Lithium ion battery electrolyte and lithium ion battery

The lithium ion battery electrolyte with a film-forming additive and unsaturated bond additive forms a stable, elastic SEI layer on the silicon-carbon electrode, reducing volume expansion and gas production, enhancing the high-temperature cycle and storage performance of silicon-containing electrodes.

CN119092829APending Publication Date: 2024-12-06XIANGHE KUNLUN NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197762.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The volume expansion and contraction of silicon-carbon negative electrodes in lithium-ion batteries during charging and discharging lead to gas production, especially at high temperatures, degrading battery performance and increasing internal resistance, which affects cycle life.

Method used

A lithium ion battery electrolyte containing a lithium salt, solvent, and additives, including a film-forming additive and a carbonate with an unsaturated bond, which forms a stable, dense network organic polymer SEI layer on the battery negative electrode interface, and the inorganic SEI layer on the battery negative electrode interface, and the inorganic SEI formed by other film-forming additives is embedded in the organic polymer skeleton to form a good lithium ion transmission channel with low internal resistance. The SEI layer is elastic, which can effectively reduce the impact of the volume expansion of the silicon-carbon negative electrode, inhibit high-temperature gas production, and improve the high-temperature cycle and high-temperature storage performance of silicon-containing negative electrode batteries.

Benefits of technology

The electrolyte forms a stable, dense organic polymer SEI layer on the battery negative electrode interface, and the inorganic SEI formed by other film-forming additives is embedded in the organic polymer skeleton to form a good lithium ion transmission channel with low internal resistance, and the SEI layer is elastic, which can effectively reduce the impact of the silicon-carbon negative electrode, inhibit high-temperature gas production, and improve the high-temperature cycle and high-temperature storage performance of silicon-containing negative electrode batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092829A_ABST
    Figure CN119092829A_ABST
Patent Text Reader

Abstract

The invention provides a lithium ion battery electrolyte and a lithium ion battery, the lithium ion battery electrolyte comprises a lithium salt, a solvent and an additive, the additive comprises a film-forming additive and an additive A, and the additive A has a structure as shown in a formula I. According to the electrolyte, the additive A which is carbonic ester containing unsaturated bonds is added into the electrolyte and is matched with the film-forming additive, so that the high-temperature cycle and high-temperature storage performance of the silicon-containing negative electrode battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery electrolytes, and in particular relates to a lithium ion battery electrolyte and a lithium ion battery. Background Art

[0002] With the growing global demand for new energy, lithium-ion batteries are widely used in electric vehicles, energy storage systems and other fields due to their high energy density, long cycle life and environmental protection. However, the performance of lithium-ion batteries is greatly affected by their electrolyte. The electrolyte is an important component of lithium-ion batteries, which directly affects the electrochemical performance, safety and stability of the battery. Among them, high-nickel positive electrode silicon-carbon negative electrode batteries are considered to be the first choice for the next generation of lithium-ion batteries due to their high energy density and long cycle life. However, the volume expansion and contraction of the silicon-carbon negative electrode during the charging and discharging process causes the battery to produce gas, especially at high temperatures, where the performance is severely degraded. The existing technical solutions optimize additives to enhance the negative electrode interface protection and reduce gas production, which usually significantly increases the internal resistance (DCIR) of the battery and affects the cycle life. Therefore, a solution to suppress gas production for low internal resistance of silicon-carbon negative electrode batteries needs to be solved urgently. Summary of the invention

[0003] In view of the deficiencies in the prior art, an object of the present invention is to provide a lithium ion battery electrolyte and a lithium ion battery.

[0004] To achieve this object, the present invention adopts the following technical solutions:

[0005] One of the purposes of the present invention is to provide a lithium ion battery electrolyte, the lithium ion battery electrolyte comprising a lithium salt, a solvent and an additive, the additive comprising a film-forming additive and an additive A, the additive A having a structure as shown in the following formula I:

[0006]

[0007] Wherein R1 is selected from substituted or unsubstituted C1-C3 straight chain alkane groups, and the substituents in the substituted C1-C3 alkane groups are selected from halogens; two R1s are the same or different;

[0008] R3 and R4 are independently selected from substituted or unsubstituted C1-C3 straight-chain alkylene groups, wherein the substituents in the substituted C1-C3 straight-chain alkylene groups are selected from halogens;

[0009] R2 is selected from substituted or unsubstituted C1-C5 straight or branched alkane groups, and the substituents in the substituted C1-C5 alkane groups are selected from halogens.

