Gel type adsorbent based on cationic surface active agent modification and application of gel type adsorbent in iodide ion adsorption
By mixing polyhydroxy amine with silane coupling agent and introducing cationic surfactant to modify it, a gel-type adsorbent with selective adsorption properties is solved, and the problems of long adsorption time and large dissolution loss in the prior art are achieved. Efficient and economical iodine ion adsorption effect.
Patent Information
- Application Number
- CN202411460954.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2025-02-21
AI Technical Summary
The equilibrium adsorption time of existing gel adsorbents is long and the dissolution loss is large during the preparation process, which affects the adsorption efficiency and economicality.
By mixing the polyhydroxy amine with a silane coupling agent, an organic gelling material is formed, and on this basis, a cationic surfactant is introduced for modification, forming a gel-type adsorbent with selective adsorption.
The adsorption equilibrium time is significantly reduced to less than 10 hours, the adsorption rate and selectivity are improved, the dissolution loss is reduced, the preparation process is simplified, and the reusability of the adsorbent is improved.
Smart Images

Figure CN119488882A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical adsorption, in particular to a gel-type adsorbent modified by a cationic surfactant and application thereof in iodide ion adsorption. Background Art
[0002] The main extraction and separation technologies of iodine include precipitation method, photocatalytic oxidation method, membrane separation method, adsorption method and ion exchange resin method. The precipitation method is simple to operate, with low equipment investment, and is suitable for low-concentration iodine ion solutions; but the selection and dosage of the precipitant need to be well controlled, otherwise it may affect the recovery rate and purity of iodine. For the photocatalytic oxidation method, seawater or brine is treated with a photocatalyst (such as TiO2, ZnO, etc.) to oxidize iodine ions into elemental iodine, and then the iodine is separated through filtration, concentration and other steps; the equipment investment is high, and the operation and maintenance are relatively complicated. The membrane used in the membrane separation method has poor selectivity and stability, and the membrane is seriously polluted, requiring frequent cleaning and replacement, and the operating cost is high. The adsorption method has a certain adsorption effect on high-concentration and low-concentration brines, but its separation and recovery is the key issue. The selection and dosage of the resin in the ion exchange resin method need to be well controlled, otherwise it may affect the recovery rate and purity of iodine, and the process of regenerating the resin is relatively complicated, requiring a certain amount of energy and chemical reagents. Overall, the adsorption method is the most suitable method for extracting iodine ions. Its advantages are: there are many types of adsorbents, and the appropriate adsorbent can be selected according to actual needs; no toxic substances are needed in the adsorption process, which is environmentally friendly; the operation of the adsorption method is simple, and it is easy to realize automation and continuous production; the separation effect of the adsorption method is good. Although the adsorption method has some disadvantages, such as the regeneration and treatment of the adsorbent is relatively complicated, its advantages still make it an iodine extraction and separation technology with broad application prospects.
[0003] The Chinese patent "Gel-type iodine ion adsorbent, preparation method and application thereof" with publication number CN 103071457 A discloses a preparation method of a gel-type iodine ion adsorbent, which mainly comprises: mixing γ-glycidyloxypropyltrimethoxysilane with polyhydroxyamine and alkaline aqueous solution to form a gel solution, and the adsorbent has an equilibrium adsorption time of about 24 hours under strong acidic conditions. The equilibrium adsorption time is long, and an alkaline aqueous solution needs to be added during the preparation process, resulting in large dissolution loss.
[0004] On this basis, this patent expands the applicable scope of silane coupling agents and adds surfactant modification to improve the selectivity and adsorption rate during the adsorption process, reducing the adsorption equilibrium time to less than 10 hours. Summary of the invention
[0005] The purpose of the present invention is to provide a gel-type adsorbent modified by a cationic surfactant and a preparation method thereof in view of the problems of long equilibrium adsorption time and large dissolution loss during the preparation process of the gel-type adsorbent in the prior art.
