Negative pole piece structure, electrode assembly, battery monomer, electrochemical device and electric equipment
By providing an active material layer, a transition metal carbon/carbon nitride layer and a solid electrolyte layer in the negative electrode sheet structure, the expansion and heat generation problems caused by the exposure of the negative electrode material are solved, and the safety and circulation performance of the battery are improved.
Patent Information
- Application Number
- CN202323078616.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2033-11-14
AI Technical Summary
The existing negative electrode sheet structures have problems such as uncontrolled expansion due to material exposure, safety risks of heat generation, and poor stability of solid-state battery systems.
A negative electrode sheet structure is designed, and at least one side of the current collector includes an active material layer, a transition metal carbon/carbon nitride layer and a solid electrolyte layer in sequence. The transition metal carbon/carbon nitride layer serves as an intermediate conductive layer and a barrier, and the solid state The electrolyte layer promotes lithium ion conduction and provides protection.
It effectively inhibits the fall of the negative electrode material, improves the battery safety and circulation performance, improves energy density and stability, and prevents the risk of lithium excretion.
Smart Images

Figure CN221994497U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of battery structure design, and in particular to a negative electrode sheet structure, an electrode assembly, a battery cell, an electrochemical device and electrical equipment. Background Art
[0002] There are many problems with the existing negative electrode plate structure design: first, the negative electrode material is exposed to the negative electrode surface and will come into direct contact with the electrolyte, the expansion of the plate cannot be suppressed, and the interface film (SEI film) will be repeatedly regenerated and broken; second, the battery is prone to generate a lot of heat after repeated charging, causing safety risks; third, ordinary negative electrode plates are difficult to maintain the high activity of the solid-state battery system and exert stable electrical performance. Therefore, it is very important to develop negative electrode plates with optimized structural design. Utility Model Content
[0003] The utility model aims at the problems in the prior art and discloses a high specific energy and high safety negative electrode sheet structure, an electrode assembly, a battery cell, an electrochemical device and an electrical equipment. The negative electrode sheet structure includes an active material layer, a transition metal carbon / carbonitride layer and a solid electrolyte layer in sequence from at least one side of the current collector to the outside. The utility model solves the problem of easy detachment of the negative electrode through the sequential design of the sheet structure, improves the safety performance of the battery, and effectively improves the energy density and cycle performance of the system.
[0004] The utility model is realized by the following technical solutions:
[0005] The present invention provides a negative electrode plate structure, which includes an active material layer, a transition metal carbon / carbonitride layer, and a solid electrolyte layer in sequence from at least one side of a current collector to the outside.
[0006] The transition metal carbon / carbonitride layer represents a transition metal carbide layer or a transition metal carbon-nitride layer.
[0007] In the design of the present invention, the transition metal carbon / carbonitride layer, on the one hand, serves as an intermediate conductive layer, which is beneficial to the capacity, and on the other hand, the transition metal carbon / carbonitride layer can block the shuttling of inactive substances and avoid side reactions caused by direct contact between active substances and solid electrolytes; the solid electrolyte layer is arranged outside the transition metal carbon / carbonitride layer to promote the conduction of lithium ions and further improve the cycle performance; the solid electrolyte layer can also form an electronic insulating layer on the surface of the negative electrode, which can play a sufficient protective role when the thermal runaway diaphragm fails, and is not prone to the risk of lithium plating, thereby improving safety performance.
[0008] As a further solution, the current collector includes one or more of copper foil, PET copper composite metal foil, aluminum foil, titanium foil, and silver foil.
[0009] As a further solution, the active material layer is selected from one or more of a graphite layer, a single silicon layer, a silicon-containing alloy layer, a silicon-carbon compound layer, and a silicon-oxygen compound layer. The active material of the graphite layer can be artificial graphite, natural graphite, composite graphite, hard carbon, soft carbon, etc. The active material layer can also contain ingredients such as a binder for the purpose of film formation. After adding other ingredients such as a binder to the active material layer, the mass proportion of the active material is not less than 80%, which is conducive to optimizing and improving the capacity.
[0010] As a further solution, the thickness of the active material layer is 20-150 μm. If the thickness is too small, the capacity and energy density of the battery will be affected; if the thickness is too large, the material is easily lost and the mechanical properties are deteriorated.
[0011] As a further solution, the transition metal carbon / carbonitride layer is a two-dimensional transition metal carbide or a two-dimensional transition metal carbon-nitride, and the transition metal is one or more of Ni, Zn, Cu, Co, Ti, and Al.
[0012] As a further solution, the thickness of the transition metal carbon / carbonitride layer is 1-12 μm. If the thickness is too small, it is difficult to play a better role; if the thickness is too large, it will hinder the electrolyte from fully infiltrating the negative electrode layer, which may cause a slight decrease in ion conductivity, and at the same time lead to a thicker negative electrode composite layer and poorer mechanical properties.