[0010] In the present invention, by using carbonate containing unsaturated bonds as additives, the carbonate has good chemical stability and thermal stability, and can form a stable, dense network organic polymer SEI layer skeleton on the battery negative electrode interface, and the inorganic SEI formed by other film-forming additives is embedded in the organic polymer skeleton to form a good lithium ion transmission channel with low internal resistance. In addition, the SEI layer is elastic, which can effectively reduce the impact of the volume expansion of the silicon-carbon negative electrode, inhibit high-temperature gas production, and improve the high-temperature cycle and high-temperature storage performance of silicon-containing negative electrode batteries.

[0011] Preferably, R1 is independently selected from the following groups or the following groups substituted with halogen: CH3-, CH3-CH2- or CH3-CH2-CH2-.

[0012] Preferably, R3 and R4 are independently selected from any one of -CH2-, -CH2-CH2-, or -CH2-CH2-CH2-.

[0013] Preferably, R2 is independently selected from the following groups or the following groups substituted with halogen: CH3-, CH3-CH2-, CH3-CH2-CH2-, CH3-CH2-CH2-CH2-, CH3-CH2-CH2-CH2-CH2-, -CH2(CH3)2, -CH2 CH2(CH3)2, -CH2(CH3)(CH2CH3), -CH2(CH2CH3)2 or -CH2(CH3)(CH2CH2CH3).

[0014] In the present invention, the halogen is selected from F, Cl, Br or I, preferably F.

[0015] Preferably, the additive A is any one of the following compounds:

[0016]

[0017] More preferably, the additive A is

[0018] In the present invention, the preparation method of the additive A comprises the following steps:

[0019] (1) reacting the compound represented by formula II with alcohol R1-OH and carbon dioxide in the presence of a composite catalyst to obtain butyne dicarbonate, wherein the composite catalyst is a combination of a metal and a metal oxide;

[0020] (2) adding an olefin compound represented by formula III to the reaction solution of step (1) to react to obtain additive A;

[0021]

[0022] Preferably, the mass ratio of the metal to the metal oxide in the composite catalyst is 1:(1-4), such as 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5 or 1:4, preferably 1:3.

[0023] Preferably, the metal in the composite catalyst is selected from any one of Fe, Ni, Cu, Zn, Mn or Sn, or a combination of at least two thereof.

[0024] Preferably, the metal oxide in the composite catalyst is selected from any one of Fe3O4, MnO2, CuO, Al2O3, MgO or V2O5, or a combination of at least two thereof.

[0025] Preferably, the amount of the composite catalyst used in step (1) is 0.2-5% by mass of the compound represented by formula II, for example 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 5%, preferably 3.5%.

[0026] Preferably, the molar ratio of the compound represented by formula II in step (1) to the alcohol R1-OH is 1:(2-2.5), for example 1:2, 1:2.1, 1:2.2, 1:2.3, 1:2.4 or 1:2.5, preferably 1:2.2.

[0027] In step (1), the carbon dioxide is added into the reaction system by gas introduction.

[0028] Preferably, the reaction in step (1) is carried out at a pressure of 0.5-5 MPa; for example, 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, 4 MPa or 5 MPa.

[0029] Preferably, the reaction temperature in step (1) is 80-120°C, for example 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C or 120°C.

[0030] Preferably, the reaction time of step (1) is 2-4 h, for example 2 h, 2.5 h, 3 h, 3.5 h or 4 h.

[0031] Preferably, the molar ratio of the olefin compound represented by formula III in step (2) to the compound represented by formula II in step (1) is (1-1.2):1, for example, 1:1, 1.01:1, 1.05:1, 1.1:1 or 1.2:1, preferably 1.05:1.

[0032] Preferably, the reaction temperature in step (2) is 70-90°C, such as 70°C, 75°C, 80°C, 85°C, or 90°C.

