Sulfide solid electrolyte glass ceramic and method for producing same

By optimizing the composition and structure of sulfide solid electrolyte glass ceramics, improving its peak intensity ratio and microcrystal particle size at a specific angle, the problem of low conductivity of existing sulfide solid electrolytes is solved, and high-performance lithium-ion batteries are realized Electrochemical properties and stability.

CN119096308APending Publication Date: 2024-12-06IDEMITSU KOSAN CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380031009.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing sulfide solid electrolyte has low ionic conductivity and is difficult to meet the needs of high-performance lithium-ion batteries.

Method used

By optimizing the composition and structure of sulfide solid electrolyte glass ceramics in CuKα ray X-ray diffraction measurement, ensuring that the peak intensity ratio exceeds 1.0 at 2θ=20.2° and 29.3° is greater than 1.0, and the raw material addition method and process are divided into two stages Synthesis to improve the particle size and crystallinity of the microcrystalline crystal.

Benefits of technology

The ionic conductivity and water resistance of sulfide solid electrolyte glass ceramics are significantly improved, and the performance of lithium-ion batteries is enhanced, especially the irreversible capacity and the stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096308A_ABST
    Figure CN119096308A_ABST
Patent Text Reader

Abstract

Provided is a sulfide solid electrolyte glass ceramic containing lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms, having peaks at diffraction angles (2 [theta]) of 20.2 DEG and 29.3 DEG in X-ray diffraction measurement using a CuK [alpha] ray, and having a value (PA / PB) of an intensity ratio of a peak intensity (PA) of the peak appearing at 2 [theta] = 20.2 DEG to a peak intensity (PB) of the peak appearing at 2 [theta] = 29.3 DEG exceeding 1.0, thus, the sulfide solid electrolyte glass ceramic has high ionic conductivity and improved water resistance, and a method for producing the sulfide solid electrolyte glass ceramic is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to sulfide solid electrolyte glass ceramics and a method for producing the same. Background Art

[0002] In recent years, with the rapid popularization of information-related devices or communication devices such as personal computers, cameras and mobile phones, the development of batteries used as their power sources has also received attention. In the past, in batteries used for such purposes, electrolytes containing flammable organic solvents were used, but by making the battery fully solid, the safety device is simplified because no flammable organic solvent is used in the battery, and the manufacturing cost and productivity are excellent. Therefore, the development of batteries in which the electrolyte is replaced by a solid electrolyte layer is carried out.

[0003] As a solid electrolyte used in a solid electrolyte layer, a sulfide solid electrolyte has been conventionally known, and it is desired to further improve the ion conductivity of the sulfide solid electrolyte.

[0004] Ion conductivity is determined by the types and composition ratios of raw materials used in the production of the solid electrolyte, the crystal form of the produced solid electrolyte, etc. For example, in order to improve the ion conductivity of a sulfide solid electrolyte, optimization of its crystal form has been studied (Patent Document 1).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-89971 Summary of the invention

[0008] Technical problem to be solved by the invention

[0009] The present invention has been completed in view of such actual conditions, and its purpose is to provide a sulfide solid electrolyte glass ceramic with high ion conductivity, and to provide an electrode composite material and a lithium ion battery using the sulfide solid electrolyte glass ceramic, as well as a method for manufacturing the sulfide solid electrolyte glass ceramic.

[0010] Solutions for solving the above technical problems

[0011] The sulfide solid electrolyte glass ceramic of the present invention is

[0012] A sulfide solid electrolyte glass ceramic comprising lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms,

[0013] In the X-ray diffraction measurement using CuKα rays, there are peaks at diffraction angles (2θ) of 20.2° and 29.3°, and the peak intensity (P A) and the peak intensity (P B ) intensity ratio value (P A / P B ) exceeds 1.0.

[0014] The method for producing the sulfide solid electrolyte glass ceramic of the present invention is as follows:

[0015] A method for manufacturing a sulfide solid electrolyte glass ceramic, comprising:

[0016] A solid electrolyte (A) is obtained by treating lithium sulfide (Li2S) and phosphorus sulfide (P2S5) by at least one selected from stirring, mixing and pulverizing;

[0017] The solid electrolyte (A) and the lithium halide are treated by at least one selected from stirring, mixing and pulverizing to obtain a solid electrolyte (B).

[0018] The electrode composite material of the present invention is

[0019] An electrode composite material comprises the sulfide solid electrolyte glass ceramic and an electrode active material.

[0020] The lithium ion battery of the present invention is

[0021] A lithium-ion battery comprises at least one of the sulfide solid electrolyte glass ceramic and the electrode composite material.

[0022] In this specification, the peak position may float within the range of ±0.5°.

[0023] Effects of the Invention

[0024] According to the present invention, it is possible to provide a sulfide solid electrolyte glass ceramic having high ion conductivity, an electrode composite material and a lithium ion battery using the sulfide solid electrolyte glass ceramic, and a method for producing the sulfide solid electrolyte glass ceramic. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a flowchart for explaining an example of a method of the production method according to the present embodiment.

[0026] Figure 2 This is a diagram for explaining the background removal and area calculation method of the 20.2° peak in X-ray diffraction (XRD) of Example 1.

[0027] Figure 3 This is a diagram for explaining the background removal and area calculation method of the 29.3° peak in X-ray diffraction (XRD) of Example 1.

[0028] Figure 4This is a diagram for explaining the background removal and area calculation method of the 20.2° peak in X-ray diffraction (XRD) of Comparative Example 1.

[0029] Figure 5 This is a diagram for explaining the background removal and area calculation method of the 29.3° peak in X-ray diffraction (XRD) of Comparative Example 1.

[0030] Figure 6 This is a diagram for explaining the method of calculating the crystallite diameter (X-ray diffraction (XRD) measurement).

[0031] Figure 7 This is a diagram for explaining the method of calculating the crystallite diameter (X-ray diffraction (XRD) measurement).

[0032] Figure 8 This is an exposure test device for evaluating water resistance.

[0033] Fig. 9 These are the results of X-ray diffraction (XRD) measurement of the solid electrolyte (A1) obtained in step (A) of Example 1.

[0034] Fig.10 These are the results of X-ray diffraction (XRD) measurement of the crystalline solid electrolyte (A2) obtained in step (A) of Example 1.

[0035] Fig.11 These are the results of X-ray diffraction (XRD) measurement of the amorphous solid electrolyte (B1) obtained in step (B) of Example 1.

[0036] Fig.12 These are the results of X-ray diffraction (XRD) measurement of the sulfide solid electrolyte glass ceramic (1) obtained in step (B) of Example 1.

[0037] Fig.13 These are the results of X-ray diffraction (XRD) measurement of the sulfide solid electrolyte glass ceramic (C1) obtained in Comparative Example 1. DETAILED DESCRIPTION

[0038] Hereinafter, an embodiment of the present invention (hereinafter sometimes referred to as "the present embodiment") is described. In addition, in this specification, the upper and lower limits of the numerical ranges of "above", "below", and "to" are numerical values ​​that can be combined arbitrarily, and the numerical values ​​of the embodiments can also be used as the upper and lower limits.

[0039] (Discovery made by the present inventors to complete the present invention)

[0040] The present inventors have conducted intensive studies to solve the above-mentioned technical problems and, as a result, have found the following matters and have completed the present invention.

[0041] As described in Patent Document 1, it is confirmed that sulfide solid electrolytes have PS4 3- As the main skeleton, a peak is observed at a specific position by XRD measurement. However, the ion conductivity of the sulfide solid electrolyte obtained by this method needs to be further improved.

[0042] The present inventors have found that the sulfide solid electrolyte glass ceramic has a peak at a specific position measured by X-ray diffraction (XRD). If the peak intensity (P A ) and the peak intensity (P B ) intensity ratio value (P A / P B ) is within a specific range, the ionic conductivity becomes larger.

[0043] Furthermore, it was found that electrode composite materials and lithium-ion batteries using these sulfide solid electrolyte glass ceramics have excellent characteristics, and it was found that the sulfide solid electrolyte glass ceramics can be obtained simply and in high yield by the above-mentioned production method.

[0044] The sulfide solid electrolyte glass ceramic has a peak at a specific position and a specific crystallite size in X-ray diffraction (XRD) measurement. A / P B The value of is within a specific range, and thus has excellent ionic conductivity, which is a phenomenon that has not been recognized so far. In addition, it can be seen that the manufacturing method of the sulfide solid electrolyte glass ceramic improves the ionic conductivity of the sulfide solid electrolyte glass ceramic by simply changing the method of adding the raw materials that have been used so far. In addition, the water resistance is also improved, and the irreversible capacity of the battery obtained thereby is excellent. This embodiment is an extremely excellent manufacturing method.

[0045] The following describes the sulfide solid electrolyte glass ceramics of the first to eleventh embodiments of the present embodiment, the manufacturing methods of the sulfide solid electrolyte glass ceramics of the twelfth to thirteenth embodiments of the present embodiment, the electrode composite material of the fourteenth embodiment, and the lithium ion battery of the fifteenth embodiment of the present embodiment.

[0046] The sulfide solid electrolyte glass ceramic of the first embodiment of the present invention is

[0047] A sulfide solid electrolyte glass ceramic comprising lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms,

[0048] In the X-ray diffraction measurement using CuKα rays, there are peaks at diffraction angles (2θ) of 20.2° and 29.3°, and the peak intensity (P A ) and the peak intensity (P B ) intensity ratio value (P A / P B ) exceeds 1.0, and the crystallite size is greater than 30 nm.

[0049] The measurement of the peak intensity by XRD using CuKα rays can be performed by, for example, the method described in Examples.

[0050] The sulfide solid electrolyte glass ceramic of the invention described in the above-mentioned Patent Document 1 focuses on the fact that it has a peak at a specific position measured by X-ray diffraction (XRD), but it is different from the sulfide solid electrolyte glass ceramic of the first embodiment in that it does not have a peak at 2θ=29.3°. This means that the sulfide solid electrolyte glass ceramic of the present embodiment includes a crystal structure different from that of the solid electrolyte described in Patent Document 1. It is known that the sulfide solid electrolyte glass ceramic of the first embodiment has a peak at a specific position, and the value of the intensity ratio of the peak intensity described later (P A / P B ) exceeds 1.0, thus having high ionic conductivity.

[0051] The reason why the sulfide solid electrolyte glass ceramic of the first scheme has excellent ion conductivity is still uncertain, but it can be considered that even if the atoms constituting the sulfide solid electrolyte glass ceramic are the same, depending on their content and manufacturing method, it will become a sulfide solid electrolyte glass ceramic with a different crystal structure, in which there is a peak at a specific peak position in the XRD measurement, and if the intensity ratio of its peak intensity is within a specific range, it becomes a sulfide solid electrolyte glass ceramic containing a large amount of crystal structure with high ion conductivity.

[0052] By increasing the crystallite diameter to 30 nm or more, the proportion of the grain boundary is reduced. Diffusion of lithium ions is suppressed at the grain boundary, so if the proportion of the grain boundary is reduced, the ion conductivity of the sulfide solid electrolyte glass ceramic is increased.

[0053] The crystallite diameter can be measured by the method described in Examples, for example.

[0054] The sulfide solid electrolyte glass ceramic according to the second aspect of the present embodiment is, in the above-mentioned first aspect,

[0055] The peak area intensity (I A ) and the peak area intensity (I B) intensity ratio value (I A / I B ) is greater than 0.78.

[0056] The peak area intensity measurement can be determined by XRD using CuKα rays, and can be carried out by, for example, the method described in Examples.

[0057] In addition to the first embodiment, in the sulfide solid electrolyte glass ceramic of the present embodiment, the value of the intensity ratio of the peak area intensity (I A / I B ) is further 0.78 or more, resulting in a sulfide solid electrolyte glass ceramic with improved ion conductivity, which is preferred.

[0058] The sulfide solid electrolyte glass ceramic according to a third aspect of the present embodiment is, in the first or second aspect,

[0059] It also has a peak at 2θ=23.6°.

[0060] In addition to the above-mentioned first aspect, a sulfide solid electrolyte glass ceramic having a peak at 2θ=23.6° is preferred because it has improved ion conductivity.

[0061] The sulfide solid electrolyte glass ceramic according to a fourth aspect of the present embodiment is, in any one of the first to third aspects,

[0062] An iodine atom is included as the halogen atom.

[0063] In addition to the first aspect described above, if the sulfide solid electrolyte glass ceramic contains iodine atoms, the ion conductivity is further improved, which is preferred. In addition, by containing halogen atoms, the water resistance described later is also improved, which is preferred.

[0064] The sulfide solid electrolyte glass ceramic of a fifth aspect of the present embodiment is, in the above-mentioned fourth aspect,

[0065] A bromine atom is also included as the halogen atom.

[0066] In addition to the fourth aspect described above, if the sulfide solid electrolyte glass ceramic further contains bromine atoms, the crystal structure is likely to form a sulfide crystalline lithium superion conductor region type II crystal structure described later, which is preferred.

[0067] The sulfide solid electrolyte glass ceramic according to a sixth aspect of the present embodiment is, in the fifth aspect described above,

[0068] The content of bromine atoms (M) contained in the sulfide solid electrolyte glass ceramic Brmol) and the content of iodine atoms (M I mol) satisfies M Br / M I The relationship is ≤1.00.

[0069] In the above-mentioned first embodiment, when the sulfide solid electrolyte glass ceramic contains bromine atoms and iodine atoms, by satisfying M Br / M I The relationship of ≤1.00 is preferred because the ion conductivity is further improved and the water resistance described later is also improved.

[0070] Bromine atom content (M Br mol) and the content of iodine atoms (M I mol) can be measured by the method described in Examples, for example.

[0071] The sulfide solid electrolyte glass ceramic according to a seventh aspect of the present embodiment is, in any one of the first to sixth aspects,

[0072] According to solid 31 P2S6 determined by P-NMR measurement 4- The phosphorus ratio is 7.5 mol % or less.

[0073] According to the research of the inventors, P2S6 4- Ingredients are easily hydrolyzed. In addition, P2S6 4- The component itself inhibits the ion conduction of Li ions and acts as a major factor in inhibiting the crystal growth of the solid electrolyte. If there is too much of this component, the crystallite size may not be sufficiently large. Therefore, if the P2S6 of the sulfide solid electrolyte glass ceramic is 4- The phosphorus ratio is preferably 7.5 mol% or less, because the water resistance and ion conductivity described below are improved. 4- The components may capture Li ions in the solid electrolyte and promote battery degradation. 4- The phosphorus ratio of the component is preferably 7.5 mol % or less because improvement in oxidation characteristics when used as a battery can be expected.

[0074] According to solid 31 P2S6 determined by P-NMR measurement 4- The phosphorus ratio can be determined by, for example, the method described in Examples.

