Modification and performance research of aqueous zinc ion battery electrolyte

By adding L-lactic acid as an additive for multipolar functional groups to the electrolyte of aqueous zinc ion batteries, the problems of growth dendrites, hydrogen evolution reactions and zinc anode corrosion are solved, which significantly improves the cycle life and electrochemical performance of the battery and simplifies the The operation process is completed.

CN119092846APending Publication Date: 2024-12-06JILIN INST OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411186965.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Water-based zinc ion batteries cause battery failure due to problems such as dendrites, hydrogen evolution reactions and zinc anode corrosion, and hydrogen generated by water decomposition seriously damages the battery, resulting in expansion and explosion.

Method used

Add L-lactic acid as an electrolyte additive to act as a multipolar functional group to improve the environment between the interface between the zinc anode and the electrolyte, reduce water activity through carboxyl and hydroxyl functional groups, inhibit the production of by-products, and inhibit water activity through hydrogen bonds .

Benefits of technology

Under the condition of current density of 1 mA·cm−2 and surface capacity of 1 mAh·cm−2, the cycle life increased from 80 h to 1600 h, which significantly improved the electrochemical performance of aqueous zinc ion batteries and simplified the operation process .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092846A_ABST
    Figure CN119092846A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of water-based zinc ion battery zinc negative electrode protection, and provides a method for adding a common and easily available reagent L-lactic acid (LA) as an additive into a water-based zinc ion battery in order to solve the problems of zinc dendrites, poor cycling stability, hydrogen evolution reaction and the like in the water-based zinc ion battery. According to the specific scheme, the LA additive is added into the zinc sulfate electrolyte, and compared with a battery without the additive, a battery using the electrolyte shows excellent performance, such as good cycle reversibility and interface stability, so that the problems of capacity fading, cycle instability and the like caused by new zinc dendritic crystal growth are solved, and the service life of the battery is prolonged. And the purpose of promoting the development and commercial application of the aqueous zinc ion battery is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of zinc negative electrode protection for aqueous zinc electrolysis, and in particular to an aqueous zinc electrolysis electrolyte additive. Background Art

[0002] Aqueous zinc-ion batteries (AZIBs) are used as a promising candidate due to their higher capacity density (5855 mAh∙cm for Zn anode). −3 , Li anode is 2061 mAh∙cm −3 ), more environmentally friendly, lower cost and looser assembly conditions will become the mainstream of future development. However, the development of AZIB is mainly limited by irregular dendrite growth, hydrogen evolution reaction and corrosion reaction. At the same time, the hydrogen produced by water decomposition during battery operation will seriously damage the battery itself and cause the battery to swell and explode.

[0003] In order to solve these problems, a large number of modification strategies have been proposed, such as coating a protective layer, applying a gel polymer electrolyte, utilizing a low eutectic solvent, and using electrolyte additives. Among them, the use of organic electrolyte additives is a common and effective method to optimize the internal environment of the battery. By forming a layer of SEI film on the surface of the zinc anode to isolate the contact between the electrode and the electrolyte, the occurrence of side reactions is fundamentally suppressed. Lactic acid is a colorless liquid that is easily soluble in water and has functional groups such as carboxyl and hydroxyl groups. LA can improve the environment of the Zn / electrolyte interface from multiple directions. Carboxyl groups can change the solvation structure, reduce the activity of water and inhibit the generation of by-products. Hydroxyl groups can make it preferentially adsorbed with the zinc anode, playing the role of electrostatic shielding and induced deposition. In addition, hydroxyl groups provide a large number of hydrogen bond donors for water molecules, which can inhibit the activity of water. Summary of the invention

[0004] In view of this, the purpose of the present invention is to solve the battery failure caused by the growth of dendrites, hydrogen evolution reaction, zinc anode corrosion and other problems in aqueous zinc ion batteries. The present invention adopts a simple and quick method to add L-lactic acid as an electrolyte additive to the electrolyte to improve the electrochemical performance of aqueous zinc ion batteries. At a current density of 1 mA∙cm -2 , with an area capacity of 1 mAh∙cm -2 Under these conditions, the cycle life can be increased from 80 h to 1600 h.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The present invention provides a method for modifying an aqueous electrolyte, and introduces multipolar functional groups into a zinc sulfate electrolyte. The concentration of the additive L-lactic acid added to the electrolyte of the present invention is 1 mol / L; The electrolyte added in the present invention should include one or more of zinc sulfate, zinc chloride, zinc nitrate or trifluoromethane zinc sulfate.