[0033] Preferably, the reaction time of step (2) is 2-4 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h.

[0034] Preferably, the reaction in step (2) is carried out at a pressure of 0.5-5 MPa, for example 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, 4 MPa or 5 MPa.

[0035] After the reaction in step (2) is completed, the reaction solution is filtered and the filtrate is purified by distillation to obtain purified compound A.

[0036] Preferably, the mass percentage of the additive A in the lithium ion battery electrolyte is 0.1-10%, such as 0.1%, 0.2%, 0.5%, 1%, 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%. As well as specific point values ​​between the above point values, the present invention will no longer exhaustively list the specific point values ​​included in the above range due to space limitations and for the sake of simplicity.

[0037] In the present invention, if the amount of additive A added is too small, when applied to a lithium-ion battery, a sufficiently stable organic SEI layer skeleton cannot be formed on the surface of the electrode material, and the structural stability of the silicon-containing negative electrode material is insufficient, which leads to poor final cycle performance of the battery; if the amount of additive A added is too high, the organic SEI layer formed on the surface of the electrode material is thicker, which affects the lithium ion transmission on the one hand, and consumes too many lithium ions on the other hand, affecting the coulombic efficiency of the lithium-ion battery and reducing the cycle life.

[0038] Preferably, the film-forming additive B includes one or a combination of at least two of carbonates, sulfates, phosphoric acids, borics, silanes, fluorocarbons, fluorosulfates, fluorophosphoric acids, fluoroborics or fluorosilanes.

[0039] In the present invention, the film-forming additive B refers to an additive that forms a solid electrolyte interface (SEI film). During the first charge and discharge process of a lithium-ion battery, the film-forming additive reacts with the electrode material and the electrolyte at the solid-liquid interface to form a passivation film covering the surface of the electrode material, namely, the SEI film. The SEI film is an electronic insulator and also a Li + Excellent conductor, Li + It can be freely embedded and removed through the SEI film. The SEI film protects the electrode material, making the material structure less likely to collapse, thereby increasing the cycle life of the electrode material.

[0040] Preferably, the film-forming additive B includes one or a combination of at least two of vinylene carbonate, 1,3-propane sultone, fluoroethylene carbonate, vinyl sulfate, tris(trimethylsilyl)phosphate or tris(trimethylsilyl)borate.

[0041] In the present invention, the combination of the film-forming additive B includes, for example, a combination of vinylene carbonate and fluoroethylene carbonate, a combination of vinylene carbonate and vinyl sulfate, or a combination of vinylene carbonate, 1,3-propane sultone and fluoroethylene carbonate.

[0042] Preferably, the mass percentage of the film-forming additive B in the lithium-ion battery electrolyte is 0.1-15%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.6%, 2%, 2.5%, 3%, 3.5%, 4%, 5%, 6%, 8%, 10%, 12% or 15%.

[0043] Preferably, the lithium salt includes one or a combination of at least two of lithium hexafluorophosphate, lithium bisoxalatoborate, lithium difluorooxalatoborate, lithium bis-(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium tetrafluoroborate or lithium difluorobisoxalatophosphate.

[0044] Preferably, the mass percentage of the lithium salt in the lithium ion battery electrolyte is 8% to 16%, for example, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5% or 16%.

[0045] Preferably, the solvent is an organic solvent.

[0046] In the present invention, the total weight of the lithium ion battery electrolyte is 100%, and the balance except for the lithium salt, the film-forming additive and the compound A is the solvent.

[0047] Preferably, the solvent comprises a carbonate-based organic solvent.

[0048] Preferably, the carbonate organic solvent includes any one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, propyl acetate, methyl acetate, ethyl propionate or propyl propionate, or a combination of at least two thereof.

[0049] In the present invention, the preparation method of the lithium ion battery electrolyte comprises the following steps: firstly, adding lithium salt into a solvent to dissolve the lithium salt, then adding a film-forming additive and an additive A, and mixing them uniformly.

[0050] A second object of the present invention is to provide a lithium ion battery, wherein the lithium ion battery comprises the lithium ion battery electrolyte as described above.

