Ultrathin foam assembly capable of conducting electricity in Z-axis direction
By introducing a closed-cell structure and fiber conductors into the foam material, an ultra-thin foam component that is conductive in the Z-axis direction is formed, which solves the problems of insufficient energy absorption, shock absorption and conductivity of traditional foam materials on AMOLED screens. Efficient shock absorption and conductive properties are achieved.
Patent Information
- Application Number
- CN202420238827.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-01-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2034-01-31
AI Technical Summary
Traditional foam materials are difficult to meet the requirements of AMOLED screens for higher energy absorption, shock absorption, and high impact resistance. They also require conductive properties in the Z-axis direction, and the sealing performance of existing conductive foam materials is insufficient.
Ultra-thin foam components that are conductive in the Z-axis direction are used, including closed-cell structures and fiber conductors. The diameter of the closed-cell structure is 20 μm ~ 80 μm, the diameter of the fiber conductors is 10 μm ~ 20 μm, and the polymer film layer is bidirectionally stretched. Stretched polyethylene terephthalate film is formed by inflating or adding expanded polymer microspheres during the molding process to form a closed-cell structure and form a tight conductive network.
It achieves higher energy absorption, shock absorption and impact resistance, and also has excellent Z-direction conductive performance and sealing performance, providing better damping and shock absorption effect.
Smart Images

Figure CN221841646U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to compressible ultra-thin shock-absorbing conductive foam, in particular to an ultra-thin foam component which is conductive in the Z-axis direction. Background Art
[0002] With the development of science and technology, people's lives cannot be separated from electronic display devices, such as mobile phones and computers. Due to the many advantages of AMOLED, AMOLED technology has a wider range of applications than LCD technology, and can be extended to the fields of electronic products, commerce, transportation, industrial control, and medical fields. Electronic equipment is prone to bumps and falls during use or transportation, so it is necessary to stick a layer of buffer material foam (such as PE foam, EVA foam, PU foam) under the AMOLED screen frame of these electronic devices to absorb the impact of the outside world. However, traditional foam materials such as PU foam, PE foam, acrylic foam and EVA foam are difficult to meet the requirements of AMOLED, such as higher energy absorption, shock absorption and high impact resistance. Moreover, with the development of OLED screens, higher requirements are put forward for acrylic foam used in SCF components, not only for higher shock absorption and buffering requirements, but also for acrylic foam to be conductive in the Z-axis direction, and the conductive resistance must be less than 0.05 ohms. At present, conductive foams are widely used in electronic products, such as conductive foam gaskets and conductive foam washers. Common conductive foam pads contain a conductive foam layer formed by plating metal on an open-cell polyurethane or polyester foam. The minimum thickness of this foam pad is about 0.5 mm, and can reach 0.3 mm after hot pressing, and the minimum is about 0.10 to 0.15 mm. The pores in this foam pad are open, so there is no sealing.
[0003] In order to obtain thin shock-absorbing foam materials with excellent Z-direction conductivity, our company has conducted in-depth research on the influencing factors and found the most optimized material formula and production process. Utility Model Content
[0004] Therefore, the utility model provides an ultra-thin foam component that is conductive in the Z-axis direction, which has higher energy absorption, shock absorption and high impact resistance capabilities, while also meeting excellent sealing performance. Since a considerable portion of the fiber conductors in the Z-axis direction form conductive paths on the upper and lower surfaces of the foam layer, the ultra-thin foam layer has excellent Z-direction conductivity.
[0005] In order to solve the above technical problems, the utility model adopts the following technical solutions:
[0006] An ultra-thin foam component that is conductive in the Z-axis direction, comprising a foam material layer that is conductive in the Z-axis direction and a polymer film layer arranged on at least one side of the foam material that is conductive in the Z-axis direction, wherein the foam material layer has a thickness of 0.07 mm to 0.4 mm, and a closed-cell structure and a fiber-type conductor are arranged in the foam material layer, wherein the diameter of the closed-cell structure is 20 μm to 80 μm.
[0007] The total volume of the closed-cell structure accounts for 20-50% of the volume of the entire conductive foam material layer, preferably 25-40%.
