Production of lithium oxide powder

By heating the lithium salt at a melting point below the lithium salt to a lower melting point below the lithium salt melting point and removing gaseous by-products, the purity and economic problems in lithium oxide production are solved, and the stability of high-purity lithium oxide powder is achieved and Convenience of collection.

CN119095797APending Publication Date: 2024-12-06ALBEMARLE CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026440.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2023-02-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing lithium oxide production process has disadvantages in terms of process conditions, product purity and economic feasibility, and it is difficult to produce relatively pure lithium oxide powder without harsh conditions.

Method used

By heating the two lithium salts at a temperature below their eutectic point to below the melting point of the lithium salt, a powder containing lithium oxide and lithium salt is formed and gaseous byproducts are removed to improve the reaction equilibrium, using non-reaction to reduce agglomeration and reduce temperature.

Benefits of technology

The production of unstable high-purity lithium oxide powder in ambient air is realized, and the introduction of impurities is avoided, and the stability and collection convenience of the product are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095797A_ABST
    Figure CN119095797A_ABST
Patent Text Reader

Abstract

A process for preparing a lithium oxide powder from a combination of lithium salts is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a process for preparing lithium oxide powder. Background Art

[0002] Lithium oxide is used in lithium batteries, glass and ceramics, and other applications. In some applications, the presence of lithium hydroxide and / or other lithium compounds as impurities in lithium oxide is undesirable.

[0003] Many methods for producing lithium oxide are known, but most suffer from one or more disadvantages in terms of process conditions, product purity and / or economic feasibility. A process that does not require harsh conditions or a large number of steps, produces relatively pure lithium oxide and is economically viable is desirable. Summary of the invention

[0004] The present invention provides lithium oxide powders containing lithium salts. If the lithium salts are coated on the lithium oxide, some of these lithium oxide powders may be slightly stable in ambient air. The present invention also provides high purity lithium oxide powders containing minimal amounts of lithium salts and not stable in ambient air.

[0005] An embodiment of the present invention is a process for producing a powder comprising lithium oxide and a lithium salt. The process comprises heating a mixture of two lithium salts at one or more temperatures ranging from about 50°C below the eutectic point of the mixture of two different lithium salts to a temperature below the melting point of the lithium salt with the lower melting point to form a powder comprising lithium oxide and a lithium salt. During the process, at least a portion of the gaseous byproducts produced by the process is removed. Optionally, a non-reactive additive is present in the mixture of the two lithium salts.

[0006] Another embodiment of the present invention is a process for converting lithium salt present in a powder comprising lithium oxide and lithium salt into lithium oxide. This process can also be viewed as a process for purifying a powder comprising lithium oxide and lithium salt by converting the lithium salt present into lithium oxide. The process comprises heating the powder comprising lithium oxide and lithium salt at one or more temperatures in the range of about 25°C below the melting point of the lithium salt to about 200°C above the melting point of the lithium salt.

[0007] Other embodiments of the present invention include powders comprising lithium oxide and a lithium salt.

[0008] These and other embodiments and features of the present invention will become more fully apparent from the ensuing description and appended claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 Photographic images of the products containing the heating step performed on the lithium salt using different reaction parameters.

[0010] Figure 2There are two x-ray powder diffraction patterns of a product formed according to the process of the present invention; one diffraction pattern is for a powder comprising lithium oxide and lithium carbonate, and one diffraction pattern is for lithium oxide without lithium carbonate.

[0011] Figure 3 is an x-ray powder diffraction pattern of a powder comprising lithium oxide and lithium carbonate formed according to the process of the present invention.

[0012] Figure 4 is the x-ray powder diffraction pattern of the product formed by heating lithium hydroxide monohydrate and lithium carbonate in the absence of non-reactive additives.

[0013] The drawings illustrate embodiments of certain aspects of the invention and are not intended to impose limitations on the scope of the invention. DETAILED DESCRIPTION

[0014] As used throughout this document, the phrase "lithium salt" includes lithium hydroxide, which is generally considered a base rather than a salt.

[0015] In the production of lithium oxide ( Li2O ) and a lithium salt powder, one of the two lithium salts has a higher melting point and the other lithium salt has a lower melting point. The lithium salt with a higher melting point is sometimes referred to as a high melting point lithium salt or a high melting point salt. The other lithium salt is sometimes referred to as a low melting point lithium salt or a low melting point salt. In this document, when referring to a specific combination of lithium salts, the low melting point salt is usually listed first.

[0016] Generally, both lithium salts used in the process of the present invention are capable of forming lithium oxide when heated at a pressure below atmospheric pressure (reduced pressure) and / or in the presence of an inert gas stream or an oxygen-containing inert gas stream.

[0017] Preferred combinations of two lithium salts in the practice of the present invention include lithium nitrate and lithium bromide; lithium hydroxide and lithium bromide; lithium bromide and lithium carbonate; lithium hydroxide and lithium carbonate; lithium bromide and lithium chloride; and lithium nitrate and lithium bromide. The preferred lithium salt combination is lithium hydroxide and lithium carbonate.

[0018] In the lithium salt combination including lithium hydroxide, the lithium hydroxide may be anhydrous lithium hydroxide or monohydrated lithium hydroxide; monohydrated lithium hydroxide is preferred. Anhydrous lithium hydroxide is preferably treated under an inert gas (i.e., without moisture, CO2 or other substances that can react with lithium hydroxide); the inert gas preferably includes one or more inert gases, typically one or more of helium, nitrogen and argon.