[0051] Preferably, the lithium ion battery comprises a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and the lithium ion battery electrolyte as described above.

[0052] Preferably, the lithium-ion battery is a silicon-containing negative electrode secondary battery.

[0053] Preferably, the positive electrode and the negative electrode include an active material, a conductive agent, a current collector and a binder, and the binder combines the active material with the conductive agent and the current collector.

[0054] In the present invention, the preparation method of the lithium ion battery comprises:

[0055] Mixing positive electrode active material, positive electrode binder, conductive agent and conductive additive to form positive electrode slurry;

[0056] A negative electrode material, a conductive additive (such as conductive carbon black), a binder (such as styrene-butadiene rubber) and an optional thickener (such as carboxymethyl cellulose) are mixed to form a negative electrode slurry;

[0057] Then, the positive electrode slurry is coated on the positive electrode current collector, and the negative electrode slurry is coated on the negative electrode current collector, and dried to obtain a positive electrode sheet and a negative electrode sheet;

[0058] The positive electrode sheet and the negative electrode sheet are packaged with a separator, and after drying, an electrolyte is injected, and the lithium-ion battery is obtained after formation.

[0059] Unless otherwise required in this application, the words "including" and "comprising" should be construed in an open, inclusive sense, ie, "including, but not limited to."

[0060] Compared with the prior art, the present invention has the following beneficial effects:

[0061] The present invention adds an additive A, a carbonate containing an unsaturated bond, to the electrolyte. Since the carbonate has good chemical stability and thermal stability, a stable and dense network organic polymer SEI layer skeleton can be formed on the battery negative electrode interface. The inorganic SEI formed by other film-forming additives is embedded in the organic polymer skeleton to form a good lithium ion transmission channel with low internal resistance. In addition, the SEI layer is elastic, which can effectively reduce the impact of the volume expansion of the silicon-carbon negative electrode, inhibit high-temperature gas production, and improve the high-temperature cycle and high-temperature storage performance of silicon-containing negative electrode batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 This is the H NMR spectrum of the carbonate of formula 1-1. DETAILED DESCRIPTION

[0063] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0064] Raw materials used in Examples 1-10 and Comparative Examples 1-2:

[0065] Solvent: The mass ratio of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) is 3:7;

[0066] Lithium salt: lithium hexafluorophosphate (LiPF6);

[0067] Film-forming additive: fluorovinylene carbonate (FEC);

[0068] About Additive A:

[0069] Examples 1 to 3 use compound A as shown in formula 1-1;

[0070]

[0071] The preparation method is as follows:

[0072] Add 100g 1,4-butynediol, 82g methanol, 3.5g composite catalyst (including metal Ni and metal oxide CuO) to the reactor, the mass ratio of metal: metal oxide in the composite catalyst is 1:3. Fill with carbon dioxide gas to 1.6MPa, heat to 110℃ and react at constant temperature and pressure for 3 hours. Release the pressure after the reaction. Add 120g 1-heptene to the reactor, flush with air and pressurize to 0.9MPa, heat to 85℃, and react at constant temperature and pressure for 3 hours. After the reaction, cool to room temperature and filter, and purify the filtrate by distillation. Obtain 326.2g of formula 1-1 carbonate, with a yield of 93.6% and a purity of 99.97%.

[0073] The product has a hydrogen nuclear magnetic resonance spectrum (instrument model Bruker AVANCE NEO 600MHz), a hydrogen spectrum (the deuterated reagent used is deuterated dimethyl sulfoxide) as shown in Figure 1 As shown, 1H NMR: δppm 0.87(3H,t,J=7.0Hz),1.23-1.48(4H,1.29(h,J=7.0Hz),1.41(tt,J=7.4, 7.0Hz)),1.97(2H,q,J=7.4Hz),2.66(2H,d,J=7.4Hz),3.77-3.87(6H,3.82 (s),3.82(s)),4.59-4.74(4H,4.65(d,J=6.6Hz),4.69(s)),5.35-5.56(3 H, 5.42 (dt, J = 15.7, 7.4Hz), 5.48 (dt, J = 15.7, 7.4Hz), 5.46 (t, J = 6.6Hz)).

