Photosensitive resin composition, dry film, cured product, printed circuit board, and laminate

By using a photosensitive resin composition containing carboxyl group-containing resin, inorganic filler and P-O bond photopolymerization initiator without aromatic rings, the gas release problem in the photosensitive resin composition is solved, and the reaction rate and reflectivity of the silicone sealant are improved. Enhanced resistance to yellowing and stability of solder resist under high temperature and high humidity conditions.

CN119095903APending Publication Date: 2024-12-06TAIYO INK MFG CO KOREALTD

Patent Information

Application Number
CN202480002122.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-27
Filing Date
2024-03-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Conventional photopolymerization initiators in existing photosensitive resin compositions produce a large amount of air release during the curing process, resulting in yellowing and incomplete curing of silicone sealants, affecting reflectivity and long-term reliability, and existing solutions such as firing processes Increased power consumption and process number.

Method used

A photopolymerization initiator with a carboxyl-containing resin without aromatic rings, an inorganic filler and a trimethylbenzoylphosphine oxide group containing a P-O bond is combined with a thiol-modified (meth)acrylate to form a photosensitive resin combination reduces gas release and increases the reaction rate of silicone sealant.

Benefits of technology

The air release amount of the photopolymerization initiator is significantly reduced, the reaction rate and reflectivity of the silicone sealant are improved, the firing process is omitted, and the anti-yellowing properties of the solder resist and the stability under high temperature and high humidity conditions are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095903A_ABST
    Figure CN119095903A_ABST
Patent Text Reader

Abstract

A photosensitive resin composition includes: (A) a carboxyl group-containing resin that does not contain an aromatic ring; (B) an inorganic filler; and (E) a photopolymerization initiator comprising a trimethylbenzoyl phosphine oxide group-containing compound having at least one P-O bond, in which outgassing of the photopolymerization initiator can be significantly reduced by the combination of the four components of the photosensitive resin composition to solve the yellowing and incomplete curing of a silicone sealant, and to improve the durability of the sealant. According to the present invention, the photopolymer initiator is added to the protective film, the reaction rate of the silicone sealant is increased, the amount of outgas transferred from the photopolymer initiator to the protective film can be reduced, and the firing step after the reflux step can be omitted to increase the reflectance, thereby solving the problems related to power consumption, having high HAST resistance and high reflectance after the HAST test, and having excellent thermal stability. According to the present invention, the photosensitive resin composition can be used to produce a solder resist, and a decrease in reflectivity under a high temperature / high humidity condition can be suppressed, so that these characteristics of the photosensitive resin composition enable the produced solder resist to exhibit an excellent effect, so that the photosensitive resin composition can effectively provide an open hole for the solder resist, thereby improving the reliability of the solder resist. And an efficient backlight unit can be realized through the solder resist with high reflectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a photosensitive resin composition, a dry film, a cured product, a printed circuit board and a laminated board, wherein the dry film has a photosensitive resin layer formed by coating and drying the photosensitive resin composition on a first film, the cured product is obtained by curing the photosensitive resin layer of the dry film, and the printed circuit board and the laminated board each include the cured product. Background Art

[0002] For printed circuit boards used in electronic devices, etc., when electronic components are mounted on the printed circuit boards, in order to prevent solder from adhering to unnecessary parts and to prevent circuit conductors from being exposed and corroded due to oxidation or moisture, a solder resist layer is usually formed on the area of ​​the board having a circuit pattern except for the connection holes.

[0003] With the lightweight and miniaturization of electronic equipment, printed circuit boards have recently had high precision and high density. Recently, the solder resist layer is usually formed by applying a photosensitive resin composition to a substrate, forming a pattern by exposure and development, and then curing the patterned resin by heating or light irradiation, which is the so-called photo solder resist.

[0004] The above-mentioned liquid photosensitive resin composition contains a solvent, and the printing and composition drying processes need to be repeated during the production process, resulting in a long working time and being environmentally unfriendly.

[0005] Instead of using a liquid photosensitive resin composition, it has been proposed to use a so-called photosensitive dry film to form a solder resist layer, which enables the drying process after applying the composition to be omitted. Lamination using a dry film reduces working time, thereby significantly shortening the manufacturing process and improving productivity, while effectively utilizing the solder resist layer even on a film board.

[0006] This dry film generally includes a laminated structure, in which a solder mask as a photosensitive resin layer is formed on a first film as a substrate, and a second film for the purpose of protection, etc. is bonded to the layer. During use, after peeling off the second film, the dry film is hot pressed onto the circuit board, and exposed on the first film, peeled off the first film, and then developed to form a patterned solder mask. Compared with using a liquid photosensitive resin composition as described above, the use of a dry film to form a solder mask can not only omit the drying process of the composition, but also improve the hole filling performance at the recessed part of the board surface, because the dry film is pressed on the circuit board, resulting in the difficulty of introducing bubbles between the board and the solder mask. In addition, the use of a dry film to form a solder mask ensures good flatness of the film, so that the chip can be effectively installed and high resolution can be achieved.

[0007] At the same time, the white solder resist has a higher reflectivity than the colored solder resist, and therefore, when the solder resist is formed using a dry film by the same method as described above, light is reflected from the surface of the solder resist during exposure, so that it is difficult for light to penetrate to the lower part of the solder resist, and a phenomenon (halo) occurs on the surface where the upper part is larger than the lower part, resulting in difficulty in realizing the pattern (for example, see patent document 1).

[0008] The solder resist layer also functions as a permanent protective film for the circuit board, and thus the solder resist composition is required to have various properties, such as alkali developability and solder heat resistance.

[0009] Furthermore, in addition to meeting the requirements as a general solder resist, the white solder resist must also have high reflectivity to minimize the reduction in reflectivity during the manufacturing process and prevent the cured product from yellowing when exposed to heat and light.

[0010] What is needed: a photosensitive resin composition that not only meets the basic requirements for a solder mask, but also meets the additional requirements for a white solder mask, has higher reflectivity and excellent yellowing resistance compared to the prior art; a dry film including a solder mask that can solve unique problems that arise during the solder mask manufacturing process; and a method for manufacturing a printed circuit board.

[0011] (Patent Document 1) Korean Patent Publication No. 10-2022-0086524. Summary of the invention

[0012] Technical issues

[0013] Conventional photopolymerization initiators (e.g., 2,4,6-trimethylbenzoyldiphenyl phosphine oxide (TPO)) contained in the photosensitive resin composition forming the solder resist generate a large amount of outgassing, and when this outgassing diffuses into the adjacent silicone sealant, the transparent silicone sealant may yellow, thereby reducing the reflectivity and causing incomplete curing of the silicone sealant. These disadvantages lead to long-term reliability problems of the board. In addition, the photopolymerization initiator can be transferred not only to the silicone sealant but also to the adjacent board.

[0014] In order to remove outgassing of the photopolymerization initiator, it has been considered to add a firing process (e.g., curing at 150°C for 6 hours) after the reflow process (e.g., at 260°C for 10 seconds), but when the photopolymerization initiator is used for a backlight unit or the like, such a firing process significantly reduces the reflectivity, resulting in increased power consumption in order to improve the reflectivity after chip mounting. In other words, the number of processes may increase and the reflectivity may also decrease.

[0015] In addition, before the firing process, a protective film (PF) can be placed on the solder resist layer to remove the photopolymerization initiator. The protective film is used to remove as much outgassing of the photopolymerization initiator as possible after the preparation of the solder resist and before the subsequent firing process, and the protective film is eliminated by peeling before the firing process. The protective film can effectively remove the photopolymerization initiator due to its high affinity for the photopolymerization initiator, so the protective film is used for the purpose of removing the photopolymerization initiator. However, this requires two processes related to the use of such a protective film and the firing process, and does not solve the reduction in reflectivity.

[0016] Various embodiments of the present disclosure provide a photosensitive resin composition, comprising: (A) a carboxyl-containing resin without an aromatic ring; (B) an inorganic filler and / or (C) a mercapto-modified (meth)acrylate; and (E) a photopolymerization initiator of a compound containing a trimethylbenzoylphosphine oxide group having at least one PO bond.

[0017] According to the photosensitive resin composition of the present disclosure, the outgassing of the photopolymerization initiator can be significantly reduced to solve the yellowing and incomplete curing of the silicone sealant and increase the reaction rate of the silicone sealant. In addition, the outgassing amount generated by the photopolymerization initiator can be suppressed to reduce the outgassing amount transferred to the protective film, and the firing process after the reflow process can be omitted to increase the reflectivity, thereby solving problems related to power consumption. In addition, the photosensitive resin composition of the present disclosure can exhibit excellent high accelerated stress test (HAST) resistance, high reflectivity after reflow, UV test or HAST test, and suppress the reduction of reflectivity under high temperature / high humidity conditions. These characteristics of the photosensitive resin composition of the present disclosure enable the produced solder resist to exert excellent effects.

[0018] Various embodiments of the present disclosure provide a dry film, a cured product, a printed circuit board, and a laminated board, all using the photosensitive resin composition.

[0019] Means of solving the problem

[0020] According to one aspect of the present disclosure, a photosensitive resin composition is provided.

[0021] The photosensitive resin composition according to one embodiment of the present disclosure may include: (A) a carboxyl-containing resin having no aromatic ring; (B) an inorganic filler; and (E) a photopolymerization initiator of a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond.

[0022] In the photosensitive resin composition according to one embodiment of the present disclosure, the photopolymerization initiator (E) of a compound containing a trimethylbenzoylphosphine oxide group having at least one PO bond may include a *-C(=O)-P(=O)R1-O-*' portion (wherein R1 is an alkyl group of 1 to 20 carbon atoms, an alkenyl group of 2 to 20 carbon atoms, an alkynyl group of 2 to 20 carbon atoms, or a cyclic group of 5 to 20 carbon atoms).

[0023] In the photosensitive resin composition according to one embodiment of the present disclosure, the (E) photopolymerization initiator of the trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond may be a trimethylbenzoylphosphine oxide group-containing polymer.

[0024] In the photosensitive resin composition according to one embodiment of the present disclosure, the polymer containing a trimethylbenzoylphosphine oxide group may have a weight average molecular weight (Mn) of 900 g / mol or more.

[0025] In the photosensitive resin composition according to one embodiment of the present disclosure, the polymer containing a trimethylbenzoylphosphine oxide group may be represented by the following Chemical Formula 1:

[0026] <Chemical Formula 1>

[0027]

[0028] a=0 to 100, b=0 to 100, and c=0 to 100.

[0029] In the photosensitive resin composition according to one embodiment of the present disclosure, the (E) photopolymerization initiator of the trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond may include an alkoxy group.

[0030] In the photosensitive resin composition according to one embodiment of the present disclosure, the (E) photopolymerization initiator of the trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond may include an ethoxy group.

[0031] In the photosensitive resin composition according to one embodiment of the present disclosure, (E) the photopolymerization initiator of a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond may be represented by the following Chemical Formula 2:

[0032] <Chemical Formula 2>

[0033]

[0034] In the photosensitive resin composition according to one embodiment of the present disclosure, the photopolymerization initiator of (E) a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond may be included in an amount of 0.01 wt % to 10 wt % relative to the total weight of the composition.

[0035] In the photosensitive resin composition according to one embodiment of the present disclosure, (A) the carboxyl-containing resin having no aromatic ring may have an unsaturated double bond.

[0036] In the photosensitive resin composition according to one embodiment of the present disclosure, the photosensitive resin composition may further include (D) a resin containing an aromatic ring.

[0037] In the photosensitive resin composition according to one embodiment of the present disclosure, (D) the resin containing an aromatic ring may be a melamine resin, a silicone resin, or a resin having a styrene main chain.

[0038] In the photosensitive resin composition according to one embodiment of the present disclosure, the photosensitive resin composition may further include (C) mercapto-modified (meth)acrylate.

[0039] In the photosensitive resin composition according to one embodiment of the present disclosure, the photosensitive resin composition may further include (F) a silane coupling agent.

[0040] In the photosensitive resin composition according to one embodiment of the present disclosure, the photosensitive resin composition may further include (G) a resin having a urethane bond.

[0041] In the photosensitive resin composition according to one embodiment of the present disclosure, the outgassing content of the photosensitive resin composition measured by thermal desorption spectroscopy (TDS) and gas chromatography-mass spectrometry (GC-MS) may be 1000 ppm or less relative to the photopolymerization initiator of (E) a compound containing a trimethylbenzoylphosphine oxide group having at least one PO bond.

[0042] In the photosensitive resin composition according to one embodiment of the present disclosure, the content of phosphorus may be 500 ppm to 5000 ppm.

[0043] The photosensitive resin composition according to one embodiment of the present disclosure may include: (A) a carboxyl-containing resin without an aromatic ring; (C) a mercapto-modified (meth)acrylate; and (E) a photopolymerization initiator of a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond.

[0044] In the photosensitive resin composition according to one embodiment of the present disclosure, the photosensitive resin composition may further include (D) a resin containing an aromatic ring.

[0045] In the photosensitive resin composition according to one embodiment of the present disclosure, the photosensitive resin composition may further include (F) a silane coupling agent.

[0046] In the photosensitive resin composition according to one embodiment of the present disclosure, the photosensitive resin composition may further include (G) a resin having a urethane bond.

[0047] The dry film according to one embodiment of the present disclosure may have a photosensitive resin layer formed by coating the photosensitive resin composition on a first film and drying the layer.

[0048] The cured product according to one embodiment of the present disclosure may be obtained by curing the photosensitive resin composition or a dry film photosensitive resin layer obtained from the photosensitive resin composition.

[0049] A printed circuit board according to one embodiment of the present disclosure may include the cured product as a solder resist.

[0050] The printed circuit board according to one embodiment of the present disclosure may further include a silicone sealant disposed on the solder resist.

[0051] In a printed circuit board according to one embodiment of the present disclosure, the silicone sealant includes an upper sealant region and a lower sealant region, and the content of the photopolymerization initiator of the (E) trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond contained in the upper sealant region or the lower sealant region is 1000 ppm or less relative to the content of the photopolymerization initiator of the (E) trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond contained in the solder resist.

[0052] A laminate according to one embodiment of the present disclosure may include: the cured product; and a protective film.

[0053] In a laminate according to one embodiment of the present disclosure, the content of the photopolymerization initiator of the (E) trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond contained in the protective film is 1000 ppm or less relative to the content of the photopolymerization initiator of the (E) trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond contained in the solder resist.

[0054] Effects of the Invention

[0055] According to some embodiments of the present disclosure, for the photosensitive resin composition, the outgassing of the photopolymerization initiator can be significantly reduced to solve the yellowing and incomplete curing of the silicone sealant and increase the reaction rate of the silicone sealant. In addition, the outgassing amount transferred from the photopolymerization initiator to the protective film can be reduced, and the firing process after the reflow process can be omitted to increase the reflectivity, thereby solving problems related to power consumption. In addition, the HAST resistance and the reflectivity after the HAST test are high, and the reduction in reflectivity under high temperature / high humidity conditions can be suppressed. These characteristics of the photosensitive resin composition of the present disclosure enable the produced solder resist to exert excellent effects.