[0075] The sulfide solid electrolyte glass ceramic according to an eighth aspect of the present embodiment is, in any one of the first to seventh aspects,

[0076] The molar fraction of Li2S (I1 Li2S ) and the molar fraction of P2S5 (I1 P2S5 ) ratio (I1 Li2S / I P2S5 ) is greater than 2.60 and less than 3.30.

[0077] Based on the first solution, the molar fraction of Li2S (I1 Li2S ) and the molar fraction of P2S5 (I1 P2S5 ) ratio (I1 Li2S / I1 P2S5 ) in a specific range, becomes P2S6 as an impurity of the solid electrolyte 4- Sulfide solid electrolyte glass ceramics with low content of components are preferred because of their improved ion conductivity and water resistance. In addition, the residual amount of Li2S is small, which also reduces the free sulfur atoms, improves the water resistance described later, and further suppresses the irreversible capacity when the battery is made, so it is preferred.

[0078] The molar fraction of Li2S (I1 Li2S ) and the molar fraction of P2S5 (I1 P2S5 ) can be determined, for example, by the method described in the embodiments.

[0079] The sulfide solid electrolyte glass ceramic according to a ninth aspect of the present embodiment is, in any one of the first to eighth aspects,

[0080] The molar fraction of Li2S (I2 Li2S ) and the molar fraction of P2S5 (I2 P2S5 ) ratio (I2 Li2S / I2 P2S5 ) is greater than 2.60 and less than 3.30.

[0081] The molar fraction (I2 Li2S ) and the molar fraction of P2S5 (I2 P2S5 ) ratio (I2 Li2S / I2 P2S5 ) In a specific range, similarly to the eighth embodiment, P2S6 which is an impurity of the solid electrolyte 4- Sulfide solid electrolyte glass ceramics with low content of components are preferred because of their improved ion conductivity and water resistance. In addition, the residual amount of Li2S is small, which also reduces the free sulfur atoms, improves the water resistance described later, and further suppresses the irreversible capacity when the battery is made, so it is preferred.

[0082] The sulfide solid electrolyte glass ceramic according to a tenth aspect of the present embodiment is, in any one of the first to ninth aspects,

[0083] The ratio of the content (mol) of lithium atoms, the content (mol) of phosphorus atoms, the content (mol) of sulfur atoms and the content (mol) of halogen atoms (content ratio) is lithium atoms:phosphorus atoms:sulfur atoms:halogen atoms = (3.20~3.70):(0.70~1.30):(3.00~5.00):(0.20~0.70).

[0084] In addition to the above-mentioned first embodiment, by including lithium atoms, phosphorus atoms, sulfur atoms and halogen atoms in specific contents, the ion conductivity is further improved, which is preferred.

[0085] The contents of lithium atoms, phosphorus atoms, sulfur atoms, and halogen atoms can be determined by, for example, the methods described in Examples.

[0086] The sulfide solid electrolyte glass ceramic according to an eleventh aspect of the present embodiment is, in any one of the first to tenth aspects,

[0087] Contains type II crystal structure of sulfide crystalline lithium superion conductor region.

[0088] In addition to the above-mentioned first embodiment, the sulfide solid electrolyte glass ceramic is preferably used because the ion conductivity is further improved by including a sulfide crystallized lithium superion conductor region of type II crystal structure.

[0089] The method for producing the sulfide solid electrolyte glass ceramic according to the twelfth aspect of the present embodiment is as follows:

[0090] A method for manufacturing a sulfide solid electrolyte glass ceramic comprises: treating lithium sulfide (Li2S) and phosphorus sulfide (P2S5) by at least one selected from stirring, mixing and pulverizing to obtain a solid electrolyte (A); treating the solid electrolyte (A) and a lithium halide by at least one selected from stirring, mixing and pulverizing to obtain a solid electrolyte (B).

[0091] According to the twelfth aspect, the sulfide solid electrolyte glass ceramics according to the first to eleventh aspects can be obtained efficiently.

[0092] That is, according to the twelfth aspect, it is possible to produce a sulfide solid electrolyte glass ceramic having improved ion conductivity.

[0093] In the conventional production method described in Patent Document 1 of synthesizing a sulfide solid electrolyte by charging all raw materials at once, it is impossible to produce a sulfide solid electrolyte glass ceramic having high crystallinity and high ion conductivity and having peaks at 2θ=20.2° and 29.3°.

[0094] In the twelfth scheme, if obtaining a solid electrolyte (A) is set as step (A), and obtaining a solid electrolyte (B) from the solid electrolyte (A) is set as step (B), then by dividing the process into at least two stages in this way, a sulfide solid electrolyte glass ceramic is synthesized to obtain a sulfide solid electrolyte glass ceramic having high crystallinity and high conductivity and having peaks at 2θ=20.2° and 29.3°.

[0095] The reasons for the improvement of crystallinity are considered as follows. It is believed that by allowing the raw materials to react fully in the synthesis of step (A), impurities or unnecessary skeletons related to performance degradation are reduced, and a solid electrolyte with few impurities is synthesized in step (B), thereby reducing impurities, and the crystallinity is improved by subsequent heating crystallization, and the electrical conductivity is also improved.

[0096] In the present embodiment, the crystallinity refers to a property of generating crystallites in the sulfide solid electrolyte and / or a property of growing and enlarging crystallites contained in the sulfide solid electrolyte.

[0097] A thirteenth aspect of the present embodiment provides a method for producing a sulfide solid electrolyte glass ceramic according to the twelfth aspect, further comprising heating the solid electrolyte (A).

[0098] By performing the above step (B) after heating the solid electrolyte (A) as described below, the crystallite size of the sulfide solid electrolyte glass ceramic becomes larger, which is preferred. As described above, increasing the crystallite size increases the ion conductivity, which is preferred.

[0099] A fourteenth aspect of the present embodiment provides a method for producing a sulfide solid electrolyte glass ceramic, in the twelfth or thirteenth aspect, further comprising heating the solid electrolyte (B).

[0100] By heating the solid electrolyte (B) as described later, the crystallite size of the sulfide solid electrolyte glass ceramic increases, which is preferable.

[0101] A method for producing a sulfide solid electrolyte glass ceramic according to a fifteenth aspect of the present embodiment is, in the twelfth to fourteenth aspects,

[0102] The solid electrolyte (B) is 31 P2S6 determined by P-NMR measurement 4- The phosphorus ratio is 15.0 mol % or less.

[0103] As mentioned above, sulfide solid electrolyte glass ceramics have PS4 as the main skeleton. 3- In addition, it also contains P2S6 4- or P2S7 4- P2S6 in solid electrolyte (B) 4- Therefore, in order to improve the ionic conductivity of the sulfide solid electrolyte glass ceramic, it is preferred to make P2S6 4- The phosphorus ratio is small.

[0104] The solid electrolyte (A) and the solid electrolyte (B) are intermediates in the production of sulfide solid electrolyte glass ceramics, and will be described in detail later.

[0105] The solid electrolyte (A) also contains P2S6 4- 、P2S7 4- etc., while the secondary skeleton is preferably P2S7 4- This is because Li2S, P2S7 are further added as needed in step (B) as described later. 4- It reacts with Li2S and easily transforms into PS4 as the main skeleton. 3- In contrast, P2S6 4- To PS4 3- The decomposition reaction is slow, in order to reduce the P2S6 that deteriorates the ionic conductivity in the solid electrolyte (B) 4- , preferably P2S6 in the solid electrolyte (A) 4- In addition, P2S6 4- It will also deteriorate water resistance, so P2S6 is preferred 4- The content is lower.

[0106] In view of the above mechanism, an in-depth study was conducted, and as a result, the following method for manufacturing a sulfide solid electrolyte glass ceramic was obtained as the method for manufacturing a sulfide solid electrolyte glass ceramic of the thirteenth scheme of the present embodiment: the solid electrolyte (A) contains Li4P2S7, and the solid electrolyte (A) contains 31 P-NMR measurements of P2S7 4- The phosphorus ratio is 20.0 mol % or more.

[0107] P2S6 4- The phosphorus ratio is determined by the solid 31 It was determined by P-NMR measurement.

[0108] The electrode composite material of the sixteenth embodiment of the present embodiment is:

[0109] An electrode composite material comprises the sulfide solid electrolyte glass ceramics of the first to eleventh embodiments and an electrode active material.

[0110] The sulfide solid electrolyte glass ceramics of the first to eleventh aspects have high ion conductivity, and thus an electrode composite material using the same has excellent ion conductivity.

[0111] The lithium ion battery of the seventeenth aspect of the present embodiment is:

[0112] A lithium-ion battery comprises at least one of the sulfide solid electrolyte glass ceramics of the first to eleventh embodiments and the electrode composite material of the sixteenth embodiment.

[0113] The sulfide solid electrolyte glass ceramic and the electrode composite material have excellent properties as described above, and therefore a battery using the electrode composite material has excellent properties.

[0114] Hereinafter, the sulfide solid electrolyte glass ceramic, the method for producing the sulfide solid electrolyte glass ceramic, the electrode composite material, and the lithium ion battery according to the present embodiment will be described in more detail based on the above-described embodiments.

[0115] [Sulfide solid electrolyte glass ceramics]

[0116] The sulfide solid electrolyte glass ceramic of the present embodiment is required to contain lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms, have peaks at 20.2° and 29.3° in X-ray diffraction (XRD) measurement using CuKα rays, and have a peak intensity (P A ) and the peak intensity (P B ) intensity ratio value (P A / P B ) exceeds 1.0, and the crystallite size is greater than 30 nm.

[0117] If P A / P B If the value is less than 1.0, the desired ion conductivity cannot be obtained. Also, if the crystallite size is less than 30 nm, the desired ion conductivity cannot be obtained.

[0118] The sulfide solid electrolyte glass ceramics of the present embodiment is preferably a sulfide solid electrolyte glass ceramics obtained by heating an amorphous sulfide solid electrolyte as described later.

[0119] In this specification, the term "sulfide solid electrolyte" refers to an electrolyte that remains solid in a nitrogen atmosphere at 25°C, contains lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms, and has ion conductivity due to lithium atoms.

[0120] “Sulfide solid electrolyte” includes both crystalline sulfide solid electrolytes and amorphous sulfide solid electrolytes having a crystal structure. In this specification, a crystalline sulfide solid electrolyte refers to a sulfide solid electrolyte in which a peak derived from a sulfide solid electrolyte is observed in an X-ray diffraction pattern in an X-ray diffraction measurement, and is a material that is independent of whether or not there is a peak derived from a raw material of the sulfide solid electrolyte. That is, the crystalline sulfide solid electrolyte includes a crystal structure derived from a sulfide solid electrolyte, and may be a part of the crystal structure derived from the sulfide solid electrolyte, or may be a whole of the crystal structure derived from the sulfide solid electrolyte. In addition, as long as the crystalline sulfide solid electrolyte has the above-mentioned X-ray diffraction pattern, it may also include an amorphous sulfide solid electrolyte in part, or it may not include an amorphous sulfide solid electrolyte. It is easier to process into a battery if it includes an amorphous component, so it is preferred. Therefore, the crystalline sulfide solid electrolyte includes the so-called glass ceramic obtained by heating the amorphous sulfide solid electrolyte to a crystallization temperature or above.

[0121] The sulfide solid electrolyte glass ceramics according to the present embodiment is a crystalline sulfide solid electrolyte which may contain an amorphous component.

[0122] In this specification, an amorphous sulfide solid electrolyte means that the X-ray diffraction pattern is a halo pattern in which substantially no peak is observed in X-ray diffraction measurement, regardless of the presence or absence of peaks derived from the raw material of the sulfide solid electrolyte or the presence or absence of a small amount of crystals inevitably generated during the operation of separating the amorphous sulfide solid electrolyte.

[0123] Furthermore, the sulfide solid electrolyte glass ceramic refers to a sulfide solid electrolyte in which a peak derived from a crystal structure of a sulfide solid electrolyte and a halo pattern derived from an amorphous sulfide solid electrolyte are observed in an X-ray diffraction pattern in X-ray diffraction measurement.

[0124] The sulfide solid electrolyte glass ceramics of the present embodiment has peaks at diffraction angles (2θ) of 20.2° and 29.3° in X-ray diffraction measurement using CuKα rays, and preferably also has a peak at 2θ=23.6°.

[0125] In addition to the above, the sulfide solid electrolyte glass ceramic of the present embodiment also has peaks near 2θ=17.5°, 18.3°, 26.1°, 27.3°, and 30.0°, and it is confirmed that the peak intensities of the peaks appearing at 20.2° and 29.3° are particularly strongly correlated with the ionic conductivity.

[0126] The peak position and the crystallite size measured by X-ray diffraction (XRD) using CuKα rays can be determined by the method described in Examples, for example.

[0127] The peak intensity is the height of the peak top from the base line (diffraction intensity) in an X-ray diffraction pattern measured by XRD, and can be determined by the method described in Examples. The peak position and the analysis intensity can be determined by the height at 2θ of the peak top.

[0128] <P A / P B >

[0129] It is known that the sulfide solid electrolyte glass ceramic of the present embodiment contains halogen atoms in its structure, but the peak intensity (P A ) and the peak intensity (P B ) different crystal structures. B The smaller the value, the higher the ionic conductivity. However, the peak intensity is a value that varies depending on the measurement conditions, etc. The inventors focused on the value of the intensity ratio (P A / P B ). It was found that the value of the intensity ratio is not easily affected by differences in measurement conditions, etc. A / P B The lithium ion migration number of the sulfide solid electrolyte glass ceramic exceeding 1.0 is high and the ion conductivity is high. The crystal structure appearing at 2θ=20.2° appears in a composition rich in iodine, and the crystallinity and ion conductivity are also high in the manufacturing method of this patent. On the other hand, the crystal structure appearing at 2θ=29.3° appears in a composition rich in bromine, the half-width of the peak is wide, and the crystallinity is low. In addition, if this phase increases, the crystallinity of the crystal at 2θ=20.2° decreases. It can be imagined that by changing the ratio of the halogens contained, the ratio of the two crystals changes. If P A / P B When the value exceeds 1.0, the ratio of the highly conductive 2θ=20.2° crystal phase increases, the crystallinity also improves, and as a result, the ion conductivity also improves.

[0130] If P A / P B When it is 1.0 or less, the desired ion conductivity cannot be obtained.

[0131] In order to improve the ionic conductivity, P A / P B The lower limit of is more preferably 1.1 or more, and further preferably 1.5 or more. A / P B The larger the value, the more preferable it is. Therefore, the upper limit is not particularly limited, but the sulfide solid electrolyte glass ceramics that can be produced are usually 20.0 or less.

[0132] P A / P BFor example, the calculation can be performed by the method described in the embodiment.