[0006] Another object of the present invention is to provide the use of the cationic surfactant-modified gel-type adsorbent in iodide ion adsorption.
[0007] The technical solution adopted to achieve the purpose of the present invention is:
[0008] A gel-type adsorbent modified by a cationic surfactant is prepared by the following method:
[0009] Step 1, mixing polyhydroxyamine and silane coupling agent to form solution A;
[0010] Step 2, adding deionized water to solution A, stirring to perform a hydrolysis reaction, and forming an organic gelling material with a three-dimensional network structure;
[0011] Step 3, aging the organic gelling material obtained in step 2, washing, drying, and grinding to obtain an adsorbent precursor;
[0012] Step 4, mixing the adsorbent precursor, the cationic surfactant with a quaternary ammonium salt group and deionized water for reaction, and collecting the solid after the reaction is completed;
[0013] Step 5, washing and drying the solid to obtain a gel-type adsorbent modified by a cationic surfactant.
[0014] In the above technical scheme, in the step 1, the polyhydroxyamine contains one or more of a hydroxyl group and an amine group, an imine group or a tertiary amine group. Preferably, the polyhydroxyamine is glycerolamine, diethanolamine, triethanolamine, dimethylethanolamine, meglumine, 2-amino-1,3-propanediol, N,N'-di(2-hydroxyethyl)-1,2-ethylenediamine, or N-(2-hydroxyethyl)-N-(3-hydroxypropyl)amine.
[0015] In the above technical solution, in step 1, the silane coupling agent is KH560, KH570 or KH170.
[0016] In the above technical solution, in step 1, the mass ratio of the polyhydroxyamine to the silane coupling agent is 1:1 to 1:5.
[0017] In the above technical solution, the mass ratio of the deionized water in step 2 to the polyhydroxyamine in step 1 is 1:1 to 8:1.
[0018] In the above technical solution, in step 2, the temperature of the hydrolysis reaction is 20 to 80° C., and the time is 1 to 10 minutes.
[0019] In the above technical solution, in step 2, after the hydrolysis reaction is completed, the excess organic reagent is removed by vacuum rotary evaporation to obtain the organic gelling material, and the vacuum rotary evaporation temperature is 60 to 85° C. and the rotation speed is 50 to 100 rpm.
[0020] In the above technical solution, in step 3, the aging temperature is room temperature and the time is 2 to 12 hours.
[0021] In the above technical solution, in step 3, the drying temperature is 40-80° C., the drying time is 8-24 hours, and the powder is sieved after grinding, and the mesh size of the sieve is 20-100 meshes.
[0022] In the above technical solution, in step 4, the cationic surfactant is hexadecyl trimethyl ammonium chloride, dodecyl dimethyl benzyl ammonium chloride or octadecyl dimethyl benzyl ammonium chloride. The introduction of positively charged quaternary ammonium salt groups on the adsorbent surface significantly enhances the electrostatic adsorption capacity of anions such as iodide ions. This modification not only improves the selectivity and hydrophilicity of the adsorbent, but also increases the surface active sites, thereby improving the adsorption capacity.
[0023] In the above technical solution, in step 4, the ratio of the mass fraction of the adsorbent precursor, the volume fraction of the cationic surfactant and the volume fraction of deionized water is 1:(0.1-0.5):1, the unit of the mass fraction is g, and the unit of the volume fraction is L.
[0024] In the above technical solution, in step 4, the reaction temperature is 40 to 60° C., and the reaction time is 2 to 8 hours.
[0025] In the above technical solution, in step 5, the drying temperature is 40 to 70° C., and the drying time is 8 to 24 hours.
[0026] Another aspect of the present invention also includes the use of the gel-type adsorbent in the adsorption and separation of iodide ions.
[0027] In the above technical solution, the adsorption equilibrium time is 6 to 8 hours.
