5,6-pentafluorophenylboric acid and an all-solid-state metal lithium battery. The polymer solid electrolyte includes a polymer matrix, a metal lithium salt and an additive, and the additive includes 2,3,4,5,6-pentafluorophenylboric acid (FFPBA). The present invention also provides an all-solid-state metal lithium battery including the polymer solid electrolyte. The present invention uses FFPBA material as a solid electrolyte additive to achieve protection of the all-solid-state metal lithium negative electrode and applicability to the high-voltage positive electrode.

[0005] However, in previous studies, the assembled all-solid-state lithium-ion batteries showed relatively low discharge capacity due to poor interface contact between the solid electrolyte membrane and the solid electrode. Therefore, the interface compatibility of these solid electrolyte membranes must be improved. PVB has good mechanical properties and is therefore widely used in solid oxide fuel cells. In the PVB molecular chain, the six-membered ring structure formed by the butyraldehyde group increases the strength of the molecular chain and simultaneously reduces the crystallinity of PVB. In addition, PVB has high viscosity, which can enhance the adhesion between the electrolyte and the electrode, thereby effectively reducing the interface resistance, improving the interface compatibility between the electrolyte and the electrode, and ultimately improving the electrochemical performance of the all-solid-state battery. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive, thereby enhancing the adhesion between the electrolyte and the electrode, thereby effectively reducing the interface resistance, improving the interface compatibility between the electrolyte and the electrode, and ultimately improving the electrochemical performance of the all-solid-state battery.

[0007] The technical solution of the present invention is: a method for recovering all elements of nickel-cobalt-manganese-lithium oxide waste, comprising the following steps:

[0008] A. MOF (UIO-67) was prepared by hydrothermal method. DMF and 4,4'-biphenyldicarboxylic acid (BPDC) powder were placed in a beaker according to appropriate proportions, and the mixed solution was ultrasonicated to completely dissolve BPDC, and then placed in a constant temperature box for heating; then, it was naturally cooled to room temperature to obtain a colorless, transparent solution with a pungent odor; then, the above solution was operated in order as follows: zirconium chloride (ZrCl4) was added, ultrasonicated, then PVP was added, ultrasonicated, then acetic acid was added, and fully mixed; poured into a reactor, the suspension was centrifuged, washed twice with detergent, and finally, dried for 12 hours to obtain a white sample powder UiO-67. In addition, the sample powder needs to be vacuum activated before use;

[0009] B. Prepare 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / zirconium complex, mix 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid, ZrCl4, and solvent according to a suitable ratio, react, filter, wash, and then dry in vacuum to obtain 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / zirconium complex; mercapto-propylene Michael addition reaction, mix 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / zirconium complex: 2-mercaptoethanol lithium, hexafluorobutyl acrylate, catalyst, and solvent according to a suitable ratio, react, neutralize with dilute hydrochloric acid to pH 7, filter, wash the solid with water, and finally dry in a vacuum oven to obtain an organometallic lithium zirconium precursor;

[0010] C. First, a certain amount of LiTFSI and organometallic lithium zirconium precursor UiO-67 were dispersed in NMP organic solvent and stirred until the powder was evenly dispersed; then, different proportions of PVB and PVDF-HFP were added to the slurry, stirred overnight at a suitable temperature, and the slurry was evenly coated on a polytetrafluoroethylene plate with a spatula and vacuum dried; finally, the dried electrolyte membrane was cut into discs with a diameter of 18 mm and transferred to a glove box for further use;

[0011] D. Assemble into a solid-state battery and test its conductivity and discharge specific capacity.

[0012] As a preferred technical solution of the present invention, in step A, the mass ratio of DMF to 4,4'-biphenyldicarboxylic acid (BPDC) powder is 0.8-1.2:2.8-3.2.

[0013] As a preferred technical solution of the present invention, in step A, the dissolving heating temperature is 120° C. and the heating time is 15 min.