[0013] As a further solution, the surface loading of the transition metal carbon / carbonitride layer is 0.5-3 mg / cm 2 When the surface loading is too small, the battery consistency will be poor and the improvement effect will be small; when the surface loading is too large, ion conduction may be hindered, causing battery polarization.
[0014] As a further solution, the transition metal carbon / carbon nitride layer is a Ti2N-Mxenes layer or a Ti3AlC2-Mxenes layer.
[0015] As a further solution, the thickness of the solid electrolyte layer is 1-20 μm. If the thickness is too small, it is difficult to improve the interface stability, and the ion transmission is not significantly improved; if the thickness is too large, the electrode structure will be thicker and the mechanical properties will deteriorate.
[0016] As a further solution, the solid electrolyte layer is one of a polymer electrolyte, an oxide electrolyte, a sulfide electrolyte, and a polymer oxide composite electrolyte. Preferably, it is a lithium lanthanum zirconium oxide (LLZO) solid electrolyte, wherein LLZO includes a cubic garnet type Li7La3Zr2O 12 (LLZO) and its Ta / Ga-doped derivatives (such as Li 6.4 LqCy 1.4 Ta 0.6 O 12 ).
[0017] As a further solution, the solid electrolyte layer is a polymer@oxide composite electrolyte, such as LLZTO and PVDF composite (LLZTO@PVDF), LLZO and PAN composite (LLZO@PAN).
[0018] As a further solution, a lithium-containing metal layer is further provided outside the solid electrolyte layer, and the lithium-containing metal layer is one or more of metallic lithium, metallic lithium foil or metallic lithium alloy foil. The lithium-containing metal layer can be used as a lithium source for pre-lithiation of the negative electrode.
[0019] As a further solution, the thickness of the lithium-containing metal layer is 5-10 μm. If the thickness is too small, it is difficult to achieve a better lithium supplement effect, and if the thickness is too large, there will be a risk of lithium precipitation, and the electrode structure will be thicker and the mechanical properties will deteriorate.
[0020] The present invention also provides an electrode assembly, a battery cell, an electrochemical device or an electrical equipment having a negative electrode plate structure.
[0021] The utility model can solve many problems of the traditional negative electrode from multiple angles through the above structural design. Compared with the prior art, it has the following characteristics and beneficial effects:
[0022] (1) The transition metal carbon / carbonitride layer has high electrical conductivity, low charge and discharge voltage, and is relatively stable in the air, which is conducive to the negative electrode capacity. The active material layer, transition metal carbon / carbonitride layer, and solid electrolyte layer are arranged in sequence on the outside of the current collector. On the one hand, the transition metal carbon / carbonitride layer serves as an intermediate conductive layer, which is conducive to the capacity. On the other hand, the transition metal carbon / carbonitride layer can block the shuttling of inactive substances and avoid direct contact side reactions between the active substance and the solid electrolyte.
[0023] (2) The solid electrolyte layer is arranged outside the transition metal carbon / carbon nitride layer to promote the conduction of lithium ions and further improve the cycle performance; the solid electrolyte layer can also form an electronic insulation layer on the surface of the negative electrode, which can provide sufficient protection when the thermal runaway diaphragm fails, making it less likely to have the risk of lithium plating, thereby improving safety performance.
[0024] (3) The optimized and limited design of the thickness of each layer is conducive to maintaining the stability of interlayer isolation and support while ensuring the matching of ion transmission and accommodation capacity of each layer, preventing problems such as capacity reduction and lithium ion accumulation and precipitation caused by imbalance of ion accommodation capacity between layers.
[0025] (4) In particular, when the present structure is designed for a silicon negative electrode plate structure, the silicon negative electrode has poor conductivity. Providing a transition metal carbon / carbon nitride layer between the active material layer and the solid electrolyte layer can significantly improve the conductivity of the silicon negative electrode material. The overall structure can better inhibit the expansion of the silicon negative electrode and the repeated rupture and formation of the SEI film. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 This is a structural schematic diagram of the negative electrode plate of Example 1 of the utility model.
[0028] Figure 2 This is a structural schematic diagram of the negative electrode plate of Example 5 of the utility model.
[0029] Figure 3 This is a graph showing the gram capacity of Example 1 of the present invention.
[0030] Figure 4 This is a graph showing the gram capacity of comparative example 1 of the present invention.
[0031] Figure 5 It is a cycle diagram of Example 1 and Comparative Example 1 of the utility model.