[0028] In the above technical scheme, after the iodine ions are adsorbed, they can be separated by desorption using a 0.01-0.1 mol / L weak alkaline solution, wherein the weak alkaline solution is an aqueous solution of Na2CO3, K2CO3, Na2SO4, or NH4HCO3.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. The present invention forms a gel-type adsorbent with selective adsorption by performing cationic surface modification on the gel-type adsorbent formed by reacting a silane coupling agent with polyhydroxyamine. The cationic head (quaternary ammonium salt group) interacts with the negative charge or polar group on the surface of the gel precursor, thereby forming a cationic modification layer on the gel surface, which helps to improve the dispersibility in aqueous media.
[0031] 2. The cationic surfactant-modified gel adsorbent (in block, granular or powdered form) of the present invention has a high adsorption capacity, a fast adsorption rate, and greatly reduces the adsorption equilibrium time. It can efficiently capture a large number of iodide ions, and has high selectivity, little interference from other ions, and has excellent adsorption performance and stability. The preparation process is simple. The present invention does not require additional addition of acid and alkali during the preparation process, has less dissolution loss, and still has a good adsorption effect under neutral conditions. It is easy to realize industrial production, and the regeneration and treatment of the adsorbent are also relatively simple and can be reused.
[0032] 3. Surface modification of the gel-like adsorbent precursor by cationic surfactants, which introduces quaternary ammonium functional groups, thereby improving the adsorption performance and selectivity, such as in Cl - :I - When the molar ratio of is 200:1, its adsorption of iodide ions can still be maintained above 96%. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Shown is the preparation process of the gel-type adsorbent of the present invention.
[0034] Figure 2 This is the morphology of the gel-type adsorbent of Example 1 (not adsorbed), wherein the magnification of A is 2500 times, and the magnification of B is 3000 times.
[0035] Figure 3 The gel-type adsorbent morphology of Example 1 (adsorption I - ), where the magnification of A is 2500 times and the magnification of B is 3000 times. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0037] Example 1
[0038] like Figure 1 As shown, a gel-type adsorbent modified by a cationic surfactant is prepared by the following method:
[0039] KH560, meglumine and water were mixed in a volume ratio of 1:2:7. After continuous stirring for 5 minutes, a uniform gel solution was formed, which was subjected to vacuum rotary evaporation at 80 rpm at 60°C. The obtained gel solution was aged for 4 hours, washed with water, and dried at 60°C for 12 hours to obtain a block gel. After grinding and sieving, an adsorbent precursor with a particle size of 25 to 90 mesh was obtained. The obtained adsorbent precursor, hexadecyltrimethylammonium chloride and water were stirred at 45°C for 6 hours in a ratio of 1g:0.2L:1L. After centrifugation and washing with water, it was dried at 65°C for 8 hours to obtain a gel-type adsorbent modified by a cationic surfactant.
[0040] The adsorbent was used to adsorb iodide ions in an acidic solution (pH=3, potassium iodide solution adjusted with dilute hydrochloric acid), the adsorption equilibrium time was 6 hours, and the adsorption capacity was 280 mg / g. The adsorbent after adsorption was eluted with a 0.05 mol / L NH4HCO3 aqueous solution at a solid-liquid ratio of 1g:0.4L, and the elution rate was 96%; after elution, it was washed with water to neutrality and then adsorbed again, and the re-adsorption capacity of iodine ions was 298 mg / g.
[0041] like Figure 2-Figure 3 As shown, the cationic surfactant-modified gel-type adsorbent obtained in this example is irregular spherical particles with a diameter of about 100 to 200 nm. The morphology of the material remains almost the same after adsorbing iodine ions, indicating that the material has a certain stability.
[0042] Example 2
[0043] A gel-type adsorbent modified by a cationic surfactant is prepared by the following method:
[0044] Mix KH570, triethanolamine and water in a volume ratio of 1:1:8. After continuous stirring for 2 minutes, a uniform gel solution is formed, which is subjected to vacuum rotary evaporation at 70°C and 60 rpm. The obtained gel solution is aged for 6 hours, washed with water, and dried at 65°C for 8 hours to obtain a block gel. After grinding and sieving, an adsorbent precursor with a particle size of 20 to 100 mesh is obtained. The obtained adsorbent precursor, dodecyl dimethyl benzyl ammonium chloride, and water are stirred at 50°C for 4 hours in a ratio of 1g:0.3L:1L. After centrifugation and washing with water, it is dried at 55°C for 9 hours to obtain a gel-type adsorbent modified by a cationic surfactant.