[0008] The fiber-type conductor has a diameter of 10 μm to 20 μm and an average aspect ratio of 5 to 30.
[0009] The fiber-type conductor is one of carbon fiber, metal-plated glass fiber, ceramic fiber, and silver- or nickel-plated glass fiber.
[0010] The fiber-type conductor is arranged between adjacent closed-cell structures and penetrates the foam material layer.
[0011] The polymer film layer is any one of biaxially stretched polyethylene terephthalate film, biaxially stretched or cast polypropylene film, polyethylene film, nylon film, polycarbonate film, polystyrene film, laminated fiber film, polyethylene terephthalate release film, polyethylene coated release paper or other release material film.
[0012] Compared with the prior art, the utility model has the following beneficial effects:
[0013] A. The conductive foam layer material provided by the utility model contains a Z-direction conductive foam material layer, and a closed-cell structure with a diameter of 20 to 80 microns and a fiber-type conductor with a diameter of 10 to 20 microns and an aspect ratio of 5 to 30 is arranged in the conductive foam material layer. The closed-cell structure can be formed in two ways: one is to use an inflation method during the molding process, and the other is to add an expanded closed-cell structure to the film-forming polymer. After coating, the fibrous conductor is evenly distributed in the wet glue layer and forms a uniformly distributed closed-cell structure. After the glue layer enters the oven, the moisture (solvent) in the wet glue layer gradually evaporates. The entire drying process will cause the coating to become thinner, and the closed-cell structure and the volume proportion of the fibrous conductor in the foam layer will gradually increase, resulting in the formation of a tighter conductive network. The presence of the closed-cell structure will squeeze the fibrous conductor and make it easy to form a Z-direction conductive foam layer structure. Since the fibrous conductor has a suitable diameter and aspect ratio, a considerable portion of the fibrous conductor in the entire foam layer will form a conductive path on the upper and lower surfaces of the foam layer after being squeezed by the expanded polymer microspheres, thereby making the ultra-thin foam layer have excellent Z-direction conductivity.
[0014] B. The foam material layer provided by the utility model is a foam material with a closed-cell structure inside, which is made of a film-forming polymer. The cells in the closed-cell structure are obtained by a physical or chemical foaming molding method and process. The pore size of the closed-cell structure is 5 to 200 microns. The cells in the closed-cell structure provide compressibility to the foam. When the foam is squeezed by an external force, the cells will deform. Since it is a closed-cell structure, part of the energy will be absorbed in the process of the cells resisting deformation. This is more conducive to providing better damping and shock absorption effects than foam with an open-cell structure.
[0015] C. The total volume of the closed-cell structure in the present invention accounts for 20-50% of the volume of the entire foam material layer. More preferably, the total volume of the closed-cell structure accounts for 25-40% of the volume of the entire foam material layer. If the volume occupied by the pores in the closed-cell structure is too small, the foam material layer will be difficult to compress, which is not conducive to the assembly of the OLED screen; if the volume occupied by the pores is too large, the damping and shock-absorbing effect of the foam material layer will be significantly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the specific implementation methods of the utility model or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 Schematic diagram of the structure of the ultra-thin foam component that is conductive in the Z-axis direction provided by the utility model
[0018] Figure 2 Schematic diagram of the cross-section of the wet adhesive layer of the foam material after coating and before drying
[0019] Figure 3 This is a schematic cross-sectional diagram of the z-direction conductive foam material layer after drying.
[0020] 1- foam material layer, 11- film-forming polymer, 12- closed-cell structure, 13- fiber-type conductor
[0021] 2-Polymer film layer DETAILED DESCRIPTION
[0022] The technical solution of the utility model will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments of the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.
[0023] like Figures 1 to 3 As shown, the utility model provides an ultra-thin foam component that is conductive in the Z-axis direction, which includes a foam material layer 1 that is conductive in the Z-axis direction and a polymer film layer 2 that is arranged on at least one side of the foam material layer 1 that is conductive in the Z-axis direction; the foam material layer 1 that is conductive in the Z-axis direction includes a film-forming polymer 11, and a closed-cell structure 12 and a fiber-type conductor 13 are arranged in the film-forming polymer 11, and the total volume of the closed-cell structure accounts for 20 to 50% of the volume of the entire conductive foam material layer 1.
