Semiconductor device and power conversion apparatus
The semiconductor device's grooved structure addresses thermal resistance and bonding reliability issues by guiding exhaust gases, enabling larger chip sizes and thinner designs with improved heat dissipation.
Patent Information
- Application Number
- CN202280093968.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2022-11-24
- Publication Date
- 2024-12-06
AI Technical Summary
Existing semiconductor devices face challenges in reducing thermal resistance and ensuring bonding reliability as chip size increases and thickness decreases, leading to issues with heat dissipation and chip warping.
A semiconductor device structure featuring a wiring layer with grooves extending from the semiconductor chip mounting area, where a sintered metal layer is formed within and outside the grooves, with varying depths and widths to facilitate gas exhaust and reduce thermal resistance.
The proposed structure effectively reduces thermal resistance and improves bonding reliability by guiding exhaust gases out of the bonding layer, allowing for larger chip sizes and thinner designs while maintaining reliability.
Smart Images

Figure CN119096338A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a semiconductor device and a power conversion apparatus. Background Art
[0002] As power conversion devices that perform power conversion and control functions in electric vehicles, railway vehicles, power generation systems, etc., semiconductor devices such as IGBT (Insulated Gate Bipolar Transistor) or MOSFET (Metal-Oxide-Semiconductor Field-Effect Transistor) are used. When the semiconductor device is working, the semiconductor chip becomes hot due to self-heating, so ensuring reliability against heat load becomes a problem. In order to meet this requirement, as a technology for improving heat dissipation performance, for example, the technology described in patent documents 1-3 is known.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-103180
[0006] Patent Document 2: International Publication No. 2017 / 002793
[0007] Patent Document 3: Japanese Patent Application Publication No. 2017-092168 Summary of the invention
[0008] Technical problem to be solved by the invention
[0009] The technology described in the above-mentioned patent document 1 is a method for providing a copper paste for non-pressurized bonding, which can obtain sufficient bonding strength even when parts with different thermal expansion coefficients are bonded without pressure, and the copper paste contains metal particles and a dispersant, the metal particles contain submicron copper particles with a volume average particle size of 0.01 μm or more and 0.8 μm or less, and micron copper particles with a volume average particle size of 2.0 μm or more and 50 μm or less, and the dispersant contains a solvent with a boiling point of 300°C or more, and the content of the solvent with a boiling point of 300°C or more is 2% by mass or more based on the total mass of the copper paste for non-pressurized bonding. In the solvent drying process, the porosity of the porous structure, which causes insufficient strength and / or increased thermal resistance of the bonding part, is reduced by ensuring the movement and deformation of the copper particles, and micro cracks are suppressed. It is generally believed that it is effective when the size of the semiconductor chip reaches a few millimeters square, but low-pressure pressurization must be performed when the chip size reaches 10 mm square. In order to deal with uneven coating, the coating thickness is increased, and the amount of gas discharged from the solvent increases, so it is necessary to pressurize with low pressure to prevent the chip from floating. In addition, a flow path for gas to be discharged from the coating layer in the center of the chip is formed, making it difficult to reduce thermal resistance.
[0010] In the technology described in the above-mentioned patent documents 2-3, a recess is arranged on the electrode surface bonded to the semiconductor chip so that when the coating thickness of the sintered metal paste is increased, the paste will not overflow from the outer edge of the chip and become unbonded peeling foreign matter, and the anchoring effect of the recess is used to improve the reliability of the bonding strength. The gas discharged from the solvent is connected to the thicker coating layer to form a flow path and is discharged to the outside, which makes it difficult to adapt to the large area of the chip and reduce the thermal resistance. In addition, as the chip area is further enlarged, the chip thickness also reaches less than 100μm, so low-pressure pressurization is required.
[0011] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a technology capable of reducing the thermal resistance of a sintered metal joint portion adapted to the increase in chip size and the decrease in thickness of a semiconductor chip.
