Perovskite solar cell and preparation method thereof
The magnetron sputtering process forms a doped perovskite layer with high uniformity in perovskite solar cells, which solves the problems of poor uniformity and many defects in the preparation of traditional perovskite layers, and significantly improves the battery performance.
Patent Information
- Application Number
- CN202411754239.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-02
- Publication Date
- 2025-03-07
AI Technical Summary
The preparation uniformity of perovskite layers in traditional perovskite solar cells is poor, with many defects, and poor doping quality, which affects the performance of the battery.
The magnetron sputtering process is used to form a doped perovskite layer on the substrate. By applying radio frequency and DC power to the perovskite target and metal target, the initial perovskite film is deposited and annealed to form a doped perovskite layer with high uniformity and few defects.
The film layer quality of the doped perovskite layer is improved, and the performance of perovskite solar cells is enhanced, including improving the photoelectric conversion efficiency and filling factor of the cells.
Smart Images

Figure CN119584832A_ABST
Abstract
Description
Technical Field
[0001] The disclosed embodiments relate to the field of solar cells, and in particular to a perovskite solar cell and a method for preparing the same. Background Art
[0002] Perovskite solar cells have the characteristics of high conversion efficiency, simple preparation process, light weight, and adjustable spectral range, and have received extensive attention from researchers at home and abroad. Since the first report, after more than ten years of development, a conversion efficiency of more than 26% has been achieved. At present, the perovskite layer in common metal perovskite solar cells is mainly prepared by solution spin coating (such as one-step spin coating, two-step spin coating), liquid phase scraping, evaporation deposition (such as dual-source co-evaporation, continuous evaporation) and liquid-assisted gas phase method, and then the perovskite layer, functional layer (such as electron transport layer or hole transport layer), metal electrode and back electrode are connected to form a complete circuit. However, the perovskite layer in traditional perovskite solar cells still has problems such as poor uniformity of large-area preparation and many defects, that is, the film quality of the perovskite layer prepared by the preparation method in the relevant technology is poor, which restricts the development of perovskite solar cells in the field of flexible solar cells and the further improvement of the photoelectric performance of the battery.
[0003] In addition, there are certain problems in the preparation of doped perovskite layers in perovskite solar cells in related technologies. For example, the preparation of mixed cation perovskite solar cells by alkali metal doping and the preparation of Pb-Sn mixed perovskite solar cells by Sn doping adopt a solution method, which faces the problems of limited solubility of some elements in organic solvents and difficulty in controlling the doping content of elements. As a result, the doping quality of doped perovskites in related technologies is poor, affecting the performance of the finally prepared perovskite solar cells.
[0004] In summary, the film quality and doping quality of the doped perovskite layer in the related art are relatively poor, so that the performance of the perovskite solar cell in the related art needs to be improved. Summary of the invention
[0005] The embodiments of the present disclosure provide a perovskite solar cell and a method for preparing the same, which can at least improve the performance of the perovskite solar cell.
[0006] According to some embodiments of the present disclosure, on the one hand, an embodiment of the present disclosure provides a method for preparing a perovskite solar cell, comprising: providing a substrate, the substrate having a first surface and a second surface relative to each other; using a magnetron sputtering process to form a doped perovskite layer on the first surface, the doped perovskite layer being doped with an alkali metal element or a tin element; wherein the step of forming the doped perovskite layer comprises: providing a perovskite target and a metal target, placing the perovskite target, the metal target and the substrate in a magnetron sputtering chamber, and heating the substrate to a preset temperature, the metal target comprising the alkali metal element or the tin element; applying an RF power supply to the perovskite target, applying a DC power supply to the metal target, and simultaneously turning on the RF power supply and the DC power supply, wherein the power of the RF power supply is less than the power of the DC power supply, so as to deposit an initial perovskite film on the first surface; annealing the initial perovskite film to convert the initial perovskite film into the doped perovskite layer.
[0007] In some embodiments, the preset temperature is 60°C to 80°C; the ratio of the power of the RF power supply to the power of the DC power supply is 1 / 10 to 1, wherein the first preset power is the power of the RF power supply, and the second power is the power of the DC power supply.
[0008] In some embodiments, the power of the RF power source is 2W to 6W, and the power of the DC power source is 6W to 20W.
[0009] In some embodiments, the process parameters of the annealing treatment include: an annealing temperature of 120° C. to 180° C., and an annealing time of 5 min to 20 min.
[0010] In some embodiments, the distance between the perovskite target and the first surface is 10 cm to 20 cm; the distance between the metal target and the first surface is 10 cm to 20 cm.
[0011] In some embodiments, the step of forming the perovskite target material includes: forming a perovskite single crystal powder by an inversion crystallization process; and grinding and pressing the perovskite single crystal powder to form the perovskite target material.
[0012] In some embodiments, the perovskite target is a MAPbI3 target; the steps of the inversion crystallization process include: preparing a mixed solution of lead iodide and methylammonium iodide in a molar ratio of 1:1 in a γ-butyrolactone solution, and stirring the mixed solution at 20°C to 30°C until it is clarified; filtering the stirred mixed solution into a clean beaker through a polytetrafluoroethylene filter, placing the beaker in an oven at 110°C to 120°C, and keeping it warm for 24h to 36h to obtain MAPbI3 single crystal powder; grinding and pressing the MAPbI3 single crystal powder to form the MAPbI3 target.
[0013] In some embodiments, the perovskite target is a CsPbI3 target; the steps of the inversion crystallization process include: preparing a mixed solution of cesium iodide and lead iodide in a molar ratio of 1:2 in a dimethyl sulfoxide solution; heating the mixed solution to 60°C to 80°C using a sand bath heating method, mixing 10g to 16g of cyclohexanol and 20g to 30g of dimethylformamide and quickly adding them to the mixed solution, slowly heating to 100°C to 120°C at a heating rate of 0.5°C / min to 2°C / min, and keeping warm for 10h to 14h to obtain a CsPbI3 single crystal powder; washing the CsPbI3 single crystal powder with the dimethylformamide at a temperature of 90°C to 110°C, and drying it in a vacuum oven; grinding and pressing the washed and dried CsPbI3 single crystal powder to form the CsPbI3 target.
[0014] In some embodiments, the step of forming the substrate includes: providing a conductive substrate, the conductive substrate including a supporting substrate and a first electrode layer, the supporting substrate being a rigid substrate or a flexible substrate; forming a first charge transport layer on a surface of the first electrode layer facing away from the supporting substrate by a spin coating process, the first surface being a surface of the first charge transport layer facing away from the first electrode layer; after forming the doped perovskite layer, the method for preparing a perovskite solar cell also includes: forming a second charge transport layer on a surface of the doped perovskite layer facing away from the substrate; forming a second electrode layer on a surface of the second charge transport layer facing away from the doped perovskite layer; wherein the first charge transport layer is one of an electron transport layer and a hole transport layer, and the second charge transport layer is the other of the electron transport layer and the hole transport layer.
[0015] According to some embodiments of the present disclosure, on the other hand, the embodiments of the present disclosure further provide a perovskite solar cell prepared by the preparation method of the above embodiments, comprising: a substrate having a first surface and a second surface relative to each other; and a doped perovskite layer, wherein the doped perovskite layer is located on the first surface of the substrate.