[0019] When the two lithium salts are lithium hydroxide and lithium carbonate, the lithium carbonate can be introduced into the lithium hydroxide by adding solid lithium carbonate or by forming the lithium carbonate in situ. The lithium carbonate can be formed in situ by reacting some of the lithium hydroxide with carbon dioxide by passing carbon dioxide gas through the lithium hydroxide, which can be done in about 5 minutes at about 50°C on a laboratory scale, or by contacting the lithium hydroxide with ambient atmosphere (air), optionally accompanied by heating, such as heating at about 50°C for about 3 hours on a laboratory scale. Another way is to allow the lithium hydroxide to contact with air for a few minutes while reducing the particle size of the lithium hydroxide; when doing so, the lithium carbonate will generally form a coating on the lithium hydroxide.

[0020] For high melting point lithium salts, the minimum amount has not been optimized, but can be about 0.1 wt% or more relative to the total weight of the mixture of low melting point lithium salts and high melting point lithium salts, typically about 0.1 wt% to about 20 wt% relative to the total weight of the mixture, preferably about 0.1 wt% to about 15 wt%, more preferably about 0.2 wt% to about 15 wt%, even more preferably about 0.3 wt% to about 12 wt%. When non-reactive additives are present, these amounts refer to the total weight of the mixture including the non-reactive additives.

[0021] When the high melting point salt is lithium carbonate, a typical amount is about 0.1 wt % or more, preferably about 0.2 wt % or more, relative to the total weight of the mixture, and is generally in the range of about 0.1 wt % to about 15 wt %, preferably about 0.1 wt % to about 12 wt %, and more preferably about 0.2 wt % to about 12 wt %. It has been observed that as the amount of lithium carbonate increases, the temperature can decrease (e.g., 410° C. for 5 wt % lithium carbonate), while lower amounts of lithium carbonate generally require higher temperatures (e.g., 420° C. for 1 wt % lithium carbonate).

[0022] One or both of the two lithium salts may be reduced to a desired average particle size before contacting the other lithium salt and the non-reactive additive (when used). Preferably, the average particle size of the two lithium salts is selected to maximize the contact between the particles of the two lithium salts, and the low melting point lithium salt preferably has an average particle size larger than the average particle size of the high melting point lithium salt. The low melting point lithium salt preferably has an average particle size in the range of about 5 μm to about 700 μm, more preferably about 10 μm to about 600 μm, and even more preferably about 15 μm to about 500 μm, while the high melting point lithium salt preferably has an average particle size in the range of about 2.5 μm to about 75 μm, more preferably about 5 μm to about 65 μm, and even more preferably about 10 μm to about 45 μm. Particle size reduction can be accomplished by conventional techniques when performed.

[0023] The optional non-reactive additive is a substance that melts above the melting point of the high melting point lithium salt and does not react with either lithium salt in the lithium salt pair or the lithium oxide. The non-reactive additive minimizes or prevents agglomeration of the lithium oxide formed during the process and permits the process to be carried out at a slightly higher temperature. In some embodiments, the presence of a non-reactive additive is preferred.

[0024] Suitable non-reactive additives include lithium oxide, quartz and inorganic oxide beads, such as silica beads or zirconium oxide beads. The non-reactive additive is preferably lithium oxide. A mixture of any two or more non-reactive additives can be used. When the non-reactive additive is lithium oxide, no purification step is required at the end of the process to remove the non-reactive additive. When the high melting point salt is lithium carbonate, the non-reactive additive is preferably a substance that melts at a temperature of about 725°C or above.

[0025] When present, the non-reactive additive is generally about 1 wt % or more relative to the gross weight of the mixture, but this is not optimized. Generally speaking, the amount of the non-reactive additive is in the range of about 1 wt % to about 90 wt %. In some embodiments, the amount of the non-reactive additive is in the range of about 20 wt % to about 90 wt %, preferably in the range of about 25 wt % to about 85 wt %, more preferably in the range of about 50 wt % to about 80 wt %. In other embodiments, the amount of the non-reactive additive is in the range of about 1 wt % to about 20 wt %, preferably in the range of about 3 wt % to about 17 wt %, more preferably in the range of about 5 wt % to about 15 wt % relative to the gross weight of the mixture.

[0026] For non-reactive additives, the average particle size is preferably in the range of about 5 μm to about 700 μm, more preferably about 10 μm to about 600 μm, and even more preferably about 15 μm to about 500 μm. In some embodiments, the average particle size of the non-reactive additive is preferably similar to or less than the average particle size of the low melting point lithium salt. Particle size reduction, when performed, can be accomplished by conventional techniques.

[0027] For two lithium salts and optional non-reactive additives, the weight percentages are determined based on the amount of material weighed, for example, on a balance or scale. In some cases, such as when the two lithium salts are lithium hydroxide and lithium carbonate, and the lithium carbonate is generated in situ, the amount of lithium carbonate is determined by x-ray powder diffraction (XRD), but it should be understood that since XRD only detects crystalline phases, there may be a certain amount of error in the XRD determination.

[0028] The order of addition or mixing of the high melting point lithium salt, the low melting point lithium salt and the optional non-reactive additive has not been observed to affect the process or the results obtained. Preferably, the low melting point lithium salt is combined with the high melting point lithium salt first (especially when the high melting point salt is lithium carbonate formed in situ), and then the non-reactive additive is introduced when used.

[0029] To mix the high melting point lithium salt, the low melting point lithium salt and the optional non-reactive additive, any conventional method or apparatus for mixing solids may be employed, such as an acoustic mixer, a ball mill (with a gas flow, e.g., air, an inert gas, or CO2), or a jet mill. When at least two of these components are soluble in the selected medium, liquid methods for mixing the two lithium salts and / or the non-reactive additive (when used) may be used; such liquid methods include spray drying of a solution, suspension, or slurry of the components, sol-gel methods, or coprecipitation of the components from a liquid.