[0024] The closed-cell structure 12 fiber-type conductor 13 polymer film layer 2 is selected from any one of biaxially stretched polyethylene terephthalate film, biaxially stretched or cast polypropylene film, polyethylene film, nylon film, polycarbonate film, polystyrene film, laminated fiber film, polyethylene terephthalate release film, polyethylene coated release paper or other release material film;
[0025] The conductive foam material layer 1 in the Z-axis direction has a loss factor of not less than 0.4 in the temperature range of 10 to 30°C; the volume resistance of the ultra-thin conductive foam component is not higher than 100 ohms; the surface resistivity of the ultra-thin conductive foam component is not less than 1 x 10 7 Ohms per square.
[0026] The conductive foam material layer 1 has a loss factor of not less than 0.4 in the temperature range of 5 to 35°C; the density of the conductive foam material layer 1 at room temperature is 0.4 to 0.9 g / cm3; the fiber conductor 13 is arranged between adjacent closed-cell structures 12 and penetrates the foam material layer, and the volume resistance of the ultra-thin conductive foam component is not higher than 10 ohms; the surface resistivity of the ultra-thin conductive foam component is not lower than 1 x 10 9 Ohms per square.
[0027] The film-forming polymer 11 is a core-shell coated structure acrylic copolymer prepared by polymerizing a monomer mixture by an emulsion polymerization method in the presence of a persulfate initiator, and the monomer mixture includes a mixture of two or more monomers selected from the group consisting of methyl (meth)acrylate, isobornyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, acrylonitrile, styrene, butadiene, etc.
[0028] The glass transition temperature Tg of the film-forming polymer 11 is (-10) to 30°C; and the film-forming polymer is copolymerized from at least two or more different monomers whose Tg difference is greater than 50°C.
[0029] The closed-cell structure 12 can be formed in two ways: one is to use an inflation method during the molding process, and the other is to add the expanded closed-cell structure 12 to the film-forming polymer. Specifically:
[0030] The method of forming a closed-cell structure 12 by inflation during the molding process: the film-forming polymer and the fiber-type conductor are placed in a vacuum screw agitator and stirred evenly, and nitrogen with a pressure of 0.1-0.3MPa is injected into the vacuum screw agitator at the same time, and the stirring rate is 100 rpm to 200 rpm. After stirring evenly, it is coated on the PET release film by a scraper coating method, and then the PET release film coated with wet glue is placed in a 90°C oven and dried for 10 minutes, and then taken out to obtain a foam release film composite sample. By setting different scraper gaps, conductive foam layered material samples with thicknesses of 50 microns, 100 microns, 200 microns and 400 microns can be obtained respectively. The schematic cross-sectional diagram of the Z-direction conductive foam material layer after drying is shown in Figure 3 As shown, the white dotted line indicates the direction of electron conduction. Due to the filling of nitrogen during the stirring process, the fiber-like conductors 13 are distributed between the bubbles, and at least a portion of the fiber-like conductors 13 penetrate the foam material layer to achieve the conductive function of the ultra-thin foam component. Here, the fiber-like conductors 13 penetrate the foam material layer, and the penetration method can be vertical penetration of the foam material layer, or it can be bent along the shape of the edge curve of the closed-cell structure and then penetrate the foam material layer. Although some of the fiber-like conductors 13 will be arranged horizontally in the finished product, most of the fiber-like conductors 13 are formed by the extrusion of the gas in the closed-cell structure 12 to penetrate the foam material layer to achieve its conductive function.
[0031] A method for adding expanded polymer microspheres to a film-forming polymer to form a closed-cell structure 12: Place the expanded polymer microspheres and fiber-type conductors 13 in a stirring paddle and stir at a low speed for 15 minutes to form a uniform dispersion, then apply it to a PET release film by scraper coating, and then put the PET release film coated with wet glue into a 90°C oven and dry it for 10 minutes before taking it out to obtain a foam release film composite sample. By setting different scraper gaps, conductive foam layered material samples with thicknesses of 50 microns, 100 microns, 200 microns and 400 microns can be obtained respectively. The schematic diagram of the cross-section of the Z-direction conductive foam material layer after drying is shown in Figure 3 As shown, the white dotted line indicates the direction of electron conduction.