[0056] For example, the photosensitive resin composition according to one aspect of the present disclosure may obtain an excellent reflectivity maintaining effect by further including titanium oxide as an inorganic filler.

[0057] According to the present disclosure, in some embodiments, a dry film, a cured product, a printed circuit board, and a laminated board, all of which use the photosensitive resin composition, may also be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1a and Figure 1b are images showing BHAST test results of dry films using the photosensitive resin compositions of Comparative Example 1 and Example 3, respectively. DETAILED DESCRIPTION

[0059] Various aspects of the disclosure will be described below.

[0060] [Photosensitive resin composition]

[0061] One aspect of the present disclosure relates to a photosensitive resin composition, including: (A) a carboxyl-containing resin without an aromatic ring; (B) an inorganic filler; and (E) a photopolymerization initiator selected from a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond.

[0062] Another aspect of the present disclosure relates to a photosensitive resin composition, comprising: (A) a carboxyl-containing resin without an aromatic ring; (C) a mercapto-modified (meth)acrylate; and (E) a photopolymerization initiator selected from a compound containing a trimethylbenzoylphosphine oxide group having at least one PO bond.

[0063] The photosensitive resin composition can suppress degassing and exhibit excellent silicone sealant reaction rate, reflectivity and HAST resistance.

[0064] For example, the photosensitive resin composition may be a composition that is cured to form a solder resist.

[0065] Next, each component of the photosensitive resin composition will be described in detail.

[0066] [(A) Carboxyl-containing resin not containing aromatic ring]

[0067] In the photosensitive resin composition according to one embodiment of the present disclosure, (A) a carboxyl-containing resin not containing an aromatic ring (hereinafter referred to as "resin (A)") may be a resin that is cured by irradiation with active energy rays to exhibit electrical insulation. Examples of the aromatic ring may include a benzene ring, a pyridine ring, a pyrimidine ring, a triazine ring, and the like.

[0068] Resin (A) can be alkaline developed by containing carboxyl groups, and has excellent resistance to discoloration or yellowing when subjected to heat or UV energy due to the absence of aromatic rings. In addition, combining resin (A) with inorganic filler (B) produces high reflectivity, less reflectivity reduction after the reflow process, and less reflectivity reduction after being subjected to a 3000-hour blue light test. Therefore, compared with other white ink compositions, the composition containing resin (A) has less reflectivity reduction caused by discoloration and yellowing, and shows excellent resistance to yellowing. For example, compared with resin (A) without aromatic rings, carboxyl-containing resins containing aromatic rings may show a relatively low initial reflectivity of the cured product, and the reflectivity is significantly reduced when subjected to heating, ultraviolet, BHAST and 85°C / 85% tests. The reason is that the aromatic rings are deformed in heat, ultraviolet, BHAST and 85°C / 85% tests, greatly resulting in a reduction in reflectivity.

[0069] For example, the resin (A) may have an unsaturated double bond. The resin (A) may be free radical-cured by ultraviolet rays, electron beams, or heat due to the presence of saturated double bonds therein.

[0070] The resin (A) is not particularly limited as long as it contains a carboxyl group but does not contain an aromatic ring. Examples thereof may be a photosensitive carboxyl group-containing resin having at least one photosensitive unsaturated double bond or a carboxyl group-containing resin having no photosensitive unsaturated double bond.

[0071] For example, a resin (any oligomer or polymer) not containing an aromatic ring from any of the following resins can be suitably used:

[0072] (1) carboxyl-containing resins obtained by copolymerization of unsaturated carboxylic acids and compounds having unsaturated double bonds;

[0073] (2) a photosensitive carboxyl group-containing resin obtained by reacting a carboxyl group-containing (meth)acrylic copolymer resin with a compound having an oxirane ring and an ethylenically unsaturated group in one molecule;

[0074] (3) a photosensitive carboxyl group-containing resin obtained by reacting a copolymer of an unsaturated monocarboxylic acid with a compound having an unsaturated double bond and a compound having one unsaturated double bond and one epoxy group in each molecule, and reacting a secondary hydroxyl group produced by the reaction with a saturated or unsaturated polyacid anhydride; and

[0075] (4) A resin containing photosensitive hydroxyl and carboxyl groups, obtained by reacting a hydroxyl-containing polymer with a saturated or unsaturated polybasic acid anhydride and then reacting compounds having one epoxy group and an unsaturated double bond in one carboxylic acid molecule produced by the reaction.

[0076] For example, the resin (A) may be a copolymer resin having a carboxyl group obtained by reacting (a) a carboxyl group-containing (meth)acrylic copolymer resin as the photosensitive carboxyl group-containing resin (2) with (b) a compound having an ethylene oxide ring and an ethylenically unsaturated group in one molecule.

[0077] For example, the carboxyl-containing (meth)acrylic copolymer resin (a) may be obtained by copolymerizing (meth)acrylic acid ester with a compound having one unsaturated group and at least one carboxyl group in one molecule, but is not limited thereto. Examples of (meth)acrylates constituting the copolymer resin (a) include: alkyl (meth)acrylates, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, and hexyl (meth)acrylate; (meth)acrylates containing hydroxyl groups, such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and caprolactone-modified 2-hydroxyethyl (meth)acrylate; and ethylene glycol-modified (meth)acrylates, such as methoxydiglycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, isooctyloxyethylene glycol (meth)acrylate, phenoxytriethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate. These may be used alone or in combination of two or more. Here, (meth)acrylate is a general term for acrylate and methacrylate, and the same applies to other similar expressions.

[0078] In addition, examples of compounds having one unsaturated group and at least one carboxyl group in one molecule may include: acrylic acid, methacrylic acid; modified unsaturated monocarboxylic acid having a chain extending between the unsaturated group and the carboxylic acid, for example, unsaturated monocarboxylic acid having an ester bond formed by β-carboxyethyl (meth) acrylate, 2-acryloyloxyethyl succinic acid, 2-acryloyloxyethyl hexahydrophthalic acid, lactone modification, etc.; modified unsaturated monocarboxylic acid having an ether bond; and those containing two or more carboxyl groups in the molecule, such as maleic acid, etc. These may be used alone or in combination of two or more.

[0079] The compound (b) having an oxirane ring and an ethylenically unsaturated group in one molecule may be any compound having an oxirane ring in one molecule, and examples thereof may include glycidyl (meth) acrylate, α-methyl glycidyl (meth) acrylate, 3,4-epoxycyclohexyl methyl (meth) acrylate, 3,4-epoxycyclohexyl ethyl (meth) acrylate, 3,4-epoxycyclohexyl butyl (meth) acrylate, 3,4-epoxycyclohexyl methylamino acrylate, etc. These may be used alone or in combination of two or more. For example, the compound (b) having an oxirane ring and an ethylenically unsaturated group in one molecule may be 3,4-epoxycyclohexyl methyl (meth) acrylate.

[0080] For example, the resin (A) may have an acid value of 30 mgKOH / g to 200 mgKOH / g. When the acid value of the resin (A) is 30 mgKOH / g or higher, the unexposed portion of the coating film of the solder resist composition can be easily removed in a weakly alkaline aqueous solution. When the acid value of the resin (A) is 200 mgKOH / g or lower, the water resistance and electrical properties of the cured film can be improved.

[0081] For example, the weight average molecular weight of the resin (A) may be 5000 g / mol to 100000 g / mol. When the weight average molecular weight of the resin (A) is 5000 g / mol or more, the deterioration of the dry touch of the coating film of the solder resist composition can be suppressed. When the weight average molecular weight of the resin (A) is 100000 g / mol or less, the deterioration of the developability and storage stability of the solder resist composition can be suppressed.

[0082] The content of the resin (A) in the photosensitive resin composition of the present disclosure may be 5wt% to 40wt%, 10wt% to 35wt% or 12wt% to 33wt% relative to the total weight of the resin composition. The composition includes solids and solvents. The content of the resin (A) may be calculated based on the solid content conversion.

[0083] When the content of the resin (A) is within the above range, excellent yellowing resistance and high reflectivity can be obtained, and a coating film of a solder resist can be formed favorably, excellent pencil hardness and adhesion can be exhibited, and a dry touch of the coating film and a reduction in undercut can be suppressed.

[0084] [(B) Inorganic filler]

[0085] The photosensitive resin composition according to one aspect of the present disclosure may obtain high reflectivity by including an inorganic filler.

[0086] Examples of inorganic fillers may include titanium oxide, zinc oxide, basic carbonate, basic sulfate, sulfate, zinc sulfide, antimony oxide, aluminum hydroxide, silicon dioxide, barium sulfate, etc. For example, when a mixture of barium sulfate and silicon dioxide is used as an inorganic filler to prepare a composition, the L value is 80 or more, the a value is -5 or more, and the b value is -5 or more. The L value can be measured by Hunter 1948. For example, when a composition is prepared by using a mixture of high-content titanium oxide and silicon dioxide as an inorganic filler, the cured product of the composition has an L value of 90 or more, an a value of -3 or more, and a b value of -3 or more, showing high whiteness and reflectivity. For example, when a composition is prepared by using at least one of titanium oxide or silicon dioxide as an inorganic filler, the L value is 95 or more, the a value is -2 or more, and the b value is -1 or more, showing the highest whiteness and reflectivity.

[0087] For example, the method for preparing titanium oxide may be any of a sulfuric acid method or a chlorine method, and may preferably be a chlorine method. For example, sulfuric acid may not be used in the preparation process. The surface treatment of titanium oxide is not particularly limited, but in the neutralization process, titanium oxide may be acid-treated with hydrochloric acid, nitric acid, phosphoric acid, acetic acid, etc. instead of sulfuric acid.

[0088] The titanium oxide may be any titanium oxide having any structure among rutile type, anatase type and ramsdellite type, which may be used alone or in combination of two or more. Among them, the ramsdellite type titanium oxide may be prepared by treating the ramsdellite type Li 0.5 TiO2 is obtained by chemical lithium oxide desorption treatment.

[0089] Among them, the use of rutile titanium oxide can further enhance heat resistance, minimize discoloration caused by light irradiation, and prevent quality degradation even in a strict use environment. In particular, heat resistance can be improved by using rutile titanium oxide that has been surface-treated with aluminum oxide such as alumina. The content of rutile titanium oxide surface-treated with aluminum oxide in the total titanium oxide is, for example, 35% or more by mass, such as 55% or more, and the upper limit is 100% or less, that is, all titanium oxide can be rutile titanium oxide surface-treated with aluminum oxide. In addition, the hardness of anatase titanium oxide is lower than that of rutile titanium oxide, so in terms of the formability of the composition, anatase titanium oxide is preferably used.

[0090] In the photosensitive resin composition of the present disclosure, the mixing amount of the inorganic filler (B) can be in the range of 30% to 70% by mass, for example, in the range of 40% to 70%, and for example, in the range of 45% to 70% relative to the total resin composition. The content of the inorganic filler (B) can be calculated based on the solid content conversion. The content of the inorganic filler (B) within the above range is conducive to high reflectivity, while the content less than the above range will cause a decrease in reflectivity, and the content exceeding the above range will cause cracking.

[0091] In the inorganic filler (B), the sulfur concentration of titanium oxide is 100ppm or less, or 50ppm or less. In addition, commercial titanium oxide with a sulfur concentration of 100ppm or less can be used, or commercial titanium oxide with a sulfur concentration of 100ppm or more can be heat treated, chemically treated or refined by washing, firing, etc. to reduce the sulfur concentration before mixing. In particular, the sulfur contained in the titanium oxide refers to all sulfur detected by analysis. This sulfur includes sulfur adsorbed on the titanium oxide and sulfur added to the titanium oxide as an impurity. In addition, the titanium oxide can have a sodium concentration of 100ppm or less, or 50ppm or less. Lower sodium concentrations may be more preferred. When exposed to moisture caused by sodium ions, excessive sodium concentrations may accelerate corrosion or oxidation of the copper substrate. For this reason, the concentration of sodium ions can be 100ppm or less.

[0092] In addition, as long as the advantages of the present disclosure are not impaired, the photosensitive resin composition of the present disclosure may include titanium oxide having a sulfur concentration of 100 ppm or more. Examples of titanium oxide having a sulfur concentration of 100 ppm or more may include CR-58, CR-90 and R-630 of ISHIHARA Co., Ltd. and R-21 of Sakai-Chem Co., Ltd., etc.

[0093] Alternatively, T-550, T-580, R-630, R-820, CR-50, CR-60, R-90 or CR-97 produced by ISHIHARA SANGYO Co., Ltd., Ti PURE R-706, R-902+, or R931 produced by DuPont Co., Ltd., TR-600, TR-700 or TR-840 produced by Fuji Titanium Industries Co., Ltd., or KR-270, KR-310 and KR-380 produced by Titanium Industries Co., Ltd., which are rutile type chloride-based titanium oxides, can be used.

[0094] When the particle size of titanium oxide is too small, fluidity may be deteriorated, and when the particle size is too large, the ability to be inserted into a small diameter substrate may be deteriorated. Taking this into account, the median particle size of titanium oxide may be in the range of 0.1 μm to 5 μm, for example, in the range of 0.1 μm to 1 μm, for example, in the range of 0.1 μm to 0.5 μm, and may be 0.36 μm. When the particle size of titanium oxide is within the above range, high reflectivity may be exhibited. The above particle size is measured using a laser diffraction method.

[0095] Among the inorganic fillers (B), examples of barium sulfate may include precipitated barium sulfate #100, precipitated barium sulfate #300, precipitated barium sulfate SS-50, BARIACE B-30, BARIACE B-31, BARIACE B-32, BARIACE B-33, BARIACE B-34, BARIFINE BF-1, BARIFINE BF-10, BARIFINE BF-20, BARIFINE BF-40 (Sakai Chemical Industry Co., Ltd.), W-1, W-6, W-10, C300 (Takehara Kagaku Kogyo Co., Ltd.), and the like.

[0096] Among the inorganic fillers (B), the silica particles are not particularly limited and can be obtained by methods known to those skilled in the art. For example, the silica particles can be produced by burning silicon powder by a vaporized metal combustion (VMC) method. According to the VMC method, a chemical salt is formed by a burner in an oxygen-containing atmosphere, a metal powder constituting a part of the target oxide particles is injected into the chemical salt in an amount sufficient to form a dust cloud, and detonation is caused to obtain oxide particles. Examples of commercially available silica include the SO series manufactured by Admatechs, the HPS series manufactured by Toagosei (HPS-0500, HPS-1000, HPS3500, etc.), and the like.

[0097] [(C) Mercapto-modified (meth)acrylate]

[0098] The photosensitive resin composition according to one aspect of the present disclosure ensures enhanced surface curing by using the mercapto-modified acrylate (C), thereby achieving improved glossiness and high reflectivity.

[0099] Furthermore, using the mercapto-modified acrylate (C) of the present disclosure together with the above-mentioned inorganic filler (B) in the photosensitive resin composition can enhance the surface curing of the photosensitive resin layer, thereby achieving higher reflectivity and higher glossiness through the enhanced surface curing.

[0100] The mercapto-modified acrylate (C) of the present disclosure is a compound modified by introducing a mercapto group into an acrylate compound, and the acrylate compound may be: a monofunctional or polyfunctional acrylate compound; or an aliphatic compound having 1 to 15 carbon atoms substituted with at least one functional group selected from an acryloyl group, an acryloyloxy group, and an acryloyloxyalkyl group; or may be, for example, pentanetriacrylate, etc.