[0133] (I A / I B )

[0134] In order to improve the ion conductivity, the peak area intensity (I A ) and the peak area intensity (I B ) intensity ratio value (I A / I B ) is preferably 0.78 or more, more preferably 0.85 or more, and further preferably 0.93 or more. The upper limit is not particularly limited, but the sulfide solid electrolyte glass ceramic that can be produced is usually 10.0 or less.

[0135] I A / I B For example, the calculation can be performed by the method described in the embodiment.

[0136] The sulfide solid electrolyte glass ceramic of the present embodiment includes a crystal structure having peaks near 2θ=20.2° and near 29.3° as a main crystal, but may also include a Li3PS4 crystal structure, a Li4P2S6 crystal structure, a Li7PS6 crystal structure, a Li7P3S 11 Crystal structure, Li7P2S8X crystal structure, Li4PS4X crystal structure, etc. (X is a halogen element) are used as other crystal structures.

[0137] Here, the term "nearby" means a range of ±0.5°, including measurement errors and deviations of the measured values ​​caused by the measuring device. That is, 2θ=20.2° means 19.7° or more and 20.7° or less.

[0138] From the perspective of obtaining higher ion conductivity, the sulfide solid electrolyte glass ceramic of the present embodiment preferably includes a sulfide crystallized lithium superion conductor region type II crystal structure. Here, the “sulfide crystallized lithium superion conductor region type II crystal structure” means that Li 4-x Ge 1-x P x S4-type sulfide crystalline lithium superion conductor region II (thio-LISICON Region II) crystal structure, and Li 4-x Ge 1-x P xAny crystal structure similar to the S4 type sulfide crystalline lithium superion conductor region II (thio-LISICON Region II) type crystal structure. In addition, the sulfide solid electrolyte glass ceramic of the present embodiment can be a sulfide solid electrolyte glass ceramic containing the sulfide crystalline lithium superion conductor region II type crystal structure, but from the viewpoint of obtaining higher ionic conductivity, it is preferred to have a sulfide crystalline lithium superion conductor region II type crystal structure as the main crystal. In this specification, "having as the main crystal" means that the proportion of the crystal structure as the object in the crystal structure is 80% or more, preferably 90% or more, and more preferably 95% or more. In addition, from the viewpoint of obtaining higher ionic conductivity, the sulfide solid electrolyte glass ceramic of the present embodiment preferably does not contain crystalline Li3PS4 (β-Li3PS4).

[0139] In the X-ray diffraction measurement using CuKα rays, the diffraction peaks of the Li3PS4 crystal structure appear, for example, at 2θ=17.5°, 18.3°, 26.1°, 27.3°, and 30.0°; the diffraction peaks of the Li4P2S6 crystal structure appear, for example, at 2θ=16.9°, 27.1°, and 32.5°; the diffraction peaks of the Li7PS6 crystal structure appear, for example, at 2θ=15.3°, 25.2°, 29.6°, and 31.0°; and the diffraction peaks of the Li7P3S 11 The diffraction peaks of the crystal structure appear near 2θ=17.8°, 18.5°, 19.7°, 21.8°, 23.7°, 25.9°, 29.6°, and 30.0°, for example. 4-x Ge 1-x P x The diffraction peaks of the S4-type sulfide crystalline lithium superion conductor region II (thio-LISICON Region II) crystal structure appear near 2θ=20.1°, 23.9°, and 29.5°, which are similar to Li 4-x Ge 1-x P x The diffraction peaks of the S4 type thio-LISICON Region II-type crystal structure appear at, for example, 2θ=20.2 and 23.6°. The peak positions may fluctuate within a range of ±0.5°.

[0140] As described above, the sulfide solid electrolyte glass ceramics of this embodiment preferably does not contain crystalline Li3PS4 (β-Li3PS4). Figure 7X-ray diffraction measurement examples of the sulfide solid electrolyte glass ceramic of the present embodiment are shown. The sulfide solid electrolyte glass ceramic of the present embodiment does not have diffraction peaks at 2θ = 17.5° and 26.1° that can be observed in crystalline Li3PS4, or even if it has them, it only has a level where the detected peaks are extremely small compared to the diffraction peaks of the sulfide crystalline lithium superionic conductor region II type crystal structure.

[0141] The above-mentioned crystal structure represented by the composition formula Li 7-x P 1- y Si y S6 and Li 7+x P 1-y Si y S6 (where x is -0.6 to 0.6 and y is 0.1 to 0.6) is cubic or orthorhombic, preferably cubic, and mainly has peaks appearing at positions of 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0° in X-ray diffraction measurement using CuKα radiation. The above-mentioned crystal structure represented by the composition formula Li 7-x-2y PS 6-x-y Cl x (0.8 ≤ x ≤ 1.7, 0 < y ≤ -0.25x + 0.5) is preferably cubic and mainly has peaks appearing at positions of 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0° in X-ray diffraction measurement using CuKα radiation. In addition, the above-mentioned crystal structure represented by the composition formula Li 7-x PS 6-x Ha x (where Ha is Cl or Br, and x is preferably 0.2 to 1.8) is preferably cubic and mainly has peaks appearing at positions of 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0° in X-ray diffraction measurement using CuKα radiation.

[0142] (crystallite grain size)

[0143] The crystallite size of the sulfide solid electrolyte glass ceramic of the present embodiment is required to be 30 nm or more. As described above, this is because high ionic conductivity cannot be obtained. From the viewpoint of improving ionic conductivity and water resistance, it is preferably 32 nm or more, more preferably 33 nm or more, further preferably 35 nm or more, further preferably 40 nm or more, more particularly preferably 70 nm or more, and further particularly preferably 76 nm or more. And as described later, by crystallizing after step (A), the crystallite size of the sulfide solid electrolyte glass ceramic can be further increased, in which case, it is particularly preferably 90 nm or more.

[0144] The upper limit is not particularly limited, but from the perspective of ease of manufacture, ease of supply, and ease of manufacture of batteries, etc., it is preferably 300 nm or less, more preferably 250 nm or less, further preferably 200 nm or less, further preferably 180 nm or less, and even more preferably 160 nm or less.

[0145] The sulfide solid electrolyte glass ceramics of the present embodiment contains lithium atoms, phosphorus atoms, sulfur atoms, and halogen atoms, and the halogen atoms are preferably at least one selected from chlorine atoms, bromine atoms, and iodine atoms.

[0146] When only one kind is contained as a halogen atom, a bromine atom or an iodine atom is preferable, and an iodine atom is more preferable.

[0147] When two halogen atoms are contained, any one of a combination of a chlorine atom and a bromine atom, a combination of a chlorine atom and a bromine atom, and a combination of a bromine atom and an iodine atom is preferred, and a combination of a bromine atom and an iodine atom is more preferred.

[0148] This is preferred because the ion conductivity is increased. In addition, the sulfide solid electrolyte glass ceramic is preferred because the water resistance is improved by containing iodine atoms.

[0149] In order to improve ion conductivity and water resistance, the sulfide solid electrolyte glass ceramics of the present embodiment preferably contains at least iodine atoms, and more preferably further contains bromine atoms.

[0150] (M Br / M I )

[0151] By making the content of bromine atoms (M Br mol) and the content of iodine atoms (M I mol) satisfies M Br / M I A relationship of ≤1.00 is preferred because the ion conductivity can be improved.

[0152] M BrThe total number of moles of bromine atoms contained in the raw materials used in producing the sulfide solid electrolyte glass ceramics is determined by M. I It depends on the total number of moles of iodine atoms contained in the raw materials used in the production of sulfide solid electrolyte glass ceramics. Br / M I , the above ionic conductivity changes significantly, and it can be seen that if M is reduced Br / M I , then P A / P B becomes larger. And if M Br / M I When M is smaller, the crystallinity is high, the crystallite size becomes larger, and the ion conductivity becomes higher, so it is preferred. Furthermore, as the crystallinity becomes higher, the water resistance described later is improved, so it is preferred. For these reasons, M Br / M I It is more preferably 0.80 or less, further preferably 0.50 or less, and further preferably 0.40 or less.

[0153] In addition, in order to increase the ionic conductivity, M Br / M I However, if the sulfide solid electrolyte glass ceramic contains a small amount of bromine atoms, the bromine atoms smaller than iodine atoms in the crystal will cause local deformation in the crystal structure, thereby observing a phenomenon that the conduction probability of a part of the ion conduction path is improved, which is preferred. Br / M I It is preferably 0 or more, more preferably greater than 0, further preferably 0.05 or more, and further preferably 0.08 or more.

[0154] M Br and M I It can be calculated from the content of each element in the raw material.

[0155] The sulfide solid electrolyte glass ceramic of this embodiment is based on the solid 31 P2S6 determined by P-NMR measurement 4- The phosphorus ratio is preferably 7.5 mol% or less. As mentioned above, P2S6 4- Easily hydrolyzed, if P2S6 4- A smaller phosphorus ratio improves water resistance, so it is preferred. In order to improve ion conductivity and water resistance, it is preferably 5.5 mol% or less, more preferably 4.0 mol% or less, further preferably 2.0 mol% or less, further preferably 1.5 mol% or less, more preferably 1.0 mol% or less, and further preferably 0.8 mol% or less. P2S6 4-The phosphorus ratio is preferably as small as possible, and the lower limit is not particularly limited, but may be substantially 0 mol % or more. Substantially 0 mol % also includes a value below the detection limit.

[0156] In the sulfide solid electrolyte glass ceramic of this embodiment, P2S7 4- The smaller the phosphorus ratio, the more preferable it is from the viewpoint of the ion conductivity of the sulfide solid electrolyte, and it is preferably 20.0% or less, more preferably 10.0% or less, and further preferably 8.0% or less, and the lower limit is preferably close to 0%.

[0157] In this manual, "main frame" refers to the PS4 3- Phosphorus ratio of the unit (PS4 3- Phosphorus ratio) exceeds 50.0%, from the perspective of high ion conductivity of sulfide solid electrolyte, PS4 3- The phosphorus ratio is preferably 60.0% or more, more preferably 70.0% or more, and even more preferably 80.0% or more. The upper limit is not particularly limited, and may be close to 100%.

[0158] In addition, in this manual, PS4 3- Unit ratio (PS4 3- Phosphorus ratio), P2S7 4- Unit ratio (P2S7 4- Phosphorus ratio) and P2S6 4- Unit ratio (P2S6 4- Phosphorus ratio) refers to the measurement of 31 P MAS NMR spectrum (solid 31 P NMR spectrum) and waveform separation, each PS4 3- Unit, P2S7 4- Unit and P2S6 4- The ratio of the unit to the overall area of ​​the peak. 31 The detailed conditions for measuring the P NMR spectrum are not particularly limited, and the measurement may be performed based on the conditions described in the Examples, for example.

[0159] (I1 Li2S / I1 P2S5 )

[0160] In the sulfide solid electrolyte glass ceramic of this embodiment, if the molar fraction of Li2S (I1 Li2S ) and the molar fraction of P2S5 (I1 P2S5 ) ratio (I1 Li2S / I1 P2S5) is 2.60 to 3.30, the ion conductivity and water resistance are improved, so it is preferably from the viewpoint of improving the ion conductivity and water resistance, more preferably 2.70 to 3.20, and further preferably 2.90 to 3.10.

[0161] (I2 Li2S / I2 P2S5 )

[0162] In the sulfide solid electrolyte glass ceramic of the present embodiment, if the molar fraction (I2 Li2S ) and the molar fraction of P2S5 (I2 P2S5 ) ratio (I2 Li2S / I2 P2S5 ) is 2.60 to 3.30, the ion conductivity and water resistance are improved, so it is preferably from the viewpoint of improving the ion conductivity and water resistance, more preferably 2.70 to 3.20, and further preferably 2.90 to 3.10.

[0163] According to the results of the examples described below, the ratio (I1 Li2S / I1 P2S5 ) and the ratio (I2 Li2S / I2 P2S5 ) is less than 10%, and further less than 9.5%, less than 7.5%, less than 5%, less than 3%, less than 1.5%, and less than 1%, which are roughly consistent. Therefore, it can be seen that according to the manufacturing method of this embodiment described later, lithium sulfide (Li2S) and phosphorus sulfide (P2S5), and solid electrolytes (A) and (B) obtained from raw materials containing them can be effectively utilized, and sulfide solid electrolyte glass ceramics with high ionic conductivity can be obtained.

[0164] If the ratio (content ratio) of the lithium atom content (mol), phosphorus atom content (mol), sulfur atom content (mol) and halogen atom content (mol) of the sulfide solid electrolyte glass ceramic of the present embodiment is, lithium atom: phosphorus atom: sulfur atom: halogen atom = (3.20~3.70): (0.70~1.30): (3.00~5.00): (0.20~0.70), it is easy to form a sulfide crystallized lithium superion conductor region II type crystal structure, so it is preferred, more preferably (3.30~3.60): (0.80~1.20): (3.50~4.50): (0.30~0.60), and further preferably (3.40~3.55): (0.90~1.10): (3.70~4.30): (0.40~0.55).

[0165] These contents can be calculated based on the contents of each element in the raw materials.

[0166] The shape of the sulfide solid electrolyte glass ceramics of the present embodiment is not particularly limited, and can be, for example, in the form of particles. The average particle size (D 50 ) For example, the range of 0.01 μm to 500 μm and 0.1 to 200 μm can be exemplified.

[0167] Average particle size (D 50 ) For example, it can be measured using a laser diffraction / scattering particle size distribution measuring device (for example, HORIBA's LA-950V2 model LA-950W2).

[0168] (Ionic conductivity)

[0169] The ionic conductivity of the sulfide solid electrolyte glass ceramic of this embodiment obtained by the manufacturing method of this embodiment is due to PS4 3- The phosphorus ratio is high and extremely high, and can usually be 0.01 mS / cm or more, more preferably 5.0 mS / cm or more, further preferably 5.4 mS / cm or more, further preferably 5.8 mS / cm or more, particularly preferably 6.0 mS / cm or more, more particularly preferably 6.8 mS / cm or more, and particularly preferably 7.2 mS / cm or more.

[0170] Water resistance (H2S generation)

[0171] The sulfide solid electrolyte glass ceramics according to the present embodiment is preferred because it exhibits high ion conductivity and is excellent in the above-mentioned water resistance.

[0172] Sulfide solid electrolytes may generate hydrogen sulfide (H2S) due to hydrolysis reaction caused by contact with moisture such as moisture in the air. "Water resistance" refers to the property of suppressing the generation of H2S even when contacting moisture in the air.

[0173] It is preferred that the amount of H2S generated is small. Among the H2S generated by the method described in the examples, if it is less than 2.0cc / g, there is no problem in practical use. It is more preferably 1.5cc / g or less, further preferably 1.0cc / g or less, further preferably 0.8cc / g or less, and particularly preferably 0.5cc / g or less. The lower limit is not particularly limited.

[0174] Hereinafter, the production method of the present embodiment will be described in more detail based on the above-mentioned embodiment.