[0032] The diameter of the closed-cell structure 12 is 5 to 200 micrometers; the total volume of the closed-cell structure accounts for 20 to 50% of the volume of the entire conductive foam material layer.
[0033] More preferably, the diameter of the closed-cell structure 12 is 20 to 80 micrometers; the total volume of the closed-cell structure accounts for 25 to 40% of the volume of the entire conductive foam material layer 1;
[0034] The fiber-like conductor 13 has a diameter range of 10 to 20 microns and an average aspect ratio of 5 to 30, where the average aspect ratio is the ratio of the average fiber length to the average fiber diameter; the added amount of the fiber-like conductor 13 is further preferably 3-15%wt of the total weight of the conductive foam material layer 1 in the Z-axis direction.
[0035] The fiber conductor 13 is selected from carbon fiber, metal-plated glass fiber, ceramic fiber, silver- or nickel-plated glass fiber; the added amount of the fiber conductor 13 is further 4-10%wt of the total weight of the conductive foam material layer in the Z-axis direction.
[0036] The volume resistance of the formed ultra-thin conductive foam component is not higher than 1 ohm; further, the surface resistivity of the ultra-thin conductive foam component is not lower than 1 x 10 11 Ohms per square.
[0037] The method for preparing the ultra-thin Z-axis conductive ultra-thin foam component used in the utility model comprises the following steps:
[0038] S1. Preparation of acrylic copolymer seed emulsion:
[0039] 20 g of butadiene, 110 g of styrene, 6 g of sodium dodecyl sulfate and 100 g of deionized water were added to a reaction kettle, heated to 50° C. and stirred continuously for emulsification for 30 minutes under nitrogen protection, 0.12 g of ammonium persulfate was dissolved in 20 g of deionized water and then added dropwise to the reaction solution while keeping the reaction apparatus under nitrogen protection, the temperature was raised to 80° C., and the reaction was continued with stirring for 3 hours to obtain a prepolymer emulsion A;
[0040] Then, 70 g of n-butyl acrylate, 2 g of sodium dodecyl sulfate and 60 g of water were weighed and added into a glass flask, and pre-emulsified for 20 minutes with slow stirring. At the same time, 0.1 g of initiator ammonium persulfate and 20 g of water were weighed and mixed and poured into a dropping funnel. At the same time, the n-butyl acrylate pre-emulsion and the ammonium persulfate aqueous solution were simultaneously added dropwise into the reactor containing the prepolymer emulsion A, and reacted at 80° C. for 3 hours to obtain emulsion B.
[0041] S2. Preparation of film-forming polymer emulsion
[0042] In a three-necked flask, 100 g of deionized water, 4 g of sodium dodecyl sulfate and 4 g of a mixed emulsifier of nonylphenol polyoxyethylene ether were added, and then 50 g of styrene and 50 g of acrylonitrile monomer were added, and stirred for pre-emulsification to obtain a styrene / acrylonitrile pre-emulsion C;
[0043] Then, 200 g of the emulsion B prepared in step S1 was used as the seed emulsion, and 20 g of the emulsion C and 0.05 g of initiator ammonium persulfate were simultaneously added dropwise, reacted at 80° C. for 4 hours, cooled and discharged, to obtain a film-forming polymer emulsion;
[0044] The viscosity of the film-forming polymer emulsion was measured to be 600 mPa.S, and the solid content was 50%. After the emulsion was dried, the glass transition temperature of the polymer was measured by differential scanning calorimetry to be 6°C.
