Electromagnetic shielding body for preparing directional electromagnetic shielding material as well as preparation method and application of electromagnetic shielding body
Through the spray-drying alternating film formation process, the carbon nanodispersion liquid is sprayed in the electromagnetic shielding material, and the problem of difficulty and high cost of thickness control of carbon nano film layer is solved, and the stability and anisotropic properties of electromagnetic shielding material are realized. promote.
Patent Information
- Application Number
- CN202411195299.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
During the preparation process of existing electromagnetic shielding materials, the thickness of the carbon nano film layer is difficult to accurately control, the process is complex and costly, which affects the stability of material performance.
The spray-drying alternating film formation process is adopted to spray the carbon nanodispersion liquid onto the conductive porous frame evenly, and the spray amount is controlled through ultrasonic spraying equipment, simplifying the process and avoiding post-liquid treatment, ensuring the precise control of the thickness of the carbon nanofilm layer.
The use of dispersion liquid is reduced, the process flow is simplified, the anisotropic performance and performance stability of electromagnetic shielding materials are improved, and the cost is reduced, which is suitable for industrial promotion.
Smart Images

Figure CN119095358A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electromagnetic shielding materials, and in particular to an electromagnetic shielding body used for preparing directional electromagnetic shielding materials, and a preparation method and application thereof. Background Art
[0002] With the continuous development of aerospace, 5G communication technology, stealth fighters, wearable flexible electronic skin and other technologies, the requirements for electromagnetic shielding, light weight, flexibility and other performance of electromagnetic shielding materials are becoming higher and higher. Polymer materials, as carriers of conductive or magnetic fillers, can reduce the mismatch of the surface impedance of composite materials due to their electrical insulation, making it easier for electromagnetic waves to enter the interior of the composite materials, thereby reducing the reflection and scattering of electromagnetic waves on the surface of the composite materials, playing the role of transmitting electromagnetic waves, and playing the role of electromagnetic wave transmission and absorption in polymer-based electromagnetic shielding composite materials. However, the quality of the electromagnetic shielding effectiveness of polymer composites mainly depends on: (1) the performance of the conductive or magnetic filler itself; (2) whether the conductive or magnetic filler can form a good conductive path between the polymer matrix and have good impedance matching.
[0003] At the same time, with the in-depth study of electromagnetic shielding mechanism by domestic and foreign researchers, it was found that the electromagnetic shielding performance of polymer matrix electromagnetic shielding composite materials also depends on the microstructure of the composite materials, and then the research on the design of composite microstructure to improve electromagnetic shielding performance was carried out to meet the application in different fields. At present, the common microstructures of polymer electromagnetic shielding composite materials mainly include: porous foam structure, multilayer structure, gradient structure, isolation structure, etc. Different microstructures will lead to different electromagnetic wave shielding mechanisms and effects, and composite materials with a single microstructure often do not have directional electromagnetic shielding performance for electromagnetic wave shielding efficiency. Therefore, research and development of electromagnetic shielding materials with directional electromagnetic shielding performance has become a research direction for technicians in this field.
[0004] In order to achieve breakthrough research in this direction, our company has introduced the patented technology of double-shielding structural materials with patent number 202110638506.5, and carried out experimental research on the construction of a pilot production line based on this patented technology. It was found that the carbon nanofilm layer in the electromagnetic shielding material is formed by vacuum-assisted filtration and then cut-assembled-packaged. This process can enhance the anisotropic properties of the electromagnetic shielding material, but the processing process is relatively complicated, and the thickness of the carbon nanofilm layer will be determined by the amount of dispersion, which makes it difficult to control the amount of dispersion and difficult to achieve precise control, affecting the stability of the performance of the electromagnetic shielding material. At the same time, the post-filtration liquid needs to be treated, and a post-liquid treatment device needs to be configured, resulting in a high cost for post-liquid treatment. Summary of the invention
[0005] Based on the above technical problems, the present invention provides an electromagnetic shielding body for preparing directional electromagnetic shielding materials, and a preparation method and application thereof. The spraying-drying alternating film-forming process is adopted to avoid post-liquid treatment and reduce the use of excessive dispersion liquid. At the same time, the film-forming effect can be guaranteed, and the carbon nanofilm layer forming process is simplified, which is easy to promote and implement in industrialization.