[0101] The mercapto-modified acrylate (C) disclosed herein may be curable or active energy ray-curable. The mercapto-modified (meth)acrylate (C) disclosed herein may be obtained by Michael addition reaction of a polyfunctional thiol compound and a stoichiometric excess of a difunctional or polyfunctional (meth)acrylate compound. Examples of polyfunctional thiol compounds include: polyfunctional thiol compounds in reaction products of polyisocyanates, such as pentaerythritol tetrakis (3-mercaptopropionate) (molecular weight: 489 g / mol), trimethylolpropane tris (3-mercaptopropionate) (molecular weight: 399 g / mol) or 1,3-bis (2-isocyanato-2-propyl) benzene tetrathiol (1,3-bis (2-isocyanato-2-propyl) benzene tetrathiol), and polyfunctional thiol compounds, such as trimethylolpropane tris (3-mercaptopropionate); polyfunctional thiol compounds in reaction products of polyisocyanates, such as isocyanates; Phorone diisocyanate, and polyfunctional thiol compounds such as trimethylolpropane tris (3-mercaptopropionate); polyfunctional thiol compounds in the reaction product of polyisocyanate, such as hexamethylene diisocyanate, and polyfunctional thiol compounds such as trimethylolpropane tris (3-mercaptopropionate); 1,6-hexanedithiol (molecular weight: 150 g / mol), ethylene glycol di-2-mercaptoacetate (molecular weight: 210 g / mol), pentaerythritol tetrakis (2-mercaptoacetate) (molecular weight: 433 g / mol) and trimethylolpropane tris (2-mercaptoacetate), ethylene glycol bis (3-mercaptopropionate) (molecular weight: 238 g / mol), etc. For example, the mercapto-modified acrylate (C) may have two or more mercapto groups or three or more mercapto groups.

[0102] The weight average molecular weight of the mercapto-modified acrylate (C) may be 5000 g / mol or less, 3000 g / mol or less, or 2000 g / mol or less. At a weight average molecular weight of 5000 g / mol or less, the mobility of the mercapto-modified (meth) acrylate molecules is reduced, thereby suppressing the degradation of the reactivity of the active energy ray-cured coating formed by the present disclosure. For example, when the coating is cured with UV-LED under the condition of deteriorated reactivity, the viscosity of the cured coating surface increases, and when a printed material is placed on the cured coating, the cured coating is likely to adhere to the printed material.

[0103] In the photosensitive resin composition of the present disclosure, the mercapto-modified (meth)acrylate may be included in an amount of 1-20 parts by weight, 1-10 parts by weight, or 1-7 parts by weight, relative to a total of 100 parts by weight of the composition.

[0104] When the content of the mercapto-modified acrylate (C) is within the above range, enhancement of surface curing, improvement of glossiness and high reflectivity can be achieved, and even after the manufacturing process, a small reduction in reflectivity and excellent crack resistance can be achieved. In addition, the degradation of glossiness caused by the degradation of surface curing can be suppressed, high reflectivity can be obtained, and the damage of the coating can be reduced by appropriate surface curing, and the resolution can be improved.

[0105] [(D) Resin containing aromatic ring]

[0106] The photosensitive resin composition of the present disclosure may include a carboxyl-containing resin (A) not containing an aromatic ring, and may further include a resin (D) containing an aromatic ring in addition to the resin (A).

[0107] The aromatic ring-containing resin (D) may exhibit excellent anti-yellowing property by combining with the resin (A). The photosensitive resin composition according to one aspect of the present disclosure may exhibit excellent anti-yellowing property by including the aromatic ring-containing resin (D) in a smaller content than the resin (A).

[0108] The aromatic ring-containing resin (D) of the present disclosure can be cured by, for example, heating to exhibit electrical insulation.

[0109] Examples of aromatic rings may include benzene rings, pyridine rings, pyrimidine rings, triazine rings, etc. Examples of aromatic ring-containing resins (D) of the present disclosure may include melamine resins, silicone resins, resins having a styrene main chain. For example, a resin having a styrene main chain may be used.

[0110] The resin (D) containing an aromatic ring may contain a carboxyl group, and may be, for example, a carboxyl-containing resin having a styrene main chain. For example, the resin (D) containing an aromatic ring may use a mixture of a carboxyl-containing resin having a styrene main chain and a carboxyl-containing resin other than the carboxyl-containing resin having a styrene main chain.

[0111] For example, when the resin (D) containing an aromatic ring is a carboxyl-containing resin having a styrene main chain, such resin does not have a photosensitive group, such as an olefinic unsaturated bond having a carboxyl group in the molecule, but has a styrene main chain in the molecule, an average molecular weight of 10000 g / mol to 50000 g / mol, and an acid value of 80 mgKOH / g to 200 mgKOH / g. Such a carboxyl-containing resin having a styrene main chain can be synthesized by copolymerization using styrene as an essential monomer. By utilizing a carboxyl-containing resin having the above-mentioned performance range, the cured coating film including the photosensitive resin composition of the present disclosure has excellent dry touch and anti-flow effect.

[0112] The carboxyl-containing resin having a styrene main chain may be, for example, a carboxyl-containing resin (any of an oligomer and a polymer) which may be obtained by copolymerization of an unsaturated carboxylic acid such as (meth) acrylic acid with a compound containing an unsaturated group selected from styrene, α-methylstyrene, a lower alkyl (meth)acrylate, isobutylene, etc. In particular, the lower alkyl group may refer to an alkyl group having 1 to 5 carbon atoms.

[0113] In the photosensitive resin composition of the present disclosure, the average molecular weight per weight of the carboxyl-containing resin having a styrene main chain varies according to the main chain of the resin, but can be 10000 g / mol to 50000 g / mol, 10000 g / mol to 25000 g / mol, 10000 g / mol to 20000 g / mol or 10000 g / mol to 17000 g / mol. A weight average molecular weight of 10000 g / mol or more can improve the anti-flow effect and dry touch (stickiness), enhance the moisture resistance of the exposed coating, inhibit the thinning of the film during the development process, and inhibit the degradation of the resolution. In addition, a weight average molecular weight of 50000 g / mol or less can improve the anti-flow effect, developability and storage stability.

[0114] In the photosensitive resin composition of the present disclosure, the acid value of the carboxyl resin may be 80 mgKOH / g to 200 mgKOH / g or 100 mgKOH / g to 180 mgKOH / g. When the acid value of the carboxyl resin having a styrene main chain is 80 mgKOH / g or higher, the softening point may be increased, thereby improving the viscosity and developing properties. When the acid value of the carboxyl resin having a styrene main chain is 200 mgKOH / g or lower, stress is not generated during the curing process by an appropriate crosslinking density, and a good coating film may be obtained.

[0115] In the photosensitive resin composition of the present disclosure, the carboxyl-containing resin having a styrene main chain has an aromatic ring, but due to the styrene main chain, the discoloration and reflectivity reduction of the cured product under light irradiation or heating can be suppressed, and excellent developability and dry touch are exhibited. The proportion of the styrene main chain in the molecule can be 10mol% to 80mol%, 10mol% to 60mol% or 10mol% to 50mol%. That is, when synthesizing a carboxyl-containing resin having a styrene main chain, 30mol% to 60mol% of styrene can be used relative to the total amount of monomers. When the proportion of the styrene main chain of the carboxyl-containing resin in the molecule is 10mol% or more, improved compatibility with other components can be obtained, and when the proportion is 80mol% or less in the molecule, good developability can be obtained.

[0116] The carboxyl resin with styrene main chain can be prepared by suspension to obtain high molecular weight. Therefore, the photosensitive resin composition using corresponding resin can have excellent dry touch (tackiness). Generally, the carboxyl resin with styrene main chain has high molecular weight when prepared by suspension polymerization, but considering the characteristics such as screen printing compatibility, dry touch and developability, the weight average molecular weight of resin can be limited in the range of 10000g / mol to 50000g / mol. Therefore, in order to control molecular weight, chain transfer agent can be used in the synthesis of carboxyl resin with styrene main chain.

[0117] In addition, in order to accelerate polymerization, a polymerization initiator can be used to synthesize a carboxyl-containing resin with a styrene main chain. Examples of polymerization initiators include benzoyl peroxide (BPO), tert-butyl peroxy-2-ethylhexanoate, 2,2'-azobis(2-methylbutyronitrile) (AMBN), etc., and a polymerization inhibitor can be benzoyl peroxide (BPO). Relative to 100wt% of the carboxyl-containing resin with a styrene main chain, the mixing amount of the polymerization initiator can be 0.1wt% to 10wt% or 0.1wt% to 6wt% in terms of solid content.

[0118] In the photosensitive resin composition of the present disclosure, the aromatic ring-containing resin (D) may be included in an amount of 0.1 wt % to 15 wt %, 1 wt % to 10 wt % or 2 wt % to 6 wt % relative to the total weight of the composition. The photosensitive resin composition includes a solid and a solvent.

[0119] When the content of the aromatic ring-containing resin (D) is within the above range, discoloration and reduction in reflectivity are suppressed, and developability and dry touch are excellent, so that the effects of improving reflectivity and preventing yellowing can be further enhanced.

[0120] [(E) Photopolymerization initiator]

[0121] The photosensitive resin composition according to one aspect of the present disclosure may include a photopolymerization initiator (E) of a compound including a trimethylbenzoylphosphine oxide group having at least one PO bond (hereinafter referred to as “photopolymerization initiator (E)”).

[0122] In 2,4,6-trimethylbenzoyldiphenylphosphine oxide (TPO) and the like widely used as conventional photopolymerization initiators, a large amount of outgassing is generated during curing, and this outgassing diffuses into the silicone sealant layer or protective film, thereby yellowing the silicone sealant, thereby reducing reflectivity and hindering the curing of the silicone sealant. There are problems with the long-term reliability of these products.

[0123] The polymer containing a trimethylbenzoylphosphine oxide group as a photopolymerization initiator has a high molecular weight and a high molecular weight, so the amount of outgassing due to heat is small even in the final curing step, reflow and sintering process using heat.

[0124] At the same time, even compounds containing trimethylbenzoylphosphine oxide having a lower molecular weight than TPO contain one or more PO bonds, resulting in enhanced intermolecular bonding (e.g., forming stronger hydrogen bonds with the remaining OH or COOH groups in the composition without reacting), thereby significantly suppressing the outgassing of the photopolymerization initiator.

[0125] For example, a compound containing a trimethylbenzoylphosphine oxide group may include three or more hydrogen-bondable sites, which may enhance the intermolecular bonding force, thereby significantly suppressing the outgassing of the photopolymerization initiator.

[0126] Therefore, this can solve the yellowing and non-curing problems of the silicone sealant, reduce the amount of outgassing of the photopolymerization initiator transferred to the protective film, and significantly increase the reaction rate of the silicone sealant.

[0127] In the case of using a photopolymerization initiator such as TPO, a separate firing process (e.g., curing at 150°C for 6 hours) is added after the reflow process to effectively remove the generated outgassing, but this firing process causes a significant decrease in reflectivity, resulting in increased power consumption when mounting the chip.

[0128] However, the use of the above-mentioned photopolymerization initiator (E) disclosed herein can omit the firing process to reduce the working time, thereby increasing productivity, reducing costs, improving reflectivity, preventing power consumption due to reduced reflectivity, minimizing the outgassing content of the photopolymerization initiator even without a protective film for removing the photopolymerization initiator, significantly improving the curing degree of silicone, improving long-term reliability, and exhibiting excellent HAST resistance and reflectivity after HAST testing. In addition, the reduction of reflectivity under high temperature / high humidity conditions can be suppressed.

[0129] The photopolymerization initiator (E) may be liquid at room temperature (20° C.) and 1 atmosphere.

[0130] The photopolymerization initiator (E) may have a PO bond.

[0131] The photopolymerization initiator (E) may include a *-C(=O)-P(=O)R1-O-*' portion (wherein R1 is an alkyl group of 1 to 20 carbon atoms, an alkenyl group of 2 to 20 carbon atoms, an alkynyl group of 2 to 20 carbon atoms, or a cyclic group of 5 to 20 carbon atoms)

[0132] When the photopolymerization initiator (E) is a polymer containing a trimethylbenzoylphosphine oxide group, the weight average molecular weight (Mn) of the polymer containing the trimethylbenzoylphosphine oxide group may be about 1000 g / mol or more. For example, the weight average molecular weight (Mn) of the polymer containing the trimethylbenzoylphosphine oxide group may be 1000 g / mol to 100000 g / mol.

[0133] The polymer containing a trimethylbenzoylphosphine oxide group may be represented by Chemical Formula 1 below.

[0134] <Chemical Formula 1>

[0135]

[0136] a=0 to 100, b=0 to 100, and c=0 to 100.

[0137] When the photopolymerization initiator (E) is a trimethylbenzoylphosphine oxide group-containing compound having a PO bond, the trimethylbenzoylphosphine oxide group-containing compound having a PO bond may include an alkoxy group.

[0138] For example, in Chemical Formula 1, a+b+c>0.

[0139] For example, the trimethylbenzoylphosphine oxide group-containing compound having a PO bond may include an ethoxy group.

[0140] The trimethylbenzoylphosphine oxide group-containing polymer having a PO bond may be represented by Chemical Formula 2 below.

[0141] <Chemical Formula 2>

[0142]

[0143] For example, the photopolymerization initiator (E) may further include at least one selected from benzoin and its alkyl ether, acetophenone, anthraquinone, thioxanthone, ketal, benzophenone, α-aminoacetophenone, acylphosphine oxide, acylphosphinate and oxime ester.

[0144] In the photosensitive resin composition of the present invention, the content of the photopolymerization initiator (E) may be 0.01 wt % to 10 wt %, 0.01 wt % to 7 wt % or 0.01 wt % to 5 wt % relative to the total composition. The photopolymerization initiator (E) contained in the above range produces sufficient photocurability on copper, resulting in good coating film curability, improved coating film properties such as chemical resistance and improved depth of curability.

[0145] The content of the photopolymerization initiator (E) within the above range results in gentle undercut and inconspicuous expansion (halo) of the upper portion, thereby resulting in excellent resolution and a large number of solder resist openings. In addition, high reflectivity can be maintained.

[0146] [(F) Silane coupling agent]

[0147] The photosensitive resin composition according to one aspect of the present disclosure may further include a silane coupling agent (F). By including the silane coupling agent (F), the photosensitive resin composition may exhibit improved crack resistance, increased reflectivity compared to the prior art, and excellent glossiness.

[0148] The silane coupling agent (F) of the present disclosure may have an organic group such as a vinyl group, a styryl group, an acryloyl group, a methacryloyl group, an isocyanurate group, an acid anhydride group, an ureide group, an epoxy group, an amino group, a methacryloyloxy group, a mercapto group, an isocyanate group, or an isocyanurate group.