[0012] Technical means of solving problems
[0013] In order to solve the above-mentioned problems, the present invention adopts the following structure.
[0014] A technology is provided, characterized in that it includes: a wiring layer; a semiconductor chip; and a sintered metal layer, which joins the semiconductor chip to the wiring layer, wherein the wiring layer has a groove extending from a semiconductor chip mounting area on which the semiconductor chip is mounted to the outside of the semiconductor chip mounting area, and in the semiconductor chip mounting area, the sintered metal layer is formed inside the groove and on the outside of the upper end of the groove, and the sintered metal layer is also formed in the groove formed on the outside of the semiconductor chip mounting area, and the depth of the groove is different near the center of the semiconductor chip mounting area and near the end of the semiconductor chip mounting area.
[0015] Effects of the Invention
[0016] According to the present invention, it is possible to provide a technique capable of reducing the thermal resistance of a sintered metal joint portion adapted to the increase in chip size and the reduction in thickness of a semiconductor chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a schematic cross-sectional view showing a main part of the semiconductor device according to the first embodiment.
[0018] Figure 2a It is a plan view showing a main part of the semiconductor device in the first embodiment.
[0019] Figure 2b It is a cross-sectional view taken along line BB of a main portion of the semiconductor device in the first embodiment.
[0020] Figure 2c It is a cross-sectional view taken along line CC of a main portion of the semiconductor device in the first embodiment.
[0021] Figure 2d Yes Description Figure 2a A top view of the mounting area of the semiconductor chip 1 is shown.
[0022] Figure 3 This is an enlarged cross-sectional view of a portion D of a main part of the semiconductor device in the first embodiment.
[0023] Figure 4 This is an enlarged cross-sectional view of a portion D of a main part of the semiconductor device in the second embodiment.
[0024] Figure 5 It is a cross-sectional view taken along line BB of a main portion of the semiconductor device in the modification of the first embodiment.
[0025] Figure 6a It is a cross-sectional view of the heat conduction analysis model of the first embodiment.
[0026] Figure 6bIt is an enlarged cross-sectional view of the E portion of the heat conduction analysis model of the first embodiment.
[0027] Figure 6c This is a cross-sectional temperature distribution diagram of the first embodiment.
[0028] Figure 7 It is a thermal resistance comparison graph of the thermal conductivity analysis result of the first embodiment.
[0029] Figure 8 1 is a circuit diagram showing an embodiment of a power conversion apparatus using the semiconductor device according to the first embodiment and the second embodiment. DETAILED DESCRIPTION
[0030] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings as appropriate. However, the present invention is not limited to the embodiments described herein, and can be appropriately combined and improved within the scope of not changing the main purpose. In addition, in the following description, the same components are marked with the same symbols, and repeated descriptions are sometimes omitted. In addition, in order to make the description clearer, the accompanying drawings are schematically represented compared with the actual form, but this is only an example and does not limit the interpretation of the present invention.
[0031] 《First Implementation Mode》
[0032] Figure 1 1 is a schematic cross-sectional view showing a main part of a semiconductor device in a first embodiment of the present invention. Figure 1 As shown, the semiconductor device 10 is a semiconductor device used in a power conversion device for power conversion and control in electric vehicles, railway vehicles, power generation systems, etc., and has a laminated structure in which a semiconductor chip 1, a circuit board (substrate) 11, and a base plate 7 are bonded to each other. Figure 1 Although not shown in the figure, a plurality of circuit boards 11 may be mounted on one base plate 7 .
[0033] The semiconductor chip 1 is, for example, a power transistor such as an IGBT (Insulated Gate Bipolar Transistor) or a MOSFET (metal-oxide-semiconductor field-effect transistor) or a diode, and is made of, for example, silicon Si, silicon carbide SiC, gallium nitride GaN, or the like.