[0006] The specific technical solution is:
[0007] One of the purposes of the present invention is to provide a method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material, comprising the following steps:
[0008] (1) cutting the melamine sponge into suitable sizes, washing and drying it, and then performing a nickel-plating conductive treatment to obtain a conductive porous skeleton;
[0009] (2) preparing a polyethylene oxide solution, and using a cell crusher to ultrasonically disperse the carbon nanotubes uniformly in the polyethylene oxide solution to obtain a carbon nanotube dispersion;
[0010] (3) Using ultrasonic spraying equipment to evenly spray the carbon nano-dispersion onto one side of the conductive porous skeleton, and after spraying, drying to obtain an electromagnetic shielding body.
[0011] The carbon nanotubes are dispersed in a polyethylene oxide solution to prepare a carbon nano dispersion, which is then sprayed on a conductive porous skeleton using an ultrasonic spraying device (for example: jlcs-2022-hdkcv), and then dried to form a carbon nano film layer, so that the carbon nano film layer and the conductive porous skeleton are jointly constructed into an electromagnetic shielding body, which not only avoids the subsequent process of bonding and assembling the conductive porous skeleton and the carbon nano film, but also avoids the influence of the change in the amount of dispersion on the thickness of the carbon nano film layer. The spraying amount is accurately controlled by using the number of spraying times and the spraying pressure and spraying distance of the ultrasonic spraying equipment, so that the thickness of the carbon nano film layer is accurately controllable, which helps to improve the performance of electromagnetic shielding structural materials.
[0012] In order to ensure the quality of the carbon nanofilm layer and improve the anisotropic performance of the electromagnetic shielding structural material, preferably, in step (3), the spraying pressure is 5-8 kPa and the spraying distance is 10-18 cm. More preferably, in step (3), the spraying pressure is 5 kPa and the spraying distance is 15 cm.
[0013] In order to improve the electromagnetic shielding performance of the electromagnetic shielding body and improve the anisotropic performance of the electromagnetic shielding body, preferably, the spraying and drying in step (3) are performed three times each.
[0014] Preferably, in step (1), the cleaning is performed by ultrasonic treatment with deionized water at 30 kHz for 10 minutes in an ultrasonic cleaning machine.
[0015] In order to improve the conductive effect of the nickel plating conductive treatment, preferably, in the step (1), before the nickel plating conductive treatment, the cleaned and dried melamine sponge is immersed in a sensitizing solution and ultrasonically sensitized for 30 minutes, removed, and ultrasonically treated with deionized water in an ultrasonic cleaning machine at 30kHz for 10 minutes, and then immersed in an activation solution for ultrasonic activation for 30 minutes, removed, and ultrasonically treated with deionized water in an ultrasonic cleaning machine at 30kHz for 10 minutes, and then dried for standby use.
[0016] More preferably, the nickel plating conductive treatment is to immerse the melamine sponge in a chemical plating solution and perform a nickel plating treatment for 3 minutes by a chemical deposition process, then remove it and wash it repeatedly with deionized water for three times, and dry it in a vacuum oven at 40° C. to constant weight.
[0017] In order to ensure that the sprayed carbon nanofilm layer is of excellent quality, preferably, in step (3), the drying is carried out in a vacuum oven at 40° C. to a constant weight.
[0018] The second purpose of the invention is to provide an electromagnetic shielding body prepared by the above-mentioned electromagnetic shielding body preparation method for preparing directional electromagnetic shielding materials. The electromagnetic shielding body sprays the carbon nanofilm layer onto the conductive porous skeleton by a spraying process, which can help reduce the difficulty of process processing and improve the anisotropic performance of the electromagnetic shielding body.
[0019] The third purpose of the invention is to provide an electromagnetic shielding body preparation method for preparing directional electromagnetic shielding materials, and the prepared electromagnetic shielding body is used for the preparation of directional electromagnetic shielding materials. Specifically, polyimide slurry is used as the encapsulation liquid, and the encapsulation liquid is sprayed on the electromagnetic shielding body by ultrasonic spraying equipment, and after the spraying is completed, it is cured at 180-190°C.
[0020] Using polyimide slurry as the encapsulation liquid to solidify and encapsulate the carbon nanofilm layer containing the porous skeleton not only utilizes the excellent temperature resistance of polyimide, enabling it to work in the temperature range of -200°C to 400°C, which helps to broaden the scope of application; it can also protect the carbon nanofilm layer sprayed on the conductive porous skeleton to avoid scratches and damage that affect the performance of the electromagnetic shielding material.