[0030] Heating the two lithium salts while removing at least a portion of the gaseous byproducts produced by the process generally results in the low melting point lithium salt forming lithium oxide. The reaction zone is where the heating of the two lithium salts (with or without non-reactive additives) occurs. Typically, the reaction zone can be an oven (e.g., a stationary oven), a kiln (such as a rotary kiln or a roller kiln), a furnace (such as a shaft furnace or a tube furnace), or a fluidized bed; a fluidized bed is sometimes preferred.

[0031] Heating can include any convenient method of achieving and maintaining the desired reaction temperature. Suitable types of heating include thermal heating, microwave heating, and optical heating (e.g., heating with a xenon arc lamp); two or more types of heating can be used. Thermal heating is often preferred.

[0032] Heating can be performed in intermittent or continuous mode. Continuous mode operation can be performed, for example, by feeding a series of reaction vessels through the reaction zone. Rotary kilns and roller kilns can be operated in continuous mode by introducing the two lithium salts at the inlet and operating the kiln so that the two lithium salts move through the kiln and exit the outlet in a continuous manner. Fluidized beds can also be operated in continuous mode.

[0033] Once the mixture is formed, heating of the mixture may be initiated. In some embodiments, the reaction zone may already be at the desired reaction temperature. In embodiments where the reaction zone is at a temperature lower than the desired reaction temperature, the mixture is heated to the desired reaction temperature preferably at a rate of about 3°C / min to about 100°C / min, preferably at a rate of about 5°C / min to about 50°C / min, more preferably at a rate of about 8°C / min to about 50°C / min; these heating rates have not been optimized. When a temperature gradient or temperature profile is used, it is recommended and preferred to optimize the heating rate to obtain a product with minimal agglomeration.

[0034] In the process of the present invention, the formation of lithium oxide from the two lithium salts is accompanied by the formation of gaseous byproducts (e.g., carbon dioxide and water). Removal of the gaseous byproducts shifts the reaction equilibrium toward the product (lithium oxide) and minimizes or prevents the reformation of the starting materials (the two lithium salts). Removal of the gaseous byproducts typically increases the reaction rate. Removal of the gaseous byproducts is typically accomplished by conducting the process under reduced pressure (less than atmospheric pressure) or in the presence of an inert gas or an oxygen-containing inert gas stream.

[0035] When used alone or as part of an oxygen-containing inert gas, the inert gas preferably comprises one or more inert gases, typically one or more of helium, nitrogen, and argon. The oxygen-containing inert gas may have any amount of oxygen; atmospheric amounts (e.g., about 21%) of oxygen are convenient, but greater or lesser amounts of oxygen may be present in the oxygen-containing inert gas and are not expected to adversely affect the reaction. The inert gas and oxygen-containing inert gas preferably contain only small or variable amounts of water and / or carbon dioxide, more preferably about 1000 ppm or less of water and about 500 ppm or less of carbon dioxide.

[0036] When the heating of the two lithium salts (in the presence or absence of non-reactive additives) is carried out in the presence of an inert gas or oxygen-containing inert gas flow, the flow rate is sufficient to remove sufficient gaseous byproducts to maintain a reaction balance that favors the product, which will vary with the heating device, reaction temperature, and the two lithium salts present in the reaction mixture. The flow rate of the inert gas or oxygen-containing inert gas is preferably in the range of about 40 sccm to about 10,000 sccm, more preferably about 500 sccm to about 7500 sccm, and even more preferably about 1000 sccm to about 6000 sccm.

[0037] When the heating of the two lithium salts (in the presence or absence of a non-reactive additive) is carried out under reduced pressure, the pressure is preferably about 608 Torr (81 kPa) or less, more preferably about 380 Torr (51 kPa) or less, still more preferably about 230 Torr (31 kPa) or less, and even more preferably about 20 Torr (2.7 kPa) or less. Optionally, an inert gas or an oxygen-containing inert gas may be fed to the reaction zone while maintaining the reduced pressure.

[0038] When the desired temperature is reached, the mixture may be heated at that temperature for the length of time required to form lithium oxide from one of the lithium salts, or the temperature may be varied during the reaction as desired. Since lithium oxide is formed during the process, the temperature may be increased to increase the conversion rate. The time is affected by the reaction temperature and the type of reaction zone. For example, in a fixed oven, the reaction may take about 20 hours to complete, while in a rotary kiln, the same reaction may take about 3 hours or less to complete.

[0039] In these processes, the two lithium salts may be present in an amount that forms a eutectic mixture in a localized spot, particularly along the interface between the two lithium salts. The temperature of the process ranges from about 50°C below the eutectic point of the two lithium salts to below the melting point of the lithium salt with the lower melting point. Preferably, the heating is carried out at one or more temperatures ranging from about 20°C below the eutectic point of the mixture of two different lithium salts to a temperature below the melting point of the lithium salt with the lower melting point. It is possible that the lower temperature of this process may be a temperature far below the eutectic point of the two lithium salts, but this parameter has not yet been optimized. Extensive melting of low-melting lithium salts is undesirable and tends to produce agglomerated powders, or solids that adhere to the reaction vessel, so temperatures several degrees lower than the melting point of the low-melting lithium salt are preferred. Melting of low-melting lithium salts can also cause corrosion of the reaction vessel, thereby introducing impurities into the product.

[0040] When the two lithium salts are lithium nitrate and lithium bromide, the temperature is preferably in the range of about 178°C to about 255°C or less, more preferably in the range of about 178°C to about 250°C. When the two lithium salts are lithium hydroxide and lithium bromide, the temperature is preferably in the range of about 225°C to about 470°C or less, more preferably in the range of about 225°C to about 465°C. When the two lithium salts are lithium bromide and lithium carbonate, the temperature is preferably in the range of about 446°C to about 550°C or less, more preferably in the range of about 446°C to about 545°C. When the two lithium salts are lithium bromide and lithium chloride, the temperature is preferably in the range of about 471°C to about 550°C or less, more preferably in the range of about 471°C to about 545°C or less.