[0149] Examples of silane coupling agents having a vinyl group may include vinyl trimethoxysilane, vinyl triethoxysilane, etc. Examples of silane coupling agents having a styrene group may include p-styrene methoxysilane, etc. Examples of silane coupling agents having a methacrylic group may include 3-methacryloxypropyl methyl dimethoxy silane, 3-methacryloxypropyl trimethoxy silane, 3-methacryloxypropyl diethoxy silane, and 3-methacryloxypropyl triethoxy silane, etc. Examples of silane coupling agents having an acrylic group may include 3-acryloxypropyl trimethoxy silane, etc. Examples of silane coupling agents having an amino group may include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxy-silyl-N-(1,3-dimethyl-butylene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane, etc. Examples of silane coupling agents having a methacryloxy group may include 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, etc. Examples of silane coupling agents having a mercapto group may include 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, etc. Examples of silane coupling agents having an isocyanate group may include 3-isocyanate propyl triethoxy silane, etc. Examples of silane coupling agents having an isocyanurate group may include tris-(trimethoxysilylpropyl)isocyanurate. Examples of silane coupling agents having an ureide group may include 3-ureidopropyltrialkoxysilane, etc. Examples of silane coupling agents having anhydride groups may include 3-(trimethoxysilyl)propyl succinic anhydride, etc.

[0150] The silane coupling agent may be a silane coupling agent having an epoxy group, and examples thereof may include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethylbisethoxysilane, and 3-glycidoxypropyltriethoxysilane.

[0151] In the photosensitive resin composition of the present disclosure, the content of the silane coupling agent (F) may be 0.1 wt % to 5 wt %, 0.3 wt % to 3 wt % or 0.4 wt % to 2 wt % relative to the total composition. The composition includes a solid and a solvent.

[0152] When the content of the silane coupling agent (E) is within the above range, the composition has excellent crack resistance, high reflectivity, excellent adhesion, and low viscosity, and thus may be suitable for film formation.

[0153] The silane coupling agent (F) may be a commercially available product, and examples thereof may include KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-1403, KBM-502, KBM-503, KBE-502, KBE-503, KBM5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103P, KBM-573, KBM-575, KBM-9659, KBM-585A, KBM-802, KBM-803, KBE-0007N, X-12-967C, and the like of Shin-Etsu Kagaku Kogyo.

[0154] [(G) Resin having urethane bond]

[0155] The photosensitive resin composition according to one aspect of the present disclosure may further include a resin (G) having a urethane bond. The resin (G) having a urethane bond may have excellent flexibility.

[0156] By using the resin (G) having a urethane bond, the photosensitive resin composition does not break even on a flexible substrate or a thin plate having a small thickness, allows lamination to a uniform thickness, and has excellent crack resistance or break resistance when subjected to external impact or bending.

[0157] The resin (G) having a urethane bond disclosed herein may include a modified urethane resin, and examples of the resin having a urethane bond may include ester-type urethane, ether-type urethane, modified urethane acrylate, modified urethane epoxy resin, silicone-modified urethane or fluorine-type modified urethane, etc., and may be, for example, a modified urethane epoxy acrylate containing an epoxy group.

[0158] The resin (G) having a urethane bond of the present disclosure can use a known compound having a urethane bond. Examples thereof can include a reaction product of an isocyanate compound (e.g., monoisocyanate, diisocyanate, and polyisocyanate) and a compound having an OH group (e.g., a monohydric alcohol, a polyol such as polyester polyol or polyether polyol, and epoxy (meth) acrylate) or a modified product thereof.

[0159] The resin (G) having a urethane bond of the present disclosure may have a carboxyl group, an epoxy group or a (meth)acryloyl group, and examples thereof may include a carboxyl group-containing resin (1), an epoxy group-containing resin (2), a (meth)acryloyl group-containing resin, etc. (3), (4), (5):

[0160] (1) Carboxyl-containing photosensitive polyurethane resins obtained by polyaddition reaction of a carboxyl-containing diol compound, a diol compound and a diisocyanate with a reaction product of a monocarboxylic acid compound having an ethylenically unsaturated double bond, for example, difunctional epoxy resin (meth)acrylates such as bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bixylenol epoxy resin or novolac epoxy resin, partial anhydrides thereof or modified products thereof;

[0161] (2) a urethane-modified epoxy resin having a urethane bond and two or more epoxy moieties in the molecule, obtained by reacting a hydroxyl-containing epoxy compound with a urethane bond-containing compound having an isocyanate group obtained by reacting a polyhydroxy compound with a polyisocyanate compound;

[0162] (3) Urethane resins obtained by a polyaddition reaction of a diisocyanate (e.g., an aliphatic diisocyanate, a branched diisocyanate, an alicyclic diisocyanate or an aromatic diisocyanate) and a diol compound (e.g., a polycarbonate-based polyol, a polyether-based polyol and a polyester-based polyol, a polyolefin polyol, an acryl polyol, an epoxy resin having a hydroxyl group (which can be used to obtain a urethane resin having an epoxy group), a bisphenol A alkylene oxide adduct diol, a compound having a phenolic hydroxyl group and an alcoholic hydroxyl group);

[0163] (4) a photosensitive polyurethane resin obtained by a polyaddition reaction of an isocyanate and a diol compound, wherein a part or all of the diisocyanate in the above (3) is replaced by a reaction product of isophorone diisocyanate and pentaerythritol triacrylate and / or a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule; and

[0164] (5) A terminal (meth)acrylated photosensitive polyurethane resin prepared by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule such as hydroxyalkyl (meth)acrylate during the synthesis of one of the resins (3) and (4).

[0165] Furthermore, as described above, one resin may have at least two types of carboxyl groups, epoxy groups, or methacryl groups.

[0166] The resin (G) having a urethane bond may be (1) in a carboxyl group-containing resin, (2) in an epoxy group-containing resin, and (5) in a (meth)acryl group-containing resin.

[0167] Diisocyanate can be, for example, an aromatic polyisocyanate, an aliphatic polyisocyanate or an alicyclic polyisocyanate. Examples of aromatic polyisocyanates can include 4,4'-diphenylmethane diisocyanate, 2,4-diisocyanate-2,6-toluene diisocyanate, naphthalene-1,5-diisocyanate-o-xylene diisocyanate, m-xylene diisocyanate, 2,4-triene dimer, etc. Examples of aliphatic polyisocyanates can include tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate and trimethyl hexamethylene diisocyanate, 4,4-methylenebis (cyclohexyl isocyanate) and isophorone diisocyanate. Examples of alicyclic polyisocyanates can include dicycloheptane triisocyanate. For example, diisocyanate can be an aliphatic isocyanate.

[0168] When the resin (G) having a urethane bond is a carboxyl-containing resin having a urethane bond, the acid value of the carboxyl-containing resin may be 40 mgKOH / G to 200 mgKOH / G or 45 mgKOH / G to 120 mgKOH / G. When the carboxyl-containing resin acid value is within the range of 40 mgKOH / G to 200 mgKOH / G, the adhesion of the cured film is ensured to promote alkali development, thereby suppressing the dissolution of the exposed area by the developing solution, so that the line will not be narrowed to a degree exceeding the required level, thereby allowing a normal resist pattern to be easily drawn.

[0169] When the resin (G) with carbamate bond is a carboxyl resin with carbamate bond, the weight average molecular weight of carboxyl resin changes according to the main chain of resin, but can be 2000g / mol to 150000g / mol, 5000g / mol to 50000g / mol or 2000g / mol to 50000g / mol. The weight average molecular weight of carboxyl resin within the above range causes good viscosity, thereby improving the moisture resistance of cured film and reducing the thinning of film in the developing process. In addition, the weight average molecular weight can cause good resolution and developability and improved storage stability within the above range.

[0170] Exemplary commercially available products of the resin (G) having a urethane bond (e.g., a carboxyl group-containing resin having a urethane bond) may include UXE-3000 (Japan Explorers Co., Ltd.), EPU-7N (urethane-modified epoxy resin; ADEKA Co., Ltd.), and Ebecryl 210 (aromatic urethane acrylate; Daicel Allnex Co., Ltd.).

[0171] In the photosensitive resin composition of the present disclosure, the content of the resin (G) having a urethane bond may be 0.1 wt % to 15 wt %, 5 wt % to 13 wt % or 8 wt % to 12 wt % relative to the total composition. The composition includes solids and solvents. When the content of the resin (G) having a urethane bond is within the above range, the composition may exhibit excellent flexibility and crack resistance, appropriate viscosity, and excellent printability and drying properties.

[0172] In the photosensitive resin composition of the present invention, the weight average molecular weight of the resin (G) having a urethane bond may be 2000 g / mol to 150000 g / mol or 2000 g / mol to 50000 g / mol. When the weight average molecular weight of the resin (G) having a urethane bond is within the above range, the composition may exhibit excellent crack resistance and flexibility.

[0173] [Other optional components]

[0174] If necessary, various additives can be added to the photosensitive resin composition of the present disclosure as optional components. Specifically, a heat curing catalyst, a dispersant, an antioxidant, a colorant, an epoxy resin, an oxetane compound, a (meth) acrylic resin and various other additives, or a mixture of two or more thereof, can be added. One or more of the following materials can be included as optional components.

[0175] <Epoxy resin>

[0176] The epoxy resin of the present disclosure may be a well-known and commonly used compound having one or more epoxy groups. For example, the epoxy resin may not overlap with the above components (A) to (G). For example, the epoxy resin may be a compound having two or more epoxy groups. Examples of epoxy resins may include monoepoxy compounds such as butyl glycidyl ether, phenyl glycidyl ether or (meth) acrylate glycidyl ether, and compounds having two or more epoxy groups in one molecule, such as bisphenol A epoxy resin, bisphenol S epoxy resin, bisphenol F epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, alicyclic epoxy resin, trimethylolpropane polyglycidyl ether, phenyl-1,3-diglycidyl ether, biphenyl-4,4'-diglycidyl ether, 1,6-hexanediol diglycidyl ether, diglycidyl ether of ethylene glycol or propylene glycol, sorbitol polyglycidyl ether, tris(2,3-epoxypropyl)isocyanurate or triglycidyl tris(2-hydroxyethyl)isocyanurate. These may be used alone or in combination of two or more depending on the desired properties.

[0177] Examples of compounds having two or more epoxy groups include bisphenol A epoxy resins such as jER828, jER834, jER1001 and jER1004 from Mitsubishi Chemical Co., Ltd., EPICLON 840, EPICLON 850, EPICLON 1050 and EPICLON 2055 from DIC Co., Ltd., Epototo D-011, YD-013, YD127 and YD-128 from Nittetsu Chemical & Materials Co., Ltd., DER317, DER331, DER661 and DER664 from Dow Chemical Japan Co., Ltd., Sumi Epoxy ESA-011, ESA-014, ELA-115 and ELA128 from Sumitomo Chemical Co., Ltd., Asahi Kasei Materials Co., Ltd. AER330, AER331, AER661 and AER664 (all trade names); brominated epoxy resins such as jERYL903 of Mitsubishi Chemical Co., Ltd., EPICLON 152 and EPICLON 165 of DIC Co., Ltd., Epototo YDE-400 and YDE-500 of Nittetsu Chemical & Materials Co., Ltd., DER542 of Dow Chemical Japan Co., Ltd., Sumitoepoxy ESB-400 and ESB-700 of Sumitomo Chemical Co., Ltd., AER711 and AER714 (all trade names) of Asahi Kasei Materials Co., Ltd.; phenolic epoxy resins such as jER152 and jER154 of Mitsubishi Chemical Co., Ltd., DEN431 and DEN438, EPICLON N-730, EPICLON N-770 and EPICLON N-865 from DIC Co., Ltd., Epototo YDC-701 and YDC-704 from Nittetsu Chemical & Materials Co., Ltd., EPPN-201, EPPN-1025, EPPN-1020, EPPN-104S, RE-306 and NC-3000 from Japan Chemical Co., Ltd., Sumi Epoxy ESCN-195X and ESCN-220 from Sumitomo Chemical Co., Ltd., AERECN-235 and ECN-299 from Asahi Kasei Materials Co., Ltd., Nittetsu Chemical & Materials Co., Ltd.'s YDCN-700-2, YDCN-700-3, YDCN-700-5, YDCN-700-7, YDCN-700-10, YDCN-704 and YDCN-704A, DIC Co., Ltd.'s EPICLON N-680, N-690 and N-695 (all trade names); bisphenol F epoxy resins, such as EPICLON 830 from DIC Co., Ltd., jER 807 from Mitsumi Chemical Co., Ltd., Epototo YDF-175 and YDF-2004 from Nittetsu Chemical & Materials Co., Ltd. (all trade names); hydrogenated bisphenol A epoxy resins, such as Epototo ST-2004, ST-2007 and ST-3000 from Nittetsu Chemical & Materials Co., Ltd. (all trade names), jER 604 from Mitsumi Chemical Co., Ltd., Nittetsu Ephotouto YH-434 of Chemical & Materials Co., Ltd.; glycidylamine type epoxy resins, such as SumiEpoxy ELM-120 (trade name) of Sumitomo Chemical Co., Ltd.; hydantoin epoxy resins; alicyclic epoxy resins, such as Celloxide 2021 (trade name) of Daicel Co., Ltd.; trihydroxyphenylmethane epoxy resins, such as YL-933 of Mitsubishi Chemical Co., Ltd. and TEN, EPPN-501 and EPPN-502 (all trade names); bis-xylenol or bisphenol epoxy resins, such as YL-6056, YX-4000 and YL-6121 of Mitsubishi Chemical Co., Ltd. or mixtures thereof (all trade names); bisphenol S epoxy resins, such as EBPS-200 of Kayaku Co., Ltd., EPX-30 of ADEKA and EXA-1514 of DIC Co., Ltd. (all trade names); bisphenol A novolac epoxy resins, such as jER 157S (trade name) of Mitsubishi Chemical Co., Ltd.; tetraphenylolethane epoxy resins, such as jER YL-931 (trade name) of Mitsubishi Chemical Co., Ltd.; heterocyclic epoxy resins, such as TEPIC (trade name) of Nissan Chemical Co., Ltd.; diglycidyl phthalate resins, such as Brenmer of Niche Oil Co., Ltd. DGT; tetraglycylyl kylenoylethane resin, such as ZX-1063 from Nittetsu Chemical & Materials Co., Ltd.; naphthyl-containing epoxy resins, such as ESN-190 and ESN-360 from Nittetsu Chemical & Materials Co., Ltd., and HP-4032, EXA-4750 and EXA-4700 from DIC Co., Ltd.; epoxy resins having a dicyclopentadiene backbone, such as HP-7200 and HP-7200H from DIC Co., Ltd.; glycidyl methacrylate copolymer epoxy resins, such as CP-50S and CP-50M from Niche Oil Co., Ltd.; copolymer epoxy resins of cyclohexylmaleimide and glycidyl methacrylate; and CTBN-modified epoxy resins (such as YR-102 and YR-450 from Nittetsu Chemical & Materials Co., Ltd.), but are not limited thereto. Among them, the compound having two or more epoxy groups may be bisphenol A epoxy resin, heterocyclic epoxy resin or a mixture thereof, instead of a resin having excellent anti-discoloration property. These epoxy resins may be used alone or in combination of two or more.

