Low-compression-ratio S355NL super-thick steel plate with thickness larger than 250-300 mm and manufacturing method thereof

By adopting the direct rolling process of large-thick continuous casting slabs, controlling chemical composition and process parameters, the problem of difficult to produce high-performance S355NL extra-thick steel plates with thicknesses exceeding 250mm in the existing technology under low compression ratio conditions is solved, and the steel plate is realized Good internal quality and excellent mechanical properties.

CN119411017AActive Publication Date: 2025-02-11JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411121144.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2025-02-11
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

It is difficult for the prior art to produce high-performance S355NL extra-thick steel plates with thicknesses exceeding 250mm under low compression ratio conditions, and the performance pass rate and flaw detection pass rate in the thickness range of 100 to 200mm are not high.

Method used

The direct rolling process of large-thick continuous casting slabs is adopted, through KR pretreatment, converter smelting, LF refining, RH refining, slab continuous casting, slow cooling, heating, rolling, slow cooling, flaw detection, normalizing, finishing and The process flow of inspection and other processes controls the chemical composition and rolling process parameters of the steel plate to ensure that the steel plate has good internal mass and mechanical properties under low compression ratio.

Benefits of technology

Under the condition of compression ratio less than 2.0, a low compression ratio high-performance S355NL extra-thick steel plate with a thickness of more than 250mm was produced. It has good internal quality, high low-temperature impact toughness and excellent layered tear resistance, meeting the energy industry Manufacturing requirements for key core components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119411017A_ABST
    Figure CN119411017A_ABST
Patent Text Reader

Abstract

The invention relates to a low-compression-ratio S355NL super-thick steel plate with the thickness larger than 250-300 mm and a manufacturing method of the low-compression-ratio S355NL super-thick steel plate. The steel plate comprises the chemical components of 0.08%-0.12% of C, 0.20%-0.40% of Si, 1.45%-1.65% of Mn, smaller than or equal to 0.005% of P, smaller than or equal to 0.001% of S, 0.02%-0.05% of Al, 0.02%-0.05% of Nb, 0.03%-0.06% of V, 0.25%-0.45% of Ni, 0.01%-0.03% of Ti and the balance Fe and inevitable impurity elements, and the carbon equivalent Ceq is smaller than or equal to 0.45%. A large-thickness thick continuous casting slab is adopted for production, and the rolling compression ratio is smaller than 2.0. The internal quality and mechanical properties of the steel plate meet the requirements that the yield strength is larger than or equal to 275 Mpa, the tensile strength is larger than or equal to 450 Mpa, the percentage elongation after fracture is larger than or equal to 22%, the transverse Charpy impact energy unit value at the temperature of-50 DEG C is larger than or equal to 100 J, and the thickness direction tensile area reduction rate is larger than or equal to 35%. And the UT flaw detection of the steel plate can meet the NB / T47013.3 I grade requirement. The metallographic microstructure of the steel plate is a uniform and fine ferrite and pearlite structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of steel plate manufacturing, and in particular relates to a low compression ratio S355NL extra-thick steel plate and a manufacturing method thereof. Background Art

[0002] With the increase of infrastructure construction projects in my country, the market demand for extra-thick steel plates is growing, and is developing towards large thickness, large unit weight, and high quality performance. S355NL extra-thick steel plates are usually used for important components in the energy field, and the design has high requirements for their service safety, so the product must have good internal quality, welding performance, and excellent low-temperature impact performance and lamellar tearing resistance.