[0041] In a more preferred embodiment where the two lithium salts are lithium nitrate and lithium bromide, the temperature is preferably in the range of about 208°C to about 255°C or less, more preferably in the range of about 208°C to about 250°C. In a more preferred embodiment where the two lithium salts are lithium hydroxide and lithium bromide, the temperature is preferably in the range of about 255°C to about 470°C or less, more preferably about 255°C to about 465°C. In a more preferred embodiment where the two lithium salts are lithium bromide and lithium carbonate, the temperature is preferably in the range of about 476°C to about 550°C or less, more preferably about 476°C to about 545°C. In a more preferred embodiment where the two lithium salts are lithium bromide and lithium chloride, the temperature is preferably in the range of about 501°C to about 550°C or less, more preferably about 501°C to about 545°C or less.

[0042] When the two lithium salts are lithium hydroxide and lithium carbonate, the temperature is preferably in the range of about 380°C to about 470°C or less, more preferably in the range of about 380°C to about 460°C. In some embodiments, the temperature is preferably in the range of about 380°C to about 425°C. In some embodiments, the temperature is varied during the process. In preferred embodiments where the temperature is varied, the temperature is slowly increased from about 380°C to about 460°C during the process.

[0043] In more preferred embodiments where the two lithium salts are lithium hydroxide and lithium carbonate, the temperature is preferably in the range of about 410°C to about 470°C or less, more preferably in the range of about 410°C to about 460°C. In some more preferred embodiments, the temperature is preferably in the range of about 410°C to about 425°C. In some embodiments, the temperature varies during the process. In some more preferred embodiments where the temperature varies, the temperature is slowly increased from about 410°C to about 460°C during the process.

[0044] It has been observed that particle size affects the reaction time and temperature required for complete conversion to lithium oxide, with larger particles requiring longer reaction times, at least when the two lithium salts are lithium hydroxide and lithium carbonate.

[0045] It has been observed that the particle size and morphology do not appear to be significantly altered by the process of the present invention. The particles are chemically altered from two lithium salts to lithium oxide and one lithium salt, where the lithium salt may form a coating on the particles. The particles of the product tend to be less dense than those of the starting material.

[0046] The product of heating the two lithium salts and the optional non-reactive additive is a powder comprising lithium oxide and one of the lithium salts (usually a high melting point lithium salt), and the product is generally a free-flowing powder. If the lithium salt is coated on the lithium oxide, some of these powders comprising one of the lithium oxide and the lithium salt may be slightly stable in ambient air.

[0047] The amount of lithium salt present in the powder comprising lithium oxide and lithium salt can be any amount ranging from slightly less than the amount present at the beginning of the process to about 0.1 wt %, depending on the reaction rate and the length of time in the reaction zone. Generally, the amount of lithium salt present in the powder comprising lithium oxide and lithium salt is about 10 wt % or less, often about 5 wt % or less, and often about 3 wt % or less.

[0048] Optionally, the powder comprising lithium oxide and lithium salt may be subjected to one or more particle size reduction techniques. Particle size reduction generally renders the product air sensitive, so it is recommended and preferred to carry out particle size reduction under an inert gas or oxygen-containing inert gas having the characteristics described above.

[0049] An advantage of the process of the present invention for forming a powder comprising lithium oxide and a lithium salt is that no bulk melting occurs during the process, which generally prevents the introduction of impurities from the reaction vessel. The process is not a solution process or a melting process, but may be a solid state reaction or a semi-solid state reaction. A small amount of local melting may occur during the process, but not to the extent that it causes observable corrosion of the reaction vessel or introduces detectable amounts of impurities.

[0050] Another advantage of the process of the present invention is that the product is obtained in powder form, which provides benefits. One of the benefits is that the product of the process does not adhere to the walls of the reaction vessel, allowing easier collection of the product.

[0051] Figure 1 The products of various processes for heating lithium hydroxide are shown. Figure 1 A shows the product of the process according to the invention, which is a free-flowing powder. Figure 1 B shows the product of the process in the absence of the non-reactive additive, which is an agglomerated powder. Figure 1 C shows the product of the process of heating lithium hydroxide without adding any other ingredients; the product appears to have melted extensively.

[0052] The relative amounts of lithium oxide and lithium salt in the product powder comprising lithium oxide and lithium salt depend to some extent on the amounts of the two lithium salts present in the mixture at the start of the process. In the product powder, the lithium salt is typically about 0.1 wt % or more, often about 0.1 wt % to about 20 wt % of the powder, preferably about 0.3 wt % to about 20 wt %, more preferably about 0.3 wt % to about 15 wt %, even more preferably about 0.3 wt % to about 10 wt %. The powder comprising lithium oxide and lithium salt is not air sensitive, and without wishing to be bound by theory, it is believed that the lithium salt forms a coating on the lithium oxide particles, possibly in a core-shell structure.

[0053] The weight percentages of lithium salt and lithium oxide are determined by x-ray powder diffraction (XRD), but it should be understood that since XRD only detects crystalline phases, a certain amount of error may exist in the XRD determination.

[0054] In the powder comprising lithium oxide and lithium salt, the lithium salt is lithium bromide, lithium carbonate, lithium chloride or lithium iodide; preferably, the lithium salt is lithium carbonate.