[0175] [Method for producing sulfide solid electrolyte glass ceramics]

[0176] The method for producing the sulfide solid electrolyte glass ceramic of the present embodiment is required to be as follows Figure 1 As shown in the figure, it includes:

[0177] A solid electrolyte (A) is obtained by treating lithium sulfide (Li2S) and phosphorus sulfide (P2S5) by at least one selected from stirring, mixing and pulverizing;

[0178] The solid electrolyte (A) and the lithium halide are treated by at least one selected from stirring, mixing and pulverizing to obtain a solid electrolyte (B).

[0179] According to the production method of this embodiment, a sulfide solid electrolyte glass ceramic having high ion conductivity can be produced by a simple production method. Furthermore, the produced sulfide solid electrolyte glass ceramic has high water resistance, and a lithium ion battery using the same has excellent battery characteristics, which is preferred.

[0180] <Step (A)>

[0181] The manufacturing method of the sulfide solid electrolyte glass ceramic of this embodiment requires that lithium sulfide (Li2S) and phosphorus sulfide (P2S5) be treated by at least one selected from stirring, mixing and crushing to obtain a solid electrolyte (A) (sometimes also recorded as process (A)), and it is more preferable to further heat the solid electrolyte (A) to crystallize it.

[0182] The manufacturing method of the sulfide solid electrolyte glass ceramic of this embodiment is different from the manufacturing method described in the above-mentioned Patent Document 1, and is to manufacture the solid electrolyte (A). This is because by using the solid electrolyte (A) as described above, P2S6, which becomes an impurity in the solid electrolyte, can be reduced. 4-phosphorus ratio, and the P2S6 can be further reduced by heating the solid electrolyte (A) as needed. 4- Phosphorus ratio, it is possible to produce a solid electrolyte (B) with improved crystallinity. 4- The phosphorus ratio can be prepared by any method and is not particularly limited.

[0183] <Process (B)>

[0184] The method for producing the sulfide solid electrolyte glass ceramic of the present embodiment requires treating the solid electrolyte (A) and the lithium halide by at least one selected from stirring, mixing and pulverizing to obtain the solid electrolyte (B) (sometimes described as step (B)).

[0185] Step (B) of the present embodiment obtains a solid electrolyte (B) by treating the solid electrolyte (A), the lithium halide and Li2S added as needed obtained in step (A) by at least one selected from stirring, mixing and pulverizing described later.

[0186] For process (B), the solid electrolyte (A) can be taken out after process (A) is completed, and lithium halide can be added to the obtained solid electrolyte (A) for treatment, or lithium halide can be added after process (A) is completed for treatment. From the viewpoint of not making the manufacturing process complicated, it is preferred to add lithium halide to the treatment device that performs process (A) after process (A) is completed for treatment. In the case of using Li2S, it is preferably added simultaneously with the lithium halide or before and after it.

[0187] As the lithium halide, it is preferred that at least lithium iodide (LiI) is contained, and it is preferred that lithium bromide (LiBr) is further contained.

[0188] <Processing>

[0189] The treatments in step (A) and step (B) of the present embodiment need to be at least one selected from stirring, mixing and pulverizing. Stirring, mixing and pulverizing may be performed alone or in combination. From the viewpoint of making the particle size of the sulfide solid electrolyte within the range described below, pulverizing is preferred.

[0190] The treatments in step (A) and step (B) may be the same or different, but are preferably the same. From the viewpoint of not complicating the production process, it is more preferable to carry out them continuously using the same treatment apparatus.

[0191] The treatment of this embodiment can be performed using a mixer, a stirrer, a pulverizer, etc. This is because the raw materials can be mixed even when a stirrer is used, and the raw materials are pulverized and mixed at the same time in a pulverizer.

[0192] As agitators and mixers, for example, a mechanical stirring mixer having stirring blades in a reaction tank and capable of stirring (also referred to as mixing brought by stirring, stirring and mixing) can be exemplified. As mechanical stirring mixers, high-speed stirring mixers, double-arm mixers, etc. can be exemplified. In addition, as high-speed stirring mixers, vertical axis rotating mixers, horizontal axis rotating mixers, etc. can be exemplified, and any type of mixer can also be used.

[0193] The shape of the stirring blade used in the mechanical stirring mixer may be a blade type, an arm type, an anchor type, a paddle type, a stirring paddle type, a belt type, a multi-stage blade type, a double-arm type, a bucket type, a double-shaft blade type, a flat blade type, a C-blade type, etc. From the viewpoint of more efficiently promoting the reaction of the raw materials, a bucket type, a flat blade type, a C-blade type, an anchor type, a paddle type, a stirring paddle type is preferred, and an anchor type, a paddle type, a stirring paddle type is more preferred.

[0194] When a mechanical stirring mixer is used, the rotation speed of the stirring blade can be appropriately adjusted according to the capacity, temperature, shape of the stirring blade, etc. of the fluid in the reaction tank, without any particular limitation, and is usually set to about 5 rpm to about 400 rpm. From the viewpoint of more efficiently promoting the reaction of the raw materials, it is preferably 10 rpm to 300 rpm, more preferably 15 rpm to 250 rpm, and further preferably 20 rpm to 200 rpm.

[0195] The temperature conditions for mixing using a mixer are not particularly limited, and are, for example, usually -30 to 120° C., preferably -10 to 100° C., more preferably 0 to 80° C., and further preferably 10 to 60° C. The mixing time is usually 0.1 to 500 hours, and is preferably 1 to 450 hours, more preferably 10 to 425 hours, further preferably 20 to 400 hours, and further preferably 30 to 375 hours from the viewpoint of making the dispersion state of the raw materials more uniform and promoting the reaction.

[0196] The method of mixing with pulverization using a pulverizer is a method conventionally adopted as a mechanical grinding method. As the pulverizer, for example, a media type pulverizer using pulverizing media can be used.

[0197] The media pulverizer is roughly divided into a container-driven pulverizer and a media-stirring pulverizer. As the container-driven pulverizer, a stirring tank, a crushing tank, or a ball mill or a bead mill in which these are combined can be cited. In addition, as the media-stirring pulverizer, there can be cited: impact pulverizers such as a cutter mill, a hammer mill, and a pin mill; tower-type pulverizers such as a tower mill; stirring tank-type pulverizers such as a grinder, a wet sand mill (aquamizer), and a sand mill; flow-through trough-type pulverizers such as a viscose mill and a coarse crusher; flow-through tube-type pulverizers; annular pulverizers such as a combined ball mill; a continuous dynamic pulverizer; various pulverizers such as a single-axis or multi-axis kneading machine. Among them, if the ease of adjusting the particle size of the obtained sulfide is considered, a ball mill or a bead mill exemplified as a container-driven pulverizer is preferred.

[0198] These pulverizers can be appropriately selected according to the desired scale, etc. For a relatively small scale, a container-driven pulverizer such as a ball mill or a bead mill can be used. In the case of large-scale or mass production, other types of pulverizers can also be used.

[0199] Furthermore, as described later, when the mixture is in a liquid state accompanied with a liquid such as a solvent or in a slurry state during mixing, a wet pulverizer capable of wet pulverization is preferred.

[0200] As wet pulverizers, wet bead mills, wet ball mills, wet vibration mills, etc. can be representatively cited. From the perspective of being able to freely adjust the conditions of the pulverization operation and being easy to handle materials with smaller particle sizes, wet bead mills using beads as pulverization media are preferred. In addition, dry pulverizers such as dry bead mills, dry ball mills, dry planetary ball mills, dry vibration mills, and dry non-media pulverizers such as jet mills can also be used.

[0201] In addition, when the object to be mixed is in a liquid state or a slurry state, a flow-through pulverizer can be used, which can be circulated as needed. Specifically, a pulverizer that circulates between a pulverizer (pulverizing mixer) for pulverizing slurry and a temperature-maintaining tank (reaction container) can be cited.

[0202] The size of the beads or balls used in the ball mill or bead mill can be appropriately selected according to the desired particle size, processing volume, etc. For example, the diameter of the beads is usually 0.05 mmφ or more, preferably 0.1 mmφ or more, more preferably 0.3 mmφ or more, and the upper limit is usually 5.0 mmφ or less, preferably 3.0 mmφ or less, and more preferably 2.0 mmφ or less. In addition, the diameter of the balls is usually 2.0 mmφ or more, preferably 2.5 mmφ or more, and more preferably 3.0 mmφ or more, and the upper limit is usually 30.0 mmφ or less, preferably 20.0 mmφ or less, and more preferably 15.0 mmφ or less.

[0203] In addition, examples of the material include metals such as stainless steel, chrome steel, and tungsten carbide; ceramics such as zirconium oxide and silicon nitride; and minerals such as agate.

[0204] When a ball mill or a bead mill is used, the rotation speed cannot be generally specified because it varies according to the scale of treatment, but is usually 10 rpm or more, preferably 20 rpm or more, and more preferably 50 rpm or more, and the upper limit is usually 1,000 rpm or less, preferably 900 rpm or less, more preferably 800 rpm or less, and further preferably 700 rpm or less.

[0205] The pulverization time in this case cannot be generally stated because it varies depending on the scale of treatment, but is usually 5 hours or more, preferably 10 hours or more, more preferably 20 hours or more, and further preferably 30 hours or more, and the upper limit is usually 300 hours or less, preferably 200 hours or less, and more preferably 100 hours or less.

[0206] By selecting the size and material of the medium (beads, balls) used, the rotation speed and time of the rotor, etc., mixing, stirring, pulverization, or a combination of these processes can be performed, and the particle size of the obtained sulfide can be adjusted.

[0207] (Solvent)

[0208] In the above-mentioned mixing, a solvent may be added to the above-mentioned raw materials for mixing. As the solvent, various solvents called organic solvents and the like can be widely used.

[0209] As the solvent, a wide range of solvents conventionally used in the production of solid electrolytes can be adopted, and examples thereof include hydrocarbon solvents such as aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, and aromatic hydrocarbon solvents.

[0210] Examples of aliphatic hydrocarbons include hexane, pentane, 2-ethylhexane, heptane, octane, decane, undecane, dodecane and tridecane. Examples of alicyclic hydrocarbons include cyclohexane and methylcyclohexane. Examples of aromatic hydrocarbon solvents include benzene, toluene, xylene, mesitylene, ethylbenzene, tert-butylbenzene, trifluoromethylbenzene and nitrobenzene.

[0211] In addition to the hydrocarbon solvents, solvents containing elements other than carbon and hydrogen, such as nitrogen, oxygen, sulfur, halogens, and other heteroelements, may be cited. Such solvents may preferably include alcohol solvents, aldehyde solvents, and ketone solvents in addition to ether solvents and ester solvents containing oxygen as a heteroelement.

[0212] As the ether solvent, for example, preferably there can be mentioned aliphatic ethers such as dimethyl ether, diethyl ether, tert-butyl methyl ether, dimethoxymethane, dimethoxyethane, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme) or diethylene glycol, triethylene glycol; alicyclic ethers such as ethylene oxide, propylene oxide, tetrahydrofuran, tetrahydropyran, dimethoxytetrahydrofuran, cyclopentyl methyl ether, dioxane; heterocyclic ethers such as furan, benzofuran, benzopyran; aromatic ethers such as methyl phenyl ether (anisole), ethyl phenyl ether, dibenzyl ether, diphenyl ether.

[0213] As the ester solvent, for example, preferably exemplified are methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate; aliphatic esters such as methyl propionate, ethyl propionate, dimethyl oxalate, diethyl oxalate, dimethyl malonate, diethyl malonate, dimethyl succinate, diethyl succinate; alicyclic esters such as methyl cyclohexanecarboxylate, ethyl cyclohexanecarboxylate, dimethyl cyclohexanedicarboxylate; heterocyclic esters such as methyl pyridinecarboxylate, methyl pyrimidinecarboxylate, acetyl lactone, propiolactone, butyrolactone, valerolactone; aromatic esters such as methyl benzoate, ethyl benzoate, dimethyl phthalate, diethyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, trimethyl trimellitate, triethyl trimellitate.

[0214] In addition, preferably, there can be mentioned alcohol solvents such as ethanol and butanol; aldehyde solvents such as formaldehyde, acetaldehyde and dimethylformamide; ketone solvents such as acetone and methyl ethyl ketone.

[0215] Examples of the solvent containing nitrogen as a heteroelement include solvents having a group containing nitrogen such as an amino group, an amide group, a nitro group, or a nitrile group. These can also be used as a complexing agent for forming a complex with the solid electrolyte.

[0216] For example, as the solvent having an amino group, preferably exemplified are aliphatic amines such as ethylenediamine, diaminopropane, dimethylethylenediamine, diethylethylenediamine, dimethyldiaminopropane, tetramethyldiaminomethane, tetramethylethylenediamine (TMEDA), and tetramethyldiaminopropane (TMPDA); alicyclic amines such as cyclopropanediamine, cyclohexanediamine, and bisaminomethylcyclohexane; heterocyclic amines such as isophoronediamine, piperazine, dipiperidylpropane, and dimethylpiperazine; and aromatic amines such as phenylenediamine, toluenediamine, naphthalenediamine, methylphenylenediamine, dimethylnaphthalenediamine, dimethylphenylenediamine, tetramethylphenylenediamine, and tetramethylnaphthalenediamine.

[0217] Also preferably, solvents containing nitrogen element such as dimethylformamide, acetonitrile, acrylonitrile and nitrobenzene can be mentioned.

[0218] As the solvent containing a halogen element as a heteroelement, preferably, dichloromethane, chlorobenzene, trifluorotoluene, chlorobenzene, chlorotoluene, bromobenzene or the like can be exemplified.

[0219] Furthermore, as the solvent containing sulfur element, dimethyl sulfoxide, carbon disulfide, etc. can be preferably exemplified.

[0220] When a solvent is used, the amount of the solvent used is preferably 100 mL or more, more preferably 500 mL or more, further preferably 1 L or more, further preferably 2 L or more, further preferably 4 L or more, and the upper limit is preferably 50 L or less, more preferably 20 L or less, further preferably 15 L or less, further preferably 12 L or less. If the amount of the solvent used is within the above range, the raw materials can be efficiently reacted.

[0221] (dry)

[0222] In the case of using a solvent for mixing, the mixing may include drying the fluid (usually a slurry) obtained by mixing after the mixing. In the case of using a complexing agent as a solvent, the sulfide can be obtained by removing the complexing agent from the complex containing the complexing agent, in the case of using a complexing agent and a solvent in combination, by removing the complexing agent from the complex containing the complexing agent and removing the solvent, and in the case of using a solvent other than the complexing agent, by removing the solvent. The obtained sulfide has PS4 3- The structure of solid electrolytes such as cells reflects ionic conductivity caused by alkali metal elements such as lithium and sodium.

[0223] The fluid obtained by mixing can be dried at a temperature corresponding to the type of solvent, for example, at a temperature equal to or higher than the boiling point of the complexing agent.