[0032] Description of reference numerals:
[0033] 1. Current collector; 2. Active material layer; 3. Transition metal carbon / carbonitride layer; 4. Solid electrolyte layer; 5. Lithium-containing metal layer. DETAILED DESCRIPTION
[0034] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other.
[0035] In the description of the present utility model, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present utility model and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present utility model. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present utility model, unless otherwise specified, "multiple" means two or more.
[0036] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installation", "connection" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0037] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments.
[0038] An exemplary structure of the high specific energy and high safety negative electrode plate structure provided by the utility model can be as follows Figure 1 As shown, from both sides of the current collector 1 to the outside, it includes an active material layer 2, a transition metal carbon / carbonitride layer 3, and a solid electrolyte layer 4, as shown in FIG. Figure 2 As shown, preferably, a lithium-containing metal layer 5 may be provided outside the solid electrolyte layer.
[0039] The material layers used in the present invention are all known material layers. The preparation of each material layer can usually be done by slurrying or depositing the main functional materials in the material layer (such as the active material material of the active material layer, the transition metal carbide material or transition metal carbon-nitride material of the transition metal carbon / carbonitride layer, and the solid electrolyte material of the solid electrolyte layer) into a film. Necessary solvents, additives or adhesives and other necessary materials can be added during the slurrying or deposition process. Examples 1 to 5 of the present invention and Comparative Examples 1 to 4 use the corresponding single side, because button batteries are usually coated on a single side. The following is a detailed introduction to each embodiment and comparative example.
[0040] Example 1
[0041] From one side of the current collector 1 to the outside, it includes an active material layer 2, a transition metal carbon / carbon nitride layer 3, and a solid electrolyte layer 4. Among them, the current collector 1 adopts an 8μm copper foil; the active material layer 2 adopts a silicon-graphite composite layer, which is specifically made by mixing silicon oxide and graphite in a mass ratio of 2:8, and slurrying with conductive carbon black (SP), carbon nanotubes (CNT), and polyacrylic acid (PAA) in a mass ratio of 95:2:1:2 and coating on the current collector, and the active material layer 2 is 50μm thick. The transition metal carbon / carbon nitride layer 3 is specifically made of commercially available Ti2N-Mxenes two-dimensional transition metal carbon-nitride uniformly coated on the surface of the dried active material layer, with a thickness of 10μm; the solid electrolyte layer 4 is made of 85% oxide solid electrolyte LLZTO and binder 15% PVDF slurry coating, with a thickness of 15μm.
[0042] Example 2
[0043] The difference from Example 1 is that the active material layer 2 adopts a graphite layer, and the graphite layer is specifically obtained by slurrying graphite and conductive carbon black (SP), carbon nanotubes (CNT), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) in a mass ratio of 96:1.5:0.5:1.5:0.5 and coating the slurry on the current collector, and the rest is the same.
[0044] Example 3
[0045] The difference from Example 2 is that the solid electrolyte layer 4 adopts a LLZO@PAN composite layer, which is specifically made by slurry coating of 85% oxide solid electrolyte LLZTO and 15% PAN binder, with a thickness of 15 μm, and the rest is the same.
[0046] Example 4
[0047] The difference from Example 2 is that the current collector 1 uses an 8 μm PET@copper composite metal foil layer, which is purchased from Guangzhou Nano New Material Technology Co., Ltd., and the rest is the same.
[0048] Example 5
[0049] The difference from Example 1 is that a 5 μm lithium foil layer is further provided on the outside of the solid electrolyte layer 4 , and the lithium foil layer is purchased from Guangzhou Nano New Material Technology Co., Ltd., and the rest is the same.
[0050] Example 6
[0051] The difference from Example 1 is that the transition metal carbon / carbonitride layer 3 adopts Ti3AlC2-Mxenes layer purchased from Beijing Beike New Materials Technology Co., Ltd., and the rest is the same.
[0052] Comparative Example 1
[0053] The difference from Example 1 is that the transition metal carbon / carbonitride layer 3 and the solid electrolyte layer 4 are not provided, and the other aspects are the same.
[0054] Comparative Example 2
[0055] The difference from Example 2 is that the transition metal carbon / carbonitride layer 3 and the solid electrolyte layer 4 are not provided, and the rest are the same.
[0056] Comparative Example 3
[0057] The difference from Example 1 is that no solid electrolyte layer 4 is provided, and the rest is the same.
[0058] Comparative Example 4
[0059] The difference from Example 1 is that the positions of the Ti2N-Mxenes layer of the transition metal carbon / carbon nitride layer 3 and the LLZTO@PVDF composite layer of the solid electrolyte layer 4 are swapped, that is, the LLZTO@PVDF composite layer of the solid electrolyte layer 4 is located on the silicon-oxygen-graphite composite layer of the active material layer 2, and the rest are the same.