[0055] Figure 2 A and Figure 3 is an x-ray powder diffraction (XRD) pattern of a powder containing lithium oxide and lithium carbonate formed according to the process described above of the present invention. In each of these diffraction patterns, there is a large peak at a 2θ value of 33.6 degrees, which is a characteristic peak of Li2O, and there is at most a very small peak at a 2θ value of 32.5 degrees, which is a characteristic peak of LiOH. Figure 4 is the XRD pattern of the product formed in the absence of the non-reactive additive; the diffraction pattern has a distinct peak at 33.6 degrees 2θ (Li2O) and a much larger peak at 32.5 degrees 2θ (LiOH).

[0056] In the process of the present invention, the surface of the reaction vessel in contact with the reactants and products can be made of any material that is corrosion resistant and inert to the reactants and products (low melting point lithium salts, high melting point lithium salts, lithium oxide, optional non-reactive additives and combinations thereof) and can withstand the temperature of the process. The surface of the reaction vessel is usually composed of an inorganic oxide (such as aluminum oxide or magnesium oxide) or a metal (such as nickel); aluminum oxide is often the preferred reaction vessel material. Other corrosion resistant materials (such as platinum or rhodium alloys) can also be used as reaction vessel materials.

[0057] When pure lithium oxide powder is required, when the lithium salt is lithium carbonate, the powder comprising lithium oxide and the lithium salt is heated to a temperature ranging from about 25° C. below the melting point of the lithium salt to about 200° C. above the melting point of the lithium salt to form lithium oxide powder.

[0058] When pure lithium oxide powder is required and the lithium salt is a lithium halide, the powder comprising lithium oxide and lithium salt is heated to a temperature ranging from about 25°C below the boiling point of the lithium salt to about 200°C above the boiling point of the lithium salt to form lithium oxide powder. The lithium halide may be lithium chloride, lithium bromide or lithium iodide.

[0059] When a non-reactive additive is used in the process of forming a powder comprising lithium oxide and a lithium salt, and the non-reactive additive is not lithium oxide, it is preferred to remove the non-reactive additive from the powder comprising lithium oxide and a lithium salt before heating the powder comprising lithium oxide and a lithium salt to a desired temperature to convert the lithium salt into lithium oxide.

[0060] For a process for preparing pure lithium oxide powder from a powder comprising lithium oxide and a lithium salt, the amount of lithium salt present in the powder comprising lithium oxide and a lithium salt is generally about 10% by weight or less, often about 5% by weight or less, and often about 3% by weight or less; typically, the amount of lithium salt in the powder comprising lithium oxide and a lithium salt is about 0.1% by weight or more. In some embodiments, the amount of lithium salt present in the powder comprising lithium oxide and a lithium salt is in the range of about 0.1% by weight to about 10% by weight, or about 0.1% by weight to about 5% by weight, or about 0.1% by weight to about 3% by weight.

[0061] Heating a powder comprising lithium oxide and a lithium salt generally converts the lithium salt into lithium oxide.

[0062] Heating the powder comprising lithium oxide and lithium carbonate to the desired reaction temperature is often carried out at a rate of about 3°C / min to about 100°C / min, preferably at a rate of about 5°C / min to about 50°C / min, and more preferably at a rate of about 8°C / min to about 50°C / min.

[0063] When the desired temperature is reached, the powder comprising lithium oxide and a lithium salt may be heated at that temperature for the length of time required to form lithium oxide from the lithium salt. During the process, the temperature may vary. The time is affected to some extent by the reaction temperature, the temperature profile of the combination of the two lithium salts and the non-reactive additive, the reaction zone, and the amount of lithium salt present. On a laboratory scale, the reaction time is in the range of about 5 minutes to about 25 hours.

[0064] When the lithium salt is lithium carbonate, the temperature of the heating process of the powder comprising lithium oxide and lithium salt is in the range of about 25°C below the melting point of the lithium salt to about 200°C above the melting point of the lithium salt, preferably about 25°C below the melting point of the lithium salt to about 175°C above the melting point of the lithium salt, more preferably about 25°C below the melting point of the lithium salt to about 100°C above the melting point of the lithium salt. Although temperatures above about 200°C above the melting point of the lithium salt can be used, they do not provide any particular advantage. When the lithium salt is lithium carbonate, the temperature is preferably in the range of about 700°C to about 900°C, more preferably in the range of about 700°C to about 800°C, and even more preferably in the range of about 700°C to about 750°C. In some preferred embodiments where the lithium salt is lithium carbonate, the temperature is preferably in the range of about 700°C to about 750°C.

[0065] In the process of forming pure lithium oxide from a powder comprising lithium oxide and a lithium salt, water is removed by heating under reduced pressure, or in the presence of an inert gas or an oxygen-containing inert gas, preferably a flowing inert gas or an oxygen-containing inert gas. The inert gas and the oxygen-containing inert gas are described above as processes for heating two lithium salts.

[0066] Preferably, the process of forming pure lithium oxide from a powder comprising lithium oxide and a lithium salt is carried out in the presence of an inert gas or an oxygen-containing inert gas flow, which will remove gaseous byproducts from the reaction zone. The flow rate of the inert gas or the oxygen-containing inert gas is preferably about 25 sccm or greater, or in the range of about 25 sccm to about 1000 sccm, more preferably about 50 sccm to about 500 sccm.

[0067] When the process is carried out under reduced pressure, the pressure is preferably about 608 Torr (81 kPa) or less, more preferably about 380 Torr (51 kPa) or less, still more preferably about 230 Torr (31 kPa) or less, and even more preferably about 20 Torr (2.7 kPa) or less. Optionally, an inert gas or an oxygen-containing inert gas may be fed to the reaction zone while maintaining the reduced pressure.

[0068] The product of heating a powder comprising lithium oxide and a lithium salt is a lithium oxide powder containing little or no lithium salt; lithium oxide is air sensitive and is generally a free-flowing powder.