[0014] As a preferred technical solution of the present invention, in step A, 40 parts of zirconium chloride (ZrCl4) are ultrasonically treated for 15 minutes, 100 parts of PVP are added, ultrasonically treated for 15 minutes, and then 80 parts of acetic acid are added.

[0015] As a preferred technical solution of the present invention, in step A, the reaction temperature is set to 120° C., and the reaction is naturally cooled to room temperature after 24 hours of reaction.

[0016] As a preferred technical solution of the present invention, in step A, the suspension is centrifuged at a speed of 8500 rpm for 3 minutes.

[0017] As a preferred technical solution of the present invention, in step A, the detergent is one or both of DMF or ethanol.

[0018] As a preferred technical solution of the present invention, in step A, the vacuum activation temperature is set at 150°C.

[0019] As a preferred technical solution of the present invention, in step A, the molar ratio of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid: ZrCl4: solvent is 1:1.1-1.5:7-10.

[0020] As a preferred technical solution of the present invention, in step A, the solvent is anhydrous methanol or ethanol, the reaction is carried out at 20°C-65°C for 30-60 minutes, and the detergent is cold methanol.

[0021] As a preferred technical solution of the present invention, in step B, the molar ratio of the 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / zirconium complex: lithium 2-mercaptoethanol: hexafluorobutyl acrylate: catalyst: solvent is 1:1.3-1.7:0.02-0.2:0.03-0.07:5-10.

[0022] As a preferred technical solution of the present invention, in step B, the solvent is anhydrous ethanol or isopropanol, the catalyst is triethylamine, and the reaction is carried out at 20°C-65°C for 30-60 minutes.

[0023] As a preferred technical solution of the present invention, in step B, the mass ratio of LiTFSI to the organic metal lithium zirconium precursor UiO-67 is 0.8-1.2:1.9-2.1.

[0024] As a preferred technical solution of the present invention, in step B, the mass ratio of PVB to PVDF-HFP is 0-3:1.

[0025] The beneficial effects achieved by the present invention using the above technical solution are as follows:

[0026] 1. Metal-organic frameworks (MOFs) have been used as fillers and introduced into polymer electrolytes to improve the electrochemical properties of electrolyte membranes. The open metal sites (OMS) of MOFs form coordination bonds with anions, thereby further improving the mobility of lithium ions.

[0027] 2. PVB has good mechanical properties and is therefore widely used in solid oxide fuel cells. In the PVB molecular chain, the hexacyclic structure formed by the butyraldehyde group increases the strength of the molecular chain and reduces the crystallinity of PVB. In addition, PVB has high viscosity, which can enhance the adhesion between the electrolyte and the electrode, thereby effectively reducing the interface resistance, improving the interface compatibility between the electrolyte and the electrode, and ultimately improving the electrochemical performance of the all-solid-state battery. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0030] Example 1

[0031] A method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB (polyvinyl butyral) additive, comprising the following steps:

[0032] A. Prepare MOF (UIO-67) by hydrothermal method. Pour 19mL of DMF and 60mg of 4,4'-biphenyldicarboxylic acid (BPDC) powder into a 50mL beaker according to the appropriate proportion. Ultrasonicate the mixed solution for 15min to completely dissolve BPDC, and then place it in a constant temperature box at 120℃ and heat it for 15min. After that, cool it naturally to room temperature to obtain a colorless, transparent solution with a pungent odor. Then, the above solution is operated in order as follows: add 40mg of zirconium chloride (ZrCl4), ultrasonicate for 15min, add 100mg of PVP, ultrasonicate for 15min, add 800μL of acetic acid, and ultrasonicate to mix thoroughly. Pour the uniform mixed solution into a 30mL reactor, set the reaction temperature to 120℃, and cool it naturally to room temperature after 24h of reaction. After that, centrifuge the obtained suspension at 8500rpm for 3min and wash it twice with DMF and alcohol. Finally, dry it in an oven at 80℃ overnight to obtain a white sample powder UiO-67. In addition, the sample powder was vacuum activated at 150 °C before use.