[0016] The technical solution provided by the embodiments of the present disclosure has at least the following advantages:
[0017] The technical solution of the preparation method of the perovskite solar cell provided in the embodiment of the present disclosure includes: providing a substrate, the substrate having a first surface and a second surface relative to each other; using a magnetron sputtering process to form a doped perovskite layer on the first surface, wherein the doped perovskite layer is doped with an alkali metal element or a tin element; wherein the step of forming the doped perovskite layer includes: providing a perovskite target material and a metal target material, placing the perovskite target material, the metal target material and the substrate in a magnetron sputtering chamber, and heating the substrate to a preset temperature, wherein the metal target material includes an alkali metal element or a tin element; applying a radio frequency power supply to the perovskite target material, applying a direct current power supply to the metal target material, and simultaneously turning on the radio frequency power supply and the direct current power supply, wherein the power of the radio frequency power supply is less than the power of the direct current power supply, so as to deposit an initial perovskite film on the first surface; and annealing the initial perovskite film to convert the initial perovskite film into a doped perovskite layer. In the preparation method of the embodiment of the present disclosure, magnetron sputtering is used to prepare the doped perovskite layer. During the magnetron sputtering process, the ions in the plasma are used to bombard the perovskite target and the metal target with high energy under electric field acceleration, so that the perovskite target and the metal target escape and deposit on the substrate in a relatively uniform and orderly manner, and a doped perovskite layer with high uniformity and fewer defects can be obtained, which can improve the film quality of the doped perovskite layer, thereby improving the performance of the perovskite solar cell. The use of high-energy ions to bombard the metal target during the magnetron sputtering process is conducive to the effective diffusion and solid solution of the alkali metal elements or tin elements in the metal target in the perovskite layer, so that the alkali metal elements or tin elements can be effectively incorporated into the perovskite layer and form a doped perovskite layer with excellent doping quality, thereby improving the performance of the perovskite solar cell. In addition, the doping content of the doped perovskite layer can be adjusted by adjusting the process parameters of magnetron sputtering, such as adjusting the power of the RF power supply or adjusting the power of the DC power supply. Therefore, the alkali metal element content or the tin element content in the doped perovskite layer prepared by magnetron sputtering can be regulated according to actual needs. The energy level structure of the perovskite solar cell can be optimized by changing the alkali metal element content or the tin element content in the doped perovskite layer, thereby improving the performance of the perovskite solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] One or more embodiments are exemplarily illustrated by pictures in the corresponding drawings, and these exemplified descriptions do not constitute a limitation on the embodiments. Unless otherwise specified, the pictures in the drawings do not constitute a scale limitation. In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the traditional technology, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 A schematic diagram of magnetron sputtering of a perovskite target and a metal target is provided for the embodiment of the present disclosure;
[0020] Figure 2 A cross-sectional view of a perovskite solar cell provided in an embodiment of the present disclosure;
[0021] Figure 3 Another cross-sectional view of a perovskite solar cell provided in an embodiment of the present disclosure;
[0022] Figure 4 This is a SEM image of the doped perovskite layer prepared in Example 1;
[0023] Figure 5 This is a SEM image of the doped perovskite layer prepared in Example 2;
[0024] Figure 6 This is a SEM image of the doped perovskite layer prepared in Example 3;
[0025] Figure 7 Schematic diagram of the preparation of materials for each film layer in the perovskite solar cell as well as the arrangement of the perovskite target material and the metal target material for Examples 1 to 14;
[0026] Figure 8 The volt-ampere characteristic curve of the perovskite solar cell prepared in Example 1;
[0027] Fig. 9 This is a graph showing the volt-ampere characteristic of the perovskite solar cell prepared in Example 2;
[0028] Fig.10 This is a graph showing the volt-ampere characteristic of the perovskite solar cell prepared in Example 3;
[0029] Fig.11 This is a graph showing the volt-ampere characteristic of the perovskite solar cell prepared in Example 4. DETAILED DESCRIPTION
[0030] As can be seen from the background technology, the film quality and doping quality of the doped perovskite layer in the related art are relatively poor, so that the performance of the perovskite solar cell in the related art needs to be improved.
[0031] In the preparation method of the embodiment of the present disclosure, magnetron sputtering is used to prepare the doped perovskite layer. During the magnetron sputtering process, the ions in the plasma are used to bombard the perovskite target and the metal target with high energy under electric field acceleration, so that the perovskite target and the metal target escape and deposit on the substrate in a relatively uniform and orderly manner, and a doped perovskite layer with high uniformity and fewer defects can be obtained, which can improve the film quality of the doped perovskite layer, thereby improving the performance of the perovskite solar cell. The use of high-energy ions to bombard the metal target during the magnetron sputtering process is conducive to the effective diffusion and solid solution of the alkali metal elements or tin elements in the metal target in the perovskite layer, so that the alkali metal elements or tin elements can be effectively incorporated into the perovskite layer to form a doped perovskite layer with excellent doping quality, thereby improving the performance of the perovskite solar cell. In addition, the doping content of the doped perovskite layer can be adjusted by adjusting the process parameters of magnetron sputtering, such as the power of the RF power supply or the power of the DC power supply. Therefore, the alkali metal element content or the tin element content in the doped perovskite layer prepared by magnetron sputtering can be regulated according to actual needs. The energy level structure of the perovskite solar cell can be optimized by changing the alkali metal element content or the tin element content in the doped perovskite layer, thereby improving the performance of the perovskite solar cell.
[0032] The following will describe the various embodiments of the present disclosure in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present disclosure, many technical details are provided in order to enable the reader to better understand the present disclosure. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solutions claimed in the present disclosure can be implemented.
[0033] Figure 1 A schematic diagram of magnetron sputtering of a perovskite target and a metal target is provided for the embodiment of the present disclosure. Figure 2 A cross-sectional view of a perovskite solar cell provided in an embodiment of the present disclosure. Figure 1 112 in the figure represents perovskite particles sputtered from the perovskite target, and 113 represents metal particles sputtered from the metal target. It can be understood that Figure 1 The numbers of sputtered perovskite particles and metal particles are for reference only; Figure 1 The direction of the arrows in the figure is the rotation direction of the metal target and the perovskite target. It can be understood that the metal target can also rotate clockwise, and the perovskite target can also rotate clockwise.
[0034] Combined with reference Figure 1 and Figure 2The preparation method of the perovskite solar cell includes: providing a substrate 100, wherein the substrate 100 has a first surface 11 and a second surface 12 opposite to each other; using a magnetron sputtering process to form a doped perovskite layer 101 on the first surface 11, wherein the doped perovskite layer 101 is doped with an alkali metal element or a tin element; wherein the step of forming the doped perovskite layer 101 includes: providing a perovskite target material 102 and a metal target material 103, placing the perovskite target material 102, the metal target material 103 and the substrate 100 In a magnetron sputtering chamber, a substrate 100 is heated to a preset temperature, and a metal target 103 includes an alkali metal element or a tin element; an RF power supply is applied to the perovskite target 102, and a DC power supply is applied to the metal target 103, and the RF power supply and the DC power supply are turned on at the same time, and the power of the RF power supply is less than the power of the DC power supply, so as to deposit an initial perovskite film 111 on the first surface 11; the initial perovskite film 111 is annealed to convert the initial perovskite film 111 into a doped perovskite layer 101.
[0035] refer to Figure 2 , the substrate 100 includes a conductive substrate 110 and a first charge transport layer 120 .
[0036] In some embodiments, the step of forming the substrate 100 includes: providing a conductive substrate 110, the conductive substrate 110 includes a supporting substrate 130 and a first electrode layer 140, and the supporting substrate 130 can be a rigid substrate or a flexible substrate; forming a first charge transfer layer 120 on the surface of the first electrode layer 140 away from the supporting substrate 130 by a spin coating process, and the first surface 11 is the surface of the first charge transfer layer 120 away from the first electrode layer 140.
[0037] The carrier substrate 130 is used to provide support for other film layers in the perovskite solar cell. The carrier substrate 130 can be a rigid substrate such as a glass substrate, a silicon substrate or a ceramic substrate, or a flexible substrate composed of any one of polyethylene terephthalate (PET), polyethylene 2,6-naphthalate (PEN), polyethersulfone (PES) and polyimide (PI).
[0038] The first electrode layer 140 is used to collect a type of carrier (electron or hole) generated by the doped perovskite layer 101 and conduct the carrier to an external circuit.
[0039] The first electrode layer 140 may be a conductive material with good light transmittance, such as ITO (Indium Tin Oxide) or FTO (Fluorine-doped Tin Oxide).
[0040] The first electrode layer 140 can be formed on the carrier substrate 130 by magnetron sputtering. With this configuration, the first electrode layer 140 and the carrier substrate 130 can have good adhesion, so that the first electrode layer 140 and the carrier substrate 130 are closely attached to each other and can together form a conductive substrate 110 with a stable structure.
[0041] Before forming the first charge transport layer 120, the preparation method further includes: ultrasonically cleaning the conductive substrate 110 with detergent, ultrapure water and anhydrous ethanol in sequence; thereafter, drying the cleaned conductive substrate 110 with nitrogen and placing it in an ultraviolet-ozone device for surface treatment to improve the wettability of the conductive substrate 110.
[0042] The first charge transport layer 120 is used to transport a type of carrier (electron or hole) generated by the doped perovskite layer 101 to the first electrode layer 140. The first charge transport layer 120 is a hole transport layer or an electron transport layer.
[0043] The preparation process of the first charge transport layer 120 includes magnetron sputtering and spin coating.
[0044] The first charge transport layer 120 may be an electron transport layer for transporting electrons, such as a ZnO (zinc oxide) layer or a SnO2 (tin oxide) layer. The first charge transport layer 120 may also be a NiO x A hole transport layer for transporting holes is formed by using a (nickel oxide) layer, Spiro-OMeTAD (2,2',7,7'-tetrakis(N,N-di(4-methoxyphenyl)amino)-9,9'-spirobifluorene) or the like.