[0069] Figure 2 B is an XRD pattern of a product formed according to the process of the present invention. In the diffraction pattern, there is a large peak (Li2O) at a 2θ value of 34 degrees; no peak of lithium carbonate is observed.

[0070] The following examples are presented for purposes of illustration and are not intended to impose limitations on the scope of the invention.

[0071] Some of the embodiments of the present invention have incomplete conversion of the low melting point lithium salt to lithium oxide. In these cases, a higher conversion to lithium oxide can be achieved by heating for a longer period of time and / or using a higher inert gas flow rate.

[0072] Example 1

[0073] Lithium hydroxide monohydrate (LiOH·H2O; 85 wt%) was combined with Li2CO3 (5 wt%) and Li2O (10 wt%) in an acoustic mixer. After mixing at ambient temperature for a few minutes, the mixture was transferred to an alumina crucible and heated to 410°C at a rate of 10°C / min and maintained at 410°C for 10 hours under argon flowing at 60 sccm. When the temperature reached 100°C, heat loss and weight loss were observed. Additional weight loss was observed during heating at 410°C for 10 hours. The mixture was cooled to ambient temperature under argon flow to obtain a free-flowing powder ( Figure 1 A) An x-ray powder diffraction pattern was collected on a sample of the cooled product. Figure 2 The obtained diffraction pattern is shown in A. In the diffraction pattern, a large peak was observed at a 2θ value of 33.6 degrees, which is a characteristic peak of Li2O. Small peaks at 2θ values ​​of 12 degrees and 22 degrees are attributed to a small amount of Li2CO3 or LiOH (LiOH comes from the reaction of lithium oxide with water vapor) in the product.

[0074] The product powder in the above step was heated to 700°C at a rate of 10°C / min in an alumina crucible and maintained at 700°C for 5 hours under argon flowing at 60 sccm. Weight loss was observed during heating at 700°C for 5 hours. The mixture was cooled to ambient temperature under argon to obtain a free-flowing powder. An x-ray powder diffraction pattern was collected on a sample of the cooled product. Figure 2 The obtained diffraction pattern is shown in B. In the diffraction pattern, a large peak was observed at a 2θ value of 34 degrees, which is a characteristic peak of Li2O, while a group of smaller peaks were observed at 38 degrees, which can also be attributed to Li2O. No peak of Li2CO3 was observed.

[0075] Example 2

[0076] Lithium hydroxide monohydrate was exposed to air at room temperature for 3 hours to form a Li2CO3 coating (about 10 wt% Li2CO3) on LiOH·H2O. The coated LiOH·H2O was combined with Li2O (10 wt%) in an acoustic mixer. After mixing at ambient temperature for a few minutes, the mixture was transferred to an alumina crucible and heated to 410°C at a rate of 10°C / min and maintained at 410°C for 15 hours under argon flowing at 60 sccm. The mixture was cooled to ambient temperature under argon flow to obtain a free-flowing powder. X-ray powder diffraction patterns were collected on a sample of the cooled product. Figure 3 The obtained diffraction pattern is shown in . In the diffraction pattern, a large peak (Li2O) was observed at a 2θ value of 33 degrees, while small peaks were observed at 2θ values ​​of 30.7 degrees and 31.7 degrees, which were attributed to a small amount of Li2CO3 in the product.

[0077] Example 3

[0078] Lithium hydroxide monohydrate was combined with Li2CO3 (10 wt%). This mixture was heated to 410°C at a rate of 10°C / min in an alumina crucible and maintained at 410°C for 5 hours under argon flowing at 60 sccm. The mixture was cooled to ambient temperature under argon flow to obtain a powder. An x-ray powder diffraction pattern was collected on a sample of the cooled product. Figure 4 The obtained diffraction pattern is shown in . In the diffraction pattern, a large peak (LiOH) was observed at a 2θ value of 32.5 degrees, while a medium-sized peak (Li2O) was observed at 33.6 degrees, and small peaks were observed at 2θ values ​​of 30.5 degrees and 31.7 degrees, which are attributed to a small amount of Li2CO3 in the product. Due to the relative sizes of the LiOH and Li2O peaks, it was concluded that LiOH was only partially converted to Li2O. Figure 1 In B an image of the product (agglomerated powder) is shown.

[0079] Example 4 - Comparative

[0080] Lithium hydroxide monohydrate powder was heated to 480°C at a rate of 10°C / min in an alumina crucible and maintained at 480°C for 5 hours under argon flowing at 60 sccm. After one hour, the conversion of LiOH to Li2O was complete. The product was cooled to ambient temperature under argon flow. The product was not a free-flowing powder. At ambient temperature, the product coated the walls of the alumina crucible. Figure 1 An image of the product is shown in C; the solid is not a powder, but rather extensive melting occurred during the process.

[0081] Example 5

[0082] Lithium hydroxide monohydrate (LiOH·H2O; 85 wt%) was combined with Li2CO3 (5 wt%) and Li2O (10 wt%) in an acoustic mixer. After mixing for a few minutes at ambient temperature, the mixture was transferred to an alumina crucible and heated to 410°C at a rate of 10°C / min and maintained at 410°C for 10 hours under argon flowing at 60 sccm. When the temperature reached 100°C, heat loss and weight loss were observed. Additional weight loss was observed during heating at 410°C for 10 hours. The mixture was cooled to ambient temperature under an argon flow to obtain a free-flowing powder. An x-ray powder diffraction pattern was collected on a sample of the cooled product. In the diffraction pattern, a large peak was observed at a 2θ value of 33.6 degrees, which is a characteristic peak of Li2O. The small peaks at 2θ values ​​of 12 degrees and 22 degrees are attributed to a small amount of Li2CO3 or LiOH in the product (LiOH comes from the reaction of lithium oxide with water vapor).