[0045] Embodiment 1:
[0046] The ultra-thin conductive foam layer material provided in this embodiment includes an ultra-thin Z-axis conductive foam material layer 1 and a polymer film layer 2 on at least one side of the conductive foam material layer. The thickness of the ultra-thin conductive foam material layer is 0.07-0.4 mm. The preparation method thereof is as follows:
[0047] 1-S3, Configuration of conductive foam material dispersion:
[0048] Weigh 1 gram of expanded hollow polyacrylonitrile copolymer microspheres of brand DS-050U purchased from Shanghai Daoxin Chemical Co., Ltd., 98 grams of the film-forming polymer emulsion prepared in step S2, 5 grams of silver-coated glass fiber purchased from Porter, USA, 0.5 grams of color paste KA100 purchased from Clariant, 0.1 grams of defoamer BYK023 purchased from BYK, and 1 gram of wetting agent WE-3650 purchased from BASF, add them into a mixing container, stir with a stirring paddle at medium and low speed for 15 minutes until a uniform dispersion is formed and set aside;
[0049] 1-S4, Preparation of Z-direction conductive foam layered materials:
[0050] After the dispersion prepared above is stirred and mixed evenly, it is coated on the PET release film by means of a scraper coating method, and then the PET release film coated with wet glue is placed in a 90°C oven and dried for 10 minutes, and then taken out to obtain a foam release film composite sample. By setting different scraper gaps, conductive foam layered material samples with thicknesses of 50 microns, 100 microns, 200 microns and 400 microns can be obtained respectively. The schematic diagram of the cross-section of the Z-direction conductive foam material layer after drying is shown in Figure 3 As shown, the white dotted line indicates the direction of electron conduction.
[0051] Four thicknesses were prepared using the formulation of Example 1 and tested separately:
[0052] The dried foam layer is peeled off from the PET release film and the thickness, density, surface resistivity, volume resistivity and foam impact absorption of the foam layer are tested.
[0053] The total volume of the closed-cell structure in this embodiment is 35% of the volume of the ultra-thin foam layer, the pore size of the closed-cell structure is 20-80 microns, and the glass transition temperature is 6°C.
[0054] Embodiment 2:
[0055] 2-S3, Configuration of conductive foam material dispersion:
[0056] Weigh 1 gram of expanded hollow polyacrylonitrile copolymer microspheres of brand DS-050U purchased from Shanghai Daoxin Chemical Co., Ltd., 98 grams of the film-forming polymer emulsion prepared in step S2, 2 grams of silver-coated glass fiber purchased from Porter, USA, 0.5 grams of color paste KA100 purchased from Clariant, 0.1 grams of defoamer BYK023 purchased from BYK, and 1 gram of wetting agent WE-3650 purchased from BASF, add them into a mixing container, stir with a stirring paddle at medium and low speed for 15 minutes until a uniform dispersion is formed and set aside;
[0057] 2-S4. Preparation of Z-direction conductive foam layered material:
[0058] The dispersion prepared above was stirred and mixed evenly, and then coated on the PET release film by scraper coating, and then the PET release film coated with wet glue was placed in a 90°C oven for drying for 10 minutes and then taken out to obtain a foam release film composite sample. By setting different scraper gaps, conductive foam layered material samples with thicknesses of 50 microns, 100 microns, 200 microns and 400 microns can be obtained respectively.
[0059] Four thicknesses were prepared using the formulation of Example 2 and tested separately:
[0060] The dried foam layer is peeled off from the PET release film and the thickness, density, surface resistivity, volume resistivity and foam impact absorption of the foam layer are tested.
[0061] The total volume of the closed-cell structure in this embodiment is 35% of the volume of the ultra-thin foam layer, the pore size of the closed-cell structure is 20-80 microns, and the glass transition temperature is 6°C.