[0003] Under the background of the country's vigorous promotion of the green, low-carbon and high-quality development strategy, domestic steel enterprises have increased their investment in the research and development of ultra-thick continuous casting slab manufacturing technology and low compression ratio rolling technology, and have achieved certain results. Publicly reported data show that the maximum thickness of steel plates produced by continuous casting billets has reached 250mm, breaking the traditional manufacturing process of ultra-thick steel plates produced by ingots, and breaking the traditional restriction that the rolling compression ratio must be greater than 3. However, due to the limitations of the thickness of the continuous casting billet, metallurgical quality and stability, the thickness of ultra-thick steel plates produced by the direct rolling process of continuous casting billets is less than 200mm, and the performance qualification rate and flaw detection qualification rate of steel plates in the thickness range of 100-200mm are generally not high. Steel plates in the thickness range of >200-250mm are produced by forging + rolling, which can significantly improve the internal quality of ultra-thick steel plates under low compression ratio conditions, but the manufacturing cycle is long, the yield rate is low, the production cost is high, and it has no promotion value. There are currently no relevant reports on the process technology of directly rolling high-performance steel plates with a thickness of >250-300mm using continuous casting billets.

[0004] Based on the above existing technologies, technicians in this field are committed to developing S355NL extra-thick steel plates with larger thickness, low compression ratio and high performance. Under rolling conditions with low compression ratio, the steel plates achieve good internal quality and excellent comprehensive mechanical properties, reduce production costs, and are suitable for mass production. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a S355NL extra-thick steel plate with a thickness of more than 250-300mm and a low compression ratio and high performance, which can be used in the manufacture of key core components in the energy industry. Under the condition of a compression ratio lower than 2.0, it has good internal quality, high low-temperature impact toughness and excellent resistance to lamellar tearing.

[0006] The technical solution adopted by the present invention to solve the above problems is: a low compression ratio and high performance S355NL extra-thick steel plate with a thickness of more than 250-300 mm, the chemical composition of the steel plate is C: 0.08-0.12%, Si: 0.20-0.40%, Mn: 1.45-1.65%, P: ≤0.005%, S: ≤0.001%, Al: 0.02-0.05%, Nb: 0.02-0.05%, V: 0.03-0.06%, Ni: 0.25-0.45%, Ti: 0.01-0.03%, the remainder is Fe and unavoidable impurity elements, the carbon equivalent Ceq is ≤0.45%, the calculation formula is: Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15, and the compression ratio of the steel plate is less than 2.0.

[0007] Furthermore, the present invention provides a S355NL extra-thick steel plate with a low compression ratio and high performance and a thickness of 250-300 mm, whose internal quality and mechanical properties meet the following requirements: yield strength ≥ 275 MPa, tensile strength ≥ 450 MPa, elongation after fracture ≥ 22%, single value of transverse Charpy impact energy at -50°C ≥ 100 J, and tensile section shrinkage in the thickness direction ≥ 35%. The steel plate UT flaw detection can meet the requirements of NB / T47013.3 Level I.

[0008] The present invention belongs to an iron-based alloy, and the main chemical elements in the steel and their functions are as follows:

[0009] C: can significantly improve the strength of the steel plate, but is not good for toughness and plasticity. Taking the strength and toughness of the steel plate into consideration, the C content in the present invention is set to 0.08-0.12%.

[0010] Mn: Manganese is a good deoxidizer and desulfurizer in the steelmaking process, which can improve the strength and toughness of steel plates. However, too high a content will cause serious segregation of continuous casting billets. The manganese content in this patent is controlled at 1.45-1.65%.

[0011] Si: It is mainly used as a reducing agent and deoxidizer during steelmaking and has a certain solid solution strengthening effect. If the content is too high, the low-temperature toughness of the steel plate will be reduced. Therefore, the Si content in the present invention is set to 0.20-0.40%.

[0012] S and P are harmful elements that increase or decrease the brittleness of steel and reduce impact toughness and welding performance. Therefore, the lower the S and P contents are, the better. In the present invention, the S content is set to ≤0.001% and the P content is set to ≤0.005%.

[0013] Ni: Nickel can significantly improve low temperature impact toughness. If the content is too high, it will have an adverse effect on the surface quality of the steel plate. At the same time, Ni is a precious alloy and its use should be limited. Considering the performance of the steel plate and the production cost, the Ni content in the present invention is set to 0.25-0.45%.