[0083] The product powder in the above step was heated to 700°C at a rate of 10°C / min in an alumina crucible and maintained at 700°C for 5 hours under argon flowing at 60 sccm. Weight loss was observed during heating at 700°C for 5 hours. The mixture was cooled to ambient temperature under argon to obtain a free-flowing powder. An x-ray powder diffraction pattern was collected on a sample of the cooled product. In the diffraction pattern, a large peak was observed at a 2θ value of 34 degrees, which is a characteristic peak of Li2O, while a group of smaller peaks were observed at 38 degrees, which can also be attributed to Li2O. No peak of Li2CO3 was observed.

[0084] Example 6

[0085] Two attempts were made in which lithium hydroxide monohydrate (LiOH·H2O; 90 wt%) was combined with Li2CO3 and Li2O (approximately 10 wt%) in an acoustic mixer. In one attempt, 0.3 wt% lithium carbonate was added; in the other attempt, 0.5 wt% lithium carbonate was added, for a total of 0.4 wt% lithium carbonate and 0.6 wt% lithium carbonate. After mixing for a few minutes at ambient temperature, each mixture was transferred to an alumina crucible and heated to 410°C at a rate of 10°C / min and maintained at 410°C for 10 hours under argon flowing at 60 sccm. When the temperature reached 100°C, heat loss and weight loss were observed. Additional weight loss was observed during heating at 410°C for 10 hours. The mixture was cooled to ambient temperature under an argon flow to obtain a free-flowing powder.

[0086] Example 7

[0087] Three attempts were made in which lithium hydroxide monohydrate (LiOH·H2O; 90 wt%) was combined with Li2CO3 and Li2O in an acoustic mixer and heated at 410°C as described in Example 6. Attempt 1 had 0.1 wt% lithium carbonate, 10 wt% lithium oxide, and unground LiOH, with an average particle size of 600 μm. Attempts 2 and 3 had 0.7 wt% lithium carbonate (0.6 wt% lithium carbonate added) and 10 wt% lithium oxide. In attempt 2, the LiOH was unground, with an average particle size of 600 μm. In attempt 3, the LiOH was ground to an average particle size of 10 μm. Attempts 2 and 3 were maintained at 410°C for 20 hours.

[0088] The products of attempts 2 and 3 were heated to 800° C. at a rate of 10° C. / min in an alumina crucible and held at 800° C. for 30 minutes under argon flowing at 60 seem. The products were cooled to ambient temperature under argon to obtain a free-flowing powder.

[0089] Example 8

[0090] An attempt was made in which unground lithium hydroxide monohydrate (LiOH.H2O; 90 wt%) was combined with 0.2 wt% Li2CO3 and 10 wt% Li2O in an acoustic mixer and heated as described in Example 6, except that the temperature was held at 418°C for 10 hours, then at 430°C for 5 hours, then at 440°C for 5 hours, and then at 450°C for 5 hours. An x-ray powder diffraction pattern was collected on a sample of the cooled product. The diffraction pattern showed that about 1.1 wt% LiOH remained in the product, indicating that stepwise heating provides a higher conversion to lithium oxide, at least for the conversion of lithium hydroxide.

[0091] Example 9

[0092] Two attempts were made in which lithium hydroxide monohydrate (LiOH.H2O; 20 wt%) was combined with 2.65 wt% Li2CO3 and 80 wt% Li2O in an acoustic mixer and heated as described in Example 6, except that the temperature was 450°C, the time was 10 hours, and the crucible was Pt / Rh / alumina. In one attempt, the LiOH was not ground, while in the other attempt, the LiOH was ball milled for 20 minutes before combining with the other ingredients.

[0093] The powder obtained from the attempt using ball-milled LiOH was partially agglomerated. An x-ray powder diffraction pattern was collected on a sample of the cooled product from the unmilled LiOH attempt; the diffraction pattern showed peaks from LiOH·H2O, indicating incomplete conversion to Li2O. An x-ray powder diffraction pattern was collected on a sample of the cooled product from the milled LiOH attempt; the diffraction pattern showed peaks from LiOH·H2O, indicating contamination from air exposure or incomplete conversion to Li2O.

[0094] Example 10

[0095] Lithium hydroxide monohydrate (LiOH·H2O, 20 g) containing Li2CO3 (0.3 wt%) in an alumina crucible was placed in a vertical furnace set at a temperature of 450°C (actual temperature about 425°C) and placed under argon flowing at 5 L / min (5000 sccm) for 3 hours. The mixture was cooled to ambient temperature under argon flow to obtain a free-flowing powder. An x-ray powder diffraction pattern was collected on a sample of the cooled product. The diffraction pattern obtained showed that the product contained 23 wt% Li2O and 77 wt% LiOH.

[0096] Components referred to by chemical name or chemical formula anywhere in this specification or its claims (whether referred to in singular or plural form) are identified as existing before contacting another substance (e.g., another component, solvent, etc.) referred to by chemical name or chemical type. It is not important what kind of chemical changes, transformations and / or reactions (if any) occur in the resulting mixture or solution, because such changes, transformations and / or reactions are the natural result of putting the specified components together under the conditions required by the present disclosure. Therefore, these components are identified as ingredients that are put together to perform the desired operation or form the desired composition. In addition, although the claims below may refer to substances, components and / or ingredients in the present tense ("comprises", "is", etc.), the substances, components or ingredients mentioned refer to their simultaneous existence just before contacting, blending or mixing with one or more other substances, components and / or ingredients according to the present disclosure for the first time. Therefore, the fact that substances, components or ingredients may lose their original properties through chemical reactions or transformations during the course of contacting, blending or mixing operations is of no practical significance if carried out in accordance with the present disclosure and the ordinary skills of a chemist.