[0062] Embodiment 3:
[0063] 2-S3, Configuration of conductive foam material dispersion:
[0064] Weigh 1 gram of expanded hollow polyacrylonitrile copolymer microspheres of brand DS-050U purchased from Shanghai Daoxin Chemical Co., Ltd., 98 grams of the film-forming polymer emulsion prepared in step S2, 7 grams of nickel-plated glass fiber purchased from Porter, USA, 0.5 grams of color paste KA100 purchased from Clariant, 0.1 grams of defoamer BYK023 purchased from BYK, and 1 gram of wetting agent WE-3650 purchased from BASF, add them into a mixing container, stir with a stirring paddle at medium and low speed for 15 minutes until a uniform dispersion is formed and set aside;
[0065] 2-S4. Preparation of Z-direction conductive foam layered material:
[0066] The dispersion prepared above was stirred and mixed evenly, and then coated on the PET release film by scraper coating, and then the PET release film coated with wet glue was placed in a 90°C oven for drying for 10 minutes and then taken out to obtain a foam release film composite sample. By setting different scraper gaps, conductive foam layered material samples with thicknesses of 50 microns, 100 microns, 200 microns and 400 microns can be obtained respectively.
[0067] Four thicknesses were prepared using the formulation of Example 3 and tested separately:
[0068] The dried foam layer is peeled off from the PET release film and the thickness, density, surface resistivity, volume resistivity and foam impact absorption of the foam layer are tested.
[0069] The total volume of the closed-cell structure in this embodiment is 35% of the volume of the ultra-thin foam layer, the pore size of the closed-cell structure is 20-80 microns, and the glass transition temperature is 6°C.
[0070] Embodiment 4:
[0071] 2-S3, Configuration of conductive foam material dispersion:
[0072] Weigh 1 gram of expanded hollow polyacrylonitrile copolymer microspheres of brand DS-050U purchased from Shanghai Daoxin Chemical Co., Ltd., 98 grams of the film-forming polymer emulsion prepared in step S2, 5 grams of nickel-plated glass fiber purchased from Porter, USA, 0.5 grams of color paste KA100 purchased from Clariant, 0.1 grams of defoamer BYK023 purchased from BYK, and 1 gram of wetting agent WE-3650 purchased from BASF, add them into a mixing container, stir with a stirring paddle at medium and low speed for 15 minutes until a uniform dispersion is formed and set aside;
[0073] 2-S4. Preparation of Z-direction conductive foam layered material:
[0074] The dispersion prepared above was stirred and mixed evenly, and then coated on the PET release film by scraper coating, and then the PET release film coated with wet glue was placed in a 90°C oven for drying for 10 minutes and then taken out to obtain a foam release film composite sample. By setting different scraper gaps, conductive foam layered material samples with thicknesses of 50 microns, 100 microns, 200 microns and 400 microns can be obtained respectively.
[0075] Four thicknesses were prepared using the formulation of Example 4 and tested separately:
[0076] The dried foam layer is peeled off from the PET release film and the thickness, density, surface resistivity, volume resistivity and foam impact absorption of the foam layer are tested.
[0077] The total volume of the closed-cell structure in this embodiment is 35% of the volume of the ultra-thin foam layer, the pore size of the closed-cell structure is 20-80 microns, and the glass transition temperature is 6°C.
[0078] Comparative Example 1:
[0079] 2-S3, Configuration of conductive foam material dispersion:
[0080] Weigh 1 gram of expanded hollow polyacrylonitrile copolymer microspheres of brand DS-050U purchased from Shanghai Daoxin Chemical Co., Ltd., 98 grams of the film-forming polymer emulsion prepared in step S2, 5 grams of nickel powder purchased from Porter, USA, 0.5 grams of color paste KA100 purchased from Clariant, 0.1 grams of defoamer BYK023 purchased from BYK, and 1 gram of wetting agent WE-3650 purchased from BASF, add them into a mixing container, stir at medium and low speed with a stirring paddle for 15 minutes until a uniform dispersion is formed and set aside;
[0081] 2-S4. Preparation of Z-direction conductive foam layered material:
[0082] The dispersion prepared above was stirred and mixed evenly, and then coated on the PET release film by scraper coating, and then the PET release film coated with wet glue was placed in a 90°C oven for drying for 10 minutes and then taken out to obtain a foam release film composite sample. By setting different scraper gaps, conductive foam layered material samples with thicknesses of 50 microns, 100 microns, 200 microns and 400 microns can be obtained respectively.
[0083] Four thicknesses were prepared using the formula of Comparative Example 1 and tested separately:
[0084] The dried foam layer is peeled off from the PET release film and the thickness, density, surface resistivity, volume resistivity and foam impact absorption of the foam layer are tested.
