Steel plate

By adjusting the chemical composition and microstructure of the steel plate, combining annealing and aging treatment, the problem of the reduction of the strength of the lithium-ion battery steel plate at high temperatures is solved. The Ni plating layer is used to enhance the stamping forming property, and the stability of the battery can structure under abnormal heating is achieved. Increased properties and high temperature intensity.

CN119095994APending Publication Date: 2024-12-06NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380034953.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-06
Filing Date
2023-10-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, the strength of the steel plate of lithium-ion batteries is significantly reduced under high temperature conditions, and the structural integrity of the battery can cannot be effectively maintained, especially in abnormal heating conditions.

Method used

By adjusting the chemical composition and microstructure of the steel plate, the residual amount of solid solution C and solid solution N in the steel plate is ensured, annealing and aging treatment are used to improve the high temperature strength, and Ni coating is formed on the surface of the steel plate to enhance stamping forming.

Benefits of technology

The high temperature strength of the steel plate under high temperature conditions of 200-300℃ has been significantly improved, ensuring the structural stability and stamping forming of the battery tank under abnormal heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005091252000000281
    Figure BDA0005091252000000281
  • Figure BDA0005091252000000291
    Figure BDA0005091252000000291
  • Figure BDA0005091252000000301
    Figure BDA0005091252000000301
Patent Text Reader

Abstract

Provided is a steel sheet having excellent high-temperature strength. A steel sheet according to the present disclosure has a chemical composition containing, in mass%, 0.040-0.070% of C, more than 0 and 0.10% or less of Si, 0.20-0.40% of Mn, more than 0 and 0.030% or less of P, more than 0 and 0.030% or less of S, 0.005-0.100% of Sol.Al, more than 0 and 0.0150% or less of N, 0.0001-0.0030% of B, 0-0.010% of Ti, 0-0.010% of Nb, 0-0.5% of Cu, 0-0.5% of Ni, 0-0.3% of Cr, and 0-0.05% of Sn, ferrite being a main phase, a grain size grade of 11.0 or more, a sheet thickness of 0.15-1.00 mm, a yield strength at room temperature of 220-500 MPa, a tensile strength of 330-550 MPa, and The aging index (AI) is 50.0 MPa or more, and the ratio of the tensile strength at 300 DEG C to the tensile strength at room temperature is 0.90 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a steel sheet, and more specifically, to a steel sheet used as a material for a battery can and subjected to a press working in a manufacturing process of the battery can. Background Art

[0002] Steel sheets are used as blanks for battery cans for secondary batteries such as lithium-ion batteries. Steel sheets for battery cans are usually formed with Ni plating or Ni diffusion plating before being processed into the shape of a battery can by stamping. Specifically, the steel sheets with the above-mentioned plating are subjected to multi-stage drawing and DI (Drawing and Ironing) processing to form the shape of a battery can.

[0003] In such a steel sheet used as a blank for battery cans and subjected to stamping, strength at room temperature after canning, stamping formability, and surface roughness resistance are required. Stamping formability refers to the property of being able to form a steel sheet while suppressing the occurrence of defects such as cracks during stamping processes such as deep drawing or DI processing. Surface roughness resistance refers to suppressing the surface roughness of the steel sheet after stamping.

[0004] In the steel plate used as the blank of the battery can and the object of stamping, the strength, stamping formability and surface roughness resistance of the battery can after canning are improved by adjusting the microstructure, grain size, and mechanical properties (yield strength, tensile strength and total elongation) at room temperature.

[0005] For example, the steel sheet disclosed in Japanese Patent No. 3516813 (Patent Document 1) contains, by mass%, C: 0.0030% or less, Si: 0.05% or less, Mn: 0.5% or less, P: 0.03% or less, S: 0.020% or less, sol.Al: 0.01-0.100%, N: 0.0070% or less, Ti: 0.01-0.050%, Nb: 0.008-0.030%, B: 0.0002-0.0007%, and the balance is Fe and inevitable elements. In this steel sheet, the grain size grade is set to 10.0 or more.

[0006] In addition, the steel sheet disclosed in Japanese Patent No. 5359709 (Patent Document 2) contains C: 0.0035-0.0080%, Si: 0.35% or less, Mn: 1.0% or less, P: 0.030% or less, S: 0.025% or less, sol.Al: 0.003-0.100%, N: 0.0100% or less, Nb: 0.040% or less, and (3-6)×C%, the remainder being Fe and inevitable impurities. In this steel sheet, the grain size grade of the recrystallized grains is also set to 11.0-13.0.

[0007] In the steel sheets disclosed in Patent Documents 1 and 2, surface roughening resistance is improved by adjusting the grain size grade.

[0008] The steel sheet disclosed in International Publication No. 2016 / 080344 (Patent Document 3) contains, by mass%, C: greater than 0.150 and less than 0.250%, Sol.Al: 0.005-0.100%, B: 0.0005-0.02%, Si: less than 0.50%, Mn: less than 0.70%, P: less than 0.070%, S: less than 0.05%, N: less than 0.0080%, Nb: less than 0.003%, Ti: less than 0.003%, and the balance is Fe and impurities. In this steel sheet, the yield strength after aging treatment is 310-370 MPa, and the total elongation is 24-30%.

[0009] In addition, the steel sheet disclosed in International Publication No. 2016 / 060248 (Patent Document 4) contains, as chemical components, by mass %, C: greater than 0.150 and less than 0.260%, Sol.Al: 0.005-0.100%, B: 0.0005-0.02%, Si: less than 0.50%, Mn: less than 0.70%, P: less than 0.070%, S: less than 0.05%, N: less than 0.0080%, Nb: less than 0.003%, Ti: less than 0.003%, and the balance is Fe and impurities. In this steel sheet, as a microstructure, ferrite and spheroidal cementite are included, the yield strength after aging treatment is 360-430 MPa, and the total elongation is 25-32%.

[0010] In the steel sheets disclosed in Patent Documents 3 and 4, the strength of the battery can after canning is improved by adjusting the yield strength, and the press formability of the steel sheets is improved by adjusting the microstructure and total elongation.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent No. 3516813

[0014] Patent Document 2: Japanese Patent No. 5359709

[0015] Patent Document 3: International Publication No. 2016 / 080344

[0016] Patent Document 4: International Publication No. 2016 / 060248 Summary of the invention

[0017] Problem that the invention aims to solve

[0018] However, in lithium-ion batteries installed in electric vehicles and the like, abnormal heat may be generated in the battery due to internal short circuits or overcharging. Assume that when abnormal heat is generated, the temperature of the battery can becomes a high temperature of about 200 to 300°C. In this specification, "high temperature" refers to 200 to 300°C. Even in the case of such abnormal heat generated in the battery can, it is preferable to maintain the strength of the battery can. Therefore, in the steel plate used as the blank of the battery can and the object of stamping, high temperature strength at 200 to 300°C is also required.

[0019] Generally, the strength of a steel sheet at high temperature is significantly lower than the strength of a steel sheet at room temperature. Patent Documents 1 to 4 do not conduct research on the high temperature strength of a steel sheet for battery cans.

[0020] An object of the present disclosure is to provide a steel sheet having excellent high temperature strength.

[0021] Solutions for solving problems

[0022] The chemical composition of the steel sheet disclosed herein contains, by mass%,

[0023] C: 0.040~0.070%,

[0024] Si: more than 0 and less than 0.10%,

[0025] Mn: 0.20~0.40%,

[0026] P: greater than 0 and less than 0.030%,

[0027] S: greater than 0 and less than 0.030%,

[0028] Sol.Al: 0.005~0.100%,

[0029] N: more than 0% and less than 0.0150%,

[0030] B: 0.0001~0.0030%,

[0031] Ti: 0~0.010%,

[0032] Nb: 0~0.010%,

[0033] Cu: 0-0.5%,

[0034] Ni: 0-0.5%,

[0035] Cr: 0 to 0.3%, and

[0036] Sn: 0~0.05%, the balance is Fe and impurities,

[0037] The steel plate has ferrite as the main phase in the microstructure, and the grain size grade of the ferrite is above 11.0.

[0038] The thickness of the steel plate is 0.15 to 1.00 mm.

[0039] The yield strength of the steel plate at room temperature is 220-500 MPa, the tensile strength at room temperature is 330-550 MPa, and the total elongation at room temperature is more than 20.0%.

[0040] The aging index AI of the steel plate is 50.0 MPa or more,

[0041] The ratio of the tensile strength of the steel sheet at 300° C. to the tensile strength at room temperature is 0.90 or more.