[0034] The circuit board 11 is composed of a first metal layer (also called a wiring layer) 3, an insulating layer 4, and a second metal layer 5. The first metal layer 3 has the function of a wiring layer of an electrode pattern for a circuit, and the material is preferably copper (Cu), copper (Cu) alloy, aluminum (Al), aluminum (Al) alloy, etc. with good electrical and thermal conductivity. The second metal layer 5 has the function of a heat diffusion plate, and the material is also, for example, Cu and / or Cu alloy, Al, Al alloy, etc. The insulating layer 4 is preferably made of a material with high insulation and thermal conductivity, such as ceramics such as aluminum nitride, aluminum oxide, and silicon nitride. The bottom plate 7 has the function of a heat dissipation surface for dissipating heat to the outside, and is preferably made of a material with high rigidity and thermal conductivity. Cu, Cu alloy, Al, Al alloy, a composite material of aluminum and silicon carbide (AlSiC), a composite material of magnesium and silicon carbide (MgSiC), etc. can be used.
[0035] The semiconductor device 10 has a chip bonding layer (also called a sintered metal layer) 2 between the semiconductor chip 1 and the first metal layer 3 of the circuit board 11, and a base plate bonding layer 6 between the circuit board 11 and the base plate 7. As the chip bonding layer 2, a material with high thermal conductivity and high heat resistance, such as a sintered bonding material of copper (Cu) nanoparticles and / or silver (Ag) nanoparticles, is used. As the base plate bonding layer 6, a material with high thermal conductivity, such as solder with lead Pb or tin Sn as the main component, is used.
[0036] The first metal layer 3 is a part of the circuit and is electrically connected to the semiconductor chip 1 and a terminal for electrical connection with the outside. The semiconductor device 10 is housed in a highly insulating resin case or the like, and the interior of the resin case is sealed with resin or silicone.
[0037] Figure 2a It is a plan view showing a main part of the semiconductor device in the first embodiment of the present invention. Figure 2b yes Figure 2a The cross-sectional view on line BB is shown. Figure 2c yes Figure 2a Cross-sectional view along line CC shown. Figure 2d Yes Description Figure 2a FIG. 1 is a top view of the mounting area RCH of the semiconductor chip.
[0038] like Figure 1 , Figure 2a , Figure 2b , Figure 2c As shown, a bonding area for bonding the semiconductor chip 1 (also referred to as the mounting area RCH of the semiconductor chip 1 or the semiconductor chip mounting area RCH) is provided on the front side of the first metal layer 3 of the circuit board 11. In the bonding area (mounting area RCH) on the front side of the first metal layer 3, a plurality of grooves 8 formed by machining, pressing, or etching are provided. Figure 2aAs shown in FIG. 1 , the length Ly8 of the groove 8 is formed to extend from the outer edge 10E of the semiconductor chip 1. That is, the wiring layer of the circuit board 11, that is, the first metal layer 3, has a plurality of grooves 8 extending from the mounting region RCH of the semiconductor chip 1 to the outer side RO of the mounting region RCH of the semiconductor chip 1. In the mounting region RCH of the semiconductor chip 1, the chip bonding layer 2 and the thin bonding layer 12 (see FIG. 1 ) as a sintered metal layer are formed inside the groove 8 and outside the upper end of the groove 8. Figure 2b , Figure 2c ) The die bonding layer 2 as a sintered metal layer is also formed in the groove 8 formed outside RO of the mounting region RCH of the semiconductor chip 1 .
[0039] like Figure 2a As shown, the semiconductor chip 1 is in a rectangular shape with four sides (OE1 to OE4) when viewed from above. The outer edge 1OE of the semiconductor chip 1 has a first side OE1 set along a first direction X, a second side OE2 opposite to the first side OE1, a third side OE3 set between the first side OE1 and the second side OE2, and a fourth side OE4 opposite to the third side OE3. The third side OE3 and the fourth side OE4 are set along a second direction Y intersecting the first direction X. The mounting area RCH of the semiconductor chip 1 set in the first metal layer 3 is the same area as the inner rectangular area surrounded by the first side OE1 to the fourth side OE4 of the semiconductor chip 1 when viewed from above.