[0178] In the photosensitive resin composition of the present disclosure, the epoxy resin may be a bisphenol-based epoxy resin, for example, a bisphenol-based epoxy resin having two or more epoxy groups. The mixed amount of the bisphenol-based epoxy resin having two or more epoxy groups used in the present disclosure may be 1 wt % to 15 wt %, 1 wt % to 10 wt % or 3 wt % to 10 wt % relative to the total composition. The composition includes a solid and a solvent.

[0179] When the content of the epoxy resin is within the above range, a coating film formed from the composition exhibits excellent adhesion, heat resistance, and pencil hardness, undergoes good curing, and can solve problems such as yellowing and difficulty in achieving high reflectivity after processing.

[0180] In the photosensitive resin composition of the present disclosure, the weight average molecular weight of the epoxy resin may be 150 g / mol to 100000 g / mol.

[0181] <Oxetane compounds>

[0182] Next, the oxetane compound will be described. The oxetane compound containing an oxetane ring is represented by the following general formula (I):

[0183]

[0184] (where R 1 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms). Specific examples of the oxetane compound may include 3-ethyl-3-hydroxymethyloxetane (DongA Synthetic Co., Ltd., trade name: OXT-101), 3-ethyl-3-(phenoxymethyl)oxetane (DongA Synthetic Co., Ltd., trade name: OXT-211), 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane (DongA Synthetic Co., Ltd., trade name: OXT-212), 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene (DongA Synthetic Co., Ltd., trade name: OXT-121) and bis(3-ethyl-3-oxetanylmethyl)ether (DongA Synthetic Co., Ltd., trade name: OXT-221). In addition, examples thereof may include phenol novolac type oxetane compounds. Such oxetane compounds may be used alone or in combination with epoxy compounds.

[0185] <(Meta) acrylic resin>

[0186] The (meth) acrylic resin is a photocurable resin. The photocurable resin is not limited as long as the resin is cured by active energy ray irradiation to exhibit electrical insulation, and may be, for example, a compound having at least one ethylenically unsaturated bond in the molecule. For example, the (meth) acrylic resin may not overlap with the above-mentioned components (A) to (G).

[0187] Compounds with ethylenically unsaturated bonds may include well-known and commonly used photopolymerizable oligomers, photopolymerizable monomers, and photopolymerizable vinyl monomers. Photopolymerizable oligomers may be unsaturated polyester-based oligomers, (meth)acrylate-based oligomers, and the like. Examples of (meth)acrylate-based oligomers may include epoxy (meth)acrylates, such as phenol novolac epoxy (meth)acrylate, cresol novolac epoxy (meth)acrylate, and bisphenol-type epoxy (meth)acrylates, urethane (meth)acrylates, epoxyurethane (meth)acrylates, polyester (meth)acrylates, polyether (meth)acrylates, polybutadiene-modified (meth)acrylates, and the like.

[0188] As the photopolymerizable monomer or the photopolymerizable vinyl monomer, well-known and commonly used monomers can be used, and examples thereof may include: styrene derivatives such as styrene, chlorostyrene and α-methylstyrene; vinyl esters such as vinyl acetate, vinyl butyrate and vinyl benzoate; ethers such as vinyl isobutyl ether, vinyl n-butyl ether, polyvinyl tert-butyl ether, vinyl n-amyl ether, vinyl isopentyl ether, vinyl n-octadecyl ether, vinyl cyclohexyl ether, ethylene glycol monobutyl ether and triethylene glycol monomethyl ether; (meth)acrylamides such as acrylamide, methacrylamide, amides, N-methylol acrylamide, N-methylol methacrylamide, N-methoxy methacrylamide, N-ethoxy methacrylamide and N-butoxy methacrylamide; aromatic compounds, such as triallyl isocyanurate, diaryl phthalates and diaryl isophthalates; (meth) acrylates, such as 2-ethylhexyl (meth) acrylate, dodecyl (meth) acrylate, tetrahydrofurfuryl (meth) acrylate, isoboroniae (meth) acrylate, (meth) acrylate phenyl (meth)acrylate and phenoxyethyl (meth)acrylate; hydroxyalkyl (meth)acrylates, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate and pentaerythritol tri(meth)acrylate; alkoxyalkylene glycol mono(meth)acrylates, such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; alkylene polyol poly(meth)acrylates, such as ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, esters, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate and dipentaerythritol hexa(meth)acrylate; polyoxyalkylene glycol poly(meth)acrylates, such as diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, ethoxylated trimethylolpropane triacrylate and propoxylated trimethylolpropane tri(meth)acrylate; poly(meth)acrylates, such as hydroxypivalic acid neopentyl glycol ester di(meth)acrylate; and isonalate-type poly(meth)acrylates, such as tris[(meth)acryloyloxyethyl]isocyanurate, which may be used alone or in combination of two or more.

[0189] In the photosensitive resin composition of the present disclosure, the (meth) acrylic resin can be an oligomer based on unsaturated polyester, an oligomer based on (meth) acrylate, etc., and can be, for example, a hexafunctional flexible acrylic oligomer. Relative to the total composition, the mixing amount of the (meth) acrylic resin can be 1wt% to 15wt%, 1wt% to 10wt% or 5wt% to 10wt%. The composition includes solids and solvents. When the content of the (meth) acrylic resin is within the above range, excellent resolution and undercut can be obtained, and the coating film can be cured to an appropriate level.

[0190] <Thermosetting catalyst>

[0191] In the composition of the present disclosure, at least any one type of curing agent or curing catalyst may be further added as a thermal curing catalyst. For example, the thermal curing catalyst may not overlap with the above-mentioned components (A) to (G).

[0192] Examples of curing agents may include polyfunctional phenolic compounds, polycarboxylic acids and their anhydrides, aliphatic or aromatic primary or secondary amines, polyamide resins, isocyanate compounds, polythio compounds, and the like. The curing agent may be, for example, a polyfunctional phenolic compound, a polycarboxylic acid and its anhydride. The use of these curing agents may ensure good processability and insulation. The polyfunctional phenolic compound may be specifically defined as long as the compound has two or more phenolic hydroxyl groups in one molecule, and may be, for example, a well-known and commonly used compound. Examples of polyfunctional phenolic compounds may include phenol novolac resins, cresol novolac resins, bisphenol A, allyl bisphenol A, bisphenol F, phenolic resins of bisphenol A, and vinyl phenol copolymer resins. The polyfunctional phenolic compound may be, for example, bisphenol A, and thus may ensure high reactivity and high heat resistance. The polyfunctional phenolic compound may be subjected to an addition reaction with at least one type of epoxy compound or octane compound in the presence of an appropriate curing catalyst. The polycarboxylic acid and its anhydride may be a compound having two or more carboxyl groups in one molecule and its anhydride, and may include, for example, (meth) acrylic acid copolymers, maleic anhydride copolymers, dibasic acid condensation products, etc. Examples of commercially available products may include Joncryl (product group name) of BASF, SMA resin (product group name) of Sartomer, and polyazelaic polyanhydride of New Japan Chemical Co., Ltd.

[0193] The curing catalyst is a compound that can become a curing catalyst in the reaction between the curing agent and the thermosetting resin, such as an epoxy compound and an oxetane compound, or a polymerization catalyst when no curing agent is used. Specific examples of the curing catalyst may include tertiary amines, tertiary amine salts, quaternary ammonium salts, tertiary phosphines, crown ether compounds, and phosphonium ylide, which may be used alone or in combination of two or more.

[0194] Examples of curing catalysts may include imidazoles, such as trade names 2E4MZ, C11Z, C17Z, and 2PZ; imidazole AZINE compounds, such as trade names 2MZ-A and 2E4MZ-A; isocyanurates of imidazoles, such as trade names 2MZ-OK and 2PZ-OK; imidazole hydroxymethyl compounds, such as trade names 2PHZ and 2P4MHZ (Shikoku Kasei Industrial Co., Ltd.); dicyandiamide and its derivatives; melamine and its derivatives; diaminomalononitrile and its derivatives; amines such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, bis(hexamethylene)triamine, triethanolamine and diaminodiphenylmethane; 1,8-diazabicyclo[5,4,0]undecene-7 (trade name DBU, San-Apro Co., Ltd.); 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5,5]undecane (trade name ATU, Ajinomoto Co., Ltd.); or organic phosphine compounds such as triphenylphosphine, tricyclohexylphosphine, tributylphosphine and methyldiphenylphosphine.

[0195] In the photosensitive resin composition of the present disclosure, the curing catalyst may be an amine-based, phosphine-based or imidazole-based curing catalyst, and may be, for example, an amine curing catalyst based on melamine. The mixing amount of the curing catalyst may be 0.1 wt % to 10 wt %, 0.1 wt % to 5 wt % or 0.1 wt % to 3 wt % relative to the total composition.

[0196] When the content of the curing catalyst is within the above range, the coating film may be sufficiently cured to exhibit excellent adhesion, pencil hardness, and heat resistance, ensure a suitable curing time, and prevent deterioration of developability.

[0197] <Antioxidants>

[0198] The photosensitive resin composition of the present disclosure may also include an antioxidant. The addition of an antioxidant can prevent the oxidative degradation of curable resins, etc., thereby inhibiting discoloration, while obtaining enhanced heat resistance and good resolution (reproducibility of line width). In other words, the white colorant can reduce the resolution by reflecting and absorbing light according to its type, but regardless of the type of the white colorant, the inclusion of an antioxidant can achieve good resolution. The antioxidant can be a free radical scavenger that neutralizes the generated free radicals, or a peroxide decomposition inhibitor that decomposes the generated peroxide into harmless substances and prevents the generation of new free radicals, and can be used alone or in two or more combinations.

[0199] Examples of antioxidants having a free radical scavenger effect may include phenolic compounds such as hydroquinone, 4-tert-butylcatechol, 2-tert-butylhydroquinone, hydroquinone monomethyl ether, 2,6-di-tert-butyl-p-cresol, 2,2-methylenebis(4-methyl-6-tert-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene and 1,3,5-tris(3′,5′-di-tert-butyl-4-hydroxybenzyl)benzene. '-di-t-butyl-4-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione (1,3,5-tris(3',5'-di-t-butyl-4-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione); quinone-based compounds such as methylquinone and benzoquinone; amine-based compounds such as bis(2,2,6,6-tetramethyl-4-piperidinyl)-sebacate and phenothiazine. For example, IRGANOX1010 (trade name, BASF Japan Co., Ltd.) and the like can be used as commercially available products.

[0200] Examples of the antioxidant having a peroxide decomposing effect may include phosphorus compounds such as triphenyl phosphite; and sulfur compounds such as pentaerythritol tetralaurylthiopropionate, dilaurylthiopropionate, and distearyl-3,3′-thiodipropionate.

[0201] For example, the antioxidant may be a phenolic compound, and the use of such a compound can suppress discoloration, enhance heat resistance, and reproduce better resolution.

[0202] Antioxidants, such as phenolic antioxidants, can be used in combination with heat-resistant stabilizers. Such a combination can show a greater effect.

[0203] Examples of the heat-resistant stabilizer may include phosphorus-based, hydroxylamine-based, and sulfur-based heat-resistant stabilizers. Such heat-resistant stabilizers may be used alone or in combination of two or more.

[0204] For example, the antioxidant may be a hydroxylamine-based antioxidant, a sulfur-based antioxidant, or a phenolic antioxidant. When a phenolic antioxidant is used, the blending amount of the phenolic antioxidant may be 0.01wt% to 5wt% or 0.03wt% to 3wt% relative to the total composition. When the blending amount of the antioxidant exceeds 0.01wt% to 1wt%, the effect caused by adding the antioxidant may be obtained with certainty. When the blending amount is 1wt% or less, a good alkalinity phenomenon may be obtained without interrupting the photoreaction, and a good dry touch or coating performance may be ensured.

[0205] <Organic solvents>

[0206] The photosensitive resin composition of the present disclosure may include an organic solvent for preparing the composition or adjusting the viscosity when applied to a substrate or a base film. Examples of the organic solvent may include: esters; aliphatic hydrocarbons such as octane and decane; petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha; and well-known and commonly used organic solvents. These organic solvents may be used alone or in combination of two or more.

[0207] <Other additives>

[0208] In addition, the photosensitive resin composition of the present disclosure may include other additives that are well known and commonly used in the field of electronic materials. Examples of other additives may include thermal polymerization inhibitors, ultraviolet absorbers, plasticizers, flame retardants, antistatic agents, anti-aging agents, antimicrobial and antifungal agents, defoamers, leveling agents, thickeners, adhesives, thixotropic agents, photoinitiator aids, sensitizers, curing accelerators, release agents, surface treatment agents, dispersants, dispersing aids, surface modifiers, stabilizers, etc.

[0209] In the photosensitive resin composition of the present disclosure, the content of phosphorus may be 500 ppm to 5000 ppm.

[0210] In the photosensitive resin composition, a phosphorus content of 500 ppm or more can improve surface curing and enhance gold plating resistance and adhesion, and a phosphorus content of 5000 ppm or less can show an effect of increasing the reaction rate of a silicone sealant.

[0211] A phosphorus content of less than 500 ppm may result in a pencil hardness of 3H, poor adhesion after gold plating, low glass content, and incomplete formation of solder resist openings (SROs). However, a phosphorus content exceeding 5000 ppm may result in a very low reaction rate of the silicone sealant, low developability and reflectivity, and incomplete formation of SROs.

[0212] [Dry film and method for producing the same]

[0213] Another aspect of the present disclosure is directed to a dry film having a photosensitive resin layer formed by coating and drying a photosensitive resin composition on a first film.

[0214] To manufacture a dry film, the composition of the present disclosure is first diluted with an organic solvent to have a properly adjusted viscosity, and then coated on the first film to a uniform thickness, for example, 40 μm to 60 μm, by a notch wheel coater, a knife coater, a lip coater, a rod coater, an extrusion coater, a reverse coater, a transfer roll coater, a gravure coater, a micro gravure coater or a spray coater, etc. Subsequently, the applied composition may be dried generally at a temperature of 40° C. to 120° C. for 1 to 30 minutes to form a photosensitive resin layer, finally manufacturing a dry film.

[0215] The thickness of the coated film is not particularly limited, but generally, the thickness after drying may be 10 μm to 150 μm, 10 μm to 80 μm, or 10 μm to 60 μm.

[0216] As the first film, a plastic film can be used, and for example, a polyester film such as polyethylene terephthalate (PET), a polyimide film, a polyamide-imide film, a polypropylene film, a polystyrene film, etc. can be used. For example, the plastic film can be polyethylene terephthalate. The thickness of the first film is not particularly limited, but generally, the thickness is appropriately selected within the range of 10 μm to 150 μm. The composition can be applied to a metal foil, such as a copper foil or an aluminum foil. The first film that has been used can be stripped with an acrylic resin (acryl), silicone, etc.

[0217] The dry film of the present disclosure is white, and thus can be used to reflect light generated from a light emitting diode (LED) or electroluminescence (EL), which is used as a light source in a lighting fixture or a backlight of a liquid crystal display, such as a mobile terminal, a laptop, a tablet computer, a monitor, a smart phone, a personal computer, or a television. The dry film of the present disclosure can be applied to LEDs, light-emitting PCBs, etc.