[0042] Effects of the Invention

[0043] The steel sheet of the present disclosure has excellent high temperature strength. DETAILED DESCRIPTION

[0044] The inventors of the present invention first studied a method for improving the strength, stamping formability, and surface roughness resistance of a battery can after canning in a steel plate that is suitable as a blank for a battery can and is the object of a stamping process. As also proposed in Patent Documents 1 to 4, the chemical composition, microstructure, grain size, and mechanical properties (yield strength, total elongation, etc.) of the steel plate at room temperature affect the strength, stamping formability, and surface roughness resistance of the battery can after canning. Therefore, the inventors of the present invention studied the chemical composition, microstructure, and grain size of the steel plate. As a result, the inventors have found that a steel sheet suitable as a blank for a battery can and a target for press working can have sufficient strength, sufficient press formability, and sufficient surface roughness resistance of a battery can after canning if the steel sheet has a chemical composition, in terms of mass%, of C: 0.040 to 0.070%, Si: greater than 0 and less than 0.10%, Mn: 0.20 to 0.40%, P: greater than 0 and less than 0.030%, S: greater than 0 and less than 0.030%, sol.Al: 0.005 to 0.100%, N: greater than 0 and less than 0. 0150% or less, B: 0.0001~0.0030%, Ti: 0~0.010%, Nb: 0~0.010%, Cu: 0~0.5%, Ni: 0~0.5%, Cr: 0~0.3%, and Sn: 0~0.05%, and the balance is Fe and impurities. In the microstructure, ferrite is the main phase, the grain size grade of ferrite is above 11.0, the plate thickness is 0.15~1.00mm, the yield strength at room temperature is 220~500MPa, the tensile strength at room temperature is 330~550MPa, and the total elongation at room temperature is above 20.0%.

[0045] The present inventors have also studied methods for improving the high temperature strength of a steel plate satisfying the above-mentioned chemical composition, microstructure, grain size grade, and plate thickness.

[0046] Among them, the present inventors have paid attention to the amount of dissolved C and dissolved N in the steel sheet. The dissolved C and dissolved N in the steel sheet reduce the stamping formability. Therefore, in the steel sheet to be subjected to stamping, the steel sheet before stamping is annealed, and then further subjected to overaging treatment, etc., to reduce the amount of dissolved C and dissolved N.

[0047] However, the inventors of the present invention thought of allowing the amount of dissolved C and dissolved N in the steel plate to remain in order to improve the high-temperature strength. The temperature range in which strength is required in the battery can is about 200 to 300°C as mentioned above. If dissolved C and dissolved N exist in the steel plate in such a high-temperature region, dynamic strain aging occurs. That is, in the above-mentioned high-temperature region, dissolved C and dissolved N diffuse moderately and fix to the dislocations in the steel plate. Therefore, it is believed that dissolved C and dissolved N contribute to the improvement of high-temperature strength at 200 to 300°C.

[0048] Therefore, the inventors of the present invention have attempted to ensure higher strength in the high temperature region of 200 to 300°C by daring to ensure a certain degree of dissolved C and dissolved N in the steel plate. Among them, it is extremely difficult to quantitatively analyze the dissolved C and dissolved N in the steel plate. Therefore, the inventors of the present invention have paid attention to the aging index AI (Aging Index) as an indicator of the dissolved C and dissolved N in the steel plate. The dissolved C and dissolved N amounts of the steel plate are related to the aging index AI. Specifically, the more dissolved C and dissolved N there are in the steel plate, the higher the aging index AI. Therefore, the dissolved C and dissolved N amounts in the steel plate can be inferred based on the aging index AI.

[0049] Therefore, the inventors of the present invention further tried to adjust the aging index AI in the steel plate satisfying the above chemical composition, microstructure, grain size grade, plate thickness and mechanical properties at room temperature. As a result, it was found that if the aging index AI is 50.0 MPa or more, the above mechanical properties at room temperature can be maintained in the steel plate having the above chemical composition, microstructure, grain size grade and plate thickness, and the high temperature strength at 200 to 300°C can be improved. Specifically, it was found that by setting the aging index AI to 50.0 MPa or more in the steel plate satisfying the chemical composition, microstructure, grain size grade, plate thickness and mechanical properties at room temperature, the ratio of the tensile strength at 300°C to the tensile strength at room temperature can be set to 0.90 or more.

[0050] The steel plate of this embodiment is completed based on the above technical ideas and has the following structure.

[0051] The chemical composition of the steel plate of the first constitution contains, by mass%,

[0052] C: 0.040~0.070%,

[0053] Si: more than 0 and 0.10% or less,

[0054] Mn: 0.20~0.40%,

[0055] P: greater than 0 and less than 0.030%,

[0056] S: greater than 0 and less than 0.030%,

[0057] Sol.Al: 0.005~0.100%,

[0058] N: more than 0% and less than 0.0150%,

[0059] B: 0.0001~0.0030%,

[0060] Ti: 0~0.010%,

[0061] Nb: 0~0.010%,

[0062] Cu: 0-0.5%,

[0063] Ni: 0-0.5%,

[0064] Cr: 0 to 0.3%, and

[0065] Sn: 0~0.05%, the balance is Fe and impurities,

[0066] In the microstructure of the steel plate, ferrite is the main phase, and the grain size grade of the ferrite is 11.0 or more.

[0067] The thickness of the steel plate is 0.15 to 1.00 mm.

[0068] The yield strength of the steel plate at room temperature is 220 to 500 MPa, the tensile strength at room temperature is 330 to 550 MPa, and the total elongation at room temperature is 20.0% or more.

[0069] The aging index AI of the steel plate is 50.0 MPa or more,

[0070] The ratio of the tensile strength of the steel sheet at 300° C. to the tensile strength at room temperature is 0.90 or more.

[0071] The steel plate of the second configuration is according to the steel plate of the first configuration, wherein:

[0072] It also has a plating layer formed on the surface.

[0073] The plating layer is composed of one or more selected from the group consisting of a Ni plating layer and a Ni diffusion plating layer.

[0074] The steel plate of the third configuration is based on the steel plate of the first or second configuration, wherein:

[0075] The above chemical composition contains

[0076] Ti: 0.001~0.010%,

[0077] Nb: 0.001~0.010%,

[0078] Cu: 0.1-0.5%,

[0079] Ni: 0.1-0.5%,

[0080] Cr: 0.1-0.3%, and

[0081] Sn: one or more selected from the group consisting of 0.01 to 0.05%.

[0082] The steel plate of the fourth configuration is the steel plate of any one of the first to third configurations, wherein:

[0083] The balance of the microstructure is composed of one or more selected from the group consisting of pearlite, cementite, bainite, and martensite.

[0084] Hereinafter, the steel sheet of the present embodiment will be described. In addition, the steel sheet of the present embodiment also includes a steel strip. In addition, unless otherwise specified, "%" related to an element means mass %.

[0085] [Features of the Steel Sheet of the Present Embodiment]

[0086] The steel plate of the present embodiment satisfies the following characteristics.

[0087] (Feature 1)

[0088] The chemical composition contains, by mass%, C: 0.040-0.070%, Si: greater than 0 and less than 0.10%, Mn: 0.20-0.40%, P: greater than 0 and less than 0.030%, S: greater than 0 and less than 0.030%, Sol.Al: 0.005-0.100%, N: greater than 0% and less than 0.0150%, B: 0.0001-0.0030%, Ti: 0-0.010%, Nb: 0-0.010%, Cu: 0-0.5%, Ni: 0-0.5%, Cr: 0-0.3%, and Sn: 0-0.05%, and the balance is Fe and impurities.

[0089] (Feature 2)

[0090] In the microstructure, ferrite is the main phase and the grain size grade is above 11.0.

[0091] (Feature 3)

[0092] The plate thickness is 0.15~1.00mm.

[0093] (Feature 4)

[0094] The yield strength at room temperature is 220 to 500 MPa, the tensile strength at room temperature is 330 to 550 MPa, and the total elongation at room temperature is 20.0% or more.

[0095] (Feature 5)

[0096] The aging index AI is 50.0 MPa or more, and the ratio of the tensile strength at 300° C. to the tensile strength at room temperature is 0.90 or more.

[0097] Hereinafter, features 1 to 5 will be described.

[0098] [For (Feature 1) Chemical composition]

[0099] The chemical composition of the steel sheet according to the present embodiment contains the following elements.

[0100] C: 0.040~0.070%

[0101] Carbon (C) exists in steel as solid solution C, which makes dynamic strain aging appear in the high temperature range of 200 to 300°C, which is the heating temperature when the battery can is short-circuited, and improves the high temperature strength of the steel plate. C also combines with other alloy elements to form carbides, which refines the grains of the steel. Due to the refinement of the grains, the surface roughness resistance of the steel plate during stamping processes such as drawing is improved. If the C content is less than 0.040%, the above effect cannot be fully obtained.

[0102] On the other hand, if the C content exceeds 0.070%, the stamping formability decreases.

[0103] Therefore, the C content is 0.040 to 0.070%.

[0104] The lower limit of the C content is preferably 0.043%, more preferably 0.045%, and further preferably 0.050%.

[0105] The upper limit of the C content is preferably 0.068%, more preferably 0.065%, and further preferably 0.060%.

[0106] The preferred range of the C content is, for example, 0.043 to 0.060%, more preferably 0.045 to 0.065%, and even more preferably 0.050 to 0.060%.

[0107] Si: more than 0 and 0.10% or less

[0108] Silicon (Si) deoxidizes steel in the steelmaking process in the steel sheet manufacturing process. However, if the Si content exceeds 0.10%, the plating adhesion to the steel sheet is reduced. In addition, the coating adhesion to the steel sheet after canning is reduced.

[0109] Therefore, the Si content is greater than 0 and is 0.10% or less.

[0110] The Si content is preferably as low as possible. However, if the Si content is reduced excessively, the manufacturing cost increases. Therefore, in consideration of normal industrial production, the preferred lower limit of the Si content is 0.01%, more preferably 0.02%, and further preferably 0.03%.

[0111] The upper limit of the Si content is preferably 0.09%, more preferably 0.08%, and further preferably 0.07%.