[0040] The length of the first side OE1 and the second side OE2 is Lx1, and the length of the third side OE3 and the fourth side OE4 is Ly1. That is, the plurality of grooves 8 are arranged side by side in the first direction X on the front side of the first metal layer 3, and the plurality of metal grooves 8 are respectively arranged to extend in the second direction Y. The length Ly8 of the groove 8 along the second direction Y is formed to be longer than the length Ly1 of the third side OE3 and / or the fourth side OE4 of the semiconductor chip 1 along the second direction Y (Ly8>Ly1). Figure 2a In the structural example of the groove 8 shown, the length Ly8 of the groove 8 is the length obtained by adding the length (Ly1) of the third side OE3 and / or the fourth side OE4 of the semiconductor chip 1, the length (Ly81) of the lower side of the groove 8 extending from the first side OE1 of the semiconductor chip 1, and the length (Ly82) of the upper side of the groove 8 extending from the second side OE2 of the semiconductor chip 1 (Ly8=Ly1+Ly81+Ly82). Ly81 and Ly82 are equal lengths in this example (Ly81=Ly82). In addition, Ly81 and Ly82 may also be different lengths (Ly81≠Ly82). The width W8 of the plurality of grooves 8 along the first direction X is the same width in this example. In addition, the width W8 of the plurality of grooves 8 along the first direction X may also be different.
[0041] Here, use Figure 2d The mounting region RCH of the semiconductor chip 1 will be described. Figure 2d Corresponding to Figure 2a The top view of FIG. 1 is a simplified top view in which the semiconductor chip 1 and the chip bonding layer 2 are removed. Figure 2d In the figure, the mounting area RCH of the semiconductor chip 1 is an area surrounded by a rectangular dotted line, and has a first side RCH1 set along a first direction X, a second side RCH2 opposite to the first side RCH1, a third side RCH3 set between the first side RCH1 and the second side RCH2, and a fourth side RCH4 opposite to the third side RCH3. The third side RCH3 and the fourth side RCH4 are set along a second direction Y intersecting the first direction X.
[0042] The mounting region RCH of the semiconductor chip 1 includes a central vicinity RCEx of the mounting region RCH and a pair of end vicinities ROEx provided at both side ends of the mounting region RCH in the first direction X. The outer side of the end vicinity ROEx of the mounting region RCH is indicated as ROx. No groove 8 is provided in the outer side ROx.
[0043] In addition, the mounting region RCH of the semiconductor chip 1 has a central vicinity RCEy of the mounting region RCH and a pair of end vicinities ROEy provided at both side ends of the mounting region RCH in the second direction Y. The outer side of the end vicinity ROEy of the mounting region RCH is represented as ROy. The extended portion of the groove 8 (the portion extending by a length Ly81 and the portion extending by a length Ly82) is provided on the outer side ROy.
[0044] use Figure 2b The depth of the plurality of grooves 8 in the first direction X is described. Figure 2b As shown, the groove 8 is formed on the front side of the first metal layer 3 so that the depth d of the groove 8 is different between the center vicinity RCEx of the mounting region RCH of the semiconductor chip 1 and the end vicinity ROEx of the mounting region RCH of the semiconductor chip 1 . Figure 2bTen grooves 8 are typically drawn. The depths d1 and d10 of the grooves 8 provided near the end ROEx are shallower than the depths d5 and d6 of the grooves 8 provided near the center RCEx (d1, d10 < d5, d6). In this example, the depth d of the groove 8 is set such that d1 < d2 < d3 < d4 < d5 and d6 > d7 > d8 > d9 > d10. That is, the depths d1 and d10 of the grooves 8 provided near the end ROEx are made shallower, and the depths d5 and d6 of the grooves 8 provided near the center RCEx are made deeper than d1 and d10. It is configured such that the depth of the groove 8 provided near the center RCEx is the deepest, and as going from near the center RCEx to near the end ROEx, the depth of the groove 8 gradually becomes shallower. The depths d5 and d6 of the grooves 8 provided near the center RCEx may be the same depth (d5 = d6), or the depths d5 and d6 may be different depths (d5 ≠ d6).