[0014] Alt: Aluminum is mainly used for deoxidation and grain refinement. The Alt content in this patent is controlled at 0.02-0.05%.

[0015] Nb, V: Niobium and vanadium microalloying elements form carbonitrides with C and N elements, which have the effect of delaying austenite recrystallization and refining ferrite grains, and can simultaneously improve the strength and toughness of the steel plate. In the present invention, the Nb content is controlled at 0.02-0.05%, and the V content is controlled at 0.03-0.06%.

[0016] Ti: forms carbonitride with C and N elements, has the effect of delaying austenite recrystallization and refining ferrite grains, and can simultaneously improve the strength and toughness of the steel plate. In the present invention, the Ti content is controlled at 0.010-0.03%.

[0017] The method for manufacturing a S355NL extra-thick steel plate with a low compression ratio and high performance and a thickness of more than 250 to 300 mm described in the present invention comprises the following contents:

[0018] The large thickness continuous casting slab is directly rolled, and the production process is: KR pretreatment → converter smelting → LF refining → RH refining → slab continuous casting → slab slow cooling → slab heating → slab slow cooling after furnace discharge → slab heating → steel plate rolling → steel plate slow cooling → flaw detection → normalizing → finishing → inspection → warehousing.

[0019] The specific operations of the main processes are as follows:

[0020] 1) Smelting process

[0021] The smelting raw materials are pre-treated with KR molten iron, and slag is removed after converter smelting, and S≤0.001%, P≤0.005%, H≤1.0ppm, O≤20ppmm, and N≤40ppm are strictly controlled; the continuous casting process adopts low superheat argon protection casting throughout the process, and the dynamic light pressure technology is used to control the segregation of the casting to Class C 0.5 level, and the looseness to 0.5 level or better; after the slab comes off the line, a hood is added for slow cooling for more than 48 hours to ensure that the hydrogen in the steel is fully diffused.

[0022] 2) Heating and rolling process

[0023] It is produced by double heating and one rolling process.

[0024] The continuous casting slab is heated in a walking beam heating furnace. In order not to affect the production rhythm, the two heating processes adopt the same process system. After the first heating, the slab is taken out of the furnace, and then quickly taken off the line to the slow cooling area for stacking and slow cooling. After the slab is naturally cooled in the air to room temperature, the continuous casting slab is loaded into the heating furnace for heating again.

[0025] Both heatings are performed in a segmented heating mode: the total heating time is 500-550 min, the temperature of the first heating section is 1000-1180°C, the temperature of the second heating section is 1160-1260°C, the temperature of the soaking section is 1150-1250°C, and the total heating time of the second heating section and the soaking section is ≥280 min.

[0026] All rolling deformation is completed on a single stand of the roughing mill. The production is carried out in full longitudinal rolling mode without controlled rolling. The rolling process adopts high permeability rolling technology, and the steel plate is naturally cooled in the air after rolling. The starting rolling temperature is 1050-1100℃, and the rolling is completed in 4-6 passes. After each rolling pass, high-pressure water is used for descaling. The temperature difference between the surface and the core of the continuous casting billet is used to achieve high permeability rolling, that is, differential temperature rolling, to ensure that the deformation coefficient of at least 2 passes is ≥0.5. After the steel plate is off the line, it is stacked and slowly cooled for ≥72 hours to fully expand hydrogen. Description: R-mill working roll radius (598mm), Δh-reduction, H-entrance thickness.

[0027] 3) Heat treatment process

[0028] The normalizing process is adopted, and the normalizing temperature is preferably controlled to be 880±10℃, the holding time coefficient is controlled to be: 2.2~2.5min / mm, and air cooling is performed; the normalizing treatment is carried out in a trolley furnace, and the steel plate is hoisted to the cooling bed as soon as possible after being taken out of the furnace to be cooled to below 200℃.