[0045] The adsorbent was used to adsorb iodide ions in an acidic solution (pH = 4, potassium iodide solution adjusted with dilute hydrochloric acid), the adsorption equilibrium time was 7h, and the adsorption capacity was 262mg / g. It was eluted with a 0.03mol / L Na2SO4 aqueous solution at a solid-liquid ratio of 1g:0.6L, and the elution rate was 97%; after elution, it was washed with water to neutrality and then adsorbed again, and the re-adsorption capacity of iodine ions was 255mg / g.
[0046] Example 3
[0047] A gel-type adsorbent modified by a cationic surfactant is prepared by the following method:
[0048] Mix KH170, dimethylethanolamine and water in a volume ratio of 1:4:5. After continuous stirring for 3 minutes, a uniform gel solution is formed, which is subjected to reduced pressure rotary evaporation at 80 rpm at 75°C. The obtained gel solution is aged for 5 hours, washed with water, and dried at 75°C for 15 hours to obtain a block gel. After grinding and sieving, an adsorbent precursor with a particle size of 25 to 75 mesh is obtained. The obtained adsorbent precursor, hexadecyltrimethylammonium chloride and water are stirred at 40°C for 5.5 hours in a ratio of 1g:0.3L:1L. After centrifugation and washing with water, it is dried at 50°C for 10 hours to obtain a gel-type adsorbent modified by a cationic surfactant.
[0049] The adsorbent was used to adsorb iodide ions in a neutral solution (pH=7, potassium iodide solution), the adsorption equilibrium time was 8h, and the adsorption capacity was 240mg / g. It was eluted with a 0.05mol / L Na2CO3 aqueous solution at a solid-liquid ratio of 1g:0.7L, and the elution rate was 95%; after elution, it was washed with water until neutral and then adsorbed again, and the re-adsorption capacity of iodine ions was 224mg / g.
[0050] Example 4
[0051] A gel-type adsorbent modified by a cationic surfactant is prepared by the following method:
[0052] KH170, N,N'-di(2-hydroxyethyl)-1,2-ethylenediamine and water were mixed in a volume ratio of 1:3:4. After continuous stirring for 2 minutes, a uniform gel solution was formed, which was subjected to vacuum rotary evaporation at 85°C and 70 rpm. The obtained gel solution was aged for 4.5 hours, washed with water, and dried at 55°C for 6 hours to obtain a block gel. After grinding and sieving, a precursor with a particle size of 30 to 120 mesh was obtained. The obtained adsorbent precursor, octadecyl dimethyl benzyl ammonium chloride, and water were stirred at 40°C for 3.5 hours in a ratio of 1g:0.4L:1L. After centrifugation and washing with water, it was dried at 60°C for 5.5 hours to obtain a gel-type adsorbent modified by a cationic surfactant.
[0053] The adsorbent was used to adsorb iodide ions in a weakly acidic solution (pH=6, potassium iodide solution adjusted with dilute hydrochloric acid), the adsorption equilibrium time was 7.5h, and the adsorption capacity was 255mg / g. It was eluted with 0.02mol / L NH4HCO3 aqueous solution at a solid-liquid ratio of 1g:0.8L, and the elution rate was 95%; after elution, it was washed with water to neutrality and then adsorbed again, and the re-adsorption capacity of iodine ions was 240mg / g.
[0054] Comparative Example 1
[0055] Compared with Example 1, no cationic surfactant modification was performed.