[0224] Furthermore, the complexing agent and the solvent used as required can be dried by volatilizing them by using a vacuum pump or the like under reduced pressure (vacuum drying) at usually 5 to 100°C, preferably 10 to 85°C, more preferably 15 to 70°C, and still more preferably around room temperature (23°C) (e.g. around room temperature ±5°C).

[0225] The fluid may also be dried by filtration using a glass filter, solid-liquid separation by decantation, or solid-liquid separation using a centrifuge. When a solvent other than a complexing agent is used, a sulfide may be obtained by solid-liquid separation. In addition, when a complexing agent is used as a solvent, after solid-liquid separation, drying based on the above-mentioned temperature conditions is performed to remove the complexing agent introduced into the complex.

[0226] Specifically, as a solid-liquid separation, the fluid is transferred to a container, and after the sulfide (or the complex (a substance that can be called a precursor of the sulfide) when the sulfide is contained) is precipitated, it is easier to remove the complexing agent and solvent to become the supernatant by decantation or by filtering using a glass filter with a pore size of about 10 to 200 μm, preferably 20 to 150 μm.

[0227] Drying may be performed after mixing and before the hydrogen treatment described below, or after the hydrogen treatment.

[0228] (Li2S and P2S5)

[0229] In the production method of this embodiment, it is necessary to use Li2S (lithium sulfide) and P2S5 (phosphorus pentasulfide).

[0230] Li2S used in this embodiment is preferably in the form of particles.

[0231] The average particle size of Li2S particles (D 50 ) is preferably 10 μm to 2000 μm, more preferably 30 μm to 1500 μm, and even more preferably 50 μm to 1000 μm. In this specification, the average particle size (D 50 ) is the particle size when the particle size distribution cumulative curve is drawn from the smallest particle to the total 50%, and the volume distribution is, for example, the average particle size that can be measured using a laser diffraction / scattering particle size distribution measuring device. In addition, for P2S5, it is also preferred to have an average particle size of the same degree as that of the Li2S particles, that is, it is preferably within the same range as the average particle size of the Li2S particles.

[0232] In this embodiment, Li2S is added in step (A) and step (B), and P2S5 is added in step (A).

[0233] In step (A), the P2S7 in the solid electrolyte (A) is 4- From the viewpoint of optimizing the content and preparing a sulfide solid electrolyte glass ceramic with high ion conductivity, it is preferred to use 0.34 mol or more of P2S5 relative to 1.00 mol of Li2S, more preferably 0.38 mol or more, further preferably 0.40 mol or more, and preferably less than 0.70 mol, more preferably less than 0.60 mol, further preferably less than 0.55 mol.

[0234] In this embodiment, in the total process of step (A) and step (B) above, the sulfide solid electrolyte glass ceramic is made of PS4 3- As the main skeleton, P2S6 in the sulfide solid electrolyte 4- From the viewpoint of reducing the phosphorus ratio and achieving high ion conductivity, it is preferred to use 0.10 mol or more of P2S5, more preferably 0.20 mol or more, further preferably 0.30 mol or more, and preferably less than 0.50 mol, more preferably less than 0.40 mol, and further preferably less than 0.35 mol, relative to 1.00 mol of Li2S used.

[0235] In this embodiment, Li2S is added at least in step (A) and step (B). 4- From the viewpoint of reducing the phosphorus ratio and achieving high ion conductivity, it is preferred to use 0.10 mol or more of Li2S for step (B), more preferably 0.20 mol or more, further preferably 0.25 mol or more, and preferably less than 0.80 mol, more preferably less than 0.70 mol, further preferably less than 0.65 mol, relative to 1.00 mol of Li2S used in step (A).

[0236] As Li2S and P2S5, commonly available commercial products may be used, or Li2S and P2S5 prepared by the method described in the Examples may be used.

[0237] From the viewpoint of improving the ionic conductivity of the sulfide solid electrolyte glass ceramic, the purity of Li2S is preferably 95 mass % or more, more preferably 98 mass % or more. 10 From the viewpoint of improving the ionic conductivity of the sulfide solid electrolyte, the purity of P2S5 is preferably 95% by mass or more, and more preferably 98% by mass or more.

[0238] (Lithium Halide)

[0239] In the present embodiment, from the viewpoint of obtaining a sulfide solid electrolyte glass ceramic having high ion conductivity, it is necessary to further add a lithium halide in the step (B) in order to introduce halogen atoms into the sulfide solid electrolyte.

[0240] The lithium halide is more preferably at least one selected from lithium chloride, lithium bromide, and lithium iodide, and further preferably a combination of lithium chloride and lithium bromide, or a combination of lithium bromide and lithium iodide.

[0241] The amount of lithium halide used may be any amount as long as it satisfies the preferred blending ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms described above.

[0242] (Solid electrolyte (A))

[0243] The solid electrolyte (A) is the solid electrolyte obtained in step (A), preferably PS4 3- or P2S7 4- The sulfide solid electrolyte with a main skeleton is preferably PS4 3- Sulfide solid electrolyte as the main skeleton.

[0244] In this manual, "main frame" refers to the PS4 3- Phosphorus ratio of the unit (PS4 3- Phosphorus ratio) exceeds 50.0%, from the perspective of high ion conductivity of sulfide solid electrolyte, PS4 3- The fraction is preferably 60.0% or more, more preferably 70.0% or more, and further preferably 80.0% or more. The upper limit is not particularly limited, and it is preferably close to 100%. However, from the viewpoint of balancing ease of manufacture and ion conductivity, it is preferably 99.5% or less, more preferably 98.0% or less, and further preferably 95.0% or less.

[0245] The solid electrolyte (A) preferably comprises P2S7 4- It may further contain a small amount of Li2S and P2S5 used as raw materials, and PS4 as the target. 3- , and P2S6 4- Among them, P2S6 4- When the content in the sulfide solid electrolyte increases, the ion conductivity decreases, so it is preferable to reduce the content.

[0246] In step (B), by further adding Li2S and lithium halide to the solid electrolyte (A) containing Li4P2S7 to obtain a sulfide solid electrolyte, the P2S6 contained in the sulfide solid electrolyte glass ceramic can be reduced. 4-Therefore, from the viewpoint of improving the ionic conductivity of the sulfide solid electrolyte glass ceramic, the solid electrolyte (A) is 31 P-NMR measurements of P2S7 4- The phosphorus ratio is preferably 20.0 mol% or more, more preferably 30.0 mol% or more, and further preferably 35.0 mol% or more based on the total amount of the solid electrolyte (A). The upper limit is not particularly limited, but due to the generation of PS4 during the treatment of step (A), 3- , and therefore, it is preferably 95.0 mol % or less, more preferably 90.0 mol % or less, and further preferably 80.0 mol % or less.

[0247] The solid electrolyte (A) may be an amorphous sulfide solid electrolyte or a crystalline sulfide solid electrolyte, but a crystalline sulfide solid electrolyte is preferred because the crystallite size of the sulfide solid electrolyte glass ceramic becomes larger.

[0248] (Solid electrolyte (B))

[0249] The solid electrolyte (B) obtained by this embodiment is a product of the step (B), is an intermediate for the production of sulfide solid electrolyte glass ceramics, contains lithium atoms, sulfur atoms and phosphorus atoms, preferably PS4 3- The main skeleton.

[0250] The solid electrolyte (B) may be a crystalline sulfide solid electrolyte or an amorphous sulfide solid electrolyte.

[0251] When the solid electrolyte (B) is a crystalline sulfide solid electrolyte, it can be used as a sulfide solid electrolyte glass ceramic, but it can also be further heated to advance crystallization.

[0252] When the solid electrolyte (B) is an amorphous sulfide solid electrolyte, it can be made into a sulfide solid electrolyte glass ceramic by heating (crystallization) as described later.

[0253] The solid electrolyte (B) contains halogen atoms. As representative solid electrolytes containing halogen atoms, for example, solid electrolytes composed of lithium sulfide, phosphorus sulfide and lithium halide, such as Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, and Li2S-P2S5-LiI-LiBr, etc., can be preferably cited; and solid electrolytes such as Li2S-P2S5-Li2O-LiI, Li2S-SiS2-P2S5-LiI, etc., which contain other atoms such as oxygen atoms and silicon atoms. From the viewpoint of obtaining higher ionic conductivity, solid electrolytes composed of lithium sulfide, phosphorus sulfide and lithium halide, such as Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, and Li2S-P2S5-LiI-LiBr, etc., are preferred.

[0254] The types of atoms constituting the solid electrolyte (B) can be confirmed by, for example, an ICP emission spectrometer.

[0255] In the case where the solid electrolyte (B) of the present embodiment is an amorphous sulfide solid electrolyte, if the solid electrolyte (B) 31 P2S6 determined by P-NMR measurement 4- The phosphorus ratio is 15.0 mol% or less, which improves ion conductivity and water resistance, so it is preferred. From the viewpoint of improving ion conductivity and water resistance, it is more preferably 10.0 mol% or less, and further preferably 7.0 mol% or less. In order to improve ion conductivity and water resistance, it is preferred not to contain P2S6 4- , so the lower limit is not particularly limited.

[0256] The solid electrolyte (B) of the present embodiment may be heated as necessary.

[0257] The solid electrolyte (B) after heating is 31 P2S6 determined by P-NMR measurement 4- The phosphorus ratio is preferably 7.5 mol% or less. As mentioned above, P2S6 4- Easily hydrolyzed, if P2S6 4- A smaller phosphorus ratio improves water resistance, so it is preferred. In order to improve ion conductivity and water resistance, it is preferably 5.5 mol% or less, more preferably 4.0 mol% or less, further preferably 2.0 mol% or less, further preferably 1.5 mol% or less, more preferably 1.0 mol% or less, and further preferably 0.8 mol% or less. P2S6 4- The phosphorus ratio is preferably as small as possible, and the lower limit is not particularly limited, but may be substantially 0 mol % or more. Substantially 0 mol % also includes a value below the detection limit.

[0258] The heated solid electrolyte (B) may be the sulfide solid electrolyte glass ceramic of the present embodiment, and may be further pulverized or the like to be a sulfide solid electrolyte glass ceramic as required.

[0259] When the solid electrolyte (B) obtained in the present embodiment has at least Li2S-P2S5, the molar ratio of Li2S to P2S5 is preferably 65-85:15-35, more preferably 70-80:20-30, and further preferably 72-78:22-28 from the viewpoint of obtaining higher ion conductivity.

[0260] In the case where the solid electrolyte (B) obtained in the present embodiment is, for example, Li2S-P2S5-LiI-LiBr, the total content of Li2S and P2S5 is preferably 60 to 95 mol%, more preferably 65 to 90 mol%, and further preferably 70 to 85 mol%. In addition, the ratio of lithium bromide to the total of lithium bromide and lithium iodide is preferably 1 to 99 mol%, more preferably 20 to 90 mol%, further preferably 40 to 80 mol%, and particularly preferably 50 to 70 mol%.

[0261] In the solid electrolyte (B) obtained in this embodiment, the mixing ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms is preferably 1.0 to 1.8: 1.0 to 2.0: 0.1 to 0.8: 0.01 to 0.6, more preferably 1.1 to 1.7: 1.2 to 1.8: 0.2 to 0.6: 0.05 to 0.5, and further preferably 1.2 to 1.6: 1.3 to 1.7: 0.25 to 0.5: 0.08 to 0.4. In addition, when bromine and iodine are used in combination as halogen atoms, the blending ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, bromine and iodine is preferably 1.0-1.8: 1.0-2.0: 0.1-0.8: 0.01-0.3: 0.01-0.3, more preferably 1.1-1.7: 1.2-1.8: 0.2-0.6: 0.02-0.25: 0.02-0.25, more preferably 1.2-1.6: 1.3-1.7: 0.25-0.5: 0.03-0.2: 0.03-0.2, and further preferably 1.35-1.45: 1.4-1.7: 0.3-0.45: 0.04-0.18: 0.04-0.18. By setting the blending ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms within the above range, it is possible to easily obtain a sulfide solid electrolyte glass ceramic having a type II crystal structure of the sulfide crystalline lithium superion conductor region described later and having higher ion conductivity.

[0262] The shape of the solid electrolyte (B) is not particularly limited, and may be, for example, a particle shape. The average particle size (D50 ) For example, the range of 0.01 μm to 500 μm and 0.1 to 200 μm can be exemplified.

[0263] The exothermic peak of the sulfide solid electrolyte glass ceramic of the present embodiment is preferably 120°C to 300°C, more preferably 150°C to 250°C, and further preferably 170°C to 220°C.

[0264] In the differential thermal analysis (DTA) of the solid electrolyte (B) serving as a manufacturing intermediate of the sulfide solid electrolyte glass ceramic of the present embodiment, if the half-width value of the exothermic peak that first appears at a temperature of 130°C or higher during the heating process is 8.0°C or lower, the ionic conductivity and water resistance are improved, so it is preferably 7.0°C or lower, more preferably 6.5°C or lower.

[0265] (heating)

[0266] The production method of the present embodiment preferably includes further heating of at least one of the solid electrolyte (A) and further heating of the solid electrolyte (B).

[0267] In order to obtain a solid electrolyte (A) which is a crystalline sulfide solid electrolyte (hereinafter also referred to as a crystalline solid electrolyte (A)) or a sulfide solid electrolyte glass ceramic, heating may be performed after obtaining a solid electrolyte (A) which is an amorphous sulfide solid electrolyte (hereinafter also referred to as an amorphous solid electrolyte (A)) or a solid electrolyte (B) which is an amorphous sulfide solid electrolyte (hereinafter also referred to as an amorphous solid electrolyte (B)).

[0268] More specifically, the solid electrolyte (A) obtained by process (A) can be heated to form a crystalline solid electrolyte (A), which can then be used as a raw material for process (B). The solid electrolyte (B) obtained by process (B) can also be heated after process (B) to form a sulfide solid electrolyte glass ceramic.

[0269] It is preferred that the solid electrolyte (A) obtained in the step (A) is heated to obtain a crystalline solid electrolyte (A) and then the step (B) is performed because the crystallite size of the sulfide solid electrolyte glass ceramic increases.

[0270] In the case of heating the amorphous solid electrolyte (B) to obtain a sulfide solid electrolyte glass ceramic, the heating temperature can be determined according to the structure of the sulfide solid electrolyte glass ceramic. Specifically, the amorphous solid electrolyte (B) is subjected to differential thermal analysis (DTA) under a temperature increase condition of 10°C / min using a differential thermal analyzer (DTA device), and the temperature of the peak top of the exothermic peak observed at the lowest temperature side at 130°C or above is used as the starting point, preferably set to a temperature lower by 5°C or more, more preferably set to a temperature lower by 7°C or more, and further preferably set to a temperature lower by 10°C or more. There is no particular restriction on the lower limit, and it is preferably set to a temperature within 30°C on the low temperature side, and more preferably set to a temperature within 25°C on the low temperature side. By setting it to such a temperature range, the sulfide solid electrolyte glass ceramic can be obtained more efficiently and reliably.