[0029] The principles of the present invention using the above process measures and applicable ranges of process parameters are as follows:

[0030] The technical difficulties of rolling high-performance extra-thick steel plates with low compression ratio of continuous casting slabs are: (1) How to improve the metallurgical quality of the continuous casting slab itself, that is, to minimize the central segregation and central porosity defects of the continuous casting slab, while fully removing the non-metallic inclusions and gas hydrogen content in the steel. (2) How to achieve rolling pressure penetration within a limited deformation range in the thickness direction to fully break up the cast structure and press the metallurgical defects in the core. The composition and process design of the present invention are developed around solving the above two technical problems. The main measures to improve the metallurgical quality of continuous casting slabs are as follows: 1) In terms of composition design, the content of segregation elements such as C, Mn, S, and P is reduced as much as possible while ensuring the strength of the steel plate; 2) In terms of production process, technical means such as dynamic light reduction of continuous casting slabs and double heating high-temperature diffusion are used to reduce the central segregation and loose defects of continuous casting slabs; The main measures adopted to achieve rolling deformation penetration are as follows: 1) Adopt a single-frame full longitudinal rolling method to extend the insulation time of the high-temperature section of the continuous casting slab, and achieve high-temperature rolling to reduce deformation resistance; 2) Increase the reduction of a single pass, adopt differential temperature rolling technology, and ensure that the deformation coefficient of at least two passes is ≥0.5.

[0031] Compared with the prior art, the advantages of the present invention are:

[0032] The present invention relates to a S355NL extra-thick steel plate with a low compression ratio and high performance and a thickness of more than 250 to 300 mm. It is produced by direct rolling of continuous casting billets. Under the condition of a compression ratio of less than 2.0, it has good internal quality, high strength, excellent low-temperature impact toughness and lamellar tear resistance. According to testing, the yield strength and tensile strength margin of the product of the present invention are above 30 MPa, the single value of the transverse Charpy impact energy at -50°C is ≥100J, and the tensile section shrinkage rate in the thickness direction is ≥35%. The UT flaw detection of the steel plate can meet the requirements of NB / T47013.3 Level I. After the normalizing treatment, the metallographic microstructure of the steel plate is a uniform and fine ferrite + pearlite mixed structure, and its typical morphology is detailed in the attached Figure 1 . BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a typical microstructure diagram (100×) of the low reduction ratio S355NL extra thick steel plate of the present invention. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0035] Example 1

[0036] The thickness of the S355NL steel plate in this embodiment is 255 mm, and its chemical composition is as follows by weight percentage: C: 0.09%, Si: 0.35%, Mn: 1.58%, P: 0.004%, S: ≤0.0008%, Al: 0.035%, Nb: 0.030%, V: 0.032%, Ni: 0.41%, Ti: 0.016%, and the remainder is Fe and unavoidable impurity elements. The carbon equivalent Ceq≤0.45%, and the calculation formula is: Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15.

[0037] The manufacturing process of the steel plate is as follows:

[0038] The thick continuous casting slab is directly rolled. The continuous casting slab is heated twice and rolled once. The production process is as follows:

[0039] KR pretreatment → converter smelting → LF refining → RH refining → slab continuous casting → slab slow cooling → slab heating → slab slow cooling after furnace exit → slab heating → steel plate rolling → steel plate slow cooling → flaw detection → normalizing → finishing → inspection → warehousing.

[0040] The specific operations of the main processes are as follows:

[0041] 1) Smelting process

[0042] The smelting raw materials are pre-treated with KR molten iron, and the slag is removed after converter smelting, and S≤0.001%, P≤0.005%, H≤1.0ppm, O≤20ppmm, and N≤40ppm are strictly controlled; the continuous casting process adopts low superheat argon protection casting throughout the process, and the casting slab segregation is controlled by dynamic soft pressure technology to be C-class 0.5 level, looseness 0.5 level or better; the slab is covered and slowly cooled for more than 48 hours after it comes off the line to ensure that the hydrogen in the steel is fully diffused. The superheat of the molten steel in the continuous casting process of this embodiment is 20°C, and the slab is tested at a low magnification, and the center segregation is C-class 0.5 level and looseness 0.5 level.