[0112] The preferred range of the Si content is, for example, 0.01 to 0.09%, more preferably 0.02 to 0.08%, and even more preferably 0.03 to 0.07%.

[0113] Mn: 0.20~0.40%

[0114] Manganese (Mn) improves the strength of the steel sheet at room temperature by solid solution strengthening. Mn also combines with S in the steel to form MnS. The formation of MnS fixes S, thereby improving the hot workability of the steel sheet. If the Mn content is less than 0.20%, the above effect cannot be fully obtained.

[0115] On the other hand, if the Mn content exceeds 0.40%, the strength of the steel sheet at room temperature increases excessively due to the solid solution strengthening of Mn. As a result, the press formability of the steel sheet decreases.

[0116] Therefore, the Mn content is 0.20 to 0.40%.

[0117] The lower limit of the Mn content is preferably 0.21%, more preferably 0.23%, and further preferably 0.25%.

[0118] The upper limit of the Mn content is preferably 0.38%, more preferably 0.36%, and further preferably 0.35%.

[0119] The preferred range of the Mn content is, for example, 0.21 to 0.38%, more preferably 0.23 to 0.36%, and further preferably 0.25 to 0.35%.

[0120] P: greater than 0 and less than 0.030%

[0121] Phosphorus (P) improves the strength of the steel sheet at room temperature by solid solution strengthening. However, if the P content exceeds 0.030%, P will be excessively segregated at the grain boundaries. As a result, the toughness and stamping formability of the steel sheet will be reduced.

[0122] Therefore, the P content is greater than 0 and is 0.030% or less.

[0123] The P content is preferably as low as possible. However, if the P content is reduced excessively, the manufacturing cost becomes high. Therefore, in consideration of normal industrial production, the preferred lower limit of the P content is 0.001%, more preferably 0.002%, and even more preferably 0.003%.

[0124] The upper limit of the P content is preferably 0.025%, more preferably 0.022%, and further preferably 0.020%.

[0125] The preferred range of the P content is, for example, 0.001 to 0.025%, more preferably 0.002 to 0.022%, and even more preferably 0.003 to 0.020%.

[0126] S: greater than 0 and less than 0.030%

[0127] Sulfur (S) reduces the hot workability, toughness and ductility of steel. If the S content exceeds 0.030%, the hot workability, toughness and ductility of steel are significantly reduced.

[0128] Therefore, the S content is greater than 0 and is 0.030% or less.

[0129] The S content is preferably as low as possible. However, if the S content is reduced excessively, the manufacturing cost becomes high. Therefore, in consideration of normal industrial production, the preferred lower limit of the S content is 0.001%, more preferably 0.002%, and further preferably 0.003%.

[0130] The upper limit of the S content is preferably 0.025%, more preferably 0.022%, and further preferably 0.020%.

[0131] The preferred range of the S content is, for example, 0.001 to 0.025%, more preferably 0.002 to 0.022%, and even more preferably 0.003 to 0.020%.

[0132] Sol.Al: 0.005~0.100%

[0133] Aluminum (Al) deoxidizes steel in the steelmaking process in the manufacturing process of steel sheets. Al also combines with N in steel to form AlN. AlN refines the crystal grains. The refinement of the crystal grains improves the surface roughness resistance of the steel sheet during stamping processes such as drawing. If the sol.Al content is less than 0.005%, the above effects cannot be fully obtained.

[0134] On the other hand, if the sol.Al content exceeds 0.100%, AlN is excessively generated. In this case, the toughness of the steel sheet decreases.

[0135] Therefore, the Al content is 0.005 to 0.100%.

[0136] The lower limit of the Al content is preferably 0.007%, more preferably 0.010%, and further preferably 0.012%.

[0137] The upper limit of the Al content is preferably 0.070%, more preferably 0.050%, more preferably 0.040%, more preferably 0.035%, more preferably 0.030%, and still more preferably 0.025%.

[0138] The preferred range of the Al content is, for example, 0.007 to 0.070%, more preferably 0.007 to 0.050%, more preferably 0.010 to 0.040%, more preferably 0.010 to 0.035%, more preferably 0.012 to 0.030%, and still more preferably 0.012 to 0.025%.

[0139] In addition, in this specification, the sol.Al content means the content of acid-soluble (sol.Al). In the steel sheet of this embodiment, the acid-insoluble Al (insol.Al) is, for example, aluminum oxide (Al2O3).

[0140] N: more than 0% and less than 0.0150%

[0141] Nitrogen (N) exists in steel as solid solution N like C, and thus makes dynamic strain aging appear in the high temperature range of 200 to 300°C, which is the heating temperature when the battery can is short-circuited, and improves the high temperature strength of the steel sheet. N also forms nitrides represented by AlN to refine the grains. As a result, the surface roughness resistance of the steel sheet during stamping such as drawing is improved.

[0142] However, when the N content exceeds 0.0150%, nitrides are excessively generated, and in this case, the toughness of the steel sheet decreases.

[0143] Therefore, the N content is greater than 0 and is 0.0150% or less.

[0144] The lower limit of the N content is preferably 0.0001%, more preferably 0.0010%, more preferably 0.0015%, more preferably 0.0020%, more preferably 0.0025%, more preferably 0.0035%, and more preferably 0.0050%.

[0145] The upper limit of the N content is preferably 0.0145%, more preferably 0.0140%, more preferably 0.0130%, more preferably 0.0120%, more preferably 0.0110%, more preferably 0.0100%, and more preferably 0.0080%.

[0146] The preferred range of the N content is, for example, 0.0001 to 0.0145%, more preferably 0.0010 to 0.0140%, more preferably 0.0015 to 0.0130%, more preferably 0.0020 to 0.0120%, more preferably 0.0025 to 0.0110%, more preferably 0.0035 to 0.0100%, and still more preferably 0.0050 to 0.0080%.

[0147] B: 0.0001~0.0030%

[0148] Boron (B) segregates at the grain boundaries and suppresses the segregation of P and S at the grain boundaries. Therefore, the press formability, hot workability and toughness of the steel sheet are improved. If the B content is less than 0.0001%, the above effects cannot be fully obtained.

[0149] On the other hand, when the B content exceeds 0.0030%, B excessively segregates at the grain boundaries or carbides of B precipitate. In this case, the hot workability and toughness of the steel sheet are reduced due to the segregation or precipitation of B.

[0150] Therefore, the B content is 0.0001 to 0.0030%.

[0151] The lower limit of the B content is preferably 0.0003%, more preferably 0.0005%, more preferably 0.0007%, more preferably 0.0010%, and still more preferably 0.0015%.

[0152] The upper limit of the B content is preferably 0.0028%, more preferably 0.0026%, more preferably 0.0024%, more preferably 0.0022%, and still more preferably 0.0020%.

[0153] The preferred range of the B content is, for example, 0.0003 to 0.0028%, more preferably 0.0005 to 0.0026%, more preferably 0.0007 to 0.0024%, more preferably 0.0010 to 0.0022%, and still more preferably 0.0015 to 0.0020%.

[0154] The balance of the chemical composition of the steel sheet of this embodiment is Fe and impurities. Impurities refer to elements mixed from raw materials such as ores and waste materials, or the manufacturing environment, when the steel sheet is manufactured industrially, and are elements allowed within a range that does not adversely affect the steel sheet of this embodiment.

[0155] [For Optional Elements]

[0156] The steel plate of this embodiment may further contain

[0157] Ti: 0~0.010%,

[0158] Nb: 0~0.010%,

[0159] Cu: 0-0.5%,

[0160] Ni: 0-0.5%,

[0161] Cr: 0-0.3%, and

[0162] Sn: One or more kinds selected from the group consisting of 0 to 0.05% may be used to replace a part of Fe.

[0163] Each of the optional elements will be described below.

[0164] [Group 1: Ti and Nb]

[0165] The chemical composition of the steel sheet of the present embodiment may also contain one or more selected from the group consisting of Ti and Nb to replace a portion of Fe. Both Ti and Nb form carbonitrides to refine the grains. As a result, the surface roughness resistance of the steel sheet during stamping such as drawing is improved. In addition, in this specification, carbonitride is a general term including carbides, nitrides, and carbonitrides.

[0166] Ti: 0~0.010%

[0167] Titanium (Ti) is an arbitrary element and may not be contained. In other words, the Ti content may be 0%.

[0168] When Ti is contained, that is, when the Ti content is greater than 0%, Ti combines with C and / or N in the steel to form Ti carbonitrides. Ti carbonitrides refine the crystal grains. As a result, the surface roughness resistance of the steel sheet during stamping such as drawing is improved. The above effect can be achieved to some extent as long as a small amount of Ti is contained.

[0169] However, when the Ti content exceeds 0.010%, Ti carbonitrides are excessively generated. In this case, the amount of dissolved C and dissolved N that contribute to dynamic strain aging in the temperature range of 200 to 300°C is excessively reduced. As a result, the high temperature strength of the steel sheet cannot be sufficiently obtained.

[0170] Therefore, the Ti content is 0 to 0.010%.

[0171] The lower limit of the Ti content is preferably 0.001%, more preferably 0.002%.

[0172] The upper limit of the Ti content is preferably 0.009%, more preferably 0.008%.

[0173] The Ti content is preferably in the range of, for example, 0.001 to 0.009%, more preferably 0.002 to 0.008%.