[0006] The concentration of the electrolyte added in the present invention is 1 mol / L.

[0007] The steps for assembling an aqueous zinc ion battery using the mixed electrolyte configured as above are as follows: Zn||Zn symmetric battery The symmetric battery uses high-purity zinc foil as electrodes after polishing and ultrasonic treatment, and the diaphragm is glass fiber; The Zn||Cu asymmetric battery uses high-purity zinc foil as the negative electrode after ultrasonic polishing, high-purity copper foil as the positive electrode, and the separator is glass fiber; The Zn||PTO full battery uses high-purity zinc foil as the negative electrode after ultrasonic polishing, and PTO as the positive electrode.

[0008] Compared with the prior art, this invention has the following benefits: The present invention introduces an additive with multipolar functional groups into the basic electrolyte. The environment of the Zn / electrolyte interface can be improved from multiple directions. The carboxyl group can change the solvation structure, reduce the activity of water and inhibit the generation of by-products. The hydroxyl group can make it preferentially adsorbed with the zinc anode, play the role of electrostatic shielding and induced deposition. In addition, the hydroxyl group provides a large number of hydrogen bond donors for water molecules, which can inhibit the activity of water. Thereby improving the electrochemical performance of the aqueous zinc ion battery. At the same time, the operation process is simple and fast, which is conducive to commercial use. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 Comparison of the battery cycling performance of Zn||Zn symmetric batteries in different electrolyte systems.

[0010] Figure 2 The constant current charge-discharge cycle curve of the Zn||Zn symmetric battery; the additive concentration in the electrolyte is 1 mol / L, and the current density is 1 mA∙cm -2 ; Figure 3 The results of the experiments are shown in Figure 2 for different electrolyte systems at a current density of 1 mA∙cm -2 , discharge depth is 1 mAh∙cm -2 X-ray diffraction (XRD) spectrum of byproducts on the surface of the negative electrode after 80 cycles under the same conditions; Figure 4 The constant current charge-discharge cycle curve of the Zn||Zn symmetric battery; the additive concentration in the electrolyte is 1 mol / L, and the current density is 5 mA∙cm -2 ; Figure 5 This is a scanning electron microscope (SEM) image of a Zn||Zn symmetric battery after 80 cycles; Figure 6 The cycling performance curve of Zn||PTO full battery at 1 A∙g -1Current density discharge; DETAILED DESCRIPTION

[0011] The present invention is described in more detail below in combination with specific implementation modes and drawings to facilitate understanding of the technical solution of the present invention, but is not intended to limit the protection scope of the present invention.

[0012] Example 1: Preparation of negative electrode: Grind the zinc sheet with 2000-mesh sandpaper, place it in an ethanol solution, ultrasonicate for 5 min, and dry it in a 60°C oven.

[0013] Preparation of electrolyte: Add 1 mol / L LA to 2 mol / L zinc sulfate solution, stir and mix well to obtain a mixed electrolyte.

[0014] The battery is assembled in the following steps: negative electrode shell, negative electrode sheet, glass fiber fully soaked in mixed electrolyte, positive electrode sheet, gasket, spring sheet, positive electrode shell and the like.

[0015] In this example, Zn||Zn symmetric batteries assembled in mixed electrolyte systems with different concentrations were tested at a current density of 5 mA∙cm -2 , discharge depth is 5 mAh∙cm -2 Cycle under the conditions, Figure 1 It can be seen that the cycle performance is best when the additive concentration is 1 mol / L. Example

[0016] Preparation of negative electrode: Grind the zinc sheet with 2000-mesh sandpaper, place it in an ethanol solution, ultrasonicate for 5 min, and dry it in a 60°C oven.