[0056] A gel-type adsorbent that has not been modified by a cationic surfactant is prepared by the following method:
[0057] KH560, meglumine and water were mixed in a volume ratio of 1:2:7. After continuous stirring for 5 minutes, a uniform gel solution was formed, and vacuum rotary evaporation was performed at 80 rpm at 60°C. The obtained gel solution was aged for 4 hours, washed with water, and dried at 60°C for 12 hours to obtain a block gel. After grinding and sieving, a gel-type adsorbent with a particle size of 25 to 90 meshes that was not modified by a cationic surfactant was obtained.
[0058] The adsorbent was used to adsorb iodide ions in an acidic solution (pH=3, potassium iodide solution adjusted with dilute hydrochloric acid), the adsorption equilibrium time was 11 h, and the adsorption capacity was 201 mg / g.
[0059] Comparative Example 2
[0060] Compared with Example 2, no cationic surfactant modification was performed.
[0061] A gel-type adsorbent that has not been modified by a cationic surfactant is prepared by the following method:
[0062] KH570, triethanolamine and water were mixed in a volume ratio of 1:1:8. After continuous stirring for 2 minutes, a uniform gel solution was formed, and vacuum rotary evaporation was performed at 70°C and 60 rpm. The obtained gel solution was aged for 6 hours, washed with water, and dried at 65°C for 8 hours to obtain a block gel. After grinding and sieving, a gel-type adsorbent with a particle size of 20 to 100 meshes that was not modified by a cationic surfactant was obtained.
[0063] The adsorbent was used to adsorb iodide ions in an acidic solution (pH=4, potassium iodide solution adjusted with dilute hydrochloric acid), the adsorption equilibrium time was 13 h, and the adsorption capacity was 184 mg / g.
[0064] Comparative Example 3
[0065] Compared with Example 3, no cationic surfactant modification was performed.
[0066] A gel-type adsorbent that has not been modified by a cationic surfactant is prepared by the following method:
[0067] KH170, dimethylethanolamine and water were mixed in a volume ratio of 1:4:5. After continuous stirring for 3 minutes, a uniform gel solution was formed, and vacuum rotary evaporation was performed at 80 rpm at 75°C. The obtained gel solution was aged for 5 hours, washed with water, and dried at 75°C for 15 hours to obtain a block gel. After grinding and sieving, a gel-type adsorbent with a particle size of 25 to 75 mesh that was not modified by a cationic surfactant was obtained.
[0068] The adsorbent was used to adsorb iodide ions in a neutral solution (pH=7, potassium iodide solution), the adsorption equilibrium time was 24 h, and the adsorption capacity was 166 mg / g.
[0069] Comparative Example 4
[0070] Compared with Example 4, no cationic surfactant modification was performed.
[0071] A gel-type adsorbent that has not been modified by a cationic surfactant is prepared by the following method:
[0072] KH170, N,N'-di(2-hydroxyethyl)-1,2-ethylenediamine and water were mixed in a volume ratio of 1:3:4. After continuous stirring for 2 minutes, a uniform gel solution was formed, and vacuum rotary evaporation was performed at 85°C and 70 rpm. The obtained gel solution was aged for 4.5 hours, washed with water, and dried at 55°C for 6 hours to obtain a block gel. After grinding and sieving, a gel-type adsorbent with a particle size of 30 to 120 mesh that has not been modified by a cationic surfactant was obtained.
[0073] The adsorbent was used to adsorb iodide ions in a weakly acidic solution (pH=6, potassium iodide solution adjusted with dilute hydrochloric acid), the adsorption equilibrium time was 16 h, and the adsorption capacity was 173 mg / g.
[0074] The adsorption equilibrium time was compared with the above embodiments and comparative examples.
[0075] Table 1 Comparison of adsorption equilibrium time
[0076] Example and comparative example number Comparative Example Example 1 11h 6h 2 13h 7h 3 24h 8h 4 16h 7.5h
[0077] The adsorption amounts were compared in combination with the above embodiments and comparative examples.