[0045] Figure 3 is Figure 2b an enlarged view of part D shown in. As Figure 3 shown, grooves 80 and 81 with different depths d2 and d3 are provided.
[0046] Use Figure 2b to illustrate the depth of the groove 8 in the second direction Y. As Figure 2c shown, in any groove 8, the depth dy3 of the groove 8 at the lower part of the central portion of the semiconductor chip 1 (i.e., near the center RCEy of the mounting area RCH of the semiconductor chip 1) is the deepest, and from the depths dy2 and dy4 of the groove 8 at the outer edge portion of the semiconductor chip 1 (i.e., near the end ROEy of the mounting area RCH of the semiconductor chip 1) to the outside of the semiconductor chip 1 (i.e., outside ROy of the mounting area RCH of the semiconductor chip 1), the depths dy1 and dy5 of the groove 8 gradually become shallower (d3 > (dy2, dy4) > (dy1, dy5)).
[0047] As Figure 2b , Figure 2c shown, the remaining area of the first metal layer 3 where the groove 8 is not formed is the front surface of the flat first metal layer 3, and the front surface of the flat first metal layer 3 and the back surface of the semiconductor chip 1 are joined by a thin bonding layer 12. The width W8 of the groove 8 is, for example, 200 μm or less, and the depth d (d1 to d10, dy1 to dy5) of the groove 8 is, for example, 200 μm or less. The thickness of the thin bonding layer 12 is, for example, about 20 μm.
[0048] The semiconductor device 10 in the first embodiment of the present invention is constructed as described above. Generally speaking, when the chip bonding layer is a sintered body containing a plurality of metal crystal grains, it becomes a porous structure. When the size and density of the pores increase, microcracks are easily generated in the bonding process during manufacturing. If used in a high temperature environment of 175 to 300°C, the bonding reliability will be reduced, the heat transfer path in the bonding layer will also be cut off, and the thermal resistance will increase.
[0049] The chip bonding layer 2 and the thin bonding layer 12 are formed as follows: metal nanoparticles such as Ag nanoparticles covered with an organic protective film are dispersed in an organic component to form a slurry to obtain a sintered bonding material (also called bonding material slurry), and the sintered bonding material is applied between the first metal layer 3 and the back of the semiconductor chip 1 by screen printing or the like, and a plurality of metal nanoparticles are sintered and bonded by heating at the required bonding temperature while applying pressure. When copper oxide particles are used to remove the oxide film and generate nanoparticles, it is preferred to use a sintered bonding material containing a reducing agent that can volatilize at the bonding temperature (60°C). The volatilization process of the reducing agent and the exhaust path of the exhaust gas generated in the sintering reaction process are the causes of the increase in pores.
[0050] In the semiconductor device 10 of the first embodiment of the present invention, the excess portion of the bonding material paste is allowed to retreat into the groove 8 under low pressure to form a thin bonding layer 12, and the exhaust gas OG generated in the volatilization process of the reducing agent and the sintering reaction process is easily guided to the outside ROy of the mounting area RCH of the semiconductor chip 1 through the groove 8 (refer to Figure 2c ), thereby reducing the pores in the thin bonding layer 12 and reducing the density. As a result, the bonding reliability in a high temperature environment such as 175 to 300° C. can be improved, and the thermal resistance in the bonding layer (2, 12) can be reduced.
[0051] The groove 8 is preferably formed by cutting using a diamond blade saw, for example. In this case, a sintered film is formed in the cutting marks formed on the sidewalls of the groove 8, and an anchoring effect can be obtained. Thus, the interface peeling of the chip bonding layer 2 formed in the groove 8 can be suppressed, and the chip size of the semiconductor chip 1 can be adapted to be larger.