[0017] Preparation of electrolyte: Add 1 mol / L LA to 2 mol / L zinc sulfate solution, stir and mix well to obtain a mixed electrolyte.

[0018] The battery is assembled in the following steps: negative electrode shell, negative electrode sheet, glass fiber fully soaked in mixed electrolyte, positive electrode sheet, gasket, spring sheet, positive electrode shell and the like.

[0019] In this example, the assembled Zn||Zn symmetric battery was charged at 1 mA∙cm -2 The cycle life was 1600 h. Figure 3 This is the XRD image after 80 cycles of this embodiment, indicating that the addition of LA can effectively inhibit the generation of by-products. Figure 4 The current density of the Zn||Zn symmetric cell is 5 mA∙cm -2 , discharge depth is 5 mAh∙cm -2From the constant current charge and discharge curve under the conditions, it can be seen that the addition of LA has excellent cycle performance. Example

[0020] Preparation of negative electrode: Grind the zinc sheet with 2000-mesh sandpaper, place it in an ethanol solution, ultrasonicate for 5 min, and dry it in a 60°C oven.

[0021] Preparation of electrolyte: Add 1 mol / L LA to 2 mol / L zinc sulfate solution, stir and mix well to obtain a mixed electrolyte.

[0022] The battery is assembled in the following steps: negative electrode shell, negative electrode sheet, glass fiber fully soaked in mixed electrolyte, positive electrode sheet, gasket, spring sheet, positive electrode shell and the like.

[0023] The battery was disassembled after 80 cycles, and the negative electrode was cleaned and then subjected to SEM testing.

[0024] After testing this embodiment, Figure 5 a is the SEM image of the zinc anode surface without additives, showing obvious zinc dendrites and collapse on the surface; Figure 5 b is the SEM image of the zinc anode surface with LA additive. It can be seen that the surface is relatively flat without large-scale collapse.

[0025] Example 4: Preparation of positive electrode: Commercial PTO powder, Ketjen black and binder PTFE were mixed in acetone solution at a mass ratio of 6:3:1 and coated on a stainless steel mesh. After drying at 80 °C for 12 h, a PTO cathode was obtained.

[0026] Preparation of negative electrode: Grind the zinc sheet with 2000-mesh sandpaper, place it in an ethanol solution, ultrasonicate for 5 min, and dry it in a 60°C oven.

[0027] Preparation of electrolyte: Add 1 mol / L LA to 2 mol / L zinc sulfate solution, stir and mix well to obtain a mixed electrolyte.

[0028] The battery is assembled in the following steps: negative electrode shell, negative electrode sheet, glass fiber fully soaked in mixed electrolyte, positive electrode sheet, gasket, spring sheet, positive electrode shell and the like.

[0029] In this example, the assembled Zn||PTO symmetric battery was heated at 1 A∙g -1 The battery was cycled at a current density of , and the coulombic efficiency was 69.02% after 250 cycles, which is much higher than that of the full battery with basic electrolyte.

Claims

1. An aqueous zinc electrolyte additive, characterized in that: A multifunctional additive is added to the aqueous electrolyte.

2. The aqueous zinc electrochemical additive according to claim 1, characterized in that: The LA concentration in the electrolyte is 1 mol / L.

3. An aqueous zinc electrolyte, characterized in that: Including the electrolyte additive described in claim 2.

4. The aqueous zinc electrolyte according to claim 3, characterized in that: The electrolyte should include one or more of zinc sulfate, zinc chloride, zinc nitrate or trifluoromethane zinc sulfate.

5. The aqueous zinc electrolyte according to claim 4, characterized in that: The electrolyte concentration is 2 mol / L.

6. An electrolyte obtained according to the configuration described in claims 1-5.

7. The aqueous zinc ion battery according to claim 6, characterized in that: The current collector is one of stainless steel mesh, titanium foil, titanium mesh or carbon cloth.

8. The aqueous zinc ion battery according to claim 6, characterized in that: The diaphragm is one of glass fiber, non-woven fabric diaphragm or filter membrane.