[0043] 2) Heating and rolling process

[0044] It is produced by double heating and one rolling process.

[0045] The continuous casting slab is heated in a walking beam heating furnace. In order not to affect the production rhythm, the two heating processes adopt the same process system. After the first heating, the slab is taken out of the furnace, and then quickly taken off the line to the slow cooling area for stacking and slow cooling. After the slab is naturally cooled in the air to room temperature, the continuous casting slab is loaded into the heating furnace for heating again.

[0046] The two heatings are performed in a segmented heating mode: the total heating time for the first heating is 510 minutes, the temperature of the first heating section is 1000-1180°C, the temperature of the second heating section is 1160-1260°C, the temperature of the equalizing section is 1150-1250°C, and the total heating time of the second heating section and the equalizing section is 300 minutes. The total heating time for the second heating is 530 minutes, the temperature of the first heating section is 1000-1180°C, the temperature of the second heating section is 1160-1260°C, the temperature of the equalizing section is 1150-1250°C, and the total heating time of the second heating section and the equalizing section is 320 minutes.

[0047] All rolling deformation is completed on a single stand of the rough rolling mill. The production is carried out in full longitudinal rolling mode without controlled rolling. The rolling process adopts high permeability rolling technology, and the steel plate is naturally cooled in the air after rolling. The starting rolling temperature is 1080℃, and the rolling is completed in 6 passes. After each rolling pass, high-pressure water is used to remove phosphorus. The temperature difference between the surface and the core of the continuous casting billet is used to achieve high permeability rolling, that is, differential temperature rolling. Among the rolling passes, the deformation coefficient of 3 passes is ≥0.5, which are 0.52, 0.57, and 0.53 respectively. After the steel plate is off the line, it is stacked and slowly cooled for ≥72 hours to fully expand hydrogen.

[0048] 3) Heat treatment process

[0049] The normalizing process is adopted, the normalizing temperature is 880±10℃, the holding time coefficient is 2.3min / mm, and the air cooling is adopted; the normalizing treatment is carried out in a trolley furnace, and the steel plate is hoisted to the cooling bed as soon as possible after being taken out of the furnace to be cooled to below 200℃.

[0050] The 255 mm thick continuous casting billet obtained by the above manufacturing process produces a low compression ratio high performance S355NL extra thick steel plate. The UT flaw detection meets the requirements of NB / T47013.3 standard level I, and has well-matched comprehensive mechanical properties, see Table 1 for details.

[0051] Example 2

[0052] The thickness of the S355NL steel plate in this embodiment is 285 mm, and its chemical composition is as follows by weight percentage: C: 0.11% S, i: 0.32%, Mn: 1.55%, P: 0.004%, S: ≤0.0006%, Al: 0.032%, Nb: 0.028%, V: 0.035%, Ni: 0.42%, Ti: 0.018%, the remainder is Fe and unavoidable impurity elements, the carbon equivalent Ceq≤0.45%, and the calculation formula is: Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15.

[0053] The manufacturing process of the steel plate is as follows:

[0054] The thick continuous casting slab is directly rolled. The continuous casting slab is heated twice and rolled once. The production process is as follows:

[0055] KR pretreatment → converter smelting → LF refining → RH refining → slab continuous casting → slab slow cooling → slab heating → slab slow cooling after furnace exit → slab heating → steel plate rolling → steel plate slow cooling → flaw detection → normalizing → finishing → inspection → warehousing.