[0052] By forming a deeper groove 8 under the center of the semiconductor chip 1 (RCEx, RCEy near the center of the mounting area RCH of the semiconductor chip 1), it is possible to ensure the storage amount of the excess bonding material paste and to alleviate the stress on the semiconductor chip 1 when cooling from the sintering temperature of 300°C to room temperature. In addition, it is possible to use a base plate 7 without warping.
[0053] (Variation Example)
[0054] Figure 5BB is a cross-sectional view of a main part of a semiconductor device in a modification of the first embodiment. Figure 5 The depth d and width W of the plurality of grooves 8 in the first direction X are described. In this modification, the depth d and width W of the grooves 8 in the second direction Y are Figure 2c Same as described in .
[0055] Figure 5 In Figure 2b The grooves 82, 83, 84, 85, and 86 are provided so that the width W8 of the plurality of grooves 8 gradually increases from the lower part of the central part (near the center RCEx) to the outer edge (near the end ROEx) of the semiconductor chip 1 (the width W82 of the groove 82> the width W83 of the groove 83> the width W84 of the groove 84> the width W85 of the groove 85> the width W86 of the groove 86). On the other hand, the grooves 82, 83, 84, 85, and 86 are provided so that the depth d of the plurality of grooves 8 gradually decreases from the lower part of the central part (near the center RCEx) to the outer edge (near the end ROEx) of the semiconductor chip 1 (the depth d82 of the groove 82< the depth d83 of the groove 83< the depth d84 of the groove 84< the depth d85 of the groove 85< the depth d86 of the groove 86).
[0056] That is, the modified example is configured such that the width W of each of the plurality of grooves (82, 83, 84, 85, 86) satisfies in the first direction X: the width W of the groove near the center RCEx is the narrowest (the width W86 of the groove 86), and the width W of the groove gradually becomes wider as it goes from the center RCEx to the end ROEx. On the other hand, the depth d of each of the plurality of grooves (82, 83, 84, 85, 86) satisfies in the first direction: the depth of the groove near the center RCEx is the deepest (the depth d86 of the groove 86), and the depth d gradually becomes shallower as it goes from the center RCEx to the end ROEx. Furthermore, the depth of each of the plurality of grooves 8 satisfies in the second direction Y: the depth near the center RCEx is the deepest, and the depth d gradually becomes shallower as it goes from the center RCEx to the outer side OE of the semiconductor chip mounting area RCH (refer to Figure 2c ).
[0057] As a result, the area of the thin bonding layer 12 can be expanded in the lower part of the central part of the semiconductor chip 1 (near the center RCEx), reducing the thermal resistance at the heat center. In addition, by providing a deeper groove 86, it is possible to ensure that the excess amount of bonding material slurry is accommodated, and at the same time, the exhaust flow path of the exhaust gas OG is ensured. Figure 2c The exhaust gas OG is exhausted in the direction of the arrow shown.
[0058] The effect of the present invention is verified using thermal conductivity analysis technology. Figure 6a is with Figure 1 Cross-sectional view of the thermal analysis model corresponding to the main parts of the semiconductor device. Figure 6b yes Figure 6a An enlarged view of section E is shown. Figure 6c is a cross-sectional temperature distribution diagram of the first embodiment. Figure 5 As described, the width and depth of the groove 8 are changed from the center to the outer edge of the chip. Assume that the semiconductor chip 1 is Si, the chip size is 20 mm square, the thickness is 0.08 mm, the thickness of the thin bonding layer 12 is 0.02 mm, the thermal conductivity is 200 W / mK, and the thermal conductivity of the bonding layer 2 filled in the groove 8 is equivalent to solder, which is 23.4 W / mK. Assume that the size of the first metal layer 3 and the second metal layer is 40 mm square, the thickness is 0.5 mm, and the thermal conductivity is 396 W / mK equivalent to copper. Assume that the thickness of the insulating layer 4 is 0.32 mm, and the thermal conductivity is 80 W / mK equivalent to silicon nitride ceramics. Assume that the thickness of the bottom plate bonding layer 6 is 0.2 mm, and the thermal conductivity is 23.4 W / mK equivalent to solder.