[0074] Example 4 uses compound A as shown in formula 1-2;

[0075]

[0076] The preparation method comprises the following steps:

[0077] Add 100g 1,4-butynediol, 82g methanol, 3.5g composite catalyst (including metal Ni and metal oxide MnO2) to the reactor, the mass ratio of metal: metal oxide in the composite catalyst is 1:3. Fill carbon dioxide gas to 1.6MPa, heat to 80℃ and react at constant temperature and pressure for 4 hours. Release the pressure after the reaction. Add 70g 1-butene to the reactor, flush with air and pressurize to 2MPa, heat to 90℃, and react at constant temperature and pressure for 2 hours. After the reaction, cool to room temperature and filter, and purify the filtrate by distillation to obtain 278.2g of formula 1-2 carbonate, with a yield of 92.8% and a purity of 99.95%.

[0078] The H NMR spectrum of the product (instrument model Bruker AVANCE NEO 600 MHz, the deuterated reagent used is deuterated dimethyl sulfoxide) data are as follows: 1 H NMR: δppm 1.53(3H,d,J=7.2Hz),2.65(2H,d,J=7.4Hz),3.77-3.87(6H,3.82(s),3.82(s)),4.59-4.74(4H,4.65(d,J= 6.6Hz), 4.69 (s)), 5.32-5.52 (3H, 5.39 (dq, J = 15.7, 7.2Hz), 5.41 (dt, J = 15.7, 7.4Hz), 5.46 (t, J = 6.6Hz)).

[0079] Example 5 uses compound A as shown in formula 1-3;

[0080]

[0081] The preparation method comprises the following steps:

[0082] Add 100g 1,4-butynediol, 118g ethanol, 3.5g composite catalyst (including metal Fe and metal oxide Fe3O4) to the reactor, the mass ratio of metal: metal oxide in the composite catalyst is 1:1. Fill with carbon dioxide gas to 3MPa, heat to 100℃ and react at constant temperature and pressure for 2 hours. Release the pressure after the reaction. Add 86g 1-pentene to the reactor, flush with air and pressurize to 4MPa, heat to 90℃, and react at constant temperature and pressure for 2 hours. After the reaction, cool to room temperature and filter, and purify the filtrate by rectification. Obtain 312g of formula 1-3 carbonate, with a yield of 89.5% and a purity of 99.81%.

[0083] The H-NMR spectrometer of the product was Bruker AVANCE NEO 600 MHz, and the deuterated reagent used was deuterated dimethyl sulfoxide (DMSO). The data are as follows: 1 H NMR: δppm 1.09(3H,t,J=7.5Hz),1.18-1.32(6H,1.24(t,J=7.1Hz),1.26(t,J=7.1Hz)),2 .07(2H,qd,J=7.5,6.9Hz),2.66(2H,d,J=7.4Hz),4.22-4.33(4H,4.27(q,J=7.1 Hz),4.28(q,J=7.1Hz)),4.59-4.74(4H,4.65(d,J=6.6Hz),4.69(s)),5.31-5. 55(3H, 5.39(dt,J=15.7,6.9Hz), 5.47(dt,J=15.7,7.4Hz), 5.46(t,J=6.6Hz)).

[0084] Example 6 uses compound A as shown in formula 1-4;

[0085]

[0086] The preparation method comprises the following steps:

[0087] Add 133g 1,4-hexynediol, 82g methanol, 4.7g composite catalyst (including metal Sn and metal oxide MgO) to the reactor, the mass ratio of metal: metal oxide in the composite catalyst is 1:3. Fill with carbon dioxide gas to 1.6MPa, heat to 110℃ and react at constant temperature and pressure for 3 hours. Release the pressure after the reaction is completed. Add 86g 1-pentene to the reactor, flush with air and pressurize to 0.9MPa, heat to 85℃, and react at constant temperature and pressure for 3 hours. After the reaction is completed, cool to room temperature and filter, and purify the filtrate by distillation to obtain 326.2g of formula 1-4 carbonate, with a yield of 93.6% and a purity of 99.97%.