[0021] Compared with the prior art, the technical effects created by the present invention are embodied in:
[0022] The carbon nanofilm layer preparation process created by the present invention is simple, and the required carbon nanofilm layer thickness can be controlled by accurately controlling the spraying pressure and the spraying distance in combination with the control of the number of spraying times, thereby reducing the difficulty of controlling the thickness of the carbon nanofilm layer preparation, and avoiding the defect that the carbon nanotube content in the carbon nanotube dispersion liquid gradually decreases with the suction filtration film-forming process, resulting in excessive dispersion liquid in the later stage, causing uneven thickness of the carbon nanofilm layer in the suction filtration film-forming process, resulting in unstable performance of the electromagnetic shielding body.
[0023] The invention is created through the introduction and experimental research of electromagnetic shielding material preparation technology. On the basis of the introduced technology, taking into account that the dispersion liquid content will change during the filtration process, resulting in poor stability of film thickness, which in turn affects the performance of the electromagnetic shielding material, ultrasonic spraying equipment is used for spraying film, which not only avoids the process of bonding and assembling the conductive porous skeleton and the carbon nanofilm layer to prepare the electromagnetic shielding body, but also avoids the defect that the dispersion liquid content changes with the film forming process and affects the film quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A process flow diagram is provided for the present invention.
[0025] Figure 2 A schematic diagram of the process flow of another embodiment of the present invention is provided. DETAILED DESCRIPTION
[0026] In order to facilitate those skilled in the art to correctly understand the present invention and enable those skilled in the art to fully understand the technical content of the present invention, the technical solution of the present invention is further explained below in conjunction with specific implementation methods and drawings. However, this explanation does not limit the scope of protection required for the present invention. The scope of protection of the present invention by those skilled in the art cannot be limited to the following explanations. Any equivalent substitutions or changes made by any those skilled in the art or persons familiar with the technology in the art based on the present invention and the technical solution and inventive concept thereof should be covered within the scope of protection of the present invention.
[0027] Explanation and explanation of terms: The "electromagnetic shielding body" used in the name of the invention is a structure containing a conductive porous skeleton and a carbon nanofilm layer without encapsulation treatment, and the electromagnetic shielding structural material is the whole after the electromagnetic shielding body is encapsulated with an encapsulation liquid (polyimide slurry). For terms not specifically pointed out and explained in the invention, the conventional understanding of the corresponding terms by those skilled in the art can be referred to.
[0028] like Figure 1 As shown, in some embodiments, a method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material comprises the following steps:
[0029] (1) The melamine sponge is cut into a suitable size (for example, cut into 3.5 cm × 2 cm × 0.2 cm according to Patent No. 202110638506.5, or cut into other sizes, for example, 3 cm × 2.5 cm × 0.3 cm, 3 cm × 2 cm × 0.2 cm, etc.), and ultrasonically treated with deionized water in an ultrasonic cleaner at 30 kHz for 10 min, and then dried in a vacuum oven at 40°C to constant weight, and then nickel-plated for conductive treatment to obtain a conductive porous skeleton; the nickel-plated conductive treatment refers to the technical content disclosed in Patent No. 202110638506.5, and the melamine sponge is immersed in a chemical plating solution and nickel-plated by a chemical deposition process for 3 minutes, and then taken out and repeatedly washed with deionized water three times, and dried in a vacuum oven at 40°C to constant weight.
[0030] (2) Prepare a polyethylene oxide solution, and use a cell crusher to ultrasonically disperse the carbon nanotubes in the polyethylene oxide solution to obtain a carbon nano dispersion; the specific preparation method refers to the technical content disclosed in Patent No. 202110638506.5.
[0031] (3) Using ultrasonic spraying equipment (e.g., models JLCS-2022-HDKCV, FS650, etc.), the carbon nano-dispersion liquid is evenly sprayed on one side of the conductive porous skeleton. After the spraying is completed, it is dried in a vacuum oven at 40° C. to a constant weight to obtain an electromagnetic shielding body.
[0032] The preparation process of the carbon nanofilm layer in the electromagnetic shielding body is simplified, the difficulty and cost of preparing the carbon nanofilm layer are reduced, which is helpful to improve the overall performance of the electromagnetic shielding body and improve the anisotropic performance of the electromagnetic shielding body after being encapsulated by the encapsulation liquid.
[0033] In some embodiments, in step (3), the spraying pressure is 5-8 kPa, and the spraying distance is 10-18 cm. In a more preferred embodiment, in step (3), the spraying pressure is 5 kPa, and the spraying distance is 15 cm.
[0034] In some embodiments, the step (3), spraying and drying are performed three times each, that is, after the carbon nano dispersion is sprayed onto one side of the conductive porous skeleton, it is dried to constant weight, and then the steps are repeated in sequence until three times are completed. This will help improve the electromagnetic shielding performance of the electromagnetic shielding body, improve the anisotropic performance of the electromagnetic shielding body, and enhance the difference in the anisotropy of the electromagnetic shielding material on the electromagnetic wave loss path.