[0174] Nb: 0~0.010%

[0175] Niobium (Nb) is an arbitrary element and may not be contained. In other words, the Nb content may be 0%.

[0176] When Nb is contained, that is, when the Nb content is greater than 0%, Nb combines with C and / or N in the steel to form Nb carbonitrides. Nb carbonitrides refine the crystal grains. As a result, the surface roughness resistance of the steel sheet during stamping such as drawing is improved. As long as a small amount of Nb is contained, the above effect can be obtained to some extent.

[0177] However, when the Nb content exceeds 0.010%, Nb carbonitrides are excessively generated. In this case, the amount of dissolved C and dissolved N that contribute to dynamic strain aging in the temperature range of 200 to 300°C is excessively reduced. As a result, the high temperature strength of the steel sheet cannot be sufficiently obtained.

[0178] Therefore, the Nb content is 0 to 0.010%.

[0179] The lower limit of the Nb content is preferably 0.001%, more preferably 0.002%.

[0180] The upper limit of the Nb content is preferably 0.009%, more preferably 0.008%.

[0181] The preferred range of the Nb content is, for example, 0.001 to 0.009%, more preferably 0.002 to 0.008%.

[0182] [Group 2: Cu, Ni, Cr and Sn]

[0183] The chemical composition of the steel sheet of this embodiment may contain one or more selected from the group consisting of Cu, Ni, Cr and Sn to replace part of Fe. These elements are all elements that may be contained in scrap when scrap is used as a raw material of the steel sheet. These elements are so-called impurity elements.

[0184] Cu: 0~0.5%

[0185] Copper (Cu) is an arbitrary element and may not be contained. That is, the Cu content may be 0%. In the steel sheet of the present embodiment, Cu is an impurity element.

[0186] When Cu is contained, that is, when the Cu content exceeds 0%, if the Cu content exceeds 0.5%, the press formability of the steel sheet decreases.

[0187] Therefore, the Cu content is 0 to 0.5%.

[0188] The Cu content is preferably as low as possible. However, if the Cu content is reduced too much, the manufacturing cost increases. Therefore, in consideration of normal industrial production, the preferred lower limit of the Cu content is 0.1%.

[0189] The upper limit of the Cu content is preferably 0.4%, more preferably 0.3%.

[0190] The preferred range of the Cu content is, for example, 0.1 to 0.4%, more preferably 0.1 to 0.3%.

[0191] Ni: 0~0.5%

[0192] Nickel (Ni) is an arbitrary element and may not be contained. That is, the Ni content may be 0%. In the steel sheet of the present embodiment, Ni is an impurity element.

[0193] When Ni is contained, that is, when the Ni content exceeds 0%, if the Ni content exceeds 0.5%, the press formability of the steel sheet decreases.

[0194] Therefore, the Ni content is 0 to 0.5%.

[0195] The Ni content is preferably as low as possible. However, if the Ni content is reduced too much, the production cost increases. Therefore, in consideration of normal industrial production, the preferred lower limit of the Ni content is 0.1%.

[0196] The upper limit of the Ni content is preferably 0.4%, more preferably 0.3%.

[0197] The preferred range of the Ni content is, for example, 0.1 to 0.4%, more preferably 0.1 to 0.3%.

[0198] Cr: 0~0.3%

[0199] Chromium (Cr) is an arbitrary element and may not be contained. That is, the Cr content may be 0%. In the steel sheet of the present embodiment, Cr is an impurity element.

[0200] When Cr is contained, that is, when the Cr content exceeds 0%, if the Cr content exceeds 0.3%, the press formability of the steel sheet decreases.

[0201] Therefore, the Cr content is 0 to 0.3%.

[0202] The Cr content is preferably as low as possible. However, if the Cr content is reduced too much, the manufacturing cost increases. Therefore, in consideration of normal industrial production, the preferred lower limit of the Cr content is 0.1%.

[0203] The preferred upper limit of the Cr content is 0.2%.

[0204] The Cr content is preferably in the range of, for example, 0.1 to 0.3%, more preferably 0.1 to 0.2%.

[0205] Sn: 0~0.05%

[0206] Tin (Sn) is an arbitrary element and may not be contained. In other words, the Sn content may be 0%. In the steel sheet of the present embodiment, Sn is an impurity element.

[0207] When Sn is contained, that is, when the Sn content exceeds 0%, if the Sn content exceeds 0.05%, Sn excessively segregates at the grain boundaries. In this case, the hot workability and toughness of the steel sheet are reduced due to the segregation of Sn.

[0208] Therefore, the Sn content is 0 to 0.05%.

[0209] The Sn content is preferably as low as possible. However, if the Sn content is reduced too much, the manufacturing cost increases. Therefore, in consideration of normal industrial production, the preferred lower limit of the Sn content is 0.01%.

[0210] The upper limit of the Sn content is preferably 0.04%, more preferably 0.03%.

[0211] The Sn content is preferably in the range of 0.01 to 0.04%, for example, and more preferably in the range of 0.01 to 0.03%.

[0212] [For (Feature 2) Microstructure]

[0213] In the steel sheet of the present embodiment, ferrite is the main phase in the microstructure, and the grain size rank is 11.0 or more. These matters will be described below.

[0214] (For the main phase of the microstructure)

[0215] In the microstructure of the steel sheet of the present embodiment, ferrite is the main phase. Here, ferrite is the main phase, which means that the area ratio of ferrite in the microstructure is 90% or more. If the main phase of the microstructure is ferrite, excellent stamping formability can be obtained.

[0216] In the microstructure, the balance other than ferrite is composed of one or more selected from the group consisting of pearlite, cementite, bainite, and martensite. Preferably, the balance of the microstructure is composed of one or more selected from the group consisting of pearlite and cementite.

[0217] The lower limit of the area ratio of ferrite in the microstructure is preferably 92%, more preferably 95%, further preferably 97%, and most preferably 100%.

[0218] (Method for determining the structure in the microstructure and method for measuring the area ratio of ferrite)

[0219] The method of determining each structure (ferrite, pearlite, cementite, bainite, and martensite) in the microstructure and the method of measuring the area ratio of ferrite are as follows.

[0220] A test piece was collected from the center of the steel plate width with the cross section parallel to the rolling direction and parallel to the plate thickness direction as an observation surface.

[0221] The observation surface was mirror-polished. The position of the mirror-polished observation surface at a depth of 4 from the surface of the steel plate in the plate thickness direction was set as the observation field. The observation field was etched with nital to reveal the microstructure.

[0222] The observation field after etching is observed with a scanning electron microscope (SEM) at 1000 times magnification. The size of the observation field is set to 100μm×100μm. In SEM observation, each organization (ferrite, pearlite, cementite, bainite and martensite) can be distinguished by organizational morphology, precipitation state of carbides, and dislocation density. For example, a organization with a layered structure can be determined as pearlite. A phase without a lower organization in the grain can be determined as ferrite. A phase that is granular and has a higher brightness can be determined as cementite. Organizations with lamellar organizations can be determined as bainite and martensite. Determine the ferrite in the observation field and find the total area of ​​ferrite.

[0223] The area ratio (%) of ferrite was determined based on the total area of ​​ferrite in the observation fields at five locations and the total area of ​​the observation fields at five locations.

[0224] (For grain size grade)

[0225] In the steel sheet of the present embodiment, the grain size grade of ferrite is 11.0 or more.

[0226] If the ferrite grains as the main phase in the microstructure are coarse, the surface roughness resistance of the steel sheet during press working such as drawing will decrease. If the ferrite grains are coarse, the in-plane anisotropy Δr will increase further, and the earing property will decrease.

[0227] In the steel sheet of the present embodiment, the ferrite grain size grade is 11.0 or more, and the ferrite grains are sufficiently fine. Therefore, in the steel sheet during the stamping process such as drawing, excellent surface roughness resistance can be obtained. In addition, in the steel sheet after the stamping process, the in-plane anisotropy Δr becomes small, and excellent lug properties can be obtained.

[0228] (Method for measuring the grain size of ferrite)

[0229] The grain size grade of ferrite in the steel sheet according to the present embodiment is determined by the following method.

[0230] A test piece was collected from the center of the steel plate in the plate width, with the cross section parallel to the rolling direction and parallel to the plate thickness direction being the observation surface.

[0231] The observation surface was mirror-polished. The observation field was set at a depth of plate thickness / 4 from the surface of the steel plate in the plate thickness direction in the mirror-polished observation surface. The observation field was etched with nitric acid to reveal the microstructure. The observation field after etching was observed with an optical microscope at 400 times. The size of the observation field was set to 300 μm×200 μm.

[0232] According to JIS G 0551 (2020), only the ferrite in the observation field is focused on and the grain size grade of ferrite is measured. At this time, the grain size grade is measured using the comparison method according to 7.2 of the same standard. The arithmetic mean of the grain size grades obtained in the observation field of 5 locations is set as the grain size grade of ferrite.

[0233] [For (Feature 3) Plate Thickness]

[0234] The steel plate of the present embodiment has a plate thickness of 0.15 to 1.00 mm.

[0235] If the plate thickness is less than 0.15 mm, the plate thickness of the hot-rolled steel plate produced needs to be reduced in the hot rolling process in the manufacturing process of the steel plate satisfying feature 1. In this case, it is difficult to adjust the finishing rolling temperature FT (°C) and the cooling rate in the hot rolling process. As a result, a sufficient aging index AI cannot be obtained in the steel plate.