[0088] The H NMR spectrum of the product (instrument model Bruker AVANCE NEO 600 MHz, the deuterated reagent used is deuterated dimethyl sulfoxide) data are as follows: 1 H NMR: δppm 1.09(3H,t,J=7.5Hz),2.07(2H,qd,J=7.5,6.9Hz),2.49-2.70(6H,2.55(t,J= 7.4Hz),2.57(td,J=7.4,7.2Hz),2.64(d,J=7.4Hz)),3.77-3.87(6H,3.82(s) ,3.82(s)),4.38-4.52(4H,4.44(t,J=7.4Hz),4.46(t,J=7.4Hz)),5.31-5.47 (3H, 5.37 (t, J = 7.2Hz), 5.39 (dt, J = 15.7, 6.9Hz), 5.40 (dt, J = 15.7, 7.4Hz)).

[0089] Example 7 uses compound A as shown in formula 1-1 and compound C as shown in formula 2-1 in a mass ratio of 1:1;

[0090]

[0091] The preparation method of the compound represented by formula 2-1 is as follows:

[0092] Add 100g 1,4-butynediol, 128g fluoromethanol, 3.5g composite catalyst (including metal Ni and metal oxide V2O5) to the reactor, the mass ratio of metal: metal oxide in the composite catalyst is 1:3. Fill with carbon dioxide gas to 1.6MPa, heat to 110℃ and react at constant temperature and pressure for 3 hours. Release the pressure after the reaction. Add 86g 1-pentene to the reactor, flush with air and pressurize to 0.9MPa, heat to 85℃, and react at constant temperature and pressure for 3 hours. After the reaction, cool to room temperature and filter, and purify the filtrate by distillation. Obtain 323.6g of formula 2-1 carbonate, with a yield of 90.4% and a purity of 99.83%.

[0093] The H NMR spectrum of the product (instrument model Bruker AVANCE NEO 600 MHz, the deuterated reagent used is deuterated dimethyl sulfoxide) data are as follows: 1 H NMR: δppm 1.09(3H,t,J=7.5Hz),2.07(2H,qd,J=7.5,6.9Hz),2.66(2H,d,J=7.4Hz),4 .28-4.41(4H,4.34(t,J=6.6Hz),4.35(t,J=6.6Hz)),4.49-4.74(8H,4.55( t,J=6.6Hz),4.55(t,J=6.6Hz),4.65(d,J=6.6Hz),4.69(s)),5.31-5.55(3 H, 5.39 (dt, J = 15.7, 6.9 Hz), 5.47 ( dt, J = 15.7, 7.4 Hz), 5.46 ( t, J = 6.6 Hz)).

[0094] Example 8 uses compound A as shown in formula 1-2 and compound C as shown in formula 2-2 in a mass ratio of 1:1;

[0095]

[0096] The preparation method of the compound shown in formula 2-2 is as follows:

[0097] Add 100g 1,4-butynediol, 82g methanol, 3.5g composite catalyst (including metal Zn and metal oxide V2O5) to the reactor, the mass ratio of metal: metal oxide in the composite catalyst is 1:3. Fill with carbon dioxide gas to 1.6MPa, heat to 110℃ and react at constant temperature and pressure for 3 hours. Release the pressure after the reaction. Add 86g 5,5,5-trifluoro-1-pentene to the reactor, flush with air and pressurize to 0.9MPa, heat to 85℃, and react at constant temperature and pressure for 3 hours. After the reaction, cool to room temperature and filter, and purify the filtrate by distillation. Obtain 343.6g of formula 2-2 carbonate, with a yield of 90.7% and a purity of 99.85%.

[0098] The H NMR spectrum of the product (instrument model Bruker AVANCE NEO 600 MHz, the deuterated reagent used is deuterated dimethyl sulfoxide) data are as follows: 1H NMR: δppm 2.31(2H,d,J=6.5Hz),2.70(2H,d,J=7.4Hz),3.77-3.87(6H,3.82(s),3.82(s)),4.59-4.74(4H,4.65(d,J= 6.6Hz), 4.69 (s)), 5.40-5.66 (3H, 5.46 (t, J = 6.6Hz), 5.49 (dt, J = 15.7, 6.5Hz), 5.58 (dt, J = 15.7, 7.4Hz)).