[0097] The present invention may comprise, consist of, or consist essentially of the materials and / or procedures described herein.

[0098] As used herein, the term "about," which modifies the quantity of an ingredient in a composition of the invention or an ingredient used in a method of the invention, refers to variations in numerical amounts that may occur, for example, in the following processes: typical measurements and liquid handling procedures used in the real world to prepare concentrates or use solutions; errors due to inadvertence in these procedures; differences in the manufacture, source, or purity of ingredients used to prepare the composition or practice the method; and the like. The term about also encompasses amounts that differ due to different equilibrium conditions of the composition resulting from a particular initial mixture. Whether or not modified by the term "about," the claims include equivalent values ​​of the quantities.

[0099] Unless expressly stated otherwise, the article "a / an" (if and as used herein) is not intended to limit the description or claims to the single element to which the article refers and should not be interpreted as limiting the description or claims to the single element to which the article refers. Instead, the article "a / an" (if and as used herein) is intended to cover one or more such elements unless the context clearly indicates otherwise.

[0100] The invention is susceptible to considerable variation in its practice.Accordingly, the foregoing description is not intended to limit the invention and should not be construed as limiting the invention to the particular examples presented above.

Claims

1. A process for producing a powder comprising lithium oxide and a lithium salt, the process comprising heating a mixture of two lithium salts at one or more temperatures ranging from about 50°C below the eutectic point of the mixture of the two lithium salts to a temperature below the melting point of the lithium salt with the lower melting point, while removing at least a portion of the gaseous by-products produced by the process, and optionally wherein a non-reactive additive is present in the mixture of the two lithium salts, to form a powder comprising lithium oxide and a lithium salt.

2. The process of claim 1, wherein the heating is performed at one or more temperatures ranging from about 20°C below the eutectic point of the mixture of two lithium salts to a temperature below the melting point of the lithium salt having the lower melting point.

3. A process as claimed in claim 1 or 2, wherein the two lithium salts are selected from lithium nitrate and lithium bromide; lithium hydroxide and lithium bromide; lithium bromide and lithium carbonate; lithium hydroxide and lithium carbonate; lithium bromide and lithium chloride; and lithium nitrate and lithium iodide.

4. The process of claim 1, wherein the two lithium salts are lithium nitrate and lithium bromide, and the temperature is in the range of about 178°C to about 255°C or less; lithium hydroxide and lithium bromide, and the temperature is in the range of about 225°C to about 470°C or less; lithium bromide and lithium carbonate, and the temperature is in the range of about 446°C to about 550°C or less; or lithium hydroxide and lithium carbonate, and the temperature is in the range of about 380°C to about 470°C or less; or Lithium bromide and lithium chloride, and the temperature is in the range of about 471°C to about 550°C or less.

5. The process of claim 4, wherein the two lithium salts are lithium hydroxide and lithium carbonate.

6. The process of any one of claims 2 to 5, wherein the two lithium salts are lithium hydroxide and lithium carbonate, and wherein the lithium carbonate is formed in situ in the presence of the lithium hydroxide.

7. The process of claim 5 or 6, wherein lithium carbonate is in an amount of about 0.1 wt. % to about 20 wt. % relative to the total weight of the mixture.

8. The process of any one of claims 5 to 7, wherein the temperature is in the range of about 380°C to about 460°C.

9. The process of any one of claims 2 to 8, wherein the lithium hydroxide is anhydrous lithium hydroxide.

10. The process of any one of claims 2 to 8, wherein the lithium hydroxide is lithium hydroxide monohydrate.

11. The process of any one of claims 1 to 10, wherein a non-reactive additive is present and is selected from quartz, silica beads, zirconium oxide beads and lithium oxide.

12. The process of any one of claims 1 to 10, wherein a non-reactive additive is present and is lithium oxide.

13. The process of any one of claims 1 to 12, wherein a non-reactive additive is present in an amount of about 1 wt % to about 90 wt % relative to the total weight of the mixture.

14. The process of any one of claims 1 to 12, wherein a non-reactive additive is present in an amount of about 20 wt % to about 90 wt % relative to the total weight of the mixture.

15. The process of any one of claims 1 to 14, wherein the process is performed in the presence of an inert gas or an oxygen-containing inert gas flowing at a rate of about 25 seem or greater.

16. The process of claim 15, wherein the inert gas is one or more of helium, nitrogen and argon.

17. The process of any one of claims 1 to 14, wherein the process is carried out at a pressure below atmospheric pressure.

18. The process of any one of claims 1 to 14, wherein the process is carried out at a pressure of about 81 kPa or less.

19. The process of claim 1, further comprising heating the powder comprising lithium oxide and lithium carbonate to a temperature in the range of about 25°C below the melting point of lithium carbonate to about 200°C above the melting point of lithium carbonate to form lithium oxide powder.

20. A process comprising heating a powder comprising lithium oxide and lithium carbonate at one or more temperatures in the temperature range of about 25°C below the melting point of lithium carbonate to about 200°C above the melting point of lithium carbonate to form lithium oxide powder.

21. The process of claim 19 or 20, wherein the temperature is in the range of about 700°C to about 900°C.

22. A process comprising heating a powder comprising lithium oxide and a lithium halide at one or more temperatures in the temperature range of about 25°C below the boiling point of the lithium halide to about 200°C above the boiling point of the lithium halide to form a lithium oxide powder.

23. A powder comprising lithium oxide and a lithium salt, wherein the lithium salt is about 0.1% by weight or more of the powder.

24. The powder of claim 23 comprising lithium oxide and lithium carbonate, wherein the lithium carbonate is about 0.3% or more by weight of the powder.

25. The powder of claim 24, wherein the lithium carbonate is from about 0.3% to about 20% by weight of the powder.