[0271] When the amorphous solid electrolyte (A) is heated to obtain the crystalline solid electrolyte (A), differential thermal analysis (DTA) is performed using a differential thermal analyzer (DTA device) under a temperature increase condition of 10°C / min, and the heat treatment is performed at a temperature near the top of the exothermic peak. The preferred heat treatment temperature is in the range of -50°C to 100°C, preferably in the range of -30°C to 80°C, and more preferably in the range of -15°C to 65°C, based on the temperature of the exothermic peak top.

[0272] The heating temperature for obtaining the crystalline sulfide solid electrolyte (A) or the sulfide solid electrolyte glass ceramic varies depending on the structure of the obtained crystalline sulfide solid electrolyte (A) or the sulfide solid electrolyte glass ceramic and cannot be generally specified, but is usually preferably 130°C or higher, more preferably 135°C or higher, and further preferably 140°C or higher. The upper limit is not particularly limited, but is preferably 350°C or lower, more preferably 330°C or lower, and further preferably 320°C or lower.

[0273] The heating time is not particularly limited as long as it is a time for obtaining the desired crystalline solid electrolyte (A) or sulfide solid electrolyte glass ceramic, and is preferably 1 minute or more, more preferably 10 minutes or more, more preferably 30 minutes or more, and more preferably 1 hour or more. In addition, the upper limit of the heating time is not particularly limited, and is preferably 24 hours or less, more preferably 10 hours or less, more preferably 5 hours or less, and more preferably 3 hours or less.

[0274] In addition, the heating is preferably carried out in an inert gas atmosphere (e.g., a nitrogen atmosphere, an argon atmosphere) or in a reduced pressure atmosphere (particularly in a vacuum). This is because it is possible to prevent the degradation (e.g., oxidation) of the product. The heating method is not particularly limited, and examples thereof include methods using a hot plate, a vacuum heating device, an argon atmosphere furnace, a firing furnace, and the like. In addition, in industry, a horizontal dryer, a horizontal vibrating fluidized dryer, and the like having a heating unit and a feeding mechanism can also be used, and the method can be selected according to the amount of heating treatment.

[0275] (crushed)

[0276] The present embodiment preferably further comprises pulverizing the solid electrolyte (A), the solid electrolyte (B) or the sulfide solid electrolyte glass ceramic, and preferably comprises a plurality of pulverizing steps. By pulverizing the solid electrolyte (A), the solid electrolyte (B) or the sulfide solid electrolyte glass ceramic, a sulfide solid electrolyte glass ceramic having a small particle size and suppressing a decrease in ionic conductivity can be obtained.

[0277] The pulverizer used for pulverization in the present embodiment is not particularly limited as long as it can pulverize particles, and for example, a media-type pulverizer using pulverizing media can be used.

[0278] As the pulverizer, a dry media pulverizer such as a dry bead mill, a dry ball mill, and a dry vibration mill, a dry non-media pulverizer such as a jet mill, etc. can be used. In the case of a slurry containing a solvent, representative examples include a wet bead mill, a wet ball mill, and a wet vibration mill. From the perspective of being able to freely adjust the conditions of the pulverization operation and being able to easily cope with materials with smaller particle sizes, a dry bead mill or a wet bead mill using beads as the pulverization medium is preferred.

[0279] The size of the beads used in the pulverizer can be appropriately selected depending on the desired particle size, processing volume, etc. For example, the diameter of the beads is usually set to about 0.05 mmφ to 5.0 mmφ, preferably 0.1 mmφ to 3.0 mmφ, and more preferably 0.3 mmφ to 1.5 mmφ.

[0280] As the pulverizer used for pulverization in the present embodiment, a machine capable of pulverizing an object using ultrasonic waves, for example, a machine called an ultrasonic pulverizer, an ultrasonic homogenizer, a probe ultrasonic pulverizer, or the like can be used.

[0281] In this case, various conditions such as the frequency of the ultrasonic wave can be appropriately selected according to the average particle size of the desired complex, and the frequency can be set, for example, to about 1 kHz to 100 kHz. From the viewpoint of more effectively pulverizing the complex, it is preferably 3 kHz to 50 kHz, more preferably 5 kHz to 40 kHz, and even more preferably 10 kHz to 30 kHz.

[0282] The power of the ultrasonic pulverizer is generally about 500 to 16,000 W, preferably 600 to 10,000 W, more preferably 750 to 5,000 W, and even more preferably 900 to 1,500 W.

[0283] The average particle size (D 50 ) can be appropriately determined as desired, and is usually 0.01 μm to 50 μm, preferably 0.03 μm to 5 μm, and more preferably 0.05 μm to 3 μm. By setting such an average particle size, it is possible to meet the requirements of small-particle solid electrolytes with an average particle size of 1 μm or less.

[0284] The pulverization time is not particularly limited as long as it is the time for the complex to reach the desired average particle size, and is usually from 0.1 hours to 100 hours. From the viewpoint of effectively making the particle size the desired size, it is preferably from 0.3 hours to 72 hours, more preferably from 0.5 hours to 48 hours, and even more preferably from 1 hour to 24 hours.

[0285] (Application of sulfide solid electrolyte glass ceramics)

[0286] The sulfide solid electrolyte glass ceramic of this embodiment has a predetermined average particle size and specific surface area, high ion conductivity, excellent battery performance, and is unlikely to generate H2S, and is therefore suitable for use in an electrode composite material for a lithium ion battery and a lithium ion battery.

[0287] This is particularly suitable when lithium is used as the conductive species. The sulfide solid electrolyte glass ceramic of this embodiment can be used for a positive electrode layer, a negative electrode layer, or an electrolyte layer.

[0288] In addition, the battery preferably uses a current collector in addition to the positive electrode layer, the electrolyte layer and the negative electrode layer, and the current collector can use a known current collector. For example, a layer obtained by coating a substance that reacts with the above-mentioned sulfide solid electrolyte glass ceramic with Au, Pt, Al, Ti or Cu can be used.

[0289] [Electrode composite materials]

[0290] The electrode composite material of the present embodiment needs to contain the above-mentioned sulfide solid electrolyte glass ceramic and an electrode active material described later.

[0291] (Electrode Active Material)

[0292] As the electrode active material, a positive electrode active material or a negative electrode active material is used, depending on whether the electrode composite material is used for a positive electrode or a negative electrode.

[0293] As the positive electrode active material, any positive electrode active material can be used without particular limitation as long as it can promote the battery chemical reaction through the relationship with the negative electrode active material, and the battery chemical reaction is accompanied by the movement of lithium ions caused by the atom adopted as the atom reflecting ionic conductivity, preferably the lithium atom. As such positive electrode active materials that can be inserted and removed by lithium ions, oxide positive electrode active materials, sulfide positive electrode active materials, etc. can be cited.

[0294] As oxide-based positive electrode active materials, preferred examples include lithium-containing transition metal composite oxides such as LMO (lithium manganese oxide), LCO (lithium cobalt oxide), NMC (lithium nickel manganese cobalt oxide), NCA (lithium nickel cobalt aluminum oxide), LNCO (lithium nickel cobalt oxide), and olivine-type compounds (LiMeNPO4, Me = Fe, Co, Ni, Mn).

[0295] Examples of the sulfide-based positive electrode active material include titanium sulfide (TiS2), molybdenum sulfide (MoS2), iron sulfide (FeS, FeS2), copper sulfide (CuS), and nickel sulfide (Ni3S2).

[0296] In addition to the above-mentioned positive electrode active material, niobium selenide (NbSe 3 ) or the like can also be used.

[0297] The positive electrode active material can be used alone or in combination of two or more.

[0298] As the negative electrode active material, any negative electrode active material that can promote the battery chemical reaction accompanied by the movement of lithium ions caused by atoms used as atoms that embody ionic conductivity, preferably metals that can form alloys with lithium atoms, their oxides, alloys of the metals and lithium atoms, etc., preferably lithium atoms, can be used without particular limitation. As such a negative electrode active material that can allow lithium ions to be inserted and removed, a substance that is known as a negative electrode active material in the battery field can be used without limitation.

[0299] Examples of such negative electrode active materials include metallic lithium such as metallic lithium, metallic indium, metallic aluminum, metallic silicon, and metallic tin, or metals capable of forming alloys with metallic lithium, oxides of these metals, and alloys of these metals with metallic lithium.

[0300] The electrode active material used in the present embodiment may have a coating layer coated on its surface.

[0301] As a material for forming the coating layer, an atom that exhibits ionic conductivity in the sulfide solid electrolyte, preferably a nitride, an oxide, or an ion conductor such as a composite of lithium atoms, can be cited. Specifically, lithium nitride (Li3N), a Li4GeO4-based structure such as Li 4-2x Zn x Conductors with LISICON crystal structures such as GeO4, and conductors with Li3PO4 skeleton structures such as Li 4-x Ge 1-x P x Conductors with sulfide-LISICON crystal structures such as S4, La 2 / 3- x Li 3x Conductors with a perovskite crystal structure such as TiO3, conductors with a NASICON crystal structure such as LiTi2(PO4)3, etc.

[0302] In addition, Li y Ti 3-y O4(0 <y<3)、Li4Ti5O 12 Lithium titanate (LTO), lithium metal oxides of metals belonging to Group 5 of the periodic table such as LiNbO3, LiTaO3, and oxide-based conductors such as Li2O-B2O3-P2O5, Li2O-B2O3-ZnO, and Li2O-Al2O3-SiO2-P2O5-TiO2.

[0303] The electrode active material having a coating layer is obtained by, for example, attaching a solution containing various atoms constituting a material forming the coating layer to the surface of the electrode active material and calcining the attached electrode active material preferably at 200° C. to 400° C.

[0304] Here, as the solution containing various atoms, for example, a solution containing alkoxides of various metals such as lithium ethoxide, titanium isopropoxide, niobium isopropoxide, tantalum isopropoxide, etc. can be used. At this time, as the solvent, an alcohol solvent such as ethanol and butanol; an aliphatic hydrocarbon solvent such as hexane, heptane, octane; an aromatic hydrocarbon solvent such as benzene, toluene, xylene, etc. can be used.

[0305] In addition, the above-mentioned attachment may be performed by dipping, spraying, or the like.

[0306] From the viewpoint of improving manufacturing efficiency and battery performance, the firing temperature is preferably 200° C. to 400° C., more preferably 250° C. to 390° C., and the firing time is usually about 1 minute to 10 hours, preferably 10 minutes to 4 hours.

[0307] As the coating rate of the coating layer, based on the surface area of ​​the electrode active material, it is preferably more than 90%, more preferably more than 95%, and further preferably 100%, that is, preferably the entire surface is coated. In addition, as the thickness of the coating layer, it is preferably more than 1nm, more preferably more than 2nm, and as the upper limit, it is preferably below 30nm, more preferably below 25nm.

[0308] The thickness of the coating layer can be measured by cross-sectional observation using a transmission electron microscope (TEM), and the coverage can be calculated from the thickness of the coating layer, elemental analysis values, and BET specific surface area.

[0309] (Other ingredients)

[0310] The electrode composite material of this embodiment may include other components such as a conductive material and a binder in addition to the above-mentioned sulfide solid electrolyte glass ceramic and electrode active material. That is, in addition to using the above-mentioned sulfide solid electrolyte glass ceramic and electrode active material, the manufacturing method of the electrode composite material of this embodiment may also use other components such as a conductive material and a binder. For other components such as a conductive agent and a binder, when mixing the above-mentioned sulfide solid electrolyte glass ceramic with the electrode active material, they can be further added to these sulfide solid electrolyte glass ceramics and the electrode active material and mixed for use.

[0311] As conductive materials, from the viewpoint of improving battery performance by improving electron conductivity, examples include artificial graphite, graphite carbon fiber, resin-fired carbon, pyrolysis vapor-grown carbon, coke, mesophase carbon microbeads, furfuryl alcohol resin-fired carbon, polyphenylene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and carbon materials that are difficult to graphitize.

[0312] By using a binder, the strength of the positive electrode and the negative electrode can be improved.

[0313] There are no particular restrictions on the binder as long as it can impart functions such as adhesion and flexibility. Examples include fluorine-based polymers such as polytetrafluoroethylene and polyvinylidene fluoride, thermoplastic elastomers such as butene rubber and styrene-butadiene rubber, acrylic resins, acrylic polyol resins, polyvinyl acetal resins, polyvinyl butyral resins, silicone resins and other resins.

[0314] The blending ratio (mass ratio) of the electrode active material and the sulfide solid electrolyte glass ceramic in the electrode composite material is preferably 99.5:0.5 to 40:60, more preferably 99:1 to 50:50, and further preferably 98:2 to 60:40 in order to improve battery performance and take manufacturing efficiency into consideration.

[0315] When containing a conductive material, the content of the conductive material in the electrode composite material is not particularly limited. If the battery performance is improved and the manufacturing efficiency is taken into consideration, it is preferably 0.5 mass % or more, more preferably 1 mass % or more, and further preferably 1.5 mass % or more. As an upper limit, it is preferably 10 mass % or less, preferably 8 mass % or less, and further preferably 5 mass % or less.

[0316] In addition, when containing a binder, the content of the binder in the electrode composite material is not particularly limited. If the battery performance is improved and the manufacturing efficiency is taken into consideration, it is preferably 1% by mass or more, more preferably 3% by mass or more, and further preferably 5% by mass or more. As an upper limit, it is preferably 20% by mass or less, preferably 15% by mass or less, and further preferably 10% by mass or less.

[0317] 〔Lithium-ion battery〕

[0318] The lithium ion battery of the present embodiment needs to include at least one selected from the sulfide solid electrolyte glass ceramic of the present embodiment and the electrode composite material.

[0319] The lithium-ion battery of the present embodiment is not particularly limited in its structure as long as it is a lithium-ion battery comprising any one of the sulfide solid electrolyte glass ceramics of the present embodiment described above and an electrode composite material comprising the sulfide solid electrolyte glass ceramics, and has the structure of a general lithium-ion battery.

[0320] As the lithium ion battery of the present embodiment, for example, a lithium ion battery having a positive electrode layer, a negative electrode layer, an electrolyte layer and a current collector is preferred. As the positive electrode layer and the negative electrode layer, the positive electrode layer and the negative electrode layer of the electrode composite material of the present embodiment are preferably used, and as the electrolyte layer, the electrolyte layer of the sulfide solid electrolyte glass ceramic of the present embodiment is preferably used.

[0321] As the current collector, any known current collector may be used. For example, a layer obtained by coating a substance that reacts with the above-mentioned solid electrolyte, such as Au, Pt, Al, Ti, or Cu, with Au or the like can be used.