[0045] In some embodiments, the first charge transport layer 120 can be a SnO2 layer, and the steps of preparing the first charge transport layer 120 include: mixing 2ml~3ml (for example, 2mL, 2.3mL, 2.5mL or 3mL) of ultrapure water with 0.2mL~0.8mL (for example, 0.2mL, 0.3mL, 0.5mL or 0.8mL) of SnO2 nanoparticle solution to form a solution, and spin coating it on the above-mentioned UV-ozone treated conductive substrate 110, the spin coating time is 20s~30s (for example, 20s, 23s, 25s, 28s or 30s), and the rotation speed of the conductive substrate 110 is 3000rpm (revolutions per minute)~5000rpm (for example, 3000rpm, 3500rpm, 4000rpm, 4500rpm or 5000rpm). After spin coating, the conductive substrate 110 is placed on a heating stage and annealed at 160° C. to 180° C. (e.g., 160° C., 165° C., 170° C., 175° C., or 180° C.) for 20 minutes to 40 minutes (e.g., 20 minutes, 25 minutes, 30 minutes, 35 minutes, or 40 minutes).
[0046] In some embodiments, the first charge transport layer 120 is NiO x The step of preparing the first charge transport layer 120 includes: adding 2 mg to 6 mg (for example, 2 mg, 3 mg, 4 mg, 5 mg or 6 mg) of NiO x Dissolve in 2mL to 3mL (e.g., 2mL, 2.3mL, 2.5mL, 2.8mL or 3mL), stir evenly, and spin-coat on the above-mentioned UV-ozone treated conductive substrate 110, the spin-coating time is 20s to 30s (e.g., 20s, 23s, 25s, 28s or 30s), and the rotation speed of the conductive substrate 110 is 2000rpm to 4000rpm (e.g., 2000rpm, 2500rpm, 3000rpm, 3500rpm or 4000rpm). After the spin coating is completed, the conductive substrate 110 is placed on a heating table and annealed at 80°C to 100°C (e.g., 80°C, 85°C, 90°C, 95°C or 100°C) for 5 minutes to 15 minutes (e.g., 5 minutes, 8 minutes, 10 minutes, 12 minutes or 15 minutes).
[0047] In some embodiments, the step of forming the perovskite target 102 includes: forming a perovskite single crystal powder by an inversion crystallization process; grinding and pressing the perovskite single crystal powder to form the perovskite target 102. The perovskite single crystal powder is prepared by the inversion crystallization process, and a perovskite target 102 with a higher purity can be prepared. The inversion crystallization process has simple steps, which is conducive to improving the preparation efficiency of perovskite solar cells.
[0048] The perovskite target 102 may be an all-inorganic metal halide target (such as CsPbI3, CsPbBr3, etc.), an organic-inorganic metal halide target (such as MAPbI3 or FAPbI3, etc.), etc.
[0049] In some embodiments, the perovskite target 102 is a MAPbI3 target; the steps of the inversion crystallization process include: preparing a mixed solution of lead iodide and methylammonium iodide in a molar ratio of 1:1 in a γ-butyrolactone solution, and stirring the mixed solution at 20°C to 30°C (for example, 20°C, 23°C, 25°C, 28°C or 30°C) until the mixed solution is clarified; filtering the stirred mixed solution into a clean beaker through a polytetrafluoroethylene filter, placing the beaker in an oven at 110°C to 120°C (for example, 110°C, 113°C, 115°C or 120°C), and keeping the temperature in an oven for 24h to 36h (for example, 24h, 26h, 28h, 30h, 32h, 34h or 36h) to obtain a MAPbI3 single crystal powder; grinding and pressing the MAPbI3 single crystal powder to form a MAPbI3 target.
[0050] In some embodiments, in some embodiments, the perovskite target 102 is a CsPbI3 target; the steps of the inversion crystallization process may include: in a dimethyl sulfoxide solution, a mixed solution of cesium iodide and lead iodide in a molar ratio of 1:2 is prepared; the mixed solution is heated to 60°C to 80°C (for example, 60°C, 65°C, 70°C, 75°C or 80°C) using a sand bath heating method, 10g to 16g (for example, 10g, 12g, 13g or 16g) of cyclohexanol and 20g to 30g (for example, 20g, 23g, 25g, 28g or 30g) of dimethylformamide are mixed and quickly added to the mixed solution, and the mixture is heated at a rate of 0.5°C / min to 2°C / min (for example, 0.5 The method comprises the following steps: slowly heating the CsPbI3 single crystal powder to 100°C-120°C (for example, 100°C, 105°C, 110°C, 115°C or 120°C) at a heating rate of 1°C / min, 1°C / min, 1.5°C / min or 2°C / min), and keeping the temperature for 10h-14h (for example, 10h, 11h, 12h, 13h or 14h) to obtain a CsPbI3 single crystal powder; washing the CsPbI3 single crystal powder with a dimethylformamide solution at a temperature of 90°C-110°C (for example, 90°C, 95°C, 100°C, 105°C or 110°C), and drying the powder in a vacuum oven; grinding and pressing the washed and dried CsPbI3 single crystal powder to form a CsPbI3 target.
[0051] In some embodiments, the preset temperature is 60° C. to 80° C., for example, 60° C., 65° C., 70° C., 75° C. or 80° C. When the preset temperature is within this range, the performance deterioration problems such as deformation of the substrate 100 or decomposition of the substrate 100 material caused by the preset temperature being too high can be avoided, and the problems such as insufficient adhesion between the doped perovskite film and the substrate 100 caused by the preset temperature being too low can also be avoided.
[0052] The metal target 103 may be a target containing an alkali metal element such as a Cs (cesium) target or a K (potassium) target, or may be a Sn target.
[0053] In some embodiments, after placing the metal target 103, the perovskite target 102 and the sample in the magnetron sputtering chamber, the vacuum degree of the sputtering chamber is adjusted to less than 10 -3 Such an arrangement can reduce the number of gas molecules in the sputtering chamber, reduce the collision between the metal particles 113 and the perovskite particles 112 and the gas molecules, and thus improve the preparation efficiency of the initial perovskite film 111 .
[0054] The power of the RF power supply of the sputtering perovskite target 102 can be less than the power of the DC power supply of the sputtering metal target 103. The lower RF power supply power helps to reduce the transition loss of the perovskite target during the sputtering process, and can also ensure the stability of sputtering and the quality of the formed film layer. Secondly, metal targets usually have higher electrical conductivity and thermal conductivity, and require higher power density to achieve effective sputtering, so a higher power DC power supply is required. The power of the RF power supply of the sputtering perovskite target 102 can be less than the power of the DC power supply of the sputtering metal target 103. Such a power setting is conducive to optimizing the energy consumption and efficiency of the entire sputtering system, ensuring that different targets can achieve the best sputtering effect during the sputtering process, while reducing the operating cost and maintenance difficulty of the equipment.
[0055] In some embodiments, the ratio of the power of the RF power supply for sputtering the perovskite target 102 to the power of the DC power supply for sputtering the metal target 103 can be 1 / 10 to 1, such as 1 / 10, 3 / 20, 3 / 10, 3 / 5 or 4 / 5. The power of the RF power supply is positively correlated with the number of the sputtered perovskite particles 112 per unit time, and the power of the DC power supply is positively correlated with the number of the sputtered metal particles 113 per unit time. Therefore, the doping content of the metal element in the doped perovskite layer 101 can be adjusted by adjusting the power ratio of the RF power supply to the power ratio of the DC power supply. When the power ratio of the RF power supply to the power ratio of the DC power supply is within the above range, the metal element in the metal target 103 can be effectively doped into the perovskite crystal to form a doped perovskite with good doping quality. When the power ratio is within the above range, the damage to the original structure of the perovskite particles 112 can be minimized while ensuring the effective doping of the metal particles 113, which helps to form a doped perovskite layer 101 with a stable structure.
[0056] In some embodiments, the power of the RF power supply is 2W to 6W, such as 2W, 3W, 4W, 5W or 6W, and the power of the DC power supply is 6W to 20W, such as 6W, 10W, 15W or 20W. The powers of the RF power supply and the DC power supply are respectively within the above ranges, which can avoid the problem of physical damage to the surface of the substrate 100 caused by sputtering of ions with too high energy due to excessive power of the RF power supply and the DC power supply, and can also avoid the problem of too low deposition rate of the perovskite layer caused by too small RF power supply and DC power supply. In other words, when the power of the RF power supply and the DC power supply are within the above ranges, a high deposition rate can be maintained without causing damage to the surface of the substrate 100, thereby improving the preparation reliability and efficiency of the perovskite solar cell.
[0057] It can be understood that the magnetron sputtering time (i.e., the length of time for turning on the RF power supply and the DC power supply at the same time) is positively correlated with the thickness of the initial perovskite film 111 formed by magnetron sputtering. The user can set the magnetron sputtering time according to actual needs. The embodiment of the present disclosure does not limit the magnetron sputtering time.
[0058] In some embodiments, the process parameters of the annealing treatment include: an annealing temperature of 120° C. to 180° C., for example, 120° C., 140° C., 160° C. or 180° C., and an annealing time of 5 min to 20 min, for example, 5 min, 10 min, 15 min or 20 min. When the process parameters of the annealing treatment are within the above range, defects and internal stress of the initial perovskite film 111 can be eliminated, which is beneficial to improving the quality of the doped perovskite layer 101.