[0236] On the other hand, if the sheet thickness exceeds 1.00 mm, sufficient press formability cannot be obtained in the steel sheet satisfying Feature 1.

[0237] Therefore, the thickness of the steel plate in the present embodiment is 0.15 to 1.00 mm.

[0238] The lower limit of the plate thickness is preferably 0.20 mm, more preferably 0.25 mm, and further preferably 0.30 mm.

[0239] The upper limit of the plate thickness is preferably 0.90 mm, more preferably 0.80 mm, and further preferably 0.70 mm.

[0240] The preferred range of the plate thickness is, for example, 0.20 to 0.90 mm, more preferably 0.25 to 0.80 mm, and even more preferably 0.30 to 0.70 mm.

[0241] The plate thickness can be measured using a laser thickness gauge (laser triangulation distance meter).

[0242] [Regarding (Characteristic 4) Mechanical properties at room temperature]

[0243] In the steel sheet of this embodiment, the yield strength at room temperature is 220 to 500 MPa, the tensile strength at room temperature is 330 to 550 MPa, and the total elongation at room temperature is 20.0% or more. In this specification, room temperature refers to 25°C.

[0244] (For room temperature yield strength and room temperature tensile strength)

[0245] When a steel sheet is used as a raw material for a battery can, for example, a certain degree of strength is required in the battery can. If the yield strength of the steel sheet at room temperature is 220 MPa or more and the tensile strength of the steel sheet at room temperature is 330 MPa or more, sufficient strength required for battery can use can be obtained.

[0246] On the other hand, if the yield strength and tensile strength of the steel sheet at room temperature are too high, sufficient press formability cannot be obtained. If the yield strength of the steel sheet at room temperature is 500 MPa or less and the tensile strength is 550 MPa or less, excellent press formability can be obtained.

[0247] Therefore, the yield strength of the steel plate at room temperature is 220 to 500 MPa, and the tensile strength of the steel plate at room temperature is 330 to 550 MPa.

[0248] The lower limit of the yield strength of the steel plate at room temperature is preferably 250 MPa, more preferably 270 MPa, and further preferably 300 MPa.

[0249] The upper limit of the yield strength of the steel plate at room temperature is preferably 480 MPa, more preferably 460 MPa, further preferably 440 MPa, further preferably 420 MPa.

[0250] The yield strength of the steel plate at room temperature is preferably in the range of, for example, 250 to 480 MPa, more preferably 270 to 460 MPa, further preferably 300 to 440 MPa, and further preferably 300 to 420 MPa.

[0251] The lower limit of the tensile strength of the steel plate at room temperature is preferably 350 MPa, more preferably 360 MPa, and further preferably 370 MPa.

[0252] The upper limit of the tensile strength of the steel plate at room temperature is preferably 530 MPa, more preferably 510 MPa, and further preferably 490 MPa.

[0253] The tensile strength of the steel plate at room temperature preferably ranges from 350 to 530 MPa, for example, more preferably from 360 to 510 MPa, and even more preferably from 370 to 490 MPa.

[0254] (For total elongation at room temperature)

[0255] When the steel sheet of this embodiment is used as a blank for a battery can, excellent stamping formability is required. If the total elongation of the steel sheet at room temperature is less than 20.0%, sufficient stamping formability cannot be obtained. Therefore, the total elongation of the steel sheet at room temperature is 20.0% or more.

[0256] The lower limit of the total elongation of the steel sheet at room temperature is preferably 21.0%, more preferably 24.0%, and further preferably 28.0%.

[0257] The upper limit of the total elongation of the steel sheet at room temperature is not particularly limited. When the steel sheet satisfies characteristics 1 to 4, the upper limit of the total elongation of the steel sheet at room temperature is, for example, 50.0%, for example, 45.0%, for example, 40.0%.

[0258] The preferred range of the total elongation of the steel sheet at room temperature is, for example, 21.0 to 50.0%, more preferably 24.0 to 45.0%, and further preferably 28.0 to 40.0%.

[0259] (Method for measuring mechanical properties at room temperature)

[0260] The yield strength, tensile strength, and total elongation at room temperature were determined as follows.

[0261] A JIS No. 5 tensile test piece was collected from the steel plate in accordance with JIS Z 2241 (2011). The parallel portion of the tensile test piece was set to be parallel to the rolling direction of the steel plate.

[0262] A tensile test was performed at room temperature in the atmosphere using the collected tensile test pieces to obtain a stress-strain curve.

[0263] The yield strength (MPa), tensile strength (MPa), and total elongation (%) at room temperature were determined from the obtained stress-strain curve, wherein the 0.2% yield strength obtained from the stress-strain curve was defined as the yield strength.

[0264] [For (Characteristic 5) Aging Index AI and High Temperature Strength]

[0265] The steel sheet of the present embodiment also has an aging index AI of 50.0 MPa or more, and a ratio of the tensile strength at 300° C. to the tensile strength at room temperature of 0.90 or more.

[0266] (For Time Index AI)

[0267] As described above, in the steel plate of the present embodiment, a predetermined amount of dissolved C and dissolved N is allowed to remain in the steel plate. As a result, dynamic strain aging occurs in the high temperature region of 200 to 300°C. Specifically, a serrated shape is generated in the stress-strain curve obtained in the tensile test at 300°C. Therefore, the high temperature strength at 200 to 300°C is improved.

[0268] When the aging index AI is 50.0 MPa or more, sufficient amounts of dissolved C and dissolved N exist in the steel sheet satisfying characteristics 1 to 4. Therefore, excellent high temperature strength can be obtained.

[0269] The lower limit of the aging index AI is preferably 52.0 MPa, more preferably 55.0 MPa, further preferably 60.0 MPa, further preferably 65.0 MPa.

[0270] The upper limit of the aging index AI is not particularly limited. The upper limit of the aging index AI is, for example, 100.0 MPa, for example, 95.0 MPa, for example, 90.0 MPa.

[0271] The preferred range of the aging index AI is, for example, 52.0 to 100.0 MPa, more preferably 55.0 to 95.0 MPa, further preferably 60.0 to 90.0 MPa, and further preferably 65.0 to 90.0 MPa.

[0272] (Measurement method of timeliness index AI)

[0273] The aging index AI is calculated using the following method.

[0274] A JIS No. 5 tensile test piece was collected from the steel plate. The parallel portion of the tensile test piece was set to be parallel to the rolling direction of the steel plate. The original cross-sectional area A (mm) of the parallel portion of the collected tensile test piece was determined.

[0275] The collected tensile test pieces were subjected to a tensile test using a tensile testing machine in accordance with JIS Z 2241 (2011) to apply a 10% prestrain to the tensile test pieces. The load F1 (kgf) at the time when the 10% prestrain was generated in the tensile test was determined.

[0276] The tensile test piece to which a pre-strain of 10% was applied was subjected to accelerated aging treatment at 100°C for 1 hour.

[0277] According to JIS Z 2241 (2011), a tensile test was performed on the tensile test piece after the accelerated aging treatment at room temperature (25° C.) in the air to determine the yield load F2 (kgf).

[0278] The obtained original cross-sectional area A of the parallel portion, the load F1, and the yield load F2 are used to determine the aging index AI (MPa) using the formula (1).

[0279] AI=(F2-F1) / A (1)

[0280] The value obtained by rounding off the second decimal place of the numerical value obtained in the formula (1) is defined as the aging index AI (MPa).

[0281] (For high temperature strength)

[0282] In the steel sheet of the present embodiment, the ratio of the tensile strength at 300°C to the tensile strength at room temperature is 0.90 or more. The tensile strength at room temperature is defined as TS RT , the tensile strength at 300℃ is defined as TS 300 In this case, the tensile strength TS at 300°C can be defined by formula (2): 300 Relative to the tensile strength TS at room temperature RT The ratio of high temperature tensile strength to TS .

[0283] R TS =TS 300 / TS RT (2)

[0284] If the high temperature tensile strength is higher than R TS If the aging index AI is 0.90 or more, a sufficiently high tensile strength is obtained even at a high temperature of 300°C. Therefore, in a battery can manufactured using the steel sheet of this embodiment as a blank, the battery can can maintain sufficient strength even when heat is generated due to a short circuit. By satisfying characteristics 1 to 4 in the steel sheet of this embodiment and setting the aging index AI to 50.0 MPa or more, the high temperature tensile strength ratio R TS Set to 0.90 or more.

[0285] High temperature tensile strength ratio R TS The preferred lower limit of is 0.93, more preferably 0.95, further preferably 0.97, further preferably 1.00.

[0286] High temperature tensile strength ratio R TS There is no particular upper limit on the steel sheet. When the steel sheet satisfies characteristics 1 to 4, the high temperature tensile strength is greater than R TS The upper limit of is, for example, 1.30, more preferably 1.25, further preferably 1.15.

[0287] High temperature tensile strength ratio R TS A preferred range of is, for example, 0.93 to 1.30, more preferably 0.95 to 1.25, further preferably 0.97 to 1.15, further preferably 1.00 to 1.15.

[0288] (High temperature tensile strength ratio R TS Measurement method)

[0289] The high temperature tensile strength ratio R is calculated as follows: TS .

[0290] The tensile strength TS of the steel sheet at room temperature was obtained by the method according to the above-mentioned (Method for measuring mechanical properties at room temperature) RT .