[0056] The specific operations of the main processes are as follows:

[0057] 1) Smelting process

[0058] The smelting raw materials are pre-treated with KR molten iron, and the slag is removed after converter smelting, and S≤0.001%, P≤0.005%, H≤1.0ppm, O≤20ppmm, and N≤40ppm are strictly controlled; the continuous casting process adopts low superheat argon protection casting throughout the process, and the casting slab segregation is controlled by dynamic soft pressure technology to be C-class 0.5 level, looseness 0.5 level or better; the slab is covered and slowly cooled for more than 48 hours after it comes off the line to ensure that the hydrogen in the steel is fully diffused. The superheat of the molten steel in the continuous casting process of this embodiment is 18°C, and the slab is tested at a low magnification, and the center segregation is C-class 0.5 level and looseness 0.5 level.

[0059] 2) Heating and rolling process

[0060] It is produced by double heating and one rolling process.

[0061] The continuous casting slab is heated in a walking beam heating furnace. In order not to affect the production rhythm, the two heating processes adopt the same process system. After the first heating, the slab is taken out of the furnace, and then quickly taken off the line to the slow cooling area for stacking and slow cooling. After the slab is naturally cooled in the air to room temperature, the continuous casting slab is loaded into the heating furnace for heating again.

[0062] The two heatings were performed in a segmented heating mode: the total heating time for the first heating was 520 minutes, the temperature of the first heating section was 1000-1180°C, the temperature of the second heating section was 1160-1260°C, the temperature of the soaking section was 1150-1250°C, and the total heating time of the second heating section and the soaking section was 315 minutes. The total heating time for the second heating was 550 minutes, the temperature of the first heating section was 1000-1180°C, the temperature of the second heating section was 1160-1260°C, the temperature of the soaking section was 1150-1250°C, and the total heating time of the second heating section and the soaking section was 330 minutes.

[0063] All rolling deformation is completed on a single stand of the roughing mill. The production is carried out in full longitudinal rolling mode without controlled rolling. The rolling process adopts high permeability rolling technology, and the steel plate is naturally cooled in the air after rolling. The starting rolling temperature is 1080℃, and the rolling is completed in 6 passes. After each rolling pass, high-pressure water is used to remove phosphorus. The temperature difference between the surface and the core of the continuous casting billet is used to achieve high permeability rolling, that is, differential temperature rolling. There are 2 passes with deformation coefficients ≥0.5, which are 0.52 and 0.61 respectively. After the steel plate is off the line, it is stacked and slowly cooled for ≥72 hours to fully expand hydrogen.

[0064] 3) Heat treatment process

[0065] The normalizing process is adopted, the normalizing temperature is 880±10℃, the holding time coefficient is 2.4min / mm, and the air cooling is adopted; the normalizing treatment is carried out in a trolley furnace, and the steel plate is hoisted to the cooling bed as soon as possible after being taken out of the furnace to be cooled to below 200℃.

[0066] The 255 mm thick continuous casting billet obtained by the above manufacturing process produces a low compression ratio high performance S355NL extra thick steel plate. The UT flaw detection meets the requirements of NB / T47013.3 standard level I, and has well-matched comprehensive mechanical properties, see Table 1 for details.

[0067] Example 3

[0068] The thickness of the S355NL steel plate in this embodiment is 300 mm, and its chemical composition is as follows by weight percentage: C: 0.10%, Si: 0.36%, Mn: 1.62%, P: 0.005%, S: ≤0.0005%, Al: 0.032%, Nb: 0.032%, V: 0.035%, Ni: 0.42%, Ti: 0.015%, and the remainder is Fe and unavoidable impurity elements. The carbon equivalent Ceq≤0.45%, and the calculation formula is: Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15.

[0069] The manufacturing process of the steel plate is as follows:

[0070] The thick continuous casting slab is directly rolled. The continuous casting slab is heated twice and rolled once. The production process is as follows:

[0071] KR pretreatment → converter smelting → LF refining → RH refining → slab continuous casting → slab slow cooling → slab heating → slab slow cooling after furnace exit → slab heating → steel plate rolling → steel plate slow cooling → flaw detection → normalizing → finishing → inspection → warehousing.