[0059] In some embodiments, the distance between the perovskite target 102 and the first surface 11 is 10 cm to 20 cm, for example, 10 cm, 12 cm, 15 cm, 17 cm or 20 cm. The distance between the perovskite target 102 and the first surface 11 is within the above range, which can avoid the perovskite particles 112 being concentratedly deposited in the central area of the substrate 100 due to being too close, and can also avoid the perovskite particles 112 being too scattered during the flight process and unable to be uniformly deposited due to being too far away. In other words, the distance between the perovskite target 102 and the first surface 11 is within the above range, which can allow the perovskite particles 112 to be uniformly deposited on the surface of the substrate 100, which is conducive to improving the uniformity of the finally manufactured doped perovskite layer 101.
[0060] The distance between the metal target 103 and the first surface 11 is 10 cm to 20 cm, for example, 10 cm, 12 cm, 15 cm, 17 cm or 20 cm. When the distance between the metal target 103 and the first surface 11 is within the above range, it is possible to avoid the metal particles 113 being concentratedly deposited in the central area of the substrate 100 due to being too close, and it is also possible to avoid the metal particles 113 being excessively scattered during flight and unable to be uniformly deposited due to being too far away. In other words, when the distance between the metal target 103 and the first surface 11 is within the above range, the metal particles 113 can be uniformly deposited on the surface of the substrate 100, which is beneficial to improving the uniformity of the doped perovskite layer 101 finally produced.
[0061] In some embodiments, the distance between the perovskite target 102 and the first surface 11 is equal to the distance between the metal target 103 and the first surface 11. Since the two targets are at the same distance from the substrate 100, the time and probability of the particles sputtered from them reaching the substrate 100 and the distribution on the surface of the substrate 100 are more similar, which can effectively avoid the component segregation caused by the distance difference, thereby obtaining a doped perovskite layer 101 with uniform composition and stable performance.
[0062] After forming the doped perovskite layer 101, the method for preparing a perovskite solar cell further includes: forming a second charge transport layer 104 on the surface of the doped perovskite layer 101 facing away from the substrate 100; forming a second electrode layer 105 on the surface of the second charge transport layer 104 facing away from the doped perovskite layer 101; wherein the first charge transport layer 120 is one of the electron transport layer and the hole transport layer, and the second charge transport layer 104 is the other of the electron transport layer and the hole transport layer.
[0063] The second charge transport layer 104 is used to transport a type of carrier (electron or hole) generated by the doped perovskite layer 101 to the second electrode layer 105. The polarity of the carriers transported by the second charge transport layer 104 is opposite to the polarity of the carriers transported by the first charge transport layer 120.
[0064] The second charge transport layer 104 may be a Spiro-OMeTAD layer, a PCBM ([6,6]-phenyl-C61-butyric acid methyl ester) layer, or the like.
[0065] The second charge transport layer 104 may be formed by a spin coating method, a chemical vapor deposition method, or the like.
[0066] In some embodiments, the second charge transport layer 104 may be a Spiro-OMeTAD layer, and the preparation steps of the second charge transport layer 104 include: weighing 400 mg to 600 mg (e.g., 400 mg, 450 mg, 500 mg, 550 mg, or 600 mg) of LiTFSI (lithium bis(trifluoromethanesulfonyl imide)) and dissolving it in 1 mL to 2 mL (e.g., 1 mL, 1.2 mL, 1.5 mL, 1.8 mL, or 2 mL) of acetonitrile solution to obtain an acetonitrile solution of LiTFSI; weighing 30 mg to 50 mg (e.g., 30 mg, 35 mg, 40 mg, 45 mg, or 50 mg) of Spiro-OMeTAD and dissolving it in 0.5 mL to 1.5 mL (e.g., 0.5 mL, 0.8 mL, 1 mL, 1.3 mL, or 1.5 mL) of chlorobenzene solution to obtain a chlorobenzene solution of Spiro-OMeTAD; Use a pipette to take 10 μL to 20 μL (10 μL, 13 μL, 15 μL, 18 μL or 20 μL) of LiTFSI acetonitrile solution and 10 μL to 20 μL of TBP (tributyl phosphate) solution in turn and add them to the Spiro-OMeTAD chlorobenzene solution to prepare a Spiro-OMeTAD mixed solution; use a pipette to take 140 μL to 160 μL (140 μL, 145 μL, 150 μL, 150 μL, 180 μL or 20 μL) of LiTFSI acetonitrile solution and 10 μL to 20 μL of TBP (tributyl phosphate) solution in turn and add them to the Spiro-OMeTAD chlorobenzene solution to prepare a Spiro-OMeTAD mixed solution; 5μL or 160μL) of Spiro-OMeTAD mixed solution is spin-coated onto the doped perovskite layer 101, and the spin coating time is 20s to 30s (for example, 20s, 23s, 25s, 28s or 30s). The rotation speed of the doped perovskite layer 101 during the spin coating process is 2000rpm to 4000rpm (for example, 2000rpm, 2500rpm, 3000rpm, 3500rpm or 4000rpm).
[0067] In some embodiments, the second charge transport layer 104 is a PCBM layer, and the preparation steps of the second charge transport layer 104 include: dissolving 30 mg to 50 mg (for example, 30 mg, 35 mg, 40 mg, 45 mg or 50 mg) of PCBM in 2 mL to 3 mL (for example, 2 mL, 2.3 mL, 2.5 mL, 2.8 mL or 3 mL) of o-dichlorobenzene solution, and spin coating it on the surface of the doped perovskite layer 101 away from the substrate 100, and the spin coating time is 20 s to 40 s (for example, 2 0s, 25s, 30s, 35s or 40s), the rotation speed of the doped perovskite layer 101 during the spin coating process is 1000rpm~2000rpm (for example, 1000rpm, 1200rpm, 1500rpm, 1800rpm or 2000rpm), and then annealed at 70℃~80℃ (for example, 70℃, 73℃, 75℃ or 80℃) for 10min~20min (for example, 10min, 12min, 15min, 18min or 20min).
[0068] The second electrode layer 105 is used to collect a type of carrier (electron or hole) generated by the doped perovskite layer 101 and conduct the carrier to an external circuit. The polarity of the carrier collected by the second electrode layer 105 is opposite to the polarity of the carrier collected by the first electrode layer 140.
[0069] The second electrode layer 105 can be a metal electrode such as gold, silver, etc., or can be a carbon electrode.
[0070] The second electrode layer 105 may be formed by a thermal evaporation method, a screen printing method, an inkjet printing method, or the like.
[0071] Figure 3 Another cross-sectional view of a perovskite solar cell provided in an embodiment of the present disclosure.
[0072] refer to Figure 3In some embodiments, the first charge transport layer 120 is a hole transport layer, the second charge transport layer 104 is an electron transport layer, and after forming the electron transport layer and before forming the second electrode layer 105, the step further includes: forming a buffer layer 106 on the surface of the second charge transport layer 104 away from the doped perovskite layer 101; the step of forming the buffer layer 106 includes: dissolving 3 mg to 5 mg (for example, 3 mg, 3.5 mg, 4 mg, 4.5 mg or 5 mg) of BCP in 2 mL to 3 mL (for example, 2 mL, 2.3 mL, 2.5 mL, 2 .8mL or 3mL) of isopropanol solution, rotating the doped perovskite layer at a rotation speed of 4000rpm to 6000rpm (for example, 4000rpm, 4500rpm, 5000rpm, 5500rpm or 6000rpm) for 20s to 30s (for example, 20s, 23s, 25s, 28s or 30s), and then annealing at 40°C to 60°C (for example, 40°C, 45°C, 50°C, 55°C or 60°C) for 9min to 12min (9min, 10min, 11min or 12min).
[0073] The buffer layer 106 can help electrons flow more smoothly from the electron transport layer to the second electrode layer 105, ensure efficient electron collection, improve the short-circuit current density and fill factor of the battery, and thus improve the photoelectric conversion efficiency of the battery. The buffer layer 106 can also adjust the energy level difference between the electron transport layer and the second electrode layer 105 to make them better match, reduce energy loss caused by energy level mismatch, and improve the performance of perovskite solar cells.
[0074] The buffer layer 106 may be a TiO 2 (titanium dioxide) nanoparticle layer or a LiF (lithium fluoride) layer, etc.
[0075] The advantages of the present application are further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present application and are not used to limit the scope of the present application. Unless otherwise specified, the various parameters involved in this specification have general meanings known in the art and can be measured by methods known in the art. For example, it is possible to test according to the method provided in the examples of the present application. In addition, the preferred ranges and options of the various different parameters provided in the various preferred embodiments can be combined arbitrarily, and the various combinations obtained therefrom are all considered to be within the scope of the disclosure of the present application.