[0033] B. Prepare 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / zirconium complex. The raw material ratio is listed in the table below. The organometallic lithium zirconium precursor is obtained by mercapto-propylene Michael addition reaction. The specific content ratio is listed in the table below.

[0034] C. First, 34 mg of LiTFSI and 68 mg of organometallic lithium zirconium precursor UiO-67 were dispersed in NMP organic solvent and then magnetically stirred at 75 ° C for 3 h until the powder was evenly dispersed. After that, 24 mg of PVB and 35 mg of PVDF-HFP were added to the slurry and stirred at 75 ° C overnight. Finally, the slurry was evenly coated on a polytetrafluoroethylene plate with a spatula and then vacuum dried at 50 ° C. Finally, the dried electrolyte membrane was cut into discs with a diameter of 18 mm and transferred to the glove box for further use. The electrolyte membranes were named UBP.

[0035] D. Assembled into a solid-state battery, its conductivity is the highest, 3.27×10 -4 S cm -1 , discharge specific capacity 154.9mAh / g.

[0036] Example 2

[0037] A method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive comprises the following steps:

[0038] The difference from Example 1 is:

[0039] The DMF is 16 mL, and the mass of 4,4'-biphenyldicarboxylic acid (BPDC) powder is 56 mg. 27.2 mg of LiTFSI and 64.6 mg of UiO-67 are dispersed in NMP organic solvent, the content of PVB is 0, and the preparation content of the modified organic metal lithium zirconium precursor is listed in the following table.

[0040] Assembled into a solid-state battery, its conductivity is 3.01×10 -4 S cm -1 , discharge specific capacity 138.6mAh / g.

[0041] Example 3

[0042] A method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive comprises the following steps:

[0043] The difference from Example 1 is:

[0044] The DMF is 22.8 mL, and the mass of 4,4'-biphenyldicarboxylic acid (BPDC) powder is 60.8 mg. 40.8 mg of LiTFSI and 71.4 mg of UiO-67 are dispersed in NMP organic solvent, the content of PVB is 48 mg, and the preparation content of the modified organic metal lithium zirconium precursor is listed in the following table.

[0045] Assembled into a solid-state battery, its conductivity is 2.58×10 -4 S cm -1 , discharge specific capacity 124.6mAh / g.

[0046] Comparative Example 1

[0047] The difference from Example 1 is as shown in the following table. The solid-state battery is assembled and its conductivity is 1.36×10 -4 Scm -1 , discharge specific capacity 124.3mAh / g.

[0048] Comparative Example 2

[0049] The difference from Example 1 is as shown in the following table. The solid-state battery is assembled and its conductivity is 1.23×10 -4 Scm -1 , discharge specific capacity 105.9mAh / g.

[0050] Table 1

[0051]

[0052] It can be seen from the above specific implementation scheme that this method effectively improves the conductivity and discharge specific capacity of the battery, and ultimately improves the electrochemical performance of the all-solid-state battery.

[0053] The present invention has been described above through specific implementation methods and examples, but these descriptions are only illustrative and should not be understood as limiting the scope of protection of the present invention. Without departing from the spirit and scope of protection of the present invention, those skilled in the art may make various improvements, modifications or equivalent substitutions to the technical solutions and implementation methods of the present invention, all of which should fall within the scope of protection of the present invention.