[0291] According to JIS G 0567 (2012), the tensile strength TS at room temperature is obtained from RT A JIS No. 5 tensile test piece was collected from the steel plate. The parallel portion of the tensile test piece was set to be parallel to the rolling direction of the steel plate.

[0292] The collected tensile test pieces were subjected to a tensile test at 300° C. in the atmosphere in accordance with JIS G 0567 (2012) to obtain a stress-strain curve.

[0293] The tensile strength TS at 300°C was calculated from the obtained stress-strain curve. 300 (MPa).

[0294] The tensile strength TS obtained using RT and tensile strength TS 300 , and based on formula (2) the high temperature tensile strength ratio R is calculated TS .

[0295] [Effects of the Steel Sheet of the Present Embodiment]

[0296] As described above, the steel plate of the present embodiment satisfies Features 1 to 4. Therefore, in the steel plate of the present embodiment, when a stamping process such as drawing is performed in the manufacturing process of the battery can, excellent stamping formability and excellent surface roughness resistance can be obtained. The steel plate of the present embodiment satisfies Features 1 to 4 as a prerequisite, and also satisfies Feature 5. Therefore, in the steel plate of the present embodiment, excellent high-temperature strength can be obtained. As a result, in a battery can manufactured using the steel plate of the present embodiment as a blank, even if heat caused by a short circuit occurs and the temperature of the battery can rises to about 200 to 300°C, the decrease in strength caused by the increase in the temperature of the battery can can be fully suppressed.

[0297] [Further Structure of the Steel Plate of the Present Embodiment]

[0298] The steel sheet of the present embodiment may further include a plating layer formed on the surface. In the present embodiment, the plating layer is composed of one or more selected from the group consisting of a Ni plating layer and a Ni diffusion plating layer.

[0299] The Ni plating layer is a plating layer in which the Ni content is 90% or more by mass%. The chemical composition of the Ni plating layer other than Ni is not particularly limited. For example, the Ni plating layer may also contain Co and / or W.

[0300] Whether or not the plating layer is a Ni plating layer can be confirmed by the following method.

[0301] A test piece including a coating is collected from a steel plate formed with a coating. An elemental analysis is performed on the coating using a fluorescent X-ray analyzer. A standard curve is prepared in advance using a standard sample of a coating with a known Ni content. The Ni content (mass %) in the coating is calculated based on the standard curve. If the obtained Ni content is 90% or more in mass %, the coating is judged to be a Ni coating.

[0302] The Ni diffusion plating layer is formed by subjecting the steel sheet on which the Ni plating layer is formed to a well-known alloying heat treatment. The Ni plating layer is formed by a well-known electroplating treatment or chemical plating treatment.

[0303] The Ni diffusion coating includes a Fe-Ni alloy layer. The Ni diffusion coating may also include a Ni coating and a Fe-Ni alloy layer formed between the Ni coating and the surface of the steel sheet. In addition, the Ni diffusion coating may also be a coating composed of a Fe-Ni alloy layer. Through alloying heat treatment, Fe in the steel sheet diffuses into the Ni coating, and Ni in the Ni coating diffuses into the steel sheet, thereby forming a Fe-Ni alloy layer.

[0304] The preferred Fe concentration of the outermost surface of the Ni diffusion plating layer is 3% or more in mass %. Here, "the outermost surface of the Ni diffusion plating layer" refers to, for example, a depth position of 0.006 μm from the Ni diffusion plating layer surface obtained based on the Ar sputtering time by glow discharge spectrometry (GDS) described later.

[0305] When the Fe concentration on the outermost surface is 3% or more, it is possible to suppress seizure between the steel sheet and the die when the steel sheet having the Ni diffusion plated layer is press-worked, thereby improving press formability.

[0306] The more preferred lower limit of the Fe concentration in the surface layer is 10%, and further preferably 15% or more.

[0307] From the viewpoint of corrosion resistance, the upper limit of the Fe concentration in the surface layer is preferably 80%, more preferably 70%, and further preferably 60%.

[0308] Whether or not the plating layer is a Ni diffusion plating layer can be determined by the following method.

[0309] A test piece including the coating was collected from a steel plate with a coating formed thereon. The coating of the test piece was subjected to a depth-direction element distribution by glow discharge spectrometry (GDS), and the Ni concentration and Fe concentration in the depth direction were measured from the surface of the coating. A high-frequency glow discharge luminescence surface analysis device was used for the measurement. The GDS measurement conditions were set as follows.

[0310] HV: Fe: 785V, Ni: 630V

[0311] Anode diameter: φ4mm

[0312] Gas: Ar

[0313] Air pressure: 600Pa

[0314] Power: 35W

[0315] As the high-frequency glow discharge light emission surface analysis device, for example, a model number: GD-Profiler2 manufactured by Horiba, Ltd. is used.

[0316] The measurement data of the depth converted from the Ar sputtering time is less than 0.006μm (6nm) sometimes contains noise due to reasons such as signal instability. That is, the measurement data of the depth converted from the Ar sputtering time is less than 0.006μm (6nm) may not be able to accurately measure the coating. Therefore, in this GDS measurement, the depth converted from the Ar sputtering time only uses data above 0.006μm. Specifically, the depth position of 0.006μm converted from the Ar sputtering time is set to the outermost surface (depth 0μm) of the coating.

[0317] Whether the plating layer is a Ni diffusion plating layer is determined based on the Ni concentration change and the Fe concentration change in the depth direction from the outermost surface obtained by GDS. For example, when the Fe concentration increases from the outermost surface toward the depth direction and the Ni concentration decreases from the outermost surface toward the depth direction, that is, in the plating layer, when the Fe concentration presents a positive gradient from the outermost surface toward the depth direction and the Ni presents a negative gradient, the plating layer is determined to be a Ni diffusion plating layer.

[0318] [Method for manufacturing steel sheet]

[0319] An example of the method for producing a steel sheet according to the present embodiment will be described. An example of the method for producing a steel sheet according to the present embodiment includes the following steps.

[0320] (Process 1) Steelmaking process

[0321] (Process 2) Hot rolling process

[0322] (Process 3) Cold rolling process

[0323] (Process 4) Annealing process

[0324] (Step 5) Plating layer forming step

[0325] Among the above steps, the plating layer forming step of step 5 is an optional step. That is, the plating layer forming step may be performed or may not be performed. Each step will be described below.

[0326] [(Process 1) Steelmaking process]

[0327] In the steelmaking process, molten steel satisfying feature 1 is produced. The produced molten steel is used to produce billets (slabs) by a casting method. For example, the slabs are produced by a well-known continuous casting method using the above-mentioned molten steel.

[0328] [(Process 2) Hot rolling process]

[0329] In the hot rolling process, the slab is hot rolled to produce a hot rolled steel sheet. The hot rolling process can be carried out using known equipment. The hot rolling process includes a rough rolling process of rough rolling the slab to produce a rough plate strip (intermediate steel plate) and a finish rolling process of finish rolling the rough plate strip to produce a hot rolled steel sheet.

[0330] In the rough rolling process, first, the slab is heated. The heated slab is rolled using a rough rolling mill to produce a rough strip. The slab heating temperature T0 is set to 1180-1250°C. If the slab heating temperature T0 is above 1180°C, the finishing temperature FT described later can be ensured. In addition, if the slab heating temperature T0 is below 1250°C, cracks such as edge cracks in the steel plate can be suppressed during the hot rolling process.

[0331] In the finishing process, the rough strip is further rolled (finishing rolling) using a finishing mill to produce a hot-rolled steel sheet. In the finishing process, the finishing temperature FT is set to 890-930°C. If the finishing temperature FT is above 890°C, the recovery and recrystallization of austenite can be promoted. Therefore, the recrystallized austenite transforms into ferrite. As a result, the in-plane anisotropy Δr of the steel sheet can be suppressed. If the finishing temperature FT is below 930°C, the coarsening of the grains can be suppressed.

[0332] After the finish rolling, the hot rolled steel sheet is cooled in a cooling zone (run-out table: ROT) and then coiled. At this time, the coiling temperature CT is set to 560 to 600°C.

[0333] If the coiling temperature CT is above 560°C, the formation of bainite is suppressed in the microstructure of the steel plate. In this case, ferrite tends to become the main phase in the microstructure of the steel plate after the annealing process described later. Moreover, the in-plane anisotropy Δr can be suppressed. On the other hand, if the coiling temperature CT is below 600°C, the excessive formation of carbonitrides can be suppressed during coiling. Therefore, the amount of dissolved C and dissolved N in the steel plate can be ensured. As a result, in the manufactured steel plate, the aging index AI becomes 50.0 MPa or more.

[0334] [(Process 3) Cold rolling process]

[0335] In the cold rolling process, the hot rolled steel sheet is pickled and then cold rolled to produce the cold rolled steel sheet. The cold rolling process can be carried out using a known device. The temperature during the cold rolling is, for example, room temperature to 200°C.

[0336] The cold rolling reduction (cold rolling rate) RR in the cold rolling process is preferably 87 to 91%. If the cold rolling rate RR is 87 to 91%, in a steel sheet having a chemical composition satisfying feature 1, the in-plane anisotropy Δr can be suppressed provided that other manufacturing conditions are also satisfied.