[0076] Example 1
[0077] Example 1 provides a formal organic-inorganic metal halide MAPb 0.8 Sn 0.2The preparation method of I3 perovskite solar cell, wherein the supporting substrate is rigid glass, the material of the first electrode layer is FTO, the transparent conductive glass formed together is the conductive substrate, the first charge transport layer (i.e., the electron transport layer) is a SnO2 layer, and the doped perovskite layer is MAPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (i.e., hole transport layer) is a Spiro-OMeTAD layer, and the second electrode layer is a metal electrode silver. The specific steps of Example 1 are as follows:
[0078] 1. The MAPbI3 target is prepared from MAPbI3 single crystal powder, which is grown by the inversion crystallization method. In the γ-butyrolactone (GBL) solution, a mixed solution of PbI2 and MAI with a molar ratio of 1:1 is prepared as the MAPbI3 single crystal growth solution, and the solution is stirred at room temperature until it is clear. The solution is filtered into a clean beaker with a polytetrafluoroethylene filter with a pore size of 0.2 mm, and the beaker is placed in an oven at 115°C and kept warm for 30 hours to obtain MAPbI3 single crystal powder. The MAPbI3 single crystal powder is ground and pressed into a cylindrical shape.
[0079] 2. The transparent conductive glass is ultrasonically cleaned with detergent, ultrapure water and anhydrous ethanol in turn. After that, the cleaned transparent conductive glass is blown dry with nitrogen and placed in a UV-ozone device for surface treatment to improve the wettability of the FTO transparent conductive glass.
[0080] 3. Spin-coat the hole transport layer on the above-treated transparent conductive glass. Mix 2.5 ml of ultrapure water and 0.5 ml of SnO2 nanoparticle solution to prepare a solution, and spin-coat it on the above-treated transparent conductive glass after UV-ozone treatment. The spin-coating time is 25 seconds and the speed is 4000 rpm. After the spin coating is completed, the transparent conductive glass is placed on a heating table and annealed at 170°C for 30 minutes to obtain a substrate.
[0081] 4. Place the substrate, MAPbI3 target and metal Sn target into the magnetron sputtering chamber. The distance between the MAPbI3 target and the substrate is 15 cm, and the distance between the metal Sn target and the substrate is 15 cm. Wait until the chamber is evacuated to a vacuum degree of less than 10 –3 Pa, the substrate was heated to 70°C. The MAPbI3 target material used a 3W RF power supply, and the metal Sn target material used a 10W DC power supply. The MAPbI3 target material and the Sn target material were sputtered simultaneously for 10 minutes to obtain an initial perovskite film. After the sputtering was completed, the initial perovskite film was placed on a heating table at 150°C for annealing for 10 minutes to obtain MAPbI3. 0.8 Sn 0.2 I3 layer.
[0082] 5. In the MAPb prepared above 0.8 Sn 0.2 Spin coat the hole transport layer on the I3 layer. The process includes the following steps: ① Weigh 500 mg of LiTFSI with a balance and dissolve it in 1.5 mL of acetonitrile solution. ② Weigh 40 mg of Spiro-OMeTAD with a balance and dissolve it in 1 mL of chlorobenzene solution. ③ Use a pipette to take 15 μL of solution ① and 15 μL of LTBP solution and add them to solution ② to prepare a Spiro-OMeTAD mixed solution. ④ Use a pipette to take 150 μL of the Spiro-OMeTAD mixed solution and spin coat it on the MAPb prepared above. 0.8 Sn 0.2 On the I3 layer, the spin coating time is 25 s and the rotation speed is 3000 rpm to obtain a hole transport layer.
[0083] 6. Place the sample with the hole transport layer deposited above into the mask, and place it into a thermal evaporation process instrument to deposit the metal electrode Ag. The deposition rate is 0.6 nm / s and the deposition thickness is 100 nm. After the deposition is completed, a formal perovskite solar cell is obtained.
[0084] Example 2
[0085] Example 2 provides a formal all-inorganic metal halide CsPb 0.8 Sn 0.2 Preparation method of I3 perovskite solar cell, wherein the supporting substrate is rigid glass, the material of the first electrode layer is FTO, the FTO transparent conductive glass together constitutes the conductive substrate, the first charge transport layer (i.e., electron transport layer) is SnO2 layer, and the doped perovskite layer is CsPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (ie, hole transport layer) is a Spiro-OMeTAD layer, and the second electrode layer is a metal electrode silver.
[0086] The preparation method of Example 2 is basically the same as that of Example 1, except that the doped perovskite layer in Example 2 is a CsPbI3 target material and a metal Sn target material formed by magnetron sputtering. 0.8 Sn 0.2 I3 layer. Among them, CsPb 0.8 Sn 0.2 The steps of I3 layer are as follows:
[0087] The CsPbI3 target was prepared from CsPbI3 single crystal powder, which was grown by an inversion crystallization method. CsI and PbI2 (1:2 molar ratio) were dissolved in a dimethyl sulfoxide (DMSO) solution by heating from room temperature to 70°C in a sand bath. Then, 13 g of cyclohexanol (CyOH) and 24 g of dimethylformamide (DMF) were mixed and quickly added to the solution. The solution was slowly heated to 110°C at a heating rate of 1°C / min. After 12 hours, CsPbI3 single crystal powder was precipitated from the solution, washed with DMF at 100°C and dried in a vacuum oven at 50°C. The crystals were then ground and pressed into a cylindrical shape.
[0088] Place the substrate, CsPbI3 target and metal Sn target in the magnetron sputtering chamber. The distance between the CsPbI3 target and the substrate is 15 cm, and the distance between the metal Sn target and the substrate is 15 cm. When the chamber is evacuated to a vacuum degree of less than 10 –3 Pa, the substrate temperature was heated to 70°C. The CsPbI3 target material used a 3W RF power supply, and the metal Sn target material used a 10W DC power supply. The CsPbI3 target material and the Sn target material were sputtered simultaneously for 10 minutes to obtain the initial perovskite film. After the sputtering was completed, the initial perovskite film was placed on a heating table at 150°C for annealing for 10 minutes to obtain the CsPb 0.8 Sn 0.2 I3 layer.
[0089] Example 3
[0090] Example 3 provides a trans-organic inorganic metal halide MAPb 0.8 Sn 0.2 Preparation method of I3 perovskite solar cell, wherein the supporting substrate is rigid glass, the material of the first electrode layer is FTO, the transparent conductive glass together constitutes the conductive substrate, and the first charge transport layer (i.e., hole transport layer) is NiO x layer, the doped perovskite layer is MAPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (i.e., electron transport layer) is a PCBM layer, the buffer layer is a BCP layer, and the second electrode layer is a metal electrode silver. The difference between Example 3 and Example 1 is that Example 3 prepares an inverted perovskite solar cell, while Example 1 prepares a formal perovskite solar cell. The specific preparation method of Example 3 is as follows:
[0091] 1. The MAPbI3 target is prepared from MAPbI3 single crystal powder, which is grown by the inversion crystallization method. In the γ-butyrolactone (GBL) solution, a mixed solution of PbI2 and MAI with a molar ratio of 1:1 is prepared as the MAPbI3 single crystal growth solution, and the solution is stirred at room temperature until it is clear. The solution is filtered into a clean beaker with a polytetrafluoroethylene filter with a pore size of 0.2 mm, and the beaker is placed in an oven at 115°C and kept warm for 30 hours to obtain MAPbI3 single crystal powder. The MAPbI3 single crystal powder is ground and pressed into a cylindrical shape.
[0092] 2. The transparent conductive glass is ultrasonically cleaned with detergent, ultrapure water and anhydrous ethanol in sequence. After that, the cleaned transparent conductive glass is blown dry with nitrogen and placed in a UV-ozone device for surface treatment to improve the wettability of the transparent conductive glass.
[0093] 3. Spin-coat the hole transport layer on the treated transparent conductive glass. x ) was dissolved in 2.5 ml of ultrapure water and spin-coated on the above-treated transparent conductive glass. The spin-coating time was 30 seconds and the rotation speed of the transparent conductive glass was 3000 rpm. After the spin coating was completed, the transparent conductive glass was placed on a heating table and annealed at 100° C. for 10 minutes to obtain a substrate.
[0094] 4. Place the above substrate, MAPbI3 target and metal Sn target into the magnetron sputtering chamber. The distance between the MAPbI3 target and the substrate is 15 cm, and the distance between the metal Sn target and the substrate is 15 cm. When the chamber is evacuated to a vacuum degree of less than 10 –3 Pa, the substrate temperature was heated to 70°C. The MAPbI3 target material used a 3W RF power supply, and the metal Sn target material used a 10W DC power supply. The MAPbI3 target material and the Sn target material were sputtered simultaneously for 10 minutes to obtain the initial perovskite film. After the sputtering was completed, the initial perovskite film was placed on a heating table at 150°C for annealing for 10 minutes to obtain the MAPbI3 target material. 0.8 Sn 0.2 I3 layer.