[0035] In certain embodiments, in step (1), the cleaning is performed by ultrasonic treatment with deionized water at 30 kHz for 10 minutes in an ultrasonic cleaning machine.
[0036] like Figure 2 As shown, in some embodiments, in step (1), before the nickel-plating conductive treatment, the cleaned and dried melamine sponge is immersed in a sensitizing solution for ultrasonic sensitization for 30 minutes, removed, and ultrasonically treated with deionized water in an ultrasonic cleaning machine at 30kHz for 10 minutes, then immersed in an activation solution for ultrasonic activation for 30 minutes, removed, and ultrasonically treated with deionized water in an ultrasonic cleaning machine at 30kHz for 10 minutes, dried, and used for standby. The performance of the electromagnetic shielding material can be improved.
[0037] In some embodiments, the nickel-plated conductive treatment is to immerse the melamine sponge in a chemical plating solution and perform a nickel-plating treatment for 3 minutes by a chemical deposition process, then remove it and wash it three times with deionized water, and dry it in a vacuum oven at 40°C to constant weight. The specific processing is carried out with reference to the technical content disclosed in Patent No. 202110638506.5.
[0038] In some embodiments, the directional electromagnetic shielding structural material is prepared by using polyimide slurry as the encapsulation liquid, and using ultrasonic spraying equipment to spray the encapsulation liquid on the electromagnetic shielding body. After spraying, it is cured at a temperature between 180-190°C.
[0039] In order to better explore the technical effects that can be brought about by the present invention, the researchers of the present invention have conducted improved experimental research on the preparation process of carbon nanofilm layers in electromagnetic shielding materials based on the technical content disclosed in Patent No. 202110638506.5, and now make the following explanation.
[0040] Example 1
[0041] Take a melamine sponge and cut it into 3.5cm×2cm×0.2cm, use deionized water to ultrasonically treat it in an ultrasonic cleaner at 30kHz for 10 minutes, and then dry it in a vacuum oven at 40°C to constant weight to obtain a melamine sponge substrate; The melamine sponge substrate is nickel-plated for 3 minutes according to the chemical deposition process in Example 1 of Patent No. 202110638506.5, then it is fished out and repeatedly washed three times with deionized water, and dried in a vacuum oven at 40°C to constant weight to obtain a conductive porous skeleton;
[0042] Weigh 20 mg of polyethylene oxide and dissolve it in 200 ml of deionized water to obtain a polyethylene oxide solution; use a cell crusher to ultrasonically disperse 200 mg of carbon nanotubes in the polyethylene oxide solution to obtain a carbon nanotube dispersion;
[0043] The carbon nano-dispersion was evenly sprayed on one side of the conductive porous skeleton using jlcs-2022-hdkcv ultrasonic spraying equipment. The spraying pressure was 5 kPa and the spraying distance (the distance between the nozzle of the ultrasonic spraying equipment and the conductive porous skeleton) was 10 cm. After spraying, it was dried in a vacuum oven at 40°C to constant weight to obtain an electromagnetic shielding body.
[0044] Example 2
[0045] On the basis of Example 1, the spraying pressure is 8 kPa, the spraying distance (the distance between the nozzle of the ultrasonic spraying equipment and the conductive porous skeleton) is 18 cm, and the rest is the same as Example 1.
[0046] Example 3
[0047] On the basis of Example 1, the spraying pressure is 6 kPa, the spraying distance (the distance between the nozzle of the ultrasonic spraying equipment and the conductive porous skeleton) is 14 cm, and the rest is the same as Example 1.
[0048] Example 4
[0049] On the basis of Example 1, the spraying pressure is 5 kPa, the spraying distance (the distance between the nozzle of the ultrasonic spraying equipment and the conductive porous skeleton) is 15 m, and the rest is the same as Example 1.
[0050] Example 5
[0051] On the basis of Example 1, the melamine sponge substrate was immersed in a sensitizing solution for ultrasonic sensitization treatment for 30 minutes, fished out, and ultrasonically treated with deionized water in an ultrasonic cleaning machine at 30kHz for 10 minutes, then immersed in an activation solution for ultrasonic activation treatment for 30 minutes, fished out, and ultrasonically treated with deionized water in an ultrasonic cleaning machine at 30kHz for 10 minutes, dried in a vacuum box at 40°C to constant weight, and then nickel-plated by a chemical deposition process to obtain a conductive porous skeleton; then the carbon nano dispersion was sprayed on the conductive porous skeleton according to the spraying process in Example 1, and the spraying and drying were performed three times each, and the rest was the same as Example 1.