[0218] In order to prepare a cured film on a printed circuit board by using a dry film, the second film for protecting the dry film is peeled off, and the exposed resin layer of the dry film is covered and attached to a substrate having a circuit by using a laminator, etc., thereby forming a resin layer on the substrate having a circuit. Subsequently, the formed resin layer may be exposed, developed, heated, and then cured to form a cured film. The second film may be peeled off at any step before or after exposure.

[0219] [Solidified product and preparation method thereof]

[0220] The cured product of the present disclosure may be obtained by curing the photosensitive resin composition of the present disclosure or the solder resist layer of the dry film of the present disclosure.

[0221] The cured product of the present disclosure can be suitably used for printed circuit boards, electronic components, etc. The cured product of the present disclosure has high crack resistance, high resolution, and outstanding dielectric properties (including low dielectric constant and low dielectric loss tangent). In addition, the cured product of the present disclosure can be excellent in heat resistance and linear expansion coefficient.

[0222] For example, the cured product of the present disclosure may be a solder resist.

[0223] The solder resist can be prepared by coating the photosensitive resin composition of the present disclosure on a substrate to form a photosensitive resin layer, selectively exposing the photosensitive resin layer by active energy rays through a photomask having a predetermined pattern, and then developing the unexposed portion with an alkaline aqueous solution (e.g., a 0.3wt% to 3wt% sodium carbonate aqueous solution) to form a pattern. Alternatively, in the case of a dry film, the first film of the dry film is peeled off, and then developed after exposure, thereby forming a patterned solder resist layer on the substrate. As long as it is within the range that does not damage the characteristics, the first film can be peeled off from the dry film before exposure, and then the exposed resin layer is exposed and developed.

[0224] [Printed circuit board and method for manufacturing the same]

[0225] The printed circuit board of the present disclosure may include a cured product of the photosensitive resin composition of the present disclosure or a cured film obtained by curing the photosensitive resin layer of the dry film of the present disclosure.

[0226] The printed circuit board of the present disclosure may include a cured product obtained from the photosensitive resin composition of the present disclosure or the photosensitive resin layer of the dry film. In the manufacturing method of the printed circuit board of the present disclosure, for example, the viscosity of the photosensitive resin composition of the present disclosure is adjusted to be suitable for the coating method by using an organic solvent, and the photosensitive resin composition is applied to a substrate by a method such as dip coating, flow coating, roller coating, rod coating, screen printing or curtain coating, and then the organic solvent included in the composition is volatilized at a temperature of 60° C. to 100° C. and dried (pre-dried) to form a non-sticky resin layer. In the case of a dry film, the resin layer is bonded to the substrate by a laminator or the like to contact the substrate, and then the first film is separated to form a resin layer on the substrate.

[0227] Examples of substrates can include not only printed circuit boards and flexible printed circuit boards having circuits formed of copper, etc., but also FR-4 substrates and all grades of copper-clad laminates (FR-4, etc.), which use copper-clad laminate materials for high-frequency circuits, utilizing paper phenol, paper epoxy, glass fiber epoxy, glass polyimide, glass fiber / epoxy, glass fiber / paper epoxy, synthetic fiber epoxy, fluoroplastic-polyethylene-polyphenylene ether, polyphenyleneoxide cyanate, etc., as well as other metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer substrates, and the like.

[0228] Lamination of the dry film on the substrate may be performed after pressurization and heating using a vacuum laminator or the like. When a substrate having a circuit is used, use of such a vacuum laminator enables the dry film to adhere to the circuit substrate regardless of unevenness on the surface of the circuit substrate, thereby preventing the mixing of bubbles and improving the reduction of dents on the substrate surface. The pressurization condition may be about 0.1 MPa to 2.0 MPa, and the temperature condition may be 40° C. to 120° C.

[0229] In addition, the cured product is post-cured by i) active energy ray irradiation followed by thermal curing (e.g., 100° C. to 220° C.), ii) thermal curing followed by active energy ray irradiation, iii) active energy ray irradiation alone, or iv) thermal curing alone, thereby forming a cured film having excellent properties such as adhesion and hardness.

[0230] The cured product of the present disclosure is cured by heating at a temperature of, for example, 100° C. to 220° C., thereby forming a cured film having excellent overall properties, such as high reflectivity, outstanding yellowing resistance, and excellent crack resistance.

[0231] The exposure device for active energy ray irradiation may be a device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury arc lamp, etc., and irradiates ultraviolet (UV) in the range of 350nm to 450nm, or a direct drawing device (for example, a laser direct imaging device in which a computer directly draws CAD data by laser) may be used. The direct drawing lamp light source or the laser light source may have a maximum wavelength in the range of 350nm to 450nm. The exposure amount for image formation varies depending on the thickness, etc., but may be generally 10mJ / cm 2 Up to 1000mJ / cm 2 or 20mJ / cm 2 Up to 800mJ / cm 2 .

[0232] Development can be performed by dipping, showering, spraying, brushing, or the like, and an alkaline aqueous solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, or amine can be used as a developing solution.

[0233] The printed circuit board of the present disclosure may include a dry film including one or more layers formed of the photosensitive resin composition.

[0234] In the formation of a printed circuit board, the dry film may be placed on a test substrate, and the dry film may be transferred to the test substrate by vacuum lamination.

[0235] Thereafter, the first film is peeled off, and the substrate to which the dry film from which the first film has been peeled off has been transferred can be UV exposed by using an exposure device. In the case of such exposure, the exposed portion (light irradiated portion) can be cured. After exposure, the substrate is cooled at room temperature, and then placed in a developing device, and the unexposed portion is developed with an alkaline aqueous solution, thereby completing the formation of the resist pattern. The substrate having a pattern formed by development is post-cured in an oven at 150°C for 1 hour to complete the substrate manufacturing. After post-curing, a reflow process is performed, followed by a chip mounting process. Then, a packaging process is performed by preparing a silicone sealant on the cured product of the photosensitive resin layer. The photosensitive resin composition disclosed herein can reduce the outgassing of the photopolymerization initiator, thereby solving the yellowing and incomplete curing of the silicone sealant formed on the cured product, and increasing the reaction rate of the silicone sealant.

[0236] In the method of manufacturing a printed circuit board including the cured product of the present disclosure, for example, the first film may be peeled off after the exposure process, followed by a lamination process.

[0237] [Silicone sealant layer and preparation method thereof]

[0238] The printed circuit board of the present disclosure may further include a silicone sealant layer disposed on the cured product (obtained by curing the photosensitive resin layer). The silicone sealant layer may be formed by coating a composition including silicone to seal and protect the printed circuit board or the solder resist layer.

[0239] In order to protect the chip portion that emits light and the photosensitive resin layer (or a cured product obtained by curing the photosensitive resin layer), the above-mentioned silicone sealant layer may be applied.

[0240] An exemplary method of preparing the silicone sealant layer will be described below.

[0241] A dam with a width of 2.0 cm, a height of 2.0 cm, and a thickness of 250-300 μm is manufactured on a printed circuit board that has been post-cured or reflowed, and then a 1:1 mixture of any silicone sealant A and B is added thereto to apply a silicone sealant with a thickness of 250 μm to 300 μm. Then, the silicone sealant is primarily cured by curing at 100° C. for 2 hours in an oven, and is secondary cured by curing at 150° C. for 4 hours in an oven, thereby preparing a silicone sealant layer.

[0242] In order to measure the physical properties of the silicone sealant layer, the reaction rate of the silicone sealant and the content of the photopolymerization initiator remaining in the silicone sealant layer can be analyzed after the silicone sealant layer is peeled off after the curing is completed. In addition, the degree of curing can be checked by measuring the curing degree (reaction rate) of the silicone sealant. The reflectivity of the silicone sealant layer can also be measured.

[0243] For example, the silicone sealant layer may include a lower sealant region close to the solder resist layer and an upper sealant region away from the solder resist layer.

[0244] For example, the content of the photopolymerization initiator (E) included in the upper sealant region or the lower sealant region may be 1000 ppm or less, 900 ppm or less, 800 ppm or less, 700 ppm or less, 600 ppm or less, or 500 ppm or less, relative to the content of the photopolymerization initiator (E) included in the solder resist layer.

[0245] The content of the photopolymerization initiator included in the upper sealant region or the lower sealant region originates from the transfer of the photopolymerization initiator included in the solder resist layer. That is, the photopolymerization initiator of the trimethylbenzoylphosphine oxide-based compound (E) having at least one PO bond disclosed in the present invention can be used to reduce the content of the photopolymerization initiator transferred to the nearby upper sealant region or the lower sealant region.

[0246] For example, when the photopolymerization initiator is transferred to the silicone sealant layer due to outgassing diffusion of the photopolymerization initiator, the silicone sealant is not completely cured due to the inhibition reaction between the phosphorus (P) component of the photopolymerization initiator and the catalyst component (e.g., platinum catalyst) of the silicone sealant layer, resulting in a decrease in the reaction rate of the silicone sealant. The decrease in the reaction rate of the silicone sealant may cause problems related to long-term reliability.

[0247] [Protective film]

[0248] The laminate of the present disclosure may include a cured product and a protective film.

[0249] In the present disclosure, in order to remove the photopolymerization initiator, a protective film may be attached after the photosensitive resin layer is post-cured to form a cured product. Due to the high affinity of the protective film to the photopolymerization initiator, the attachment of the protective film can effectively remove the photopolymerization initiator remaining in the solder resist layer. Removing the residual photopolymerization initiator can reduce the content of the photopolymerization initiator remaining after the flow and firing processes. When the silicone sealant is coated on the cured product layer, the reduction in the content of the photopolymerization initiator leads to an increase in the reaction rate of the silicone sealant, and the increased reaction rate can significantly improve long-term reliability.

[0250] The protective film may be, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, a surface-treated paper, etc. The thickness of the protective film is not particularly limited, but may be, for example, 10 μm to 150 μm.

[0251] For example, the content of the photopolymerization initiator (E) included in the protective film may be 1000 ppm or less relative to the content of the photopolymerization initiator (E) included in the solder resist layer.

[0252] The content of the photopolymerization initiator included in the protective film originates from the transfer of the photopolymerization initiator included in the solder resist layer. That is, the photopolymerization initiator of the trimethylbenzoylphosphine oxide-based compound (E) having at least one PO bond disclosed in the present invention can be used to reduce the content of the photopolymerization initiator transferred to the nearby protective film.

[0253] <Example>

[0254] Hereinafter, the present disclosure will be described in detail with reference to Examples. The present disclosure is not limited to the following Examples.

[0255] <Synthesis Example 1: Alkali-soluble resin A, copolymer resin>

[0256] In a flask equipped with a thermometer, a stirrer, a dropping funnel and a reflux condenser, 325.0 parts by weight of dipropylene glycol monomethyl ether as a solvent was heated to 110° C., and a mixture of 174.0 parts by weight of methacrylic acid, 174.0 parts by weight of ε-caprolactone-modified methacrylic acid (average molecular weight: 314), 77.0 parts by weight of methyl methacrylate, 222.0 parts by weight of dipropylene glycol monomethyl ether, and 12.0 parts by weight of tert-butyl peroxy-2-ethylhexanoate (perbutylated-O of Nichiyu) as a polymerization catalyst was added dropwise over 3 hours, and stirred at 110° C. for 3 hours, and then the polymerization catalyst was deactivated to obtain a resin solution. The resin solution was cooled, and then 289.0 parts by weight of cyclopolymer M100 (Daicel), 3.0 parts by weight of triphenylphosphine and 1.3 parts by weight of hydroquinone monomethyl ether were added. The temperature was raised to 100° C., and the mixture was stirred to perform a ring-opening addition reaction of the epoxy ring, thereby obtaining a resin solution A. The obtained resin solution A had a solid content of 54.5 wt %, and an acid value of the solid content of 79.8 mgKOH / g.

[0257] <Synthesis Example 2: Resin Solution D>

[0258] In an internal pressure vessel equipped with a thermometer, a cooling tube and an agitator, 200 parts by weight of deionized water and 0.3 parts by weight of sodium sulfate were injected and confirmed to be dissolved. Then, 5 parts by weight of benzoyl peroxide (BPO) as a polymerization initiator and 5 parts by weight of α-methylstyrene dimer (MSD) as a chain transfer agent were added to a mixture including 10.4 parts by weight of methyl methacrylate (MMA), 5 parts by weight of n-butyl acrylate (n-BA), 24.6 parts by weight of methacrylic acid (MAA) and 60 parts by weight of styrene, and fully dissolved. Thereafter, a dispersant was added to a concentration of 300 ppm, and the inside of the kiln was replaced with nitrogen by sufficient stirring, and then the temperature was raised to carry out suspension polymerization. After the polymerization was completed, the obtained suspension was filtered through a 30 μm mesh and dried under hot air at 40°C to obtain a granular resin. The obtained particulate resin (copolymer resin) was sufficiently dissolved using dipropylene glycol methyl ether (DPM) as an organic solvent to achieve a solid concentration of 50 wt %, and this solution was referred to as resin solution D. The solid acid value was 160 mgKOH / g.

[0259] <Synthesis Example 3: Carboxyl-containing cresol novolac epoxy acrylate resin A-2>

[0260] In a four-necked flask equipped with a stirrer and a reflux condenser, 220 parts by mass of a cresol novolac type epoxy resin was placed, and 214 parts by mass of carbitol acetate was added and then dissolved by heating. Then, 0.1 parts by mass of hydroquinone as a polymerization inhibitor and 2.0 parts by mass of dimethylbenzylamine as a reaction catalyst were added to prepare a mixture. The mixture was heated to 95°C to 105°C, and 72 parts by mass of acrylic acid was slowly added dropwise, and then reacted for 16 hours. The reaction product was cooled to 80°C to 90°C, and then 106 parts by mass of tetrahydrophthalic anhydride was added to react for 8 hours, then cooled, and then the contents were taken out.

[0261] The photosensitive resin having ethylenically unsaturated bonds and carboxyl groups thus obtained had a nonvolatile content of 64%, a solid acid value of 84.4 mgKOH / g, and a weight average molecular weight (Mw) of about 7500. Hereinafter, the resin is referred to as (A-2). The weight average molecular weight of the obtained resin was measured by GPC.

[0262] Preparation of photosensitive resin composition

[0263] Table 1

[0264] Content of each component of the photosensitive resin composition (unit: based on mass percentage relative to the total composition, each value is rounded to three decimal places, provided that in Example 2, the weight percentage is calculated relative to the total weight of the composition of Example 1).

[0265]

[0266]

[0267]

[0268]

[0269]

[0270] Preparation of dry film of photosensitive resin composition

[0271] Each composition of the examples and comparative examples was coated on a first film (PET film; XD-500P manufactured by Toray Co., Ltd., film thickness: 25 μm) to a uniform thickness (50 μm) by using a notch wheel coater in a clean room. (2) The coated resin composition was dried in four temperature chambers ranging from 40° C. to 120° C. (Chamber 1: 60° C., Chamber 2: 80° C., Chamber 3: 100° C., Chamber 4: 100° C.). (3) The appropriately dried coating film on the first film was combined with a second film (polypropylene, PP film) to prepare a dry film. Specifically, the thickness of the dry coating film was 60 μm.