[0072] The specific operations of the main processes are as follows:

[0073] 1) Smelting process

[0074] The smelting raw materials are pre-treated with KR molten iron, and the slag is removed after converter smelting, and S≤0.001%, P≤0.005%, H≤1.0ppm, O≤20ppmm, and N≤40ppm are strictly controlled; the continuous casting process adopts low superheat argon protection casting throughout the process, and the casting slab segregation is controlled by dynamic soft pressure technology to be C-class 0.5 level, looseness 0.5 level or better; the slab is covered and slowly cooled for more than 48 hours after it comes off the line to ensure that the hydrogen in the steel is fully diffused. The superheat of the molten steel in the continuous casting process of this embodiment is 17°C, and the slab is tested at a low magnification, and the center segregation is C-class 0.5 level and looseness 0.5 level.

[0075] 2) Heating and rolling process

[0076] It is produced by double heating and one rolling process.

[0077] The continuous casting slab is heated in a walking beam heating furnace. In order not to affect the production rhythm, the two heating processes adopt the same process system. After the first heating, the slab is taken out of the furnace, and then quickly taken off the line to the slow cooling area for stacking and slow cooling. After the slab is naturally cooled in the air to room temperature, the continuous casting slab is loaded into the heating furnace for heating again.

[0078] The two heatings were performed in a segmented heating mode: the total heating time for the first heating was 540 minutes, the temperature of the first heating section was 1000-1180°C, the temperature of the second heating section was 1160-1260°C, the temperature of the soaking section was 1150-1250°C, and the total heating time of the second heating section and the soaking section was 325 minutes. The total heating time for the second heating was 545 minutes, the temperature of the first heating section was 1000-1180°C, the temperature of the second heating section was 1160-1260°C, the temperature of the soaking section was 1150-1250°C, and the total heating time of the second heating section and the soaking section was 345 minutes.

[0079] All rolling deformation is completed on a single stand of the roughing mill. The production is carried out in full longitudinal rolling mode without controlled rolling. The rolling process adopts high permeability rolling technology. The steel plate is naturally cooled in the air after rolling. The starting rolling temperature is 1080℃, and the rolling is completed in 6 passes. After each rolling pass, high-pressure water is used to remove phosphorus. The temperature difference between the surface and the core of the continuous casting billet is used to achieve high permeability rolling, that is, differential temperature rolling. There are 2 passes with deformation coefficients ≥0.5, which are 0.51 and 0.56 respectively. After the steel plate is off the line, it is stacked and slowly cooled for ≥72 hours to fully expand hydrogen.

[0080] 3) Heat treatment process

[0081] The normalizing process is adopted, the normalizing temperature is 880±10℃, the holding time coefficient is 2.5min / mm, and the air cooling is adopted. The normalizing treatment is carried out in a trolley furnace, and the steel plate is hoisted to the cooling bed as soon as possible after being taken out of the furnace to be cooled to below 200℃.

[0082] The 300 mm thick continuous casting billet produced by the above manufacturing process produces a low compression ratio high performance S355NL extra thick steel plate. The UT flaw detection meets the requirements of NB / T47013.3 standard level I, and has well-matched comprehensive mechanical properties, see Table 1 for details.

[0083] Table 1 Mechanical properties of the steel plates produced in each embodiment

[0084]

[0085] Note: The numbers in () are average values.

Claims

1. A S355NL extra-thick steel plate with a thickness of >250-300mm and a low compression ratio, characterized in that: The chemical composition of the steel plate is calculated by weight as follows: C: 0.08-0.12%, Si: 0.20-0.40%, Mn: 1.45-1.65%, P: ≤0.005%, S: ≤0.001%, Al: 0.02-0.05%, Nb: 0.02-0.05%, V: 0.03-0.06%, Ni: 0.25-0.45%, Ti: 0.01-0.03%, the balance is Fe and unavoidable impurity elements, carbon equivalent Ceq≤0.45%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15, where the element symbol is the percentage of the corresponding element.