Claims

1. A method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive, characterized in that The following steps are involved: A. MOF (UIO-67) was prepared by hydrothermal method. DMF and 4,4'-biphenyldicarboxylic acid (BPDC) powder were placed in a beaker according to appropriate proportions, and the mixed solution was ultrasonicated to completely dissolve BPDC, and then placed in a constant temperature box for heating; then, it was naturally cooled to room temperature to obtain a colorless, transparent solution with a pungent odor; then, the above solution was operated in order as follows: zirconium chloride (ZrCl4) was added, ultrasonicated, then PVP was added, ultrasonicated, then acetic acid was added, and fully mixed; poured into a reactor, the suspension was centrifuged, washed twice with detergent, and finally, dried for 12 hours to obtain a white sample powder UiO-67. In addition, the sample powder needs to be vacuum activated before use; B. Prepare 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / zirconium complex, mix 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid, ZrCl4, and solvent according to a suitable ratio, react, filter, wash, and then dry in vacuum to obtain 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / zirconium complex; mercapto-propylene Michael addition reaction, mix 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / zirconium complex: 2-mercaptoethanol lithium, hexafluorobutyl acrylate, catalyst, and solvent according to a suitable ratio, react, neutralize with dilute hydrochloric acid to pH 7, filter, wash the solid with water, and finally dry in a vacuum oven to obtain an organometallic lithium zirconium precursor; C. First, a certain amount of LiTFSI and organometallic lithium zirconium precursor UiO-67 were dispersed in NMP organic solvent and stirred until the powder was evenly dispersed; then, different proportions of PVB and PVDF-HFP were added to the slurry, stirred overnight at a suitable temperature, and the slurry was evenly coated on a polytetrafluoroethylene plate with a spatula and vacuum dried; finally, the dried electrolyte membrane was cut into discs with a diameter of 18 mm and transferred to a glove box for further use; D. Assemble into a solid-state battery and test its conductivity and discharge specific capacity.

2. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 1, characterized in that: In step A, the mass ratio of DMF to 4,4'-biphenyldicarboxylic acid (BPDC) powder is 0.8-1.2:2.8-3.

2.

3. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 1, characterized in that: In step A, the dissolving heating temperature is 120° C. and the heating time is 15 min.

4. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 1, characterized in that: In step A, 40 parts of zirconium chloride (ZrCl4) are ultrasonically treated for 15 minutes, 100 parts of PVP are added, ultrasonically treated for 15 minutes, and then 80 parts of acetic acid are added.

5. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 1, characterized in that: In step A, the reaction temperature is set at 120° C., and the mixture is naturally cooled to room temperature after reacting for 24 hours.

6. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 1, characterized in that: In step A, the suspension is centrifuged at 8500 rpm for 3 min.

7. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 1, characterized in that: In step A, the detergent is one or both of DMF and ethanol.

8. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 1, characterized in that: In step A, the vacuum activation temperature is set at 150°C.

9. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 1, characterized in that: In step A, the molar ratio of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid: ZrCl4: solvent is 1:1.1-1.5:7-10.

10. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 3, characterized in that: In step A, the solvent is anhydrous methanol or ethanol, the reaction is carried out at 20° C.-65° C. for 30-60 minutes, and the detergent is cold methanol.

11. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 3, characterized in that: In step B, the molar ratio of 2'-amino-[1,1':4',1"-terphenyl]-4,4"-dicarboxylic acid / zirconium complex: lithium 2-mercaptoethanol: hexafluorobutyl acrylate: catalyst: solvent is 1:1.3-1.7:0.02-0.2:0.03-0.07:5-10.

12. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 3, characterized in that: In step B, the solvent is anhydrous ethanol or isopropanol, the catalyst is triethylamine, and the reaction is carried out at 20° C.-65° C. for 30-60 minutes.

13. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 3, characterized in that: In step C, the mass ratio of LiTFSI to the organic metal lithium zirconium precursor UiO-67 is 0.8-1.2:1.9-2.

1.

14. The method for preparing a composite electrolyte for an all-solid-state lithium metal battery using a PVB additive according to claim 3, characterized in that: In step C, the mass ratio of PVB to PVDF-HFP is 0-3:1.

Citation Information

Patent Citations

  • Magnesium metal organic complex and preparation method thereof

    CN108314628A

  • Metal organic framework-polymer composite solid electrolyte as well as preparation method and application thereof

    CN113937363A

  • High-viscosity composite solid electrolyte membrane as well as preparation method and application thereof

    CN117936891A

  • Electrolyte used in electrochemical device

    CN1282989A

  • Electrodes having electrode additive for high performance batteries and applications of same

    WO2020167725A1

Cited By

  • Ionic liquid additive for solid-state lithium metal battery electrolyte and application of ionic liquid additive

    CN119518075A