[0078] Table 2 Comparison of adsorption capacity
[0079] Example and comparative example number Comparative Example Example 1 201mg / g 298mg / g 2 184mg / g 255mg / g 3 166mg / g 224mg / g 4 173mg / g 240mg / g
[0080] The adsorbent prepared in the above examples and comparative examples was placed in a mixed aqueous solution of potassium iodide and potassium chloride, wherein Cl - :I - =200:1, and the selectivity of iodide ions was compared.
[0081] Table 3 Comparison of iodide ion selectivity
[0082]
[0083]
[0084] The above is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A gel-type adsorbent modified by a cationic surfactant, characterized in that: Prepared by the following method: Step 1, mixing polyhydroxyamine and silane coupling agent to form solution A; Step 2, adding deionized water to solution A, stirring to perform a hydrolysis reaction, and forming an organic gelling material with a three-dimensional network structure; Step 3, aging the organic gelling material obtained in step 2, washing, drying, and grinding to obtain an adsorbent precursor; Step 4, mixing the adsorbent precursor, the cationic surfactant with a quaternary ammonium salt group and deionized water for reaction, and collecting the solid after the reaction is completed; Step 5, washing and drying the solid to obtain a gel-type adsorbent modified by a cationic surfactant.
2. The gel-type adsorbent according to claim 1, characterized in that: In the step 1, the polyhydroxyamine contains one or more of a hydroxyl group and an amine group, an imine group or a tertiary amine group. Preferably, the polyhydroxyamine is glycerolamine, diethanolamine, triethanolamine, dimethylethanolamine, meglumine, 2-amino-1,3-propanediol, N,N'-di(2-hydroxyethyl)-1,2-ethylenediamine, N-(2-hydroxyethyl)-N-(3-hydroxypropyl)amine, and the silane coupling agent is KH560, KH570 or KH170.
3. The gel-type adsorbent according to claim 1, characterized in that: In the step 1, the mass ratio of the polyhydroxyamine to the silane coupling agent is 1:1 to 1:
5.
4. The gel-type adsorbent according to claim 1, characterized in that: The mass ratio of the deionized water in step 2 to the polyhydroxyamine in step 1 is 1:1 to 8:
1.
5. The gel-type adsorbent according to claim 1, characterized in that: In the step 2, the temperature of the hydrolysis reaction is 20 to 80° C., and the time is 1 to 10 minutes. After the hydrolysis reaction is completed, the excess organic reagent is removed by vacuum rotary evaporation to obtain the organic gelling material. The temperature of the vacuum rotary evaporation is 60 to 85° C., and the speed is 50 to 100 rpm.
6. The gel-type adsorbent according to claim 1, characterized in that: In the step 3, the aging temperature is room temperature, the time is 2 to 12 hours, the drying temperature is 40 to 80° C., the drying time is 8 to 24 hours, and the powder is sieved after grinding, and the mesh size of the sieve is 20 to 100 meshes.
7. The gel-type adsorbent according to claim 1, characterized in that: In the step 4, the cationic surfactant is hexadecyltrimethylammonium chloride, dodecyldimethylbenzylammonium chloride or octadecyldimethylbenzylammonium chloride.
8. The gel-type adsorbent according to claim 1, characterized in that: In step 4, the ratio of the mass fraction of the adsorbent precursor, the volume fraction of the cationic surfactant and the volume fraction of deionized water is 1:(0.1-0.5):1, the unit of the mass fraction is g, the unit of the volume fraction is L, the reaction temperature is 40-60°C, and the reaction time is 2-8h.
9. Use of the gel-type adsorbent according to any one of claims 1 to 8 in adsorption and separation of iodide ions.
10. The use according to claim 9, characterized in that The adsorption equilibrium time is 6 to 8 hours. After the iodine ions are adsorbed, the iodine ions can be separated by desorption using a 0.01 to 0.1 mol / L weak alkaline solution. The weak alkaline solution is an aqueous solution of Na2CO3, K2CO3, Na2SO4, or NH4HCO3.
Citation Information
Patent Citations
Gel type iodine ion adsorbent and preparation method and application thereof
CN103071457A