[0095] 5. Spin-coat an electron transport layer on the prepared doped perovskite layer. Dissolve 40 mg of PCBM in 2.5 mL of o-dichlorobenzene solution and spin-coat it on the prepared doped perovskite layer. The spin-coating time is 30 s at a speed of 1500 rpm, and then anneal at 75 ° C for 15 min to obtain an electron transport layer. Dissolve 4 mg of BCP in 2.5 mL of isopropanol, rotate at 5000 rpm for 25 s, and then anneal at 50 ° C for 10 min to obtain a buffer layer.
[0096] 6. Place the sample with the electron transport layer deposited on it into the mask, and place it into a thermal evaporation process instrument to deposit the metal electrode Ag at a deposition rate of 0.6nm / s and a deposition thickness of 100nm. After the metal electrode Ag deposition is completed, an inverse perovskite solar cell can be obtained.
[0097] Example 4
[0098] Example 4 provides a trans-all-inorganic metal halide CsPb 0.8 Sn 0.2 Preparation method of I3 perovskite solar cell, wherein the supporting substrate is rigid glass, the material of the first electrode layer is FTO, the transparent conductive glass together constitutes the conductive substrate, and the first charge transport layer (i.e., hole transport layer) is NiO x layer, the doped perovskite layer is CsPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (ie, electron transport layer) is a PCBM layer, the buffer layer is a BCP layer, and the second electrode layer is a metal electrode silver.
[0099] The preparation method of Example 4 is basically the same as that of Example 3, except that the doped perovskite layer in Example 4 is a CsPbI3 target formed by magnetron sputtering and a metal Sn target. 0.8 Sn 0.2 I3 layer. Among them, CsPb 0.8 Sn 0.2 The steps of I3 layer are as follows:
[0100] The CsPbI3 target was prepared from CsPbI3 single crystal powder, which was grown by an inversion crystallization method. CsI and PbI2 (1:2 molar ratio) were dissolved in a dimethyl sulfoxide (DMSO) solution by heating from room temperature to 70°C in a sand bath. Then, 13 g of cyclohexanol (CyOH) and 24 g of dimethylformamide (DMF) were mixed and quickly added to the solution. The solution was slowly heated to 110°C at a heating rate of 1°C / min. After 12 hours, CsPbI3 single crystal powder was precipitated from the solution, washed with DMF at 100°C and dried in a vacuum oven at 50°C. Then, the crystals were ground and pressed into a cylindrical shape.
[0101] Place the substrate, CsPbI3 target and metal Sn target in the magnetron sputtering chamber. The distance between the CsPbI3 target and the substrate is 15 cm, and the distance between the metal Sn target and the substrate is 15 cm. When the chamber is evacuated to a vacuum degree of less than 10 –3Pa, the substrate temperature was heated to 70°C. The CsPbI3 target material used a 3W RF power supply, and the metal Sn target material used a 10W DC power supply. The CsPbI3 target material and the Sn target material were sputtered simultaneously for 10 minutes to obtain an initial perovskite film. After the sputtering was completed, the initial perovskite film was placed on a heating table at 150°C for annealing for 10 minutes to obtain CsPb 0.8 Sn 0.2 I3 layer.
[0102] Example 5
[0103] Example 5 provides a formal organic-inorganic metal halide MAPb 0.8 Sn 0.2 Preparation method of I3 perovskite solar cell, wherein the supporting substrate is PET, the material of the first electrode layer is ITO, the flexible substrate composed of PET and ITO is a conductive substrate, the first charge transport layer (i.e., electron transport layer) is a SnO2 layer, and the doped perovskite layer is MAPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (ie, hole transport layer) is a Spiro-OMeTAD layer, and the second electrode layer is a metal electrode silver.
[0104] The preparation method of Example 5 is substantially the same as that of Example 1, except that the conductive substrate of Example 5 is different from that of Example 1. Specifically, in Example 5, a flexible supporting substrate PET and ITO together constitute the conductive substrate, while in Example 1, a rigid glass and FTO together constitute the conductive substrate.
[0105] Example 6
[0106] Example 6 provides a trans-organic inorganic metal halide MAPb 0.8 Sn 0.2 The preparation method of I3 perovskite solar cell, wherein the supporting substrate is PET, the material of the first electrode layer is ITO, the flexible substrate composed of PET and ITO is a conductive substrate, and the first charge transport layer (i.e., hole transport layer) is NiO x layer, the doped perovskite layer is MAPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (ie, electron transport layer) is a PCBM layer, the buffer layer is a BCP layer, and the second electrode layer is a metal electrode silver.
[0107] The preparation method of Example 6 is substantially the same as that of Example 3, except that the conductive substrate of Example 6 is different from that of Example 3. Specifically, in Example 6, a flexible supporting substrate PET and ITO together constitute the conductive substrate, while in Example 3, a rigid glass and FTO together constitute the conductive substrate.
[0108] Example 7
[0109] Example 7 provides a formal organic-inorganic metal halide MAPb 0.8 Sn 0.2 The preparation method of I3 perovskite solar cell, wherein the supporting substrate is flexible glass, the material of the first electrode layer is ITO, the flexible conductive glass together constitutes the conductive substrate, the first charge transport layer (i.e., the electron transport layer) is a SnO2 layer, and the doped perovskite layer is MAPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (ie, hole transport layer) is a Spiro-OMeTAD layer, and the second electrode layer is a metal electrode silver.
[0110] The preparation method of Example 7 is substantially the same as that of Example 1, except that the conductive substrate of Example 7 is different from that of Example 1. Specifically, in Example 7, flexible glass and ITO together constitute the conductive substrate, while in Example 1, rigid glass and FTO together constitute the conductive substrate.
[0111] Example 8
[0112] Example 8 provides a formal all-inorganic metal halide CsPb 0.8 Sn 0.2 Preparation method of I3 perovskite solar cell, wherein the supporting substrate is flexible glass, the material of the first electrode layer is ITO, the flexible conductive glass together constitutes the conductive substrate, the first charge transport layer (i.e., electron transport layer) is SnO2 layer, and the doped perovskite layer is CsPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (ie, hole transport layer) is a Spiro-OMeTAD layer, and the second electrode layer is a metal electrode silver.
[0113] The preparation method of Example 8 is substantially the same as that of Example 2, except that the conductive substrate of Example 8 is different from that of Example 2. Specifically, in Example 8, flexible glass and ITO together constitute the conductive substrate, while in Example 2, rigid glass and FTO together constitute the conductive substrate.
[0114] Example 9
[0115] Example 9 provides a trans-organic inorganic metal halide MAPb 0.8 Sn 0.2 Preparation method of I3 perovskite solar cell, wherein the supporting substrate is flexible glass, the material of the first electrode layer is ITO, the flexible conductive glass together constitutes the conductive substrate, and the first charge transport layer (i.e., hole transport layer) is NiO x layer, the doped perovskite layer is MAPb0.8 Sn 0.2 I3 layer, the second charge transport layer (ie, electron transport layer) is a PCBM layer, the buffer layer is a BCP layer, and the second electrode layer is a metal electrode silver.
[0116] The preparation method of Example 9 is substantially the same as that of Example 3, except that the conductive substrate of Example 9 is different from that of Example 1. Specifically, in Example 9, flexible glass and ITO together constitute the conductive substrate, while in Example 3, rigid glass and FTO together constitute the conductive substrate.
[0117] Example 10
[0118] Example 10 provides a trans-all-inorganic metal halide CsPb 0.8 Sn 0.2 Preparation method of I3 perovskite solar cell, wherein the supporting substrate is flexible glass, the material of the first electrode layer is ITO, the flexible conductive glass together constitutes the conductive substrate, and the first charge transport layer (i.e., hole transport layer) is NiO x layer, the doped perovskite layer is CsPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (ie, electron transport layer) is a PCBM layer, the buffer layer is a BCP layer, and the second electrode layer is a metal electrode silver.
[0119] The preparation method of Example 10 is substantially the same as that of Example 4, except that the conductive substrate of Example 10 is different from that of Example 4. Specifically, in Example 10, flexible glass and ITO together constitute the conductive substrate, while in Example 4, rigid glass and FTO together constitute the conductive substrate.
[0120] Embodiment 11
[0121] Embodiment 11 provides a formal organic-inorganic metal halide Cs 0.2 MA 0.8 The preparation method of PbI3 perovskite solar cell, wherein the supporting substrate is PET, the material of the first electrode layer is ITO, the flexible substrate composed of PET and ITO is a conductive substrate, the first charge transport layer (i.e., electron transport layer) is a SnO2 layer, and the doped perovskite layer is Cs 0.2 MA 0.8 PbI3 layer, the second charge transport layer (ie, hole transport layer) is a Spiro-OMeTAD layer, and the second electrode layer is a metal electrode silver.