[0099] In Example 9, compound C represented by formula 2-1 was used.

[0100] In Example 10, compound C represented by formula 2-2 is used.

[0101] Embodiment 11

[0102] Compound A represented by Formula 1-1 was used, and the film-forming additive was replaced by 1,3-propane sultone. The selection of other substances was the same as that in Example 1.

[0103] Example 12

[0104] Compound A shown in Formula 1-1 was used, and the film-forming additive was replaced with vinyl sulfate. The selection of other substances was the same as in Example 1.

[0105] Embodiment 13

[0106] Compound C represented by Formula 2-1 was used, and the film-forming additive was replaced by tris(trimethylsilyl)phosphate. The selection of other substances was the same as that in Example 1.

[0107] Embodiment 14

[0108] Compound C shown in Formula 2-1 is used, and the film-forming additive is replaced with tris(trimethylsilyl)borate, and the selection of other substances is the same as in Example 1

[0109] Comparative Example 1 does not use compound A;

[0110] In Comparative Example 2, an excess amount of compound A represented by Formula 1-1 was used.

[0111] The amounts of each raw material added in the electrolytes of Examples 1 to 8 and Comparative Examples 1 to 2 are shown in Table 1.

[0112] Table 1

[0113]

[0114]

[0115] The lithium ion battery electrolyte prepared in Examples 1 to 8 and Comparative Examples 1-2 is used to prepare a lithium ion battery, and the preparation method is as follows:

[0116] Nickel cobalt manganese oxide (NCM811), positive electrode binder (PVDF), carbon (C) and conductive carbon black (Super-P) were mixed in a mass ratio of 95.5:2:1:1.5, and N-methylpyrrolidone (NMP) solvent was added to prepare a positive electrode slurry with a solid content of 50%;

[0117] Silicon carbon (SiC), conductive carbon black (Super-P), carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 95.9:0.5:1.5:2.1, and water was added as a solvent to prepare a negative electrode slurry with a solid content of 40%;

[0118] The positive electrode slurry is coated on the aluminum foil current collector, and the negative electrode slurry is coated on the copper foil current collector, and after drying, the positive electrode sheet and the negative electrode sheet are obtained;

[0119] Then the positive electrode sheet and the negative electrode sheet were packaged with a polyethylene separator, dried, and injected with 6.5 g of the electrolyte prepared in Examples 1 to 8 and Comparative Examples 1 to 2. After formation, the lithium-ion battery was obtained, and its electrical properties were tested.

[0120] Performance Testing:

[0121] (1) 45°C cycle capacity retention rate: The prepared lithium-ion battery was placed at room temperature and connected to a battery testing system (Xinwei testing system CT-ZWJ-4'S-T-1U). After charging to 4.2 V at 1C (the charging cut-off current was 0.05C), it was discharged to 2.75 V at 1C. The charge and discharge process was repeated for 800 cycles to test the capacity retention rate of the lithium-ion battery.

[0122] (2) 60℃ high temperature storage: The prepared lithium-ion battery was placed at room temperature and connected to a battery test system (Xinwei test system CT-ZWJ-4'S-T-1U). After charging to 4.2V at 1C (charging cut-off current is 0.05C), it was placed in a 60℃ oven for constant temperature storage. After 7 days, it was taken out and cooled to room temperature. The capacity retention rate and internal resistance (DCIR) of the lithium-ion battery were tested. The volume of the battery before and after storage was measured by the drainage method, and the volume difference was the gas production.

[0123] The test results of lithium ion batteries prepared using the lithium ion battery electrolytes prepared in Examples 1 to 8 and Comparative Examples 1 to 2 are shown in Table 2.

[0124] Table 2

[0125]

[0126] It can be seen that the lithium-ion battery electrolyte of the present invention can make the battery's 45°C cycle capacity retention rate above 85%, 60°C 7-day capacity retention rate above 92%, 60°C 7-day DCIR growth rate below 5.5%, 60°C 7-day gas production below 1.2 cm 3 Compared with the comparative example, the high temperature cycle and high temperature storage performance of silicon-containing negative electrode batteries are significantly improved when compound A is added in a reasonable amount.