[0085] The total volume of the closed-cell structure in this embodiment is 35% of the volume of the ultra-thin foam layer, the pore size of the closed-cell structure is 20-80 microns, and the glass transition temperature is 6°C.
[0086] Comparative Example 2:
[0087] 2-S3, Configuration of conductive foam material dispersion:
[0088] Weigh 1 gram of expanded hollow polyacrylonitrile copolymer microspheres of brand DS-050U purchased from Shanghai Daoxin Chemical Co., Ltd., 98 grams of the film-forming polymer emulsion prepared in step S2, 10 grams of nickel powder purchased from Porter, USA, 0.5 grams of color paste KA100 purchased from Clariant, 0.1 grams of defoamer BYK023 purchased from BYK, and 1 gram of wetting agent WE-3650 purchased from BASF, add them into a mixing container, stir at medium and low speed with a stirring paddle for 15 minutes until a uniform dispersion is formed and set aside;
[0089] 2-S4. Preparation of Z-direction conductive foam layered material:
[0090] The dispersion prepared above was stirred and mixed evenly, and then coated on the PET release film by scraper coating, and then the PET release film coated with wet glue was placed in a 90°C oven for drying for 10 minutes and then taken out to obtain a foam release film composite sample. By setting different scraper gaps, conductive foam layered material samples with thicknesses of 50 microns, 100 microns, 200 microns and 400 microns can be obtained respectively.
[0091] Four thicknesses were prepared using the formula of Comparative Example 2 and tested separately:
[0092] The dried foam layer is peeled off from the PET release film and the thickness, density, surface resistivity, volume resistivity and foam impact absorption of the foam layer are tested.
[0093] The total volume of the closed-cell structure in this embodiment is 35% of the volume of the ultra-thin foam layer, the pore size of the closed-cell structure is 20-80 microns, and the glass transition temperature is 6°C.
[0094] The test results of the embodiments and comparative examples:
[0095]
[0096] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention of the utility model.
Claims
1. An ultra-thin foam component that is conductive in the Z-axis direction, comprising a foam material layer (1) that is conductive in the Z-axis direction and a polymer film layer (2) disposed on at least one side of the foam material layer (1) that is conductive in the Z-axis direction, characterized in that: The thickness of the foam material layer (1) is 0.07 mm to 0.4 mm. The foam material layer (1) comprises a film-forming polymer (11). The film-forming polymer (11) is provided with a closed-cell structure (12) and a fiber-type conductor (13). The diameter of the closed-cell structure (12) is 20 μm to 80 μm.
2. The ultra-thin foam component that is conductive in the Z-axis direction according to claim 1, characterized in that: The total volume of the closed-cell structure accounts for 20 to 50% of the volume of the entire foam material layer (1).
3. The ultra-thin foam component that is conductive in the Z-axis direction according to claim 2, characterized in that: The total volume of the closed-cell structure accounts for 25-40% of the volume of the entire foam material layer (1).
4. The ultra-thin foam component capable of conducting electricity in the Z-axis direction according to claim 1, characterized in that: The fiber-type conductor (13) has a diameter of 10 μm to 20 μm and an average aspect ratio of 5 to 30.
5. The ultra-thin foam component capable of conducting electricity in the Z-axis direction according to claim 4, characterized in that: The fiber-type conductor (13) is one of carbon fiber, metal-plated glass fiber, ceramic fiber, and silver- or nickel-plated glass fiber.
6. The ultra-thin foam component capable of conducting electricity in the Z-axis direction according to claim 1, characterized in that: The fiber-type conductor (13) is arranged between adjacent closed-cell structures (12) and penetrates the foam material layer.
7. The ultra-thin foam component capable of conducting electricity in the Z-axis direction according to claim 1, characterized in that: The polymer film layer (2) is any one of a biaxially stretched polyethylene terephthalate film, a biaxially stretched or cast polypropylene film, a polyethylene film, a nylon film, a polycarbonate film, a polystyrene film, a laminated fiber film, a polyethylene terephthalate release film or a polyethylene coated release paper.