[0059] The thickness of the bottom plate 7 is 3 mm, and the thermal conductivity is 396 W / mK, which is equivalent to copper. The heat transfer boundary condition (heat transfer rate 30000 W / m2K) is set for the heat dissipation surface of the bottom plate 7, and the other parts are heat-insulated. The semiconductor chip 1 is heated uniformly at 1 kW. The temperature distribution at this time is Figure 6c . Figure 6c Represents isotherms. Figure 6c In the example, the temperature T1 near the center of the semiconductor chip 1 is in the temperature range of about 61°C to 56°C, the temperature T2 near the end of the semiconductor chip 1 is in the temperature range of about 38°C to 30°C, and the temperature T3 near the end of the first metal layer 3 is in the temperature range of about 15°C to 7°C. Figure 6a At the thermal resistance evaluation position 9 shown, the thermal resistance of the bonding layer 12 is evaluated based on the temperature difference from the semiconductor chip 1 to the bottom surface of the first metal layer 3 .
[0060] Figure 7 This is a comparison graph of thermal resistances of the thermal conductivity analysis results of the first embodiment. Figure 7 is Figure 6a At the thermal resistance evaluation position 9 shown, the thermal resistance of the die bonding layer 12 is evaluated based on the temperature difference from the front surface of the semiconductor chip 1 to the bottom surface of the first metal layer 3 at the center of the semiconductor chip 1 . Figure 7 In FIG. 8 , the vertical axis represents the thermal resistance Rth (K / kW) between chip electrodes (between semiconductor chip 1 and first metal layer 3 ), and the horizontal axis represents the width W (mm) of groove 8 . Figure 7 The results of analyzing the present invention (71) and comparative examples 1-6 are shown in FIG.
[0061] Here, the chip bonding layer 12 of Comparative Example 1 (72) is a grooveless solder bonding (thickness 0.1 mm). The chip bonding layer 12 of Comparative Example 2 (73) is a grooveless sintering bonding (thickness 0.2 mm, thermal conductivity 100 W / mK). As comparative examples with grooves and uniform groove width and depth, Comparative Examples 3-6 were adopted. The depth of the groove in Comparative Example 3 (74) was 0.08 mm. The depth of the groove in Comparative Example 4 (75) was 0.12 mm. The depth of the groove in Comparative Example 5 (76) was 0.16 mm. The depth of the groove in Comparative Example 6 (77) was 0.20 mm. Therefore, it can be seen that according to the present invention (71), the thermal resistance between chip electrodes can be reduced.
[0062] Second Implementation Method
[0063] Figure 4 is Figure 2b The schematic configuration diagram of the second embodiment is shown in the enlarged view of the D portion of FIG. In the second embodiment, the inclined surface 31 is provided on the side of the grooves 80 and 81 near the semiconductor chip 1 .
[0064] According to the second embodiment, the bonding slurry of the bonding layers 2, 12, etc. during manufacturing can be easily evacuated. In addition, stress concentration before and after the heating process can be suppressed. Furthermore, cracks in the semiconductor chip 1 can be prevented. The method for forming the groove 8 is preferably cutting processing using a diamond blade saw (Dual type). In this case, by first forming a V-shaped groove and then processing it into a deep groove, grooves 80, 81 having an inclined surface 31 on one side near the semiconductor chip 1 can be formed. A sintered film will be formed in the cutting marks formed on the side walls of the grooves 80, 81, and an anchoring effect can be obtained.