[0122] The preparation method of Example 11 is substantially the same as that of Example 5, except that the doped perovskite layer in Example 11 is CsPb formed by magnetron sputtering of MAPbI3 target and metal Cs target. 0.8 Sn0.2 I3 layer. Among them, CsPb 0.8 Sn 0.2 The steps of I3 layer are as follows:
[0123] The MAPbI3 target is prepared from MAPbI3 single crystal powder, which is grown by the inversion crystallization method. In the γ-butyrolactone (GBL) solution, a mixed solution of PbI2 and MAI with a molar ratio of 1:1 is prepared as the MAPbI3 single crystal growth solution, and the solution is stirred at room temperature until it is clear. The solution is filtered into a clean beaker with a polytetrafluoroethylene filter with a pore size of 0.2 mm, and the beaker is placed in an oven at 115°C and kept warm for 30 hours to obtain MAPbI3 single crystal powder. The MAPbI3 single crystal powder is ground and pressed into a cylindrical shape.
[0124] Place the substrate, MAPbI3 target and metal Cs target in the magnetron sputtering chamber. The distance between the MAPbI3 target and the substrate is 15 cm, and the distance between the metal Cs target and the substrate is 15 cm. When the chamber is evacuated to a vacuum degree of less than 10 –3 Pa, the substrate temperature was heated to 70°C. The MAPbI3 target material used a 3W RF power supply, and the metal Cs target material used a 10W DC power supply. The MAPbI3 target material and the Cs target material were sputtered simultaneously for 10 minutes to obtain the initial perovskite film. After the sputtering was completed, the initial perovskite film was placed on a heating table at 150°C for annealing for 10 minutes to obtain CsPb 0.8 Sn 0.2 I3 layer.
[0125] Example 12
[0126] Embodiment 12 provides a trans-organic inorganic metal halide MAPb 0.8 Sn 0.2 The preparation method of I3 perovskite solar cell, wherein the supporting substrate is PET, the material of the first electrode layer is ITO, the flexible substrate composed of PET and ITO is a conductive substrate, and the first charge transport layer (i.e., hole transport layer) is NiO x layer, the doped perovskite layer is MAPb 0.8 Sn 0.2 I3 layer, the second charge transport layer (ie, electron transport layer) is a PCBM layer, the buffer layer is a BCP layer, and the second electrode layer is a metal electrode silver.
[0127] The preparation method of Example 12 is substantially the same as that of Example 6, except that the doped perovskite layer in Example 12 is CsPb formed by magnetron sputtering of MAPbI3 target and metal Cs target. 0.8 Sn 0.2I3 layer. Among them, CsPb 0.8 Sn 0.2 The steps of I3 layer are as follows:
[0128] The MAPbI3 target is prepared from MAPbI3 single crystal powder, which is grown by the inversion crystallization method. In the γ-butyrolactone (GBL) solution, a mixed solution of PbI2 and MAI with a molar ratio of 1:1 is prepared as the MAPbI3 single crystal growth solution, and the solution is stirred at room temperature until it is clear. The solution is filtered into a clean beaker with a polytetrafluoroethylene filter with a pore size of 0.2 mm, and the beaker is placed in an oven at 115°C and kept warm for 30 hours to obtain MAPbI3 single crystal powder. The MAPbI3 single crystal powder is ground and pressed into a cylindrical shape.
[0129] Place the substrate, MAPbI3 target and metal Cs target in the magnetron sputtering chamber. The distance between the MAPbI3 target and the substrate is 15 cm, and the distance between the metal Cs target and the substrate is 15 cm. When the chamber is evacuated to a vacuum degree of less than 10 –3 Pa, the substrate temperature was heated to 70°C. The MAPbI3 target material used a 3W RF power supply, and the metal Cs target material used a 10W DC power supply. The MAPbI3 target material and the Cs target material were sputtered simultaneously for 10 minutes to obtain the initial perovskite film. After the sputtering was completed, the initial perovskite film was placed on a heating table at 150°C for annealing for 10 minutes to obtain CsPb 0.8 Sn 0.2 I3 layer.
[0130] Example 13
[0131] Example 13 provides a formal organic-inorganic metal halide MAPb 0.9 Sn 0.1 The preparation method of I3 perovskite solar cell, wherein the supporting substrate is rigid glass, the material of the first electrode layer is FTO, the transparent conductive glass formed together is the conductive substrate, the first charge transport layer (i.e., the electron transport layer) is a SnO2 layer, and the doped perovskite layer is MAPb 0.9 Sn 0.1 I3 layer, the second charge transport layer (ie, hole transport layer) is a Spiro-OMeTAD layer, and the second electrode layer is a metal electrode silver.
[0132] The preparation method of Example 13 is substantially the same as that of Example 1, except that, in Example 13, when magnetron sputtering the MAPbI3 target and the Sn target, the MAPbI3 target uses a 6W RF power supply, and the metal Sn target uses a 10W DC power supply. In Example 1, when magnetron sputtering the MAPbI3 target and the Sn target, the MAPbI3 target uses a 3W RF power supply, and the metal Sn target uses a 10W DC power supply.
[0133] Embodiment 14
[0134] Example 14 provides a formal organic-inorganic metal halide MAPb 0.6 Sn 0.4 The preparation method of I3 perovskite solar cell, wherein the supporting substrate is rigid glass, the material of the first electrode layer is FTO, the transparent conductive glass formed together is the conductive substrate, the first charge transport layer (i.e., the electron transport layer) is a SnO2 layer, and the doped perovskite layer is MAPb 0.6 Sn 0.4 I3 layer, the second charge transport layer (ie, hole transport layer) is a Spiro-OMeTAD layer, and the second electrode layer is a metal electrode silver.
[0135] The preparation method of Example 14 is substantially the same as that of Example 1, except that, in Example 14, when magnetron sputtering the MAPbI3 target and the Sn target, the MAPbI3 target uses a 3W RF power supply, and the metal Sn target uses a 20W DC power supply. In Example 1, when magnetron sputtering the MAPbI3 target and the Sn target, the MAPbI3 target uses a 3W RF power supply, and the metal Sn target uses a 10W DC power supply.
[0136] Figure 4 This is a SEM (Scanning Electron Microscope) image of the doped perovskite layer prepared in Example 1. Figure 5 This is the SEM image of the doped perovskite layer prepared in Example 2. Figure 6 This is the SEM image of the doped perovskite layer prepared in Example 3.
[0137] Combined with reference Figures 4 to 6 The doped perovskite layers prepared in Examples 1 to 3 can be seen to have obvious grain structures, which indicates that the doped perovskite layers have good crystallinity, and good crystallinity usually means higher carrier mobility, so that the perovskite solar cell can have good performance.
[0138] Table 1 Performance test results of the prepared flexible perovskite solar cells.
[0139] Table 1
[0140]
[0141]
[0142] Among them, in Table 1, the forward sweep (FS) is the scanning of the electrode potential of the perovskite solar cell from a lower potential to a higher potential, the reverse sweep (RS) is the scanning of the electrode potential of the perovskite solar cell from a higher potential to a lower potential, Voc (Open-Circuit Voltage) is the open-circuit voltage of the perovskite solar cell, Jsc (Short-Circuit Current Density) is the short-circuit current density of the perovskite solar cell, FF (FillFactor) is the fill factor of the perovskite solar cell, and PCE (Power Conversion Efficiency) is the photoelectric conversion efficiency of the perovskite solar cell.
[0143] Figure 7 Schematic diagram of the preparation of materials for each film layer in the perovskite solar cell as well as the arrangement of the perovskite target material and the metal target material for Examples 1 to 14; Figure 8 The volt-ampere characteristic curve of the perovskite solar cell prepared in Example 1; Fig. 9 This is a graph showing the volt-ampere characteristic of the perovskite solar cell prepared in Example 2; Fig.10 This is a graph showing the volt-ampere characteristic of the perovskite solar cell prepared in Example 3; Fig.11 This is a graph showing the volt-ampere characteristic of the perovskite solar cell prepared in Example 4. Figure 8 to Figure 11 The black line FS in the figure represents the volt-ampere characteristic curve measured by scanning the electrode potential of the perovskite solar cell from a lower potential to a higher potential, and the red line RS represents the volt-ampere characteristic curve measured by scanning the electrode potential of the perovskite solar cell from a higher potential to a lower potential.
[0144] Combined with reference table 1, Figures 7 to 11, the PCEs of the perovskite solar cells prepared in Examples 1 to 14 were higher than 13% in both forward and reverse scans, which indicates that the uniformity of the doped perovskite layer prepared by magnetron sputtering in the disclosed embodiments is good, and the perovskite solar cell containing the doped perovskite layer prepared by magnetron sputtering has excellent photoelectric performance. Moreover, whether a formal perovskite solar cell or an inverted perovskite solar cell is prepared, whether the supporting substrate in the perovskite solar cell is a rigid substrate or a flexible substrate, and whether the material of the first electrode layer in the perovskite solar cell is ITO or FTO, a high photoelectric conversion efficiency can be achieved, which indicates that the method of preparing the doped perovskite layer by magnetron sputtering is feasible and can be adapted to perovskite solar cells of different structures.