[0322] Example

[0323] Next, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples at all.

[0324] (1) Explain the measurement method.

[0325] (1-1) X-ray diffraction (XRD) measurement (XRD pattern)

[0326] The obtained solid electrolyte was measured by XRD measurement.

[0327] The powder of the solid electrolyte prepared in each example was filled into a groove of 20 mm in diameter and 0.2 mm in depth, and flattened with glass to prepare a sample. The sample was sealed with a kapton film for XRD so as not to be exposed to air, and then measured.

[0328] The powder X-ray diffraction measurement apparatus D2 PHASER manufactured by BRUKER CO., LTD. was used and the measurement was carried out under the following conditions.

[0329] Tube voltage: 30kV

[0330] Tube current: 10mA

[0331] X-ray wavelength: Cu-Kα ray

[0332] Optical system: Concentration method

[0333] Slit composition: Soller slit 4° (same for incident and receiving sides), divergence slit 1mm, Kβ filter (Ni plate 0.5%), air scattering screen (3mm)

[0334] Detector: Semiconductor detector

[0335] Measuring range: 2θ = 10-60 degrees

[0336] Step width, scanning speed: 0.05deg, 0.05deg / sec

[0337] From the obtained XRD pattern, a peak appearing at 2θ=20.2° and a peak appearing at 2θ=29.3° were confirmed.

[0338] That is, a straight line baseline is set for the peak shape obtained by XRD measurement, and the difference between the intensity of each point and the baseline is obtained to prepare an XRD curve. For the peak appearing at 2θ = 20.2°, a straight line baseline is set and subtracted in the range of 19.2 to 20.7°, and the peak maximum value in the range of 20.2±0.3° is taken as the peak intensity. For the area surrounded by the baseline and the curve of the XRD pattern, the peak of the function described later is set at 20.2±0.2° and curve fitting is performed, and the area of ​​the peak thus obtained is taken as the peak area intensity (refer to Figure 2 and Figure 4). In addition, for the peak appearing at 2θ=29.3°, a straight line baseline was set and subtracted in the range of 27.8 to 30.6°, and the peak maximum value in the range of 29.3°±0.3° was taken as the peak intensity. Two peaks of the function described later were set at 28.7±0.2° and 29.3±0.2° and a curve fitting was performed, and the area of ​​the 29.3° peak was taken as the peak area intensity (refer to Figure 3 and Figure 5 ).

[0339] Find the peak intensity (P A ) and peak area intensity (I A ), the peak intensity of the peak appearing at 2θ = 29.3° (P B ) and peak area intensity (I B ), and calculate P based on these values A / P B and I A / I B .

[0340] (1-2) X-ray diffraction (XRD) measurement (crystal size)

[0341] The crystallite size (L) was determined by the method of P. Scherrer et al. Specifically, the crystallite size (L) was determined by calculation using the result measured in the same manner as in (1-1) using the following formula.

[0342] Crystallite size (L) = Kλ / (β·cosθ)

[0343] K: 0.9 was used as a constant.

[0344] λ: (Cu-Kα ray)

[0345] β: Calculated according to β = wB.

[0346] w: The half-width of the 23.6° peak obtained by measurement

[0347] B: Device constant (measured in the same manner as in (1-1) for a standard substance (silicon), and obtained from the peak at 2θ=28.5°: B=0.1497°)

[0348] w (the half width obtained by measurement) is calculated as follows. That is, a straight line baseline is set for the peak shape obtained by XRD measurement (refer to Figure 6 ), obtain the difference between the intensity of each point and the baseline, and make an XRD curve (refer to Figure 7). The XRD curve is set to a formula consisting of a Lorentz function L(x) and a Gaussian function G(x) (f(x) = (1-α) × L(x) + α × G(x)), and the parameters A, w, x0 and α are determined by curve fitting.

[0349] [Number 1]

[0350]

[0351] (1-3) Solid 31 P-NMR measurements

[0352] Device: ECZ400R (manufactured by Japan Electronics Co., Ltd.)

[0353] Observation core: 31 P

[0354] Observation frequency: 161.994MHz

[0355] Measuring temperature: room temperature

[0356] Pulse sequence: Single pulse

[0357] 90° pulse width: 3.2μs

[0358] Waiting time after FID measurement until the next pulse is applied: 60s

[0359] MAS (Magic Angle Spinning) speed: 11kHz

[0360] Total times: 64 times

[0361] Measuring range: 250ppm~-150ppm

[0362] Sample volume: 100 mg

[0363] External standard: NH4H2PO4 (chemical shift 1.00ppm)

[0364] (1-3-1) Case of amorphous sulfide solid electrolyte

[0365] according to 31 The P-NMR spectrum was waveform separated by using the nonlinear least square method to extract the peak signal from each phosphorus-containing structure. The ratio of phosphorus contained in each phosphorus-containing structure among all phosphorus (phosphorus ratio, mol%) was measured. In addition, the chemical shift of each phosphorus-containing structure was waveform separated as shown in Table 1. The area (Sp1, Sp2, etc.) in the table represents the area of ​​the peak after waveform separation.

[0366] [Table 1]

[0367] Table 1

[0368] Attribution Chemical shift (ppm) Functions used for optimization area <![CDATA[PS4 3- Glass]]> 82-85 Gaussian function Sp1 <![CDATA[P2S6 4- Glass]]> 102-108 Gaussian function Sp2 <![CDATA[P2S7 4- Glass]]> 91.4 Gaussian function Sp3

[0369] PS4 3- Phosphorus ratio (%): 100×Sp1 / (Sp1+Sp2+Sp3)

[0370] P2S6 4- Phosphorus ratio (%): 100×Sp2 / (Sp1+Sp2+Sp3)

[0371] P2S7 4- Phosphorus ratio (%): 100×Sp3 / (Sp1+Sp2+Sp3)

[0372] (1-3-2) Crystalline Solid Electrolyte (A)

[0373] Table 2 was used as the chemical shift of each phosphorus-containing structure, and the phosphorus ratio was determined by the method according to (1-3-1).

[0374] [Table 2]

[0375] Table 2

[0376] Attribution Chemical shift (ppm) Functions used for optimization area <![CDATA[P2S7 4- Glass]]> 91.4 Gaussian function Sp1 <![CDATA[P2S7 4- Crystal]]> 90-91 Gaussian function Sp2 <![CDATA[PS4 3- Crystal]]> 86-87.5 Pseudo-Vogt function Sp3

[0377] In addition, P2S7 4- The phosphorus ratio is defined as P2S7 4- The ratio of glassy phosphorus to P2S7 4- The sum of the ratios of crystalline phosphorus.

[0378] Furthermore, it is not possible to fully optimize the PS4 with a pseudo-Vogt function. 3- In the case of crystalline peaks, two pseudo-Vogt functions were used for separation.

[0379] (1-3-3) Case of the sulfide solid electrolyte glass ceramic of the present invention

[0380] Table 3 was used as the chemical shift of each phosphorus-containing structure, and the phosphorus ratio was determined by the method according to (1-3-1).

[0381] [Table 3]

[0382] Table 3

[0383] Attribution Chemical shift (ppm) Functions used for optimization area <![CDATA[P2S6 4- Glass]]> 102-108 Gaussian function Sp1 RII similar crystals① Fixed at the peak position of 88.5-91.7 Gaussian function Sp2 β-like crystal 86-87 Gaussian function Sp3

[0384] (1-4) Ionic conductivity measurement

[0385] In this example, the measurement of ion conductivity was performed as follows.

[0386] The sulfide solid electrolyte is formed into a 10 mm diameter (cross-sectional area S: 0.785 cm 2), round particles with a height (L) of 0.1 to 0-3 cm are used to make a sample. The top and bottom of the sample are taken as electrode terminals, and the AC impedance method is used for measurement at 25°C (frequency range: 1MHz to 100Hz, amplitude: 10mV) to obtain a Cole-Cole plot. Near the right end of the arc observed in the high-frequency side area, the real part Z'(Ω) at the point where -Z"(Ω) is the smallest is taken as the bulk resistance R(Ω) of the electrolyte, and the ionic conductivity σ(S / cm) is calculated according to the following formula.

[0387] R=ρ(L / S)

[0388] σ=1 / ρ

[0389] (1-5) Water resistance evaluation (H2S generation)

[0390] Exposure test device (refer to Figure 8 ) is composed of the following components as main components connected by tubes (not shown): a flask 10 for humidifying nitrogen, a static mixer 20 for mixing humidified nitrogen with non-humidified nitrogen, a dew point meter 30 (M170 / DMT152 manufactured by VAISALA) for measuring the water content of the mixed nitrogen, a double reaction tube 40 for setting a measurement sample, a dew point meter 50 for measuring the water content of nitrogen discharged from the double reaction tube 40, and a hydrogen sulfide measuring device 60 (Model 3000RS manufactured by AMI) for measuring the concentration of hydrogen sulfide contained in the discharged nitrogen. The temperature of the flask 10 is set to 10° C. by a cooling tank 11.

[0391] In addition, the tubes connecting the components use Teflon (registered trademark) tubes with a diameter of 6 mm. Figure 8 The tube labels are omitted and the flow of nitrogen is indicated by arrows instead.

[0392] The evaluation steps are described below.

[0393] In a nitrogen glove box set at a dew point of -80°C, about 0.15 g of a powder sample 41 was weighed, placed inside a reaction tube 40 sandwiched with quartz wool 42, and sealed.

[0394] Nitrogen is supplied from a nitrogen source (not shown) at 0.02 MPa into the apparatus 1. A portion of the supplied nitrogen is supplied to the flask 10 through the two-way branch pipe BP to be humidified. The other portion is directly supplied to the static mixer 20 as unhumidified nitrogen. In addition, the supply amount of nitrogen to the flask 10 is adjusted by a needle valve V.

[0395] The dew point is controlled by adjusting the flow rate of unhumidified nitrogen and humidified nitrogen with a flow meter FM with a needle valve. Specifically, the flow rate of unhumidified nitrogen is set to 800 mL / min, and the flow rate of humidified nitrogen is set to 10 to 30 mL / min, and they are supplied to the static mixer 20 for mixing, and the dew point of the mixed gas (a mixture of unhumidified nitrogen and humidified nitrogen) is confirmed by a dew point meter 30.

[0396] After the dew point was adjusted to -20°C, the three-way stopcock 43 was rotated to allow the mixed gas to flow inside the reaction tube 40 for 2 hours. The amount of hydrogen sulfide contained in the mixed gas that passed through the sample 41 was measured using a hydrogen sulfide measuring device 60. The amount of hydrogen sulfide generated during this period was converted to an amount per 1g of sample and calculated (unit: cc / g). In addition, in order to remove hydrogen sulfide, the measured gas was passed through an alkaline trap 70.

[0397] After the sample is exposed for a predetermined time, the supply of humidified nitrogen is stopped, and the reaction tube 40 is sealed with non-humidified nitrogen.

[0398] (1-6) Determination of composition using inductively coupled plasma (ICP) emission spectrometry

[0399] The powder of the sulfide solid electrolyte was weighed and collected in a vial in an argon atmosphere. A KOH alkaline aqueous solution was added to the vial, and the sample was dissolved while paying attention to the capture of the sulfur component, and appropriately diluted to prepare a measurement solution. The obtained measurement solution was measured using a Paschen Runge ICP-OES device (SPECTROARCOS manufactured by SPECTRO) to determine the composition.

[0400] The standard curve solutions were prepared using 1000 mg / L standard solutions for ICP measurement for Li, P, and S, 1000 mg / L standard solution for ion chromatography for Br, and potassium iodide (special grade reagent) for I.

[0401] Two measurement solutions were prepared for each sulfide solid electrolyte, and four measurements were performed with each measurement solution to calculate the average value. The composition was determined from the average value of the measured values ​​of the two measurement solutions. The ratio of the molar fraction of Li2S (I2Li2S) to the molar fraction of P2S5 (I2P2S5) (I2Li2S / I2P2S5) was calculated from the obtained element ratio.

[0402] (2) Example of Preparation of Lithium Sulfide (Li2S) and Phosphorus Pentasulfide (P2S5)

[0403] (2-1) Example of Preparation of Lithium Sulfide (Li2S)

[0404] (2-1-1) Preparation of Li2S

[0405] As a non-aqueous medium, 303.8 kg of toluene (manufactured by Sumitomo Corporation) obtained by dehydration (measured by a Karl Fischer titrator to confirm that the water content was less than 100 ppm) was added to a 500 L (liter) stainless steel reactor under a nitrogen flow, and then 33.8 kg of anhydrous lithium hydroxide (manufactured by Honjo Chemical Co., Ltd.) was added, and stirred at 131 rpm for 2 hours at 95°C using a twinstir stirring blade to prepare a slurry.

[0406] Then, stirring was continued, hydrogen sulfide (manufactured by Sumitomo Seika Co., Ltd.) was blown into the slurry at a supply rate of 100 L / min, and the temperature was raised to 104°C. A azeotropic gas of water and toluene was continuously discharged from the reactor. The azeotropic gas was condensed by a condenser outside the system to dehydrate. During this period, an amount of toluene equal to the distilled toluene was continuously supplied to keep the reaction liquid level constant.

[0407] The amount of water in the condensate gradually decreased, and no distilled water was observed 24 hours after the introduction of hydrogen sulfide. During the reaction, the solid was dispersed in toluene and stirred, and there was no water separated from the toluene.

[0408] Then, the hydrogen sulfide was switched to nitrogen, and nitrogen was circulated at 100 L / min for 1 hour.

[0409] The obtained solid component was filtered and dried to obtain Li2S as a white powder. 50 It is 412μm.

[0410] (2-1-2) Crushing of Li2S

[0411] The Li2S obtained in (2-1-1) was pulverized in a nitrogen atmosphere using a pin mill (100UPZ manufactured by Hosokawa Micron Co., Ltd.) equipped with a quantitative feeder. The feeding rate was 80 g / min, and the rotation speed of the disk was 18000 rpm.

[0412] D of Li2S after crushing 50 It is 7.7μm.

[0413] (2-2) Example of Preparation of Phosphorus Pentasulfide (P2S5)

[0414] (2-2-1) Crushing of P2S5

[0415] In (2-1-2), P2S5 (manufactured by Thermofos, D 50 =125 μm) was used instead of the Li2S obtained in (2-1-1), and the pulverization was carried out in the same manner.

[0416] D of P2S5 after crushing50 It is 8.7μm.

[0417] (Example 1)

[0418] Process (A)

[0419] 0.488 g (45.947 g / mol, 0.01062 mol) of Li2S produced in (2-1-2), 1.012 g (222.272 g / mol, 0.00455 mol) of P2S5 produced in (2-2-1) and 10 (about 32 g) zirconia balls with a diameter of 10 mm were added to a zirconia can (45 mL) of a planetary ball mill (manufactured by FRITSCH: Model P-7), which was completely sealed to form an argon atmosphere in the can. Without heating or cooling, the rotation speed of the planetary ball mill was set to 370 rpm for 40 hours of treatment (mechanical grinding) to obtain a powder (solid electrolyte (A1)).