[0052] Polyimide slurry is used as the encapsulation liquid, and the encapsulation liquid is sprayed on the electromagnetic shielding body obtained in Examples 1-5 using an ultrasonic spraying device according to the spraying pressure and spraying distance of the corresponding embodiment. After the spraying is completed, the temperature is set between 180-190°C for curing to obtain a directional electromagnetic shielding structural material. The obtained directional electromagnetic shielding structural material is incident with electromagnetic waves from both the front and back sides to detect EMI SE T Each group was tested three times and the average value was taken (one decimal place was retained). The test results are shown in Table 1.
[0053] Table 1
[0054]
[0055] As can be seen from Table 1, the invention sprays the carbon nanotube dispersion on the conductive porous skeleton to form an electromagnetic shielding body through a spraying process, which can not only avoid the defect of affecting the film quality due to the change of the dispersion content during the film forming process, and avoid the packaging process of assembling the carbon nanofilm layer and the conductive porous skeleton to form an electromagnetic shielding body, but also ensure that the anisotropy of the electromagnetic shielding structural material is significantly different. At the same time, the invention helps to improve the anisotropic performance through proper control of the spraying process parameters; sensitizing and activating the melamine sponge substrate will help to enhance the anisotropy and broaden the potential application environment of the electromagnetic shielding material.
[0056] The invention creates other matters that are not covered, and can be realized by conventional technical means with reference to the prior art or common knowledge known to those skilled in the art. For example, the preparation of nickel plating solution, the preparation of sensitizing solution, the preparation of activation solution, etc. can all be prepared with reference to the technical content disclosed in patent number 202110638506.5. Another example: the encapsulation liquid is yellow polyimide slurry (YPI).
Claims
1. A method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material, characterized in that: The following steps are involved: (1) cutting the melamine sponge into suitable sizes, washing and drying it, and then performing a nickel-plating conductive treatment to obtain a conductive porous skeleton; (2) preparing a polyethylene oxide solution, and uniformly dispersing the carbon nanotubes in the polyethylene oxide solution using a cell crusher ultrasound to obtain a carbon nanotube dispersion; (3) Using ultrasonic spraying equipment, the carbon nano-dispersion liquid is evenly sprayed on the conductive porous skeleton. After the spraying is completed, it is dried to obtain an electromagnetic shielding body.
2. The method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material according to claim 1, wherein: In the step (3), the spraying pressure is 5-8 kPa and the spraying distance is 10-18 cm.
3. The method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material according to claim 1 or 2, characterized in that: In the step (3), the spraying pressure is 5 kPa and the spraying distance is 15 cm.
4. The method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material according to claim 1 or 2, characterized in that: In the step (3), spraying and drying are performed three times each.
5. The method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material according to claim 1, wherein: In the step (1), before the nickel plating conductive treatment, the cleaned and dried melamine sponge is immersed in a sensitizing solution and ultrasonically sensitized for 30 minutes, removed, and ultrasonically treated with deionized water in an ultrasonic cleaning machine at 30kHz for 10 minutes, then immersed in an activation solution and ultrasonically activated for 30 minutes, removed, and ultrasonically treated with deionized water in an ultrasonic cleaning machine at 30kHz for 10 minutes, dried, and set aside.
6. The method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material according to claim 1 or 5, characterized in that: The nickel plating conductive treatment is to immerse the melamine sponge in a chemical plating solution and perform a nickel plating process for 3 minutes through a chemical deposition process, then remove it and repeatedly wash it with deionized water three times, and dry it in a vacuum oven at 40° C. to constant weight.
7. The method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material according to claim 1, wherein: In the step (3), the drying is carried out in a vacuum oven at 40° C. to a constant weight.
8. An electromagnetic shielding body prepared by the method for preparing an electromagnetic shielding body of directional electromagnetic shielding material according to any one of claims 1 to 7.
9. The electromagnetic shielding body prepared by the method for preparing an electromagnetic shielding body for preparing a directional electromagnetic shielding material according to claim 8 is used for preparing a directional electromagnetic shielding material.
10. The use according to claim 9, characterized in that Polyimide slurry is used as the encapsulation liquid, and ultrasonic spraying equipment is used to spray the encapsulation liquid on the electromagnetic shielding body. After the spraying is completed, it is cured at 180-190° C.