[0145] Referring to Example 1 and Example 13 in Table 1, the difference between the preparation method of Example 1 and the preparation method of Example 13 is that the RF power supply of the magnetron sputtering MAPbI3 target material in Example 13 is twice the RF power supply of the magnetron sputtering MAPbI3 target material in Example 1, and the DC power supply power of the sputtering Sn target material is the same, so that the number of MAPbI3 particles sputtered per unit time in Example 13 is twice the number of MAPbI3 particles sputtered per unit time in Example 1, and the number of Sn particles sputtered per unit time in Example 1 and Example 13 is the same, so that Example 13 obtains a MAPbI3 with half the Sn doping content compared with Example 1. 0.9 Sn 0.1 I3 doped perovskite layer. The PCE values of Example 13 under forward scanning or reverse scanning are lower than the PCE values of Example 1 under forward scanning and reverse scanning, which can illustrate that the doping content of Example 1 has a better effect on the energy level optimization of the perovskite solar cell, making the perovskite solar cell of Example 1 have better performance. It can also be explained that the embodiments of the present disclosure can provide a method for changing the power of the perovskite target material to adjust the content of the metal target material element doped in the doped perovskite layer, and can adjust the photoelectric efficiency of the finally obtained perovskite solar cell.
[0146] Referring to Example 1 and Example 14 in Table 1, the difference between the preparation method of Example 1 and the preparation method of Example 14 is that the DC power supply of the magnetron sputtering Sn target material in Example 14 is twice the DC power supply of the magnetron sputtering Sn target material in Example 1, and the RF power supply power of the sputtering MAPbI3 target material is the same, so that the number of Sn particles sputtered per unit time in Example 14 is twice the number of Sn particles sputtered per unit time in Example 1, and the number of MAPbI3 particles sputtered per unit time in Example 1 and Example 14 is the same, so that Example 14 obtains MAPbI3 with double the Sn doping content compared with Example 1. 0.6 Sn 0.4The PCE value of Example 14 under forward scanning or reverse scanning is different from the PCE values of Example 1 under forward scanning and reverse scanning, which can illustrate that the disclosed embodiments can provide a method for adjusting the content of metal target elements doped in the doped perovskite layer by changing the power of the perovskite target material, so as to change the photoelectric efficiency of the final perovskite solar cell.
[0147] It is understandable that Example 13 and Example 14 only illustrate the schematic diagram of adjusting the power supply power of the perovskite target alone or adjusting the power supply power of the metal target alone. In fact, the power of both can be adjusted at the same time to change the power ratio of the two to adjust the content of the metal target element doped in the doped perovskite layer, which can change the photoelectric efficiency of the solar cell finally obtained. Regarding the optimal content of the metal target element doped in the doped perovskite layer for improving the performance of the perovskite cell, there are certain differences between different perovskite targets and different metal targets. The embodiments of the present disclosure provide a method for adjusting the doping content of the metal target element, so that researchers can optimize the energy level structure of the perovskite solar cell by adjusting the content of the metal target element, thereby improving the performance of the perovskite solar cell.
[0148] In summary, the embodiments of the present disclosure can adjust the content of the metal target element doped in the doped perovskite layer by adjusting the power supply power of the sputtering perovskite target or the power supply power of the sputtering metal target, so as to optimize the energy level structure of the perovskite solar cell and improve the performance of the perovskite solar cell.
[0149] Correspondingly, another embodiment of the present disclosure further provides a perovskite solar cell prepared by the preparation method of any of the above embodiments. For the parts that are the same or corresponding to the previous embodiment, reference can be made to the corresponding description of the previous embodiment, and will not be described in detail below.
[0150] refer to Figure 2 The perovskite solar cell includes: a substrate 100 and a doped perovskite layer 101 , the substrate 100 has a first surface 11 and a second surface 12 opposite to each other; the doped perovskite layer 101 is located on the first surface 11 of the substrate 100 .
[0151] Those skilled in the art can understand that the above-mentioned embodiments are specific examples for realizing the present disclosure, and in practical applications, various changes can be made to them in form and details without departing from the spirit and scope of the present disclosure. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present disclosure, so the protection scope of the present disclosure shall be based on the scope defined in the claims.
Claims
1. A method for preparing a perovskite solar cell, characterized in that: include: providing a substrate having opposing first and second sides; Using a magnetron sputtering process, forming a doped perovskite layer on the first surface, wherein the doped perovskite layer is doped with an alkali metal element or a tin element; Wherein, the step of forming the doped perovskite layer comprises: Providing a perovskite target material and a metal target material, placing the perovskite target material, the metal target material and the substrate in a magnetron sputtering chamber, and heating the substrate to a preset temperature, wherein the metal target material includes the alkali metal element or the tin element; Applying a radio frequency power supply to the perovskite target material and a direct current power supply to the metal target material, and turning on the radio frequency power supply and the direct current power supply at the same time, wherein the power of the radio frequency power supply is less than the power of the direct current power supply, so as to deposit an initial perovskite film on the first surface; The initial perovskite film is annealed to convert the initial perovskite film into the doped perovskite layer.
2. The method for preparing a perovskite solar cell according to claim 1, characterized in that: The preset temperature is 60° C. to 80° C.; the ratio of the power of the radio frequency power source to the power of the direct current power source is 1 / 10 to 1.
3. The method for preparing a perovskite solar cell according to claim 2, characterized in that: The power of the radio frequency power source is 2W to 6W, and the power of the direct current power source is 6W to 20W.
4. The method for preparing a perovskite solar cell according to claim 1, characterized in that: The process parameters of the annealing treatment include: an annealing temperature of 120° C. to 180° C., and an annealing time of 5 min to 20 min.
5. The method for preparing a perovskite solar cell according to claim 1, characterized in that: The distance between the perovskite target and the first surface is 10 cm to 20 cm; the distance between the metal target and the first surface is 10 cm to 20 cm.
6. The method for preparing a perovskite solar cell according to claim 1, characterized in that: The steps of forming the perovskite target material include: Forming perovskite single crystal powder by an inversion crystallization process; The perovskite single crystal powder is ground and pressed to form the perovskite target.
7. The method for preparing a perovskite solar cell according to claim 6, characterized in that: The perovskite target is a MAPbI3 target; The steps of the inversion crystallization process include: In the γ-butyrolactone solution, a mixed solution of lead iodide and methylammonium iodide in a molar ratio of 1:1 is prepared, and the mixed solution is stirred at 20° C. to 30° C. until it becomes clear; The mixed solution after stirring is filtered through a polytetrafluoroethylene filter into a clean beaker, and the beaker is placed in an oven at 110° C. to 120° C. and kept warm for 24 h to 36 h to obtain MAPbI3 single crystal powder; The MAPbI3 single crystal powder is ground and pressed to form the MAPbI3 target.
8. The method for preparing a perovskite solar cell according to claim 6, characterized in that: The perovskite target is a CsPbI3 target; The steps of the inversion crystallization process include: In dimethyl sulfoxide solution, a mixed solution of cesium iodide and lead iodide in a molar ratio of 1:2 is prepared; Heat the mixed solution to 60°C to 80°C by sand bath heating, mix 10g to 16g of cyclohexanol and 20g to 30g of dimethylformamide and quickly add them to the mixed solution, slowly heat to 100°C to 120°C at a heating rate of 0.5°C / min to 2°C / min, and keep warm for 10h to 14h to obtain CsPbI3 single crystal powder; Washing the CsPbI3 single crystal powder with the dimethylformamide at a temperature of 90° C. to 110° C., and drying in a vacuum oven; The cleaned and dried CsPbI3 single crystal powder is ground and pressed to form the CsPbI3 target material.
9. The method for preparing a perovskite solar cell according to claim 1, characterized in that: The steps of forming the substrate include: Providing a conductive substrate, wherein the conductive substrate comprises a supporting substrate and a first electrode layer, wherein the supporting substrate is a rigid substrate or a flexible substrate; forming a first charge transport layer on a surface of the first electrode layer facing away from the supporting substrate by a spin coating process, wherein the first surface is a surface of the first charge transport layer facing away from the first electrode layer; After forming the doped perovskite layer, the method for preparing the perovskite solar cell further comprises: forming a second charge transport layer on a surface of the doped perovskite layer facing away from the substrate; forming a second electrode layer on a surface of the second charge transport layer facing away from the doped perovskite layer; The first charge transport layer is one of an electron transport layer and a hole transport layer, and the second charge transport layer is the other of the electron transport layer and the hole transport layer.
10. A perovskite solar cell prepared by the method for preparing a perovskite solar cell according to any one of claims 1 to 9, characterized in that: include: a substrate having opposing first and second sides; A doped perovskite layer is located on the first surface of the substrate.
Citation Information
Cited By
Solar cell module, preparation method thereof and solar cell
CN120112135A