[0420] The obtained powder (solid electrolyte (A1)) was measured by X-ray diffraction (XRD) (refer to Fig. 9 ) can be confirmed as an amorphous solid electrolyte.

[0421] Heating (crystallization) process (first time)

[0422] The entire amount of the solid electrolyte (A1) obtained in the step (A) was heated at 300° C. for 3 hours in an electric furnace in a glove box set to an argon atmosphere.

[0423] Then, the mixture was slowly cooled and ground with a mortar in a glove box under an argon atmosphere to obtain a powder (crystalline solid electrolyte (A2)). The results of X-ray diffraction (XRD) measurement are shown in Fig.10 .

[0424] Process (B)

[0425] 1.001 g of the solid electrolyte (A2) obtained in step (A) was weighed, and 0.093 g (0.00202 mol) of Li2S and 0.406 g (133.845 g / mol, 0.00304 mol) of LiI as a lithium halide were added thereto, and an amorphous solid electrolyte (B1) was obtained in the same manner as in the above step (A). The results of X-ray diffraction (XRD) measurement of the amorphous solid electrolyte (B1) are shown in Fig.11 In addition, through solid 31 P-NMR measurement and evaluation of P2S6 4- Phosphorus ratio (see Table 5).

[0426] Heating (crystallization) process

[0427] The entire amount of the amorphous solid electrolyte (B1) obtained in the step (B) was heated at 180° C. for 2 hours using a hot plate in a glove box set to an argon atmosphere.

[0428] Thereafter, the mixture was slowly cooled and pulverized with a mortar in a glove box under an argon atmosphere to obtain a powder (sulfide solid electrolyte glass ceramic (1)).

[0429] The obtained powder was measured by X-ray diffraction (XRD) (refer to Fig.12 ), peaks derived from a crystal structure similar to type II in the sulfide crystalline lithium superion conductor region were observed at 2θ = 20.2°, 23.6°, and 29.3°. Fig.12 It was confirmed that the raw materials of Li2S and LiI were consumed, and it was found that a sulfide solid electrolyte glass ceramic containing less of these raw materials as impurities was obtained.

[0430] (Comparative Example 1)

[0431] An amorphous solid electrolyte (C1) is obtained in the same manner as in the above step (B) of Example 1, except that 0.451 g (0.00981 mol) of Li2S produced in (2-1-2), 0.727 g (0.00327 mol) of P2S5 produced in (2-2-1), 0.109 g (0.00082 mol) of LiI as a lithium halide, and 0.213 g (86.845 g / mol, 0.00245 mol) of LiBr are added.

[0432] Crystallization process

[0433] The entire amount of the obtained amorphous sulfide solid electrolyte (C1) was heated at 190° C. for 2 hours using a hot plate in a glove box set to an argon atmosphere.

[0434] Then, the mixture was slowly cooled and pulverized with a mortar in a glove box under an argon atmosphere to obtain a powder (sulfide solid electrolyte glass ceramic (C1)).

[0435] The obtained powder was measured by X-ray diffraction (XRD) (refer to Fig.13 ), a peak originating from a crystal structure similar to the type II region of sulfide crystalline lithium superion conductor was observed, confirming that it was a sulfide solid electrolyte glass ceramic.

[0436] (Comparative Example 2)

[0437] 1.070 g of the solid electrolyte (A2) obtained by heating the solid electrolyte (A1) obtained in step (A) is weighed, and 0.100 g (0.00218 mol) of Li2S is added thereto, and further 0.109 g (0.00082 mol) of LiI as a lithium halide is added, and further 0.213 g (86.845 g / mol, 0.00245 mol) of LiBr is added. Except for this, the amorphous solid electrolyte (C2) 2 is obtained in the same manner as in the above step (B) of Example 1.

[0438] The entire amount of the obtained amorphous sulfide solid electrolyte (C2) was heated at 180° C. for 2 hours using a hot plate in a glove box set in an argon atmosphere to obtain a sulfide solid electrolyte glass ceramic (C2).

[0439] The obtained powder was subjected to X-ray diffraction (XRD) measurement, and a peak derived from a crystal structure similar to that of the type II region of the sulfide crystalline lithium superion conductor was observed.

[0440] (Comparative Example 3)

[0441] 0.440 g (0.00958 mol) of Li2S produced in (2-1-2), 0.709 g (0.00319 mol) of P2S5 produced in (2-2-1), 0.213 g (0.00159 mol) of LiI as lithium halide, 0.138 g (0.00159 mol) of LiBr, 53 g of zirconia balls with a diameter of 2 mm, and solvent ethylbenzene (5 mL) were added to a zirconia can (45 mL) of a planetary ball mill (manufactured by FRITSCH: Model P-7), which was completely sealed to form an argon atmosphere in the can. The rotation speed of the planetary ball mill was set to 500 rpm without heating and cooling, and the treatment (mechanical grinding) was performed for 40 hours. The obtained slurry was dried at room temperature under vacuum and then heated at 80°C to obtain a powder (amorphous solid electrolyte (C3)).

[0442] The obtained powder was confirmed to be an amorphous solid electrolyte by X-ray diffraction (XRD) measurement.

[0443] Crystallization process

[0444] The entire amount of the obtained amorphous sulfide solid electrolyte (C3) was heated at 203° C. for 2 hours using a hot plate in a glove box set to an argon atmosphere.

[0445] Then, the mixture was slowly cooled and pulverized with a mortar in a glove box under an argon atmosphere to obtain a powder (sulfide solid electrolyte glass ceramic (C3)).

[0446] The obtained powder was subjected to X-ray diffraction (XRD) measurement, and a peak derived from a crystal structure similar to that of the type II region of the sulfide crystalline lithium superion conductor was observed.

[0447] (Examples 2 to 10)

[0448] Sulfide solid electrolyte glass ceramics (2) to (10) were obtained in the same manner as in Example 1, except that the solid electrolyte (A2), Li2S, LiI, LiBr and their amounts used in step (B) of Example 1, and the heating temperature in the crystallization step were set to the contents described in Table 4. In Table 4, electrolyte A2 refers to the amount (g) of the crystalline solid electrolyte (A2) used in step (B). In Comparative Examples 1 and 3, no crystalline solid electrolyte (A2) was used, and Li2S, P2S5 and lithium halide were treated uniformly. Therefore, the amount of electrolyte A2 used was recorded as "-". P2S5 in Table 4 represents the amount of P2S5 used at this time. In Examples 1 to 10 and Comparative Example 2, P2S5 was not used in step (B), so it was recorded as "-".

[0449] In these, similarly to the sulfide solid electrolyte glass ceramic (1), peaks derived from a crystal structure similar to the sulfide crystalline lithium superion conductor region type II were observed at 2θ=20.2°, 23.6°, and 29.3°.

[0450] [Table 4]

[0451] Table 4

[0452]

[0453] Table 4 shows the contents (mol) of sulfur atoms, phosphorus atoms and halogen atoms relative to the content (mol) of lithium atoms of the sulfide solid electrolyte glass ceramics obtained in Examples 1 to 10 and Comparative Examples 1 to 3, calculated from the contents of each element in the raw materials.

[0454] In addition, P A / P B ,I A / I B 、M Br / M I 、P2S6 4 - Phosphorus ratio and I1 Li2S / I1 P2S5 The results are shown in Table 5, and the crystallite size, ion conductivity, and H2S generation amount are shown in Table 6. Blank areas in Tables 5 and 6 indicate that no measurement was performed.

[0455] [Table 5]

[0456] Table 5

[0457]

[0458] [Table 6]

[0459] Table 6

[0460]

[0461] It can be seen that the sulfide solid electrolyte glass ceramics of Examples 1 to 10 have high ionic conductivity and are suitable as materials for lithium ion batteries, etc. In addition, the ratio I1Li2S / I1P2S5 calculated from the content of each element in the raw material and the ratio I2Li2S / I2P2S5 measured using an inductively coupled plasma (ICP) emission spectrometer have composition deviations of 9.1% and 5.6% in Examples 1 and 8, respectively, but the deviation is about 2% in other examples, and it is confirmed that it is roughly consistent with the ratio in the raw material. Therefore, it is confirmed that according to the manufacturing method of this embodiment, lithium sulfide (Li2S) and phosphorus sulfide (P2S5), as well as solid electrolytes (A) and (B) obtained from raw materials containing them, can be effectively utilized, and sulfide solid electrolyte glass ceramics with high ionic conductivity can be obtained.

[0462] The sulfide solid electrolyte glass ceramic (C1) of Comparative Example 1 is different from the sulfide solid electrolyte glass ceramic of the present embodiment in that it is produced by a production method that does not include step (A). A / P B The sulfide solid electrolyte glass ceramic (C1) has a lower ionic conductivity than the sulfide solid electrolyte glass ceramic of the embodiment. It can be seen that if P A / P B If it is less than 1.0, the effect of the present invention will not be achieved.

[0463] The sulfide solid electrolyte glass ceramic (C2) of Comparative Example 2 is prepared by changing the amount of LiI and LiBr used. A / P B becomes 0.7, confirming that the sulfide solid electrolyte glass ceramic (C2) has lower ion conductivity than the sulfide solid electrolyte glass ceramic of the embodiment. In addition, it is known that in Comparative Example 2, although step (A) is included, P A / P B Since the value is 1.0 or less, the crystallite size does not increase.

[0464] Since the amount of LiI and LiBr used in the sulfide solid electrolyte glass ceramic (C3) of Comparative Example 3 was adjusted, P A / P B is 1.0, because P A / P BThe ion conductivity is low because the sulfide solid electrolyte glass ceramic (C3) of Comparative Example 3 is higher than that of the sulfide solid electrolyte glass ceramics of Examples 2 to 4. 4- The phosphorus ratio is high and the amount of H2S produced is poor.

[0465] Furthermore, it was confirmed that the sulfide solid electrolyte glass ceramics of Examples 1 to 10 were smaller than the sulfide solid electrolyte glass ceramics of Comparative Examples 1 to 3, and the generation of H 2 S was suppressed.

[0466] Industrial Applicability

[0467] According to this embodiment, a crystalline sulfide solid electrolyte having high ion conductivity and excellent battery performance can be produced. The crystalline sulfide solid electrolyte obtained by the production method of this embodiment is suitable for lithium ion batteries, especially batteries used in information-related devices or communication devices such as personal computers, video cameras and mobile phones.

Claims

1. A sulfide solid electrolyte glass ceramic, characterized in that: Contains lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms, In the X-ray diffraction measurement using CuKα rays, there are peaks at diffraction angles (2θ) of 20.2° and 29.3°, and the peak intensity (P A ) and the peak intensity (P B ) intensity ratio value (P A / P B ) exceeds 1.0, and the crystallite size is greater than 30 nm.

2. The sulfide solid electrolyte glass ceramic according to claim 1, characterized in that: The peak area intensity (I A ) and the peak area intensity (I B ) intensity ratio value (I A / I B ) is greater than 0.

78.

3. The sulfide solid electrolyte glass ceramic according to claim 1 or 2, characterized in that: It also has a peak at 2θ=23.6°.

4. The sulfide solid electrolyte glass ceramic according to any one of claims 1 to 3, characterized in that An iodine atom is included as the halogen atom.

5. The sulfide solid electrolyte glass ceramic according to claim 4, characterized in that: A bromine atom is also included as the halogen atom.

6. The sulfide solid electrolyte glass ceramic according to claim 5, characterized in that: The content of bromine atoms (M) contained in the sulfide solid electrolyte glass ceramic Br mol) and the content of iodine atoms (M I mol) satisfies M Br / M I The relationship is ≤1.

00.

7. The sulfide solid electrolyte glass ceramic according to any one of claims 1 to 6, characterized in that According to solid 31 P2S6 determined by P-NMR measurement 4- The phosphorus ratio is 7.5 mol % or less.

8. The sulfide solid electrolyte glass ceramic according to any one of claims 1 to 7, characterized in that The molar fraction of Li2S (I 1 Li2S ) and the molar fraction of P2S5 (I 1 P2S5 ) ratio (I1 Li2S / I 1 P2S5 ) is greater than 2.60 and less than 3.

30.

9. The sulfide solid electrolyte glass ceramic according to any one of claims 1 to 8, characterized in that The molar fraction of Li2S (I 2 Li2S ) and the molar fraction of P2S5 (I 2 P2S5 ) ratio (I2 Li2S / I 2 P2S5 ) is greater than 2.60 and less than 3.

30.

10. The sulfide solid electrolyte glass ceramic according to any one of claims 1 to 9, characterized in that The ratio of the content (mol) of lithium atoms, the content (mol) of phosphorus atoms, the content (mol) of sulfur atoms and the content (mol) of halogen atoms, that is, the content ratio is lithium atoms:phosphorus atoms:sulfur atoms:halogen atoms = (3.20~3.70):(0.70~1.30):(3.00~5.00):(0.20~0.70).

11. The sulfide solid electrolyte glass ceramic according to any one of claims 1 to 10, characterized in that: Contains type II crystal structure of sulfide crystalline lithium superion conductor region.

12. A method for producing a sulfide solid electrolyte glass ceramic, the method for producing a sulfide solid electrolyte glass ceramic according to any one of claims 1 to 11, characterized in that: include: A solid electrolyte (A) is obtained by treating lithium sulfide (Li2S) and phosphorus sulfide (P2S5) by at least one selected from stirring, mixing and pulverizing; The solid electrolyte (A) and the lithium halide are treated by at least one selected from stirring, mixing and pulverizing to obtain a solid electrolyte (B).

13. The method for producing a sulfide solid electrolyte glass ceramic according to claim 12, wherein: Also included is heating the solid electrolyte (A).

14. The method for producing a sulfide solid electrolyte glass ceramic according to claim 12 or 13, characterized in that: Also included is heating the solid electrolyte (B).

15. The method for producing a sulfide solid electrolyte glass ceramic according to any one of claims 12 to 14, characterized in that: The solid electrolyte (B) is 31 P2S6 determined by P-NMR measurement 4- The phosphorus ratio is 15.0 mol % or less.

16. An electrode composite material, characterized in that: A sulfide solid electrolyte glass ceramic comprising the sulfide solid electrolyte glass ceramic according to any one of claims 1 to 11 and an electrode active material.

17. A lithium ion battery, characterized in that: Contains at least one of the sulfide solid electrolyte glass ceramic according to any one of claims 1 to 11 and the electrode composite material according to claim 16.

Citation Information

Patent Citations

  • Sulfide solid electrolytic material, lithium solid battery, and manufacturing method of sulfide solid electrolytic material