[0060] The negative electrode plate layer settings of Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 1.
[0061] After the prepared electrode pieces are thoroughly dried, they are assembled into button cells, and the electrical performance of the assembled button cells is tested. The test conditions are: when the active material is a silicon-containing negative electrode, 0.1C constant current discharge to 0.005V; 0.1C constant current charge to 0.8V; when the active material is graphite, 0.1C constant current discharge to 0.005V; 0.1C constant current charge to 1.5V. The test results are shown in Table 1 and Figure 3-5 shown.
[0062] Table 1 Pole layer settings and performance tests of the utility model embodiments and comparative examples
[0063]
[0064] As shown in Table 1, the gram capacity, first effect and cycle performance of Examples 1 to 6 are better than those of Comparative Examples 1 to 4. Figure 3-Figure 5 It can be seen that the battery gram capacity of the layered electrode in Example 1 of the utility model is higher at 595.5 mAh / g, and the capacity retention rate of the battery with the layered electrode is greater than 90% when it is cycled at 0.5C for 100 cycles, and the battery consistency is very good; while the comparative example 1 does not have the transition metal carbon / carbonitride layer 3 and the solid electrolyte layer 4, and its gram capacity is 572.6 mAh / g, and the capacity retention rate of the battery after 100 cycles is only about 83%.
[0065] Comparing Example 1 with Example 5, Example 5 has a higher gram capacity of 598.2 mAh / g due to the fact that a 5 μm lithium foil layer is further provided on the outside of the solid electrolyte layer 4, and the first efficiency is also significantly improved compared with Example 1, indicating that the lithium foil layer provided on the outside has a significant effect on lithium supplementation.
[0066] Comparing Example 1 with Comparative Example 3, since the solid electrolyte layer 4 is not provided in Comparative Example 3, the gram capacity, first efficiency and cycle performance are inferior to those of Example 1 as a whole.
[0067] Comparing Example 1 with Comparative Example 4, since the positions of the Ti2N-Mxenes layer of the transition metal carbon / carbon nitride layer 3 and the LLZTO@PVDF composite layer of the solid electrolyte layer 4 are swapped, although the gram capacity and the first efficiency are not reduced much, the cycle performance is significantly reduced. This is because the solid electrolyte layer 4 is arranged outside the transition metal carbon / carbon nitride layer 3 and is in more complete contact with the electrolyte, which can better promote the conduction of lithium ions and further improve the cycle performance.
[0068] It should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A negative electrode plate structure, characterized in that: From at least one side of the current collector to the outside, it includes an active material layer, a transition metal carbon / carbonitride layer, and a solid electrolyte layer in sequence.
2. A negative electrode plate structure according to claim 1, characterized in that: The current collector includes one or more of copper foil, PET copper composite metal foil, aluminum foil, titanium foil, and silver foil.
3. A negative electrode plate structure according to claim 1, characterized in that: The active material layer is selected from one or more of a graphite layer, a single silicon layer, a silicon-containing alloy layer, a silicon-carbon compound layer, and a silicon-oxygen compound layer.
4. A negative electrode plate structure according to claim 1, characterized in that: The thickness of the active material layer is 20-150 μm.
5. The negative electrode plate structure according to claim 1, characterized in that: The thickness of the transition metal carbon / carbonitride layer is 1-12 μm; The surface loading of the transition metal carbon / carbonitride layer is 0.5-3 mg / cm 2 .
6. A negative electrode plate structure according to claim 1, characterized in that: The transition metal carbon / carbon nitride layer is a Ti2N-Mxenes layer or a Ti3AlC2-Mxenes layer.
7. A negative electrode plate structure according to claim 1, characterized in that: The thickness of the solid electrolyte layer is 1-20 μm.
8. The negative electrode sheet structure according to claim 1, characterized in that: The solid electrolyte layer is one of a polymer electrolyte, an oxide electrolyte, a sulfide electrolyte, and a polymer@oxide composite electrolyte.
9. A negative electrode plate structure according to claim 8, characterized in that: The solid electrolyte layer is a polymer oxide composite electrolyte.
10. A negative electrode plate structure according to claim 8, characterized in that: A lithium metal layer is also provided outside the solid electrolyte layer.
11. A negative electrode plate structure according to claim 10, characterized in that: The thickness of the lithium metal layer is 5-10 μm.
12. An electrode assembly, characterized in that: A negative electrode sheet structure having any one of claims 1 to 9.
13. A battery cell, characterized in that: A negative electrode sheet structure having any one of claims 1 to 9.
14. An electrochemical device, characterized in that: A negative electrode sheet structure having any one of claims 1 to 9.
15. An electrical equipment, characterized in that: A negative electrode sheet structure having any one of claims 1 to 9.