[0272] Evaluation Example 1: Measurement of outgassing content, silicone sealant reaction rate, and photopolymerization initiator content

[0273] 1. Determination of gas release content

[0274] The photosensitive resin composition of each example and comparative example was laminated on a PET film using a vacuum laminator (CVP-300, Nichigo-Morton) with a first chamber temperature of 60° C., a vacuum pressure of 3 hPa and a vacuum time of 10 seconds to prepare a dry film, and then the PET film was peeled off.

[0275] The DI exposure device manufactured by Screen was used at 300mJ / cm 2 The whole surface was exposed under 400 ° C. and measured by an integrated photometer, while using Kodak Step Tablet No. 2 (41 steps) with 23 steps as a photomask. Subsequently, development was performed at 30 ° C. for 60 seconds with a 1.0% Na2CO3 aqueous solution under a spray pressure of 0.2 MPa. Thereafter, curing was performed in an oven at 150 ° C. for 60 minutes to obtain a cured product of a photosensitive resin layer.

[0276] A powder sample was collected from the manufactured resist layer and placed in a thermal desorption unit (TDU) manufactured by GERSTEL Co., Ltd. Specifically, the powder sample was heated at 150° C. for 60 minutes, starting from 30° C. at a temperature increase rate of 60° C. / min, by using helium as a purge gas (50 ml / min), and then desorbed and collected at −50° C. The collected outgassing components were separated and analyzed in a gas chromatograph mass spectrometer (8890 / 5977B) manufactured by Agilent Technologies Co., Ltd. to be quantified as a conversion rate of n-dodecane, and then the weight percentage of the outgassing components was measured based on the weight of the photopolymerization initiator included in the cured product of the photosensitive resin layer.

[0277] The measurement conditions in the gas chromatography are as follows: Column: Capillary column DB-1MS, manufactured by Agilent Technologies (length 30 m, inner diameter 0.25 mm, thickness 0.25 μm), detector: MS (ITQ900), carrier gas: helium, injector temperature: 300° C., detector temperature: 230° C., column temperature conditions: initial temperature 50° C., maintained at 50° C. for 2 minutes after sample injection, heated to 300° C. at a rate of 12° C. / sec. and maintained at 300° C. for 10 minutes.

[0278] In addition, as described below, a silicone sealant (obtained by laminating a dry film of a photosensitive resin composition on a FR-4Cu film and then peeling off the PET) was formed on the substrate and then heated at 100° C. for 2 hours and at 150° C. for 4 hours for curing.

[0279] The outgassing content, silicone reaction rate, and content of the photopolymerization initiator transferred to the silicone sealant and the protective film in each of Examples and Comparative Examples were measured and shown in the following Table 2. The respective measuring methods refer to the following description.

[0280] [Measurement method of outgassing amount]

[0281] The peak of the photopolymerization initiator was studied by TD-GCMS analysis. The unit of the peak was expressed as μg / g, indicating the amount of gas (μg) in n-dodecane produced per 1g of sample, and the total outgassing amount of the photopolymerization initiator peak was measured. In particular, the ratio of the peak area of ​​the photopolymerization initiator to the area of ​​n-dodecane as the REF of GC-MS was calculated (the calculation formula is provided below).

[0282] Calculation formula: photopolymerization initiator analysis peak area / n-dodecane measurement peak area.

[0283] 2. Measurement of silicone sealant reaction rate and photopolymerization initiator content

[0284] [Calculation of silicone sealant reaction rate and photopolymerization initiator content]

[0285] (1) Each dry film of the photosensitive resin composition (white solder resist composition) was laminated on the FR-4Cu film by using a vacuum laminator (CVP-300, Nichigo-Morton) with the temperature of the first chamber at 60°C under the conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and then the PET film was peeled off.

[0286] The DI exposure device manufactured by Screen was used at 300mJ / cm 2 The photosensitive resin layer was exposed under 400 ° C and measured by an integrated photometer while using Kodak Step Tablet No. 2 (41 steps) with 23 steps as a photomask. Subsequently, the development was carried out at 30 ° C for 60 seconds with a 1.0% Na2CO3 aqueous solution under a spray pressure of 0.2 MPa. Thereafter, curing was carried out in an oven at 150 ° C for 60 minutes to obtain a cured product (solder resist layer) of the photosensitive resin layer.

[0287] A dam with a width of 2.0 cm, a height of 2.0 cm, and a thickness of 250-300 μm was manufactured and then attached to both ends of the cured product of the photosensitive resin layer on the FR-4Cu film. A 1:1 mixture of silicone sealants A and B was added to the space formed by the dam to laminate a silicone sealant layer with a thickness of 250 μm to 300 μm thereon. Thereafter, the silicone sealant was primarily cured by curing at 100°C in an oven for 2 hours, and secondary cured by curing at 150°C in an oven for 4 hours. After completing the secondary curing, a knife was used to separate the interface between the cured product of the photosensitive resin layer and the silicone sealant layer. Then, the reaction rates of the upper and lower sealant regions of the silicone sealant layer and the degree of curing of the silicone sealant in the silicone sealant layer were measured on a ZnSe crystal plate using an FT-IR system.

[0288] [Calculation method of silicone reaction rate]

[0289] 1) Silicone samples that were not subjected to primary and secondary curing and silicone samples that were subjected to secondary curing (upper and lower parts) were prepared.

[0290] 2) Uncured silicone and cured silicone were placed on a ZnSe crystal plate and FT-IR measurements were performed.

[0291] 3) By comparing the Si-H peak of the cured silicone with the adjacent region (2160 -1 ) to calculate the reaction rate, while using the uncured silicone as the REF (calculation formula provided below).

[0292] Calculation formula: Si-H peak height of cured silicone / Si-H peak height of uncured silicone × 100

[0293] (2) The content of the photopolymerization initiator was measured using gel permeation chromatography while using the silicone sealant separated by a knife.

[0294] Specifically, 0.05 g of the analyte sample as the secondary post-curing silicone sealant was separated from the silicone sealant layer formed on the cured product of the photosensitive resin layer with a knife. 0.05 g of the analyte sample was dissolved in 10.0 g of THF and then filled into a vial. In order to dissolve the undissolved photosensitive resin composition in the solution, an ultrasonic vibrator was used for 5 minutes to prepare the sample. Thereafter, 100 μl of the sample was injected into a gel permeation chromatography (GPC) device and the analysis was completed.

[0295] [Calculation of the content of the photopolymerization initiator transferred to the protective film]

[0296] The PF protective film was attached to the secondary cured silicone sealant and placed at a temperature of 40°C and a humidity of 90% for 24 hours. Then, the PF protective film was peeled off, and then a 0.05g sample was separated from the silicone sealant layer formed on the cured product of the photosensitive resin layer with a knife as an analyte sample of the PF protective film. 0.05g of the analyte sample was dissolved in 5.0g of tetrahydrofuran (THF) and then loaded into a vial. In order to dissolve the undissolved photosensitive resin composition in the solution, an ultrasonic vibrator was used for 5 minutes to prepare the sample. Thereafter, 100μl of the sample was injected into a gel permeation chromatography (GPC) device and the analysis was completed.

[0297] [Gel Permeation Chromatography (GPC) Measurement Method and Measurement Conditions for Photopolymerization Initiator Content Analysis]

[0298] The sampled sample was injected into the GPC equipment (GPC equipment name: E2695 water separation module, detector: 2998PDA / 2414RI, flow rate: 0.5 ml / min, column: HSP gel HR MB-L 2.0 and HSP gel HR1.0, measurement temperature: 4°C, mobile phase: THF). Regarding the calculation method, the peak at the absorption wavelength of 382 nm of TPO as a photopolymerization initiator was quantified and analyzed. The sampled analyte sample and TPO were used as REF photopolymerization initiator samples. The same procedure was performed on samples containing 1 ppm, 10 ppm and 100 ppm TPO to obtain a calibration curve, and the calibration curve results obtained at each concentration were used to quantify the photopolymerization initiator included in the sample.

[0299] (Evaluation of outgassing amount)

[0300] ◎: Outgassing content <500ppm

[0301] ○: 500ppm≤gas release content<1000ppm

[0302] △: 1000ppm≤gas release content<2000ppm

[0303] X: 2000ppm≤gas release content

[0304] (Evaluation of the reaction rate of silicone sealants)

[0305] ◎: 70% ≤ upper silicone sealant reaction rate

[0306] ○: 55%≤ Upper silicone sealant reaction rate<70%

[0307] △: 40%≤ Upper silicone sealant reaction rate<55%

[0308] X: Reaction rate of silicone sealant <40%

[0309] (Evaluation of the reaction rate of silicone sealants)

[0310] ◎: 50% ≤ silicone sealant reaction rate

[0311] ○: 40% ≤ silicone sealant reaction rate <50%

[0312] △: 30% ≤ silicone sealant reaction rate <40%

[0313] X: Reaction rate of silicone sealant <30%

[0314] (Content of photopolymerization initiator transferred to sealant)

[0315] ◎: Photopolymerization initiator content <300ppm

[0316] ○: 300ppm≤Photopolymerization initiator content<500ppm

[0317] △: 500ppm≤Photopolymerization initiator content<700ppm

[0318] X: 700ppm≤Photopolymerization initiator content

[0319] Table 2

[0320]

[0321] Referring to Table 2, the outgassing contents of Examples 1 to 10 including photopolymerization initiator 1 or 2 are significantly lower than the outgassing contents of Comparative Examples 1 to 4, 6, and 7. This significant reduction in outgassing of the photopolymerization initiator can solve the yellowing problem of the silicone sealant and greatly improve the reaction rate of the silicone sealant. The reduction in the amount of photopolymerization initiator transferred to the silicone sealant can improve the long-term reliability and stability of the product.

[0322] In Comparative Examples 1 to 4, 6 and 7 using TPO as a photopolymerization initiator, as described above, the transferred photopolymerization initiator TPO remains at a content of 700 ppm or more in the silicone sealant, resulting in reduced reflectivity and reaction rate of the silicone sealant and problems associated with long-term reliability of the product.

[0323] In Examples 1 and 2, where only Omnipol TP is used as the photopolymerization initiator, the outgassing content of the photopolymerization initiator and the content of the photopolymerization initiator transferred to the silicone sealant are significantly reduced, thereby maintaining high reflectivity, increasing the reaction rate in the sealant area, and improving the long-term reliability and stability of the product.

[0324] In Examples 3 to 10 using Omnirad TPO L as a photopolymerization initiator, the outgassing content and the content of photopolymerization initiator transferred to the silicone sealant are significantly reduced, thereby maintaining high reflectivity, increasing the reaction rate in the sealant area, and improving the long-term reliability and stability of the product.

[0325] Next, a protective film (PF) was formed on the silicone sealant and kept at 40°C / 90% humidity for 24 hours, and only the protective film was peeled off. Then, the content of the photopolymerization initiator transferred to the protective film was measured using gel permeation chromatography, as shown in Table 3 below.

[0326] (Evaluation of Photopolymerization Initiator Content)

[0327] ◎: Photopolymerization initiator content <500ppm

[0328] ○: 500ppm≤Photopolymerization initiator content<2000ppm

[0329] △: 2000ppm≤Photopolymerization initiator content<4000ppm

[0330] X: 4000ppm≤Photopolymerization initiator content

[0331] Table 3

[0332]

[0333]

[0334] Referring to Table 3 and Table 2, the outgassing content of Examples 1 to 10 including photopolymerization initiator 1 or 2 is significantly lower than the outgassing content of Comparative Examples 1 to 4, 6 and 7 including other photopolymerization initiators, and thus the content of photopolymerization initiator transferred not only to the silicone sealant but also to the protective film is greatly reduced. Specifically, compared with Comparative Examples 1-4, 6 and 7, Examples 1-10 show a significant reduction in the photopolymerization initiator transferred to the protective film (PF). This indicates that the use of the photopolymerization initiator represented by Chemical Formulas 1 and 2 reduces outgassing, and the reduction in outgassing prevents the transfer of the photopolymerization initiator to the silicone sealant and the protective film, and therefore, the use of the photopolymerization initiator defined in the present disclosure can increase the reflectivity and improve the reaction rate and degree of curing of the silicone sealant, thereby improving long-term reliability.

[0335] Evaluation Example 2: BHAST Test

[0336] Each dry film prepared in Examples 3 and 4 and Comparative Examples 1 to 4 was laminated on a substrate having a comb electrode (line / space=50μm / 50μm) using a vacuum laminator (CVP-300, Nichigo-Morton) at a first chamber temperature of 60°C, a vacuum pressure of 3hPa and a vacuum time of 10 seconds, and then pressed under a pressure of 0.2MPa and a pressing time of 10 seconds to obtain an evaluation substrate. The PET film was peeled off, and then exposed using a DI exposure device (Screen) with an exposure dose obtained in Step Tablet (41 steps) 23 steps, and then developed (mass 1% Na2CO3, 30°C, 0.2MPa) for 60 seconds to complete the substrate manufacturing. After the substrate manufacturing was completed, the substrate was subjected to BHAST for 250 hours in a chamber under the conditions of 110°C, 85% and 20V to evaluate insulation reliability, BHAST resistance and reflectivity, etc.

[0337] The BHAST test results are shown in Figure 1A and Figure 1B.

[0338] After the BHAST test, the reflectance was measured and is shown in the following Table 4. The reflectance was measured at a wavelength of 450 nm using a spectrophotometer (CM-2600d, Konica Minolta Sensing Co., Ltd.).

[0339] ◎: 90% ≤ reflectivity

[0340] ○: 87% ≤ reflectivity < 90%

[0341] △: 84% ≤ reflectivity < 87%

[0342] X: Reflectivity < 84%

[0343] In addition, a HAST resistance test was performed and the results are shown in Table 4 below.

[0344] Each dry film prepared in the embodiments and comparative examples was laminated on a substrate having a comb-shaped electrode (line / space = 50 μm / 50 μm) using a vacuum laminator (CVP-300, Nichigo-Morton Co., Ltd.) at a first chamber temperature of 60°C, a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and then pressed under a pressure of 0.2 MPa and a pressing time of 10 seconds to obtain an evaluation substrate.

[0345] The PET film was peeled off and then 2The exposure was measured by an integrated photometer under a spray pressure of 0.2 MPa. Then, a 1.0% Na2CO3 aqueous solution was used for development at 30°C for 60 seconds, and a cured coating of a dry film cured at 150°C for 60 minutes in an oven was formed to manufacture a HAST evaluation substrate. The evaluation substrate was placed in a high temperature and high humidity bath at a temperature of 110°C and a humidity of 85%, charged at a voltage of 20V, and subjected to a 250-hour high accelerated stress test (HAST) in the bath. After 250 hours, the discoloration and elution of the cured coating of the dry film were evaluated according to the following evaluation criteria (equipment manufacturer: Espec Co., Ltd., ion migration system, equipment name: NY IM1064).

[0346] ○: No peeling, discoloration or elution was observed.

[0347] X: Peeling, discoloration, or elution is often observed with the naked eye.

[0348] Table 4

[0349]

[0350] Referring to Table 4, the reflectivity after HAST test in Examples 3 and 4 is higher than that in Comparative Examples 1 to 4. In addition, compared with Comparative Examples 1 to 4, Examples 3 and 4 show higher reflectivity, very low copper oxidation and corrosion, and no peeling, discoloration or dissolution after HAST test.