[0337] [(Step 4) Annealing step]

[0338] In the annealing process, the cold-rolled steel sheet is annealed. For annealing, for example, continuous annealing is performed. The annealing process can be performed using known equipment. In the annealing process, the annealing temperature T1 is 720 to 820°C. If the annealing temperature T1 is above 720°C, the unrecrystallized structure can be sufficiently reduced. Therefore, in the microstructure of the steel sheet after manufacture, ferrite becomes the main phase. On the other hand, if the annealing temperature T1 is below 820°C, the coarsening of the recrystallized grains can be sufficiently suppressed. Therefore, in the microstructure of the steel sheet after manufacture, the grain size grade of ferrite becomes above 11.0. The holding time t1 of the annealing temperature T1 is, for example, 20 to 60 seconds.

[0339] In the annealing step, the steel sheet after being held at the annealing temperature T1 for a period of time t1 is cooled in two stages as follows.

[0340] (1st stage cooling)

[0341] The average cooling rate CR of the steel sheet in the first temperature range from the annealing temperature T1 to 650°C T1-650 Set it to 8°C / sec or less.

[0342] (2nd stage cooling)

[0343] The average cooling rate CR in the second temperature range from 650°C to 250°C of the steel plate 650-250 Set to 15 to 30°C / second.

[0344] Hereinafter, the first-stage cooling and the second-stage cooling will be described.

[0345] (For the first stage of cooling)

[0346] The first temperature range (temperature range of the steel sheet from the annealing temperature T1 to 650° C.) is a temperature range in which phase transformation can occur in the microstructure of the steel sheet satisfying the first characteristic.

[0347] If the average cooling rate CR T1-650 When the temperature is higher than 8°C / sec, structures other than ferrite (for example, hard structures such as bainite and martensite) are easily generated. In this case, the ferrite area ratio in the microstructure of the produced steel sheet is less than 90%, and ferrite does not become the main phase.

[0348] If the average cooling rate CR T1-650 When the temperature is 8°C / sec or less, the formation of structures other than ferrite can be sufficiently suppressed. Therefore, in the microstructure of the manufactured steel sheet, the ferrite area ratio is 90% or more, and ferrite becomes the main phase.

[0349] (For the second stage of cooling)

[0350] The second temperature range (temperature range of the steel sheet from 650° C. to 250° C.) is a temperature range where phase transformation and precipitation of precipitates can occur.

[0351] If the average cooling rate CR 650-250 If the temperature is less than 15°C / sec, carbonitrides are excessively generated. In this case, sufficient amounts of dissolved C and dissolved N cannot be ensured in the steel sheet after manufacture. Therefore, the aging index AI of the steel sheet after manufacture is less than 50.0 MPa.

[0352] On the other hand, if the average cooling rate CR 650-250 When the heating rate is higher than 30° C. / sec, structures other than ferrite (for example, hard structures such as bainite and martensite) are easily generated. As a result, sufficient total elongation cannot be obtained in the steel sheet.

[0353] If the average cooling rate CR 650-250 If the cooling rate in the second temperature range is 15 to 30°C / sec, then the cooling rate in the second temperature range is appropriate. In this case, sufficient solid phase C and dissolved N can be ensured in the manufactured steel plate on the premise of satisfying other manufacturing conditions. Therefore, in the manufactured steel plate, the aging index AI becomes 50.0 MPa or more.

[0354] The average cooling rate CR is calculated as follows: T1-650 and the average cooling rate CR 650-250 In the continuous annealing furnace, multiple thermometers are arranged along the conveying path. These thermometers are used to measure the temperature of the steel plate when it passes through the continuous annealing furnace at various locations. Based on the temperature measurement results at various locations and the steel plate passing time between various locations, the average cooling rate CR in the first temperature zone is calculated. T1-650 (°C / sec) and the average cooling rate CR in the second temperature range 650-250 (℃ / sec).

[0355] [(Step 5) Plating layer forming step]

[0356] The plating layer forming step is an optional step and may not be performed. When a steel sheet having a Ni plating layer or a Ni diffusion plating layer is produced, the plating layer forming step is performed.

[0357] When the Ni plating layer is formed on the surface of the steel sheet, the Ni plating layer forming step is performed after the annealing step. Specifically, the steel sheet after the annealing step is immersed in a Ni plating bath to perform electroplating or chemical plating. A well-known Ni plating bath can be used for the Ni plating bath. The Ni plating bath is selected from the group consisting of, for example, a Watt bath, a sulfuric acid bath, an aminosulfonic acid bath, a Wood bath, a fluoroboride bath, a chloride bath, and a citric acid bath.

[0358] The thickness (or adhesion amount) of the Ni plating layer formed on the surface of the steel sheet is not particularly limited. The thickness of the Ni plating layer is, for example, 0.3 to 5.0 μm. The Ni adhesion amount of the Ni plating layer is, for example, 2.7 to 44.5 g / m 2 .

[0359] The amount of Ni deposited on the coating can be determined by elemental analysis using the above-mentioned fluorescent X-ray analyzer. Specifically, a test piece including the coating is collected from a steel plate formed with the coating. An elemental analysis is performed on the surface of the coating using a fluorescent X-ray analyzer. A standard curve is prepared in advance using a standard sample of the coating with a known Ni deposit. The Ni deposited on the coating (g / m 2 ). In addition, the thickness (μm) of the plating layer can be obtained based on the Ni deposition amount.

[0360] When a Ni diffusion coating is formed on the surface of a steel sheet, a Ni coating forming process is performed before an annealing process. Specifically, the steel sheet after the cold rolling process and before the annealing process is immersed in a Ni plating bath to perform electroplating or chemical plating. The Ni coating is formed by the above process. The above annealing process is performed on the steel sheet on which the Ni coating is formed. In the annealing process, Fe in the steel sheet diffuses into the Ni coating, and Ni in the Ni coating diffuses into the steel sheet. As a result, a Ni diffusion coating containing an Fe-Ni alloy layer is formed.

[0361] [Other processes than the above]

[0362] The method for producing a steel sheet according to the present embodiment may include performing a temper rolling (skin pass rolling) step after the annealing step. The temper rolling step is an optional step and may not be performed.

[0363] In the temper rolling process, the steel sheet after the annealing process is subjected to temper rolling. The reduction rate of the temper rolling is, for example, 0.5 to 5.0%. If the reduction rate is 0.5% or more, the yield point elongation can be sufficiently suppressed in the steel sheet after manufacture. In this case, the tensile strain generated when the stamping process (deep drawing) is implemented can be suppressed. If the reduction rate is 5.0% or less, a sufficient total elongation can be obtained. Therefore, sufficient stamping formability can be obtained in the steel sheet after manufacture.

[0364] The steel sheet of the present embodiment can be manufactured by the above-described manufacturing method.

[0365] Example

[0366] The effects of the steel sheet of the present embodiment will be described in more detail below using examples. These examples are examples for confirming the effects of the steel sheet of the present embodiment, and are not intended to limit the steel sheet of the present disclosure.

[0367] Steel sheets having the chemical compositions shown in Table 1 (Table 1A and Table 1B) were manufactured by the following method.

[0368] [Table 1A]

[0369] Table 1A

[0370]

[0371] [Table 1B]

[0372] Table 1B

[0373]

[0374] "-" in Table 1B means that the content of the corresponding element is below the impurity level. For example, the Ti content of steel number A means "0"% when the fourth decimal place is rounded off. The Cu content of steel number A means "0"% when the second decimal place is rounded off.

[0375] Specifically, in the steelmaking process, slabs of each steel number are manufactured. In the hot rolling process, the manufactured slabs are subjected to hot rolling (rough rolling and finish rolling) to manufacture hot rolled steel sheets. The slab heating temperature T0 (°C), the finish rolling temperature FT (°C), and the coiling temperature CT (°C) in the hot rolling process are as shown in Table 2.

[0376] [Table 2]

[0377] Table 2

[0378]

[0379] In the cold rolling process, the hot rolled steel sheet is cold rolled to produce a cold rolled steel sheet of plate thickness. The cold rolling rate RR (%) in the cold rolling process is as shown in Table 2. The plate thickness of the cold rolled steel sheet of test number 11 is 0.20 mm. The plate thickness of the cold rolled steel sheet of test number 12 is 0.80 mm. The plate thickness of the cold rolled steel sheets of test numbers other than test numbers 11 and 12 is 0.30 mm.

[0380] The cold-rolled steel sheet was subjected to a coating forming step to form a Ni coating on the front and back surfaces of the cold-rolled steel sheet. Specifically, Ni electroplating was performed under well-known conditions. In any test number, the Ni coating weight of the Ni coating was 13.0 g / m2 on each single surface. 2 As described above, the adhesion amount of the Ni plating layer was determined by elemental analysis using a fluorescent X-ray analyzer.

[0381] The steel sheet with the Ni plating layer was subjected to an annealing process. The annealing temperature T1, annealing time t1, and average cooling rate CR in the annealing process are T1-650 (℃ / sec), and the average cooling rate CR650-250 (°C / sec) as shown in Table 2.

[0382] The steel sheets after the annealing step were subjected to a temper rolling step. The reduction ratio in the temper rolling was 1.2% in all the test numbers.