2. The S355NL extra-thick steel plate with a thickness of >250-300 mm and a low compression ratio and high performance according to claim 1, characterized in that: The internal quality and mechanical properties of the steel plate meet the following requirements: yield strength ≥275Mpa, tensile strength ≥450Mpa, elongation after fracture ≥22%, single value of transverse Charpy impact energy at -50℃ ≥100J, tensile section shrinkage in thickness direction ≥35%; UT flaw detection of the steel plate can meet the requirements of NB / T47013.3 Level I; the metallographic microstructure of the steel plate is uniform and fine ferrite + pearlite structure.

3. A method for manufacturing the steel plate according to claim 1, characterized in that: Including the following processes: 1) Molten steel smelting The smelting raw materials are pre-treated with KR molten iron, and the slag is removed after converter smelting to control the molten steel S≤0.001%, P≤0.005%, H≤1.0ppm, O≤20ppmm, and N≤40ppm; the continuous casting process adopts low superheat argon protection casting throughout the process, and the dynamic soft pressure technology is used to control the segregation of the cast billet to Class C 0.5 and the looseness to 0.5 or better; the slab is covered and slowly cooled for more than 48 hours after it comes off the line to ensure that the hydrogen in the steel is fully diffused; 2) Heating and rolling The production process is two-time heating and one-time rolling. The same process system is used for the two heatings. After the first heating, the slab is taken out of the furnace and then quickly taken off the line to the slow cooling area for stacking and slow cooling. After the billet is naturally cooled to room temperature in the air, the continuous casting slab is loaded into the heating furnace for the second heating. All rolling deformation is completed on a single stand of the roughing mill. The production is carried out in full longitudinal rolling mode without controlled rolling. The rolling reduction ratio is less than 2.

0. The rolling process adopts high permeability rolling technology. The steel plate is naturally cooled in the air after rolling. The starting rolling temperature is 1050-1100℃. The rolling is completed in 4-6 passes. After each rolling pass, high-pressure water is used for descaling. The temperature difference between the surface and the core of the continuous casting billet is used to achieve high permeability rolling, that is, differential temperature rolling, to ensure that the deformation coefficient of at least 2 passes is ≥0.5; the steel plate is stacked and slowly cooled for ≥72 hours after it comes off the line to fully expand hydrogen; 3) Heat treatment process The normalizing process is adopted. After the steel plate is normalized and heated out of the furnace, it is lifted to the cooling bed as soon as possible and cooled to below 200℃.

4. The method according to claim 3, characterized in that: In step 2), both heating steps are performed in a segmented heating mode: the total heating time is 500-550 min, the temperature of the first heating section is 1000-1180°C, the temperature of the second heating section is 1160-1260°C, the temperature of the soaking section is 1150-1250°C, and the total heating time of the second heating section and the soaking section is ≥280 min.

5. The method according to claim 3, characterized in that: Normalizing treatment is carried out in a trolley furnace, the normalizing temperature is 880±10℃, the holding time coefficient is 2.2~2.5min / mm, and air cooling is used.

Citation Information

Patent Citations

  • Steel plates for 355MPa-level easy-to-weld ocean platform and production process of steel plates

    CN103194677A

  • Hydroelectric normalized high strength steel sheet with great thickness and easy to weld and production method thereof

    CN103451530A

  • Low-compression-ratio high-performance ultra-thick steel plate produced by continuous casting billet and manufacturing method of steel plate

    CN105755375A

  • S355NL low-carbon high-toughness low alloy steel plate of 250 mm thickness and manufacturing method thereof

    CN105925893A

  • Low-carbon extra-thick low-yield-ratio steel S355NL for reel and manufacturing method of low-carbon extra-thick low-yield-ratio steel S355NL

    CN106119713A