[0351] Evaluation Example 3: Reflectivity Test (After Reflow and UV Treatment)

[0352] Each of the dry films prepared in Examples 1 to 4 and Comparative Examples 1 to 7 was laminated on a copper substrate using a vacuum laminator (CVP-300, Nichigo-Morton Co., Ltd.) at a first chamber temperature of 60° C., a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and then pressed under a pressure of 0.2 MPa and a pressing time of 10 seconds.

[0353] The PET film was peeled off and then the DI exposure device manufactured by Screen was used at 300 mJ / cm 2The exposure was carried out under 400 ° C and measured by an integrated photometer, while Kodak Step Tablet No. 2 (41 steps) was used to set 23 steps as a photomask. Subsequently, under a spray pressure of 0.2 MPa, development was carried out at 30 ° C for 60 seconds with a 1.0% Na2CO3 aqueous solution. After that, curing was carried out in an oven at 150 ° C for 60 minutes to obtain a substrate. The reflectivity of the coating surface of the obtained substrate at a wavelength of 450nm was measured by using a spectrophotometer (CM-2600d, KonicaMinolta Sensing Co., Ltd.). Reflow was carried out one to three times at 260 ° C for 10 seconds, and the reflectivity was measured. The results are shown in Table 5. After post-curing, at 500mJ / cm 2 The UV was passed through the integrated photometer three times under the conditions of , and the reflectance was measured each time. The results are shown in Table 6.

[0354] ◎: 90% ≤ reflectivity

[0355] ○: 87% ≤ reflectivity < 90%

[0356] △: 84% ≤ reflectivity < 87%

[0357] X: Reflectivity < 84%

[0358] Table 5

[0359]

[0360]

[0361] The initial reflectivity without performing the reflow process and the reflectivity at 450 nm after the reflow process once, twice and three times and after the reflow process once and the firing process in Examples 1 to 4 are higher than those in Comparative Examples 1 to 7, indicating that the reflectivity reduction after reflow or firing is minimized.

[0362] Specifically, for Examples 1 to 4, Omnipol TP or Omnirad TPO-L was used as a photopolymerization initiator, resulting in a small amount of outgassing, which had little effect on the silicone sealant, so the firing process could be omitted. Therefore, high reflectivity could be obtained even after reflow.

[0363] However, for Comparative Examples 1 to 7, in order to be applied to backlight unit products, since the TPO photopolymerization initiator affects the curability of the silicone sealant, a firing process for removing TPO is required after the reflow process. In addition, the implementation of the firing process leads to a significant reduction in reflectivity.

[0364] In summary, Examples 1 to 4 show excellent reflectivity at an equal or higher level than Comparative Examples 1 to 7 even when applied to actual products, and as previously discussed in Table 2, show excellent reaction rate and degree of curing of the silicone sealant, thereby improving the long-term durability and stability of the product.

[0365] Table 6

[0366] Reflectivity evaluation after post-curing and UV treatment

[0367]

[0368]

[0369]

[0370] Regarding the reflectivity at 450 nm, Examples 1 to 4 showed higher initial reflectivity than Comparative Examples 1 to 6, and showed a similar trend even after being treated with 500 mJ of UV three times. The reflectivity of Examples 1 to 4 after the UV treatment three times was 90.2 to 90.6, but the reflectivity of Comparative Examples 1 to 4 after the UV treatment three times was 73 to 89.7, which may be caused by the deterioration of yellowing.

[0371] Evaluation Example 4: Test in a chamber at 85°C and 85% humidity and reflectivity test in a HS chamber

[0372] Each of the dry films prepared in Examples 2 to 4 and Comparative Example 1 was laminated using a vacuum laminator (CVP-300, Nichigo-Morton Co., Ltd.) at a first chamber temperature of 60° C., a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and then pressed under a pressure of 0.2 MPa and a pressing time of 10 seconds to obtain an evaluation substrate.

[0373] The PET film was peeled off and then measured by an integrated photometer at 300 mJ / cm 2 The substrate was exposed under 0.2 MPa of spray pressure. Subsequently, it was developed at 30 ° C for 60 seconds with 1.0% Na2CO3 aqueous solution. After that, it was cured in an oven at 150 ° C for 60 minutes to obtain a substrate. Under the conditions of 85 ° C temperature and 85% humidity, the obtained substrate was placed in a chamber (HIFLEX, temperature and humidity chamber, provided by ETAC) and placed for 1000 hours. The reflectivity of the substrate placed in the HS chamber for 1000 hours was measured using a spectrophotometer (CM-2600d, Konica Minolta Sensing Co., Ltd.) at a wavelength of 450nm. The results are shown in Table 7.

[0374] ◎: 90% ≤ reflectivity

[0375] ○: 87% ≤ reflectivity < 90%

[0376] △: 84% ≤ reflectivity < 87%

[0377] X: Reflectivity < 84%

[0378] Table 7

[0379] Reflectivity evaluation after being placed in a chamber at a temperature of 85°C and a humidity of 85%

[0380]

[0381]

[0382] Even when evaluated for a long time under high temperature and high humidity conditions, Examples 2 to 4 showed a small decrease in the reflectance at 450 nm even under high temperature and high humidity conditions.

[0383] After evaluation under high temperature and high humidity conditions, the b values ​​in Examples 2 to 4 are smaller than that in Comparative Example 1. This indicates that under high temperature and high humidity conditions, Examples 2 to 4 experience less yellowing than Comparative Example 1. Even under high temperature and high humidity conditions, Examples 2 to 4 experience less yellowing than Comparative Example 1 and thus may be more advantageous as a material for a backlight unit.

[0384] Evaluation Example 5: General Performance Evaluation

[0385] <Manufacturing of Evaluation Substrate>

[0386] Each of the photosensitive resin compositions prepared in the examples and comparative examples was laminated on a PET film using a vacuum laminator (CVP-300, Nichigo-Morton Co., Ltd.) at a first chamber temperature of 60° C., a vacuum pressure of 3 hPa, and a vacuum time of 10 seconds, and then pressed under a pressure of 0.2 MPa and a pressing time of 10 seconds to obtain an evaluation substrate. The PET film was peeled off, and then a DI exposure device manufactured by Screen Co., Ltd. was used at 300 mJ / cm 2 The substrate was exposed at 400 ° C and measured by an integrated photometer, while using Kodak Step Tablet No. 2 (41 steps) with 23 steps as a photomask. Subsequently, the substrate was developed at 30 ° C for 60 seconds with a 1.0% Na2CO3 aqueous solution under a spray pressure of 0.2 MPa, and post-cured in an oven at 150 ° C to manufacture a substrate.

[0387] <Pencil hardness>

[0388] For the substrate, a pencil of B to 9H that had been polished to flatten the tip of the core was pressed at an angle of about 45° to record the hardness of the pencil without peeling off the coating film.

[0389] <Adhesion>

[0390] Mark 1 mm (10 × 10) checkerboard squares on the substrate, completely stick transparent tape on the checkerboard squares, immediately peel off the tape while holding one end of the tape at right angles to the substrate, and then check the number of checkerboard squares that were not completely peeled off. Use the number of remaining checkerboard squares as the numerator and the total number of checkerboard squares (100) as the denominator to record the result.

[0391] PASS: At least 95% of the board squares remain.

[0392] NG: Fewer than 95% of the board squares remain.

[0393] <Glossiness evaluation>

[0394] The glossiness of the coating surface of the substrate at an angle of 60° was measured using a gloss colorimeter (BYK E-4430).

[0395] <Solder Heat Resistance>

[0396] Immerse the substrate in a 288°C solder bath for 10 seconds. Then, mark 1 mm (10×10) checkerboard squares on the substrate and completely stick transparent tape to the checkerboard squares, immediately peel it off while holding one end of the tape at a right angle to the substrate, and then check the number of checkerboard squares that were not completely peeled off. Use the number of remaining checkerboard squares as the numerator and the total number of checkerboard squares (100) as the denominator to record the result.

[0397] PASS: At least 95% of the board squares remain.

[0398] NG: Fewer than 95% of the board squares remain.

[0399] Table 8

[0400]

[0401] Comparative Example 5 had a small amount of photopolymerization initiator, resulting in incomplete surface curing, and thus showed a pencil hardness as low as 3H, a significant decrease in glossiness to 72, NG adhesion and solder heat resistance, and unfavorable developability. Comparative Example 6 had an excessively high content of photopolymerization initiator, resulting in good surface curing to ensure excellent adhesion and solder heat resistance, but poor developability due to increased curability, which may cause problems in the formation of SRO. Example 7 showed an improved pencil hardness of up to 6H and significantly improved adhesion and solder heat resistance, and Example 8 showed an improved pencil hardness of up to 6H and significantly improved adhesion and solder heat resistance.

[0402] Evaluation Example 6: Analysis of phosphorus content in photosensitive resin composition

[0403] 1) Accurately weigh each photosensitive resin composition of Examples 1 to 8 and Comparative Examples 1 to 6 to 0.1 g in a beaker, then add 2 mL of nitric acid and heat on a hot plate to react. 2) The sample was temporarily placed on a hot plate and cooled to room temperature, and 0.03 mL of hydrochloric acid in a hot state was added to react. 3) Thereafter, the nitric acid solution of the sample was not allowed to evaporate completely, leaving only a small amount. The residue was cooled to room temperature and then completely dissolved in 1 mL of concentrated nitric acid added again. The sample was completely dissolved and then diluted with ultrapure water. 4) The phosphorus (P) concentration of the Examples and Comparative Examples was analyzed under wavelength conditions of 213.617 nm and 214.914 nm by using an ICP-OES analysis system (Optima series, manufactured by Perkin Elmer Co., Ltd.).

[0404] Table 9

[0405]

[0406] The compositions of Examples 1 to 8 and Comparative Examples 1 to 4 were detected to have a phosphorus concentration of about 3000 ppm. Since Comparative Example 5 did not use a phosphorus-containing photopolymerization initiator, its phosphorus content was detected to be as low as 430 ppm. The phosphorus content of Comparative Example 6 was detected to be 5500 ppm.

Claims

1. A photosensitive resin composition comprising: (A) a carboxyl-containing resin that does not contain an aromatic ring; (B) inorganic fillers; and (E) A photopolymerization initiator of a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond.

2. The photosensitive resin composition according to claim 1, wherein (E) the photopolymerization initiator of the trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond comprises a *-C(=O)-P(=O)R1-O-*' portion (wherein, R1 is an alkyl group of 1 to 20 carbon atoms, an alkenyl group of 2 to 20 carbon atoms, an alkynyl group of 2 to 20 carbon atoms, or a cyclic group of 5 to 20 carbon atoms). 3 . The photosensitive resin composition according to claim 1 , wherein the photopolymerization initiator (E) of the trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond is a trimethylbenzoylphosphine oxide group-containing polymer. 4 . The photosensitive resin composition according to claim 3 , wherein the polymer containing a trimethylbenzoylphosphine oxide group has a weight average molecular weight (Mn) of 900 g / mol or more.

5. The photosensitive resin composition according to claim 3, wherein the polymer containing trimethylbenzoylphosphine oxide groups is represented by the following Chemical Formula 1: <Chemical Formula 1> a=0 to 100, b=0 to 100, and c=0 to 100. 6 . The photosensitive resin composition according to claim 1 , wherein the photopolymerization initiator of (E) the trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond comprises an alkoxy group. 7 . The photosensitive resin composition according to claim 1 , wherein the photopolymerization initiator of (E) the trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond comprises an ethoxy group.

8. The photosensitive resin composition according to claim 1, wherein (E) the photopolymerization initiator of a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond is represented by the following Chemical Formula 2: <Chemical Formula 2> 9 . The photosensitive resin composition according to claim 1 , wherein the photopolymerization initiator of (E) a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond is included in an amount of 0.01 wt % to 10 wt % relative to the total weight of the composition. 10 . The photosensitive resin composition according to claim 1 , wherein (A) the carboxyl-containing resin having no aromatic ring has an unsaturated double bond. 11 . The photosensitive resin composition according to claim 1 , further comprising (D) a resin containing an aromatic ring. 12 . The photosensitive resin composition according to claim 11 , wherein (D) the aromatic ring-containing resin is a melamine resin, a silicone resin or a resin having a styrene main chain. 13 . The photosensitive resin composition according to claim 1 , further comprising (C) a mercapto-modified (meth)acrylate. 14 . The photosensitive resin composition according to claim 1 , further comprising (F) a silane coupling agent. 15 . The photosensitive resin composition according to claim 1 , further comprising (G) a resin having a urethane bond.

16. The photosensitive resin composition according to claim 1, wherein the outgassing content of the photosensitive resin composition measured by thermal desorption spectroscopy (TDS) and gas chromatography-mass spectrometry (GC-MS) is 1000 ppm or less relative to (E) the photopolymerization initiator of a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond. 17 . The photosensitive resin composition according to claim 1 , wherein the content of phosphorus is 500 ppm to 5000 ppm.

18. A photosensitive resin composition comprising: (A) a carboxyl-containing resin that does not contain an aromatic ring; (B) mercapto-modified (meth)acrylate; and (E) A photopolymerization initiator of a trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond. 19 . The photosensitive resin composition according to claim 18 , further comprising (D) a resin containing an aromatic ring. 20 . The photosensitive resin composition according to claim 18 , further comprising (F) a silane coupling agent. 21 . The photosensitive resin composition according to claim 18 , further comprising (G) a resin having a urethane bond. 22 . A dry film having a photosensitive resin layer formed by applying the photosensitive resin composition according to claim 1 to a first film and drying it. 23 . A cured product obtained by curing the photosensitive resin composition according to claim 1 or a photosensitive resin layer for a dry film obtained from the photosensitive resin composition.

24. A printed circuit board comprising the cured product of claim 23 as a solder resist.

25. The printed circuit board of claim 24, further comprising a silicone sealant disposed on the solder resist.

26. The printed circuit board of claim 25, wherein the silicone sealant comprises an upper sealant region and a lower sealant region, and The content of the photopolymerization initiator of the (E) trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond contained in at least one of the upper sealant region or the lower sealant region is 1000 ppm or less relative to the content of the photopolymerization initiator of the (E) trimethylbenzoylphosphine oxide group-containing compound having at least one PO bond contained in the solder resist.

27. A laminate comprising: The cured product according to claim 23; and Protective film.

28. A laminate according to claim 27, wherein the content of the photopolymerization initiator of the compound containing a trimethylbenzoylphosphine oxide group having at least one PO bond (E) contained in the protective film is 1000 ppm or less relative to the content of the photopolymerization initiator of the compound containing a trimethylbenzoylphosphine oxide group having at least one PO bond (E) contained in the solder resist.

Citation Information

Patent Citations

  • Optically achromatized acoustooptic deflection apparatus

    EP0000104A1

  • Process for preventing polymer buildup in a polymerization reactor

    EP0000400A1

  • Process for preparing butyl-p-benzoylbenzoates

    EP0000502A1

  • 1-Methylisoguanosin, processes and intermediates for its preparation, its pharmaceutical compositions and their preparation

    EP0000770A2

  • Tipping vehicle

    EP0001020A1

Cited By

  • Photosensitive resin composition, photosensitive dry film, cured film and circuit board

    CN119916643A