[0127] The applicant declares that the present invention illustrates the lithium-ion battery electrolyte and lithium-ion battery of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A lithium ion battery electrolyte, characterized in that: The lithium-ion battery electrolyte comprises a lithium salt, a solvent and an additive, wherein the additive comprises an additive A and a film-forming additive B, and the additive A has a structure as shown in the following formula I: Wherein R1 is selected from substituted or unsubstituted C1-C3 straight chain alkane groups, and the substituents in the substituted C1-C3 alkane groups are selected from halogens; two R1s are the same or different; R3 and R4 are independently selected from substituted or unsubstituted C1-C3 straight-chain alkylene groups, wherein the substituents in the substituted C1-C3 straight-chain alkylene groups are selected from halogens; R2 is selected from substituted or unsubstituted C1-C5 straight or branched alkane groups, and the substituents in the substituted C1-C5 alkane groups are selected from halogens.

2. The lithium ion battery electrolyte according to claim 1, characterized in that: The R1 is independently selected from the following groups or the following groups substituted with halogen: CH3-, CH3-CH2- or CH3-CH2-CH2-. Preferably, R3 and R4 are independently selected from any one of -CH2-, -CH2-CH2-, or -CH2-CH2-CH2-. Preferably, R2 is independently selected from the following groups or the following groups substituted with halogen: CH3-, CH3-CH2-, CH3-CH2-CH2-, CH3-CH2-CH2-CH2-, CH3-CH2-CH2-CH2-CH2-, -CH2(CH3)2, -CH2 CH2(CH3)2, -CH2(CH3)(CH2CH3), -CH2(CH2CH3)2 or -CH2(CH3)(CH2CH2CH3).

3. The lithium ion battery electrolyte according to claim 1 or 2, characterized in that: The additive A is any one of the following compounds: More preferably, the additive A is 4. The lithium ion battery electrolyte according to any one of claims 1 to 3, characterized in that: The mass percentage of the additive A in the lithium ion battery electrolyte is 0.1-10%.

5. The lithium ion battery electrolyte according to any one of claims 1 to 4, characterized in that: The film-forming additive B comprises one or a combination of at least two of carbonates, sulfates, phosphoric acids, borics, silanes, fluorocarbons, fluorosulfates, fluorophosphoric acids, fluoroborics or fluorosilanes; Preferably, the film-forming additive B includes one or a combination of at least two of vinylene carbonate, 1,3-propane sultone, fluoroethylene carbonate, vinyl sulfate, tris(trimethylsilyl)phosphate or tris(trimethylsilyl)borate.

6. The lithium ion battery electrolyte according to any one of claims 1 to 5, characterized in that: The mass percentage of the film-forming additive B in the lithium-ion battery electrolyte is 0.1-15%.

7. The lithium ion battery electrolyte according to any one of claims 1 to 6, characterized in that: The lithium salt includes one or a combination of at least two of lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium tetrafluoroborate or lithium difluorobis(oxalatophosphate); Preferably, the mass percentage of the lithium salt in the lithium ion battery electrolyte is 8% to 16%.

8. The lithium ion battery electrolyte according to any one of claims 1 to 7, characterized in that: The solvent is an organic solvent; Preferably, the solvent comprises a carbonate organic solvent; Preferably, the carbonate organic solvent includes any one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, propyl acetate, methyl acetate, ethyl propionate or propyl propionate, or a combination of at least two thereof; Preferably, the total weight of the lithium-ion battery electrolyte is 100%, and the balance, except for the lithium salt, the film-forming additive and the compound A, is the solvent.

9. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium-ion battery electrolyte according to any one of claims 1 to 8.

10. The lithium ion battery according to claim 9, characterized in that: The lithium ion battery comprises a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and a lithium ion battery electrolyte according to any one of claims 1 to 8. Preferably, the lithium-ion battery is a secondary battery containing a silicon negative electrode; Preferably, the positive electrode and the negative electrode respectively include an active material, a conductive agent, a current collector and a binder.