[0065] 《Third Implementation Mode》
[0066] Figure 8 1 is a circuit diagram showing an embodiment of a power conversion device 30 using the semiconductor device 10 of the first embodiment and the second embodiment. The power conversion device 30 includes a plurality of semiconductor devices 10, and waveform signals of different timings are input to the gates of at least two of them. The semiconductor device 10 includes two IGBT power transistors in this example. An inverter device is shown in the circuit of this example, but in addition to the inverter device, it can also be applied to a power conversion device 30 of a motor or the like. The power conversion device 30 including the inverter device and the motor can be installed in a high-speed vehicle and an electric vehicle as their power source. By applying the semiconductor device 10 of the first embodiment and the second embodiment to the power conversion device 30, the thermal resistance of the sintered metal joint portion adapted to the enlarged chip size and thinned chip size of the semiconductor chip 1 can be reduced, so that a power conversion device 30 with an improved rated current can be provided, and long-term reliability can be ensured.
[0067] As mentioned above, the invention made by the present inventors has been specifically described based on the embodiments. However, the present invention is not limited to the above-mentioned embodiment and embodiments, and various modifications can be made.
[0068] Description of Reference Numerals
[0069] 1: semiconductor chip, 2: chip bonding layer (sintered metal layer), 3: first metal layer (wiring layer), 4: insulating layer, 5: second metal layer, 6: base plate bonding layer, 7: base plate, 8, 80, 81, 82, 83, 84, 85, 86: groove, 9: thermal resistance evaluation position, 10: semiconductor device, 11: circuit board, 12: thin bonding layer, 30: power conversion device, 31: inclined surface.
Claims
1. A semiconductor device, characterized in that: include: Wiring layer; Semiconductor chips; and a sintered metal layer that bonds the semiconductor chip to the wiring layer, wherein The wiring layer has a groove extending from a semiconductor chip mounting region where the semiconductor chip is mounted to the outside of the semiconductor chip mounting region. The sintered metal layer is formed inside the groove and outside the upper end of the groove in the semiconductor chip mounting region. The sintered metal layer is also formed in the groove formed on the outer side of the semiconductor chip mounting area. The depth of the groove is different between the vicinity of the center of the semiconductor chip mounting region and the vicinity of the end of the semiconductor chip mounting region.
2. The semiconductor device according to claim 1, wherein: The depth of the groove is deeper near the center of the semiconductor chip mounting region and near the end of the semiconductor chip mounting region, and is shallower near the end of the semiconductor chip mounting region.
3. The semiconductor device according to claim 2, wherein: The width of the groove is narrower near the center of the semiconductor chip mounting region and near the end of the semiconductor chip mounting region, and is wider near the end of the semiconductor chip mounting region.
4. The semiconductor device according to any one of claims 1 to 3, characterized in that: An inclined surface is provided at an upper end of the groove near the semiconductor chip.
5. The semiconductor device according to claim 1, wherein: The slot includes a plurality of slots, The plurality of grooves are arranged side by side in a first direction, Each of the plurality of grooves is provided to extend in a second direction intersecting the first direction.
6. The semiconductor device according to claim 5, wherein: The depth of each of the plurality of grooves satisfies that, in the first direction, the depth is deepest near the center and gradually becomes shallower as it moves from the center to the end.
7. The semiconductor device according to claim 6, wherein: The depth of each of the plurality of grooves satisfies that, in the second direction, the depth is deepest near the center and gradually becomes shallower as it moves from the center toward the outer side of the semiconductor chip mounting region.
8. The semiconductor device according to claim 7, wherein: The widths of the plurality of grooves are the same in the first direction.
9. The semiconductor device according to claim 7, wherein: The width of each of the plurality of grooves satisfies that the width near the center is the narrowest and the width gradually increases from the center to the end portions.
10. The semiconductor device according to claim 7 or 8, characterized in that: An upper end of each of the plurality of grooves has an inclined surface near the semiconductor chip.
11. A power conversion device, characterized in that: comprising the semiconductor device as claimed in claim 1, The semiconductor chip is an IGBT or MOSFET power transistor, or a diode.