[0383] The steel plates of each test number were manufactured using the above process. The steel plates of each test number were provided with Ni diffusion coatings on the front and back surfaces. In addition, the plate thickness of the steel plate of test number 11 (the plate thickness of the steel plate excluding the Ni diffusion coating) was 0.20 mm. The plate thickness of the steel plate of test number 12 was 0.80 mm. The plate thickness of the steel plates of other test numbers except test numbers 11 and 12 was 0.30 mm.

[0384] [Evaluation test]

[0385] The following evaluation tests were performed on the steel plates of the respective test numbers.

[0386] (Test 1) Microstructure observation test

[0387] (Test 2) Ferrite grain size measurement test

[0388] (Test 3) Mechanical properties evaluation test at room temperature

[0389] (Test 4) Time Index AI Measurement Test

[0390] (Test 5) High temperature tensile strength ratio R TS Measurement test

[0391] Hereinafter, each test will be described.

[0392] [(Test 1) Microstructure observation test]

[0393] Based on the method described in the above (method for determining the structure in the microstructure and the method for measuring the area ratio of ferrite), the main phase in the microstructure of the steel plate of each test number is determined, and the area ratio (%) of ferrite is calculated. The results are shown in the "Main Phase" column of the "Microstructure" column in Table 3. In this column, "F" means that the main phase of the microstructure is ferrite, and the area ratio of ferrite is more than 90%. "B" in this column means that the main phase of the microstructure is bainite, and the area ratio of bainite is more than 90% (that is, the area ratio of ferrite is less than 10%). In this column, "F+B" means that although the total area ratio of ferrite and bainite is more than 90%, the area ratio of ferrite and the area ratio of bainite are both less than 90%. In addition, in test number 12, the area ratio of ferrite is larger than the area ratio of bainite.

[0394] [Table 3]

[0395] Table 3

[0396]

[0397] [(Test 2) Ferrite grain size measurement test]

[0398] The ferrite grain size grade of the steel plate of each test number was obtained based on the method described in the above-mentioned (Method for measuring the grain size grade of ferrite). The obtained grain size grade is indicated in the "Grain size grade" column of the "Microstructure" column in Table 3. In addition, in the steel plates of test numbers 18, 23 and 24, ferrite is not the main phase in the microstructure. Therefore, in the steel plates of these test numbers, the grain size grade of ferrite was not measured (indicated by "-" in the "Grain size grade" column in Table 3).

[0399] [(Test 3) Mechanical properties evaluation test at room temperature]

[0400] The yield strength YS at room temperature of the steel plate of each test number was determined based on the method described in the above (Method for measuring mechanical properties at room temperature) RT (MPa), tensile strength TS at room temperature RT (MPa), and the total elongation EL at room temperature RT (%) The yield strength YS RT , tensile strength TS RT And the total elongation EL RT The room temperature yield strength YS RT (MPa)" column, "Room temperature tensile strength TS RT (MPa)" column, and "Room temperature total elongation EL RT (%)"column.

[0401] [(Test 4) Time-Effect Index AI Measurement Test]

[0402] The aging index AI (MPa) of the steel plate of each test number was determined based on the method described in the above (Method for measuring aging index AI). The obtained aging index AI is shown in the "AI (MPa)" column of Table 3.

[0403] [(Test 5) High temperature tensile strength ratio R TS Measurement test]

[0404] Based on the above (high temperature tensile strength ratio R TS The high temperature tensile strength ratio R of the steel plate of each test number was calculated by the method described in the measurement method of TS The obtained high temperature tensile strength is R TS Indicated in Table 3, “R TS (TS 300 / TSRT )"column.

[0405] [Evaluation results]

[0406] The evaluation results are shown in Table 3. Referring to Table 3, in the steel sheets of test numbers 1 to 12, characteristics 1 to 5 are satisfied. Therefore, in these steel sheets, predetermined strength is obtained, sufficient stamping formability and surface roughness resistance are obtained. In addition, excellent high temperature strength is obtained in these steel sheets.

[0407] On the other hand, in test number 13, the C content is too low. Therefore, the grain size of ferrite is too low. In addition, the aging index AI is too low. Therefore, the tensile strength TS at room temperature is RT and high temperature tensile strength ratio R TS Too low to obtain sufficient high temperature strength.

[0408] In test number 14, the C content was too high. Therefore, the tensile strength TS at room temperature RT Therefore, the total elongation EL at room temperature RT If the pressure drop is too low, sufficient stamping performance cannot be achieved.

[0409] In test number 15, the N content was too high. Therefore, the tensile strength TS at room temperature RT Therefore, the total elongation EL at room temperature RT Too low to obtain sufficient stamping formability.

[0410] In test number 16, the Ti content is too high. Therefore, the aging index AI is too low. Therefore, the high temperature tensile strength is lower than R TS The total elongation EL at room temperature is too low to obtain sufficient high temperature strength. RT Too low to obtain sufficient stamping formability.

[0411] In test number 17, the Nb content is too high. Therefore, the aging index AI is too low. Therefore, the high temperature tensile strength is lower than R TS The total elongation EL at room temperature is too low to obtain sufficient high temperature strength. RT If the pressure drop is too low, sufficient stamping performance cannot be achieved.

[0412] In test number 18, although the chemical composition satisfied characteristic 1, the coiling temperature CT was too low. Therefore, bainite became the main phase in the microstructure of the steel sheet. As a result, the tensile strength TS at room temperature was RT Too high, the total elongation EL at room temperature RT Too low. Therefore, sufficient stamping formability cannot be obtained. Moreover, the high temperature tensile strength is lower than RTS Too low to obtain sufficient high temperature strength.

[0413] In test number 19, although the chemical composition satisfies characteristic 1, the coiling temperature CT is too high. Therefore, the aging index AI is low. As a result, the high temperature tensile strength is lower than R TS Too low to obtain sufficient high temperature strength.

[0414] In test numbers 20 and 21, although the chemical composition satisfied characteristic 1, the cooling rate CR in the temperature range from 650°C to 250°C in the annealing process was 650-250 Slower. Therefore, the aging index AI is lower. As a result, the high temperature tensile strength is higher than R TS Too low to obtain sufficient high temperature strength.

[0415] In Test No. 22, although the chemical composition satisfied Feature 1, the cooling rate CR in the temperature range from 650°C to 250°C during the annealing process was 650-250 Therefore, the aging index AI is lower. As a result, the high temperature tensile strength is higher than R TS The total elongation EL at room temperature is too low to obtain sufficient high temperature strength. RT As a result, sufficient stamping properties cannot be obtained.

[0416] In test numbers 23 and 24, although the chemical composition satisfied characteristic 1, in the annealing process, the cooling rate CR of the steel sheet in the temperature range from the annealing temperature T1 to 650°C was T1-650 Faster. In the microstructure of the steel plate, not only ferrite but also bainite is generated, and the ferrite area ratio is less than 90%. Therefore, the total elongation EL at room temperature is RT Too low. Therefore, sufficient stamping formability cannot be obtained. In addition, the aging index AI is low. As a result, the high temperature tensile strength is lower than R TS Too low to obtain sufficient high temperature strength.

[0417] The embodiments of the present disclosure have been described above. However, the above embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above embodiments, and the above embodiments can be appropriately modified and implemented within the scope of the present disclosure.

Claims

1. A steel sheet, the chemical composition of which contains, by mass%, C: 0.040~0.070%, Si: more than 0 and less than 0.10%, Mn: 0.20~0.40%, P: greater than 0 and less than 0.030%, S: greater than 0 and less than 0.030%, Sol.Al: 0.005~0.100%, N: more than 0% and less than 0.0150%, B: 0.0001~0.0030%, Ti: 0~0.010%, Nb: 0~0.010%, Cu: 0-0.5%, Ni: 0-0.5%, Cr: 0 to 0.3%, and Sn: 0~0.05%, The balance is Fe and impurities. The steel plate has ferrite as the main phase in the microstructure, and the grain size grade of the ferrite is above 11.

0. The thickness of the steel plate is 0.15 to 1.00 mm. The yield strength of the steel plate at room temperature is 220 to 500 MPa, the tensile strength at room temperature is 330 to 550 MPa, and the total elongation at room temperature is greater than 20.0%. The aging index AI of the steel plate is 50.0 MPa or more, The ratio of the tensile strength of the steel sheet at 300° C. to the tensile strength at room temperature is 0.90 or more.

2. The steel plate according to claim 1, wherein: It also has a coating formed on the surface. The plating layer is composed of one or more selected from the group consisting of a Ni plating layer and a Ni diffusion plating layer.

3. The steel plate according to claim 1, wherein: The chemical composition contains a Ti: 0.001~0.010%, Nb: 0.001~0.010%, Cu: 0.1-0.5%, Ni: 0.1-0.5%, Cr: 0.1-0.3%, and Sn: one or more selected from the group consisting of 0.01 to 0.05%.

4. The steel plate according to claim 1, wherein: The balance of the microstructure is composed of one or more selected from the group consisting of pearlite, cementite, bainite, and martensite.

Citation Information

Patent Citations

  • High strength steel sheet and method for producing same

    CN107614729A

  • High tensile cold-rolled steel sheet having excellent strain aging hardening properties

    CN1366559A

  • Production of cold rolled steel sheet excellent in baking hardenability at low temperature

    JP1993171286A

  • High strength cold rolled steel sheet having superior local ductility and stable baking hardenability of coating, produced by continuous annealing

    JP1995216502A

  • High-strength cold-rolled steel sheet and manufacturing method therefor

    JP2009019231A