Adhesive tape
By designing a multi-layer structure and marking printing layer in the tape, the problem of residual glue contamination and insignificance of marking after pasting is solved, and the effect of tape being pasted at a predetermined position is achieved and easy to remove and marking is achieved.
Patent Information
- Application Number
- CN202420561543.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2034-03-21
AI Technical Summary
Existing tapes are prone to residual glue contamination after being pasted and the product identification is not significant, which affects the appearance of the adhered and consumer identification.
A tape including a first pressure-sensitive adhesive layer, a foamed resin layer, a second pressure-sensitive adhesive layer, a first release layer, a base material layer and a second release layer are designed, and the second release layer is sequentially from top to bottom. A marking printing layer is provided on the release layer, and the surface area of the marking printing layer accounts for 5 to 30% of the surface area of the substrate layer. Through a specific layer thickness and material combination, the tape is easy to remove and the marking is significant.
The tape is pasted at a predetermined position and is easy to remove after use, leaving no residual glue. At the same time, the product logo is significant, meeting the needs for appearance and recognition.
Smart Images

Figure CN222064413U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the field of adhesive tapes, and in particular relates to an adhesive tape used for electronic equipment. Background Art
[0002] At present, in industries such as the electronics industry, a method of applying an adhesive tape is generally used to fix components or parts, or to protect a forming surface or prevent contamination of the forming surface.
[0003] However, conventional adhesive tapes currently have the following problems: they are prone to produce residual adhesive contamination on the adherend, affecting the appearance of the adherend; and the product logo is not obvious, making it difficult for consumers to identify it. Utility Model Content
[0004] Problems to be solved by utility models
[0005] The utility model aims to provide an adhesive tape which can be kept stuck on a predetermined sticking position of an adherend, is easy to remove after use, does not cause residual adhesive pollution to the adherend and has a clear product mark.
[0006] Solutions for solving problems
[0007] In order to achieve the above-mentioned object, the utility model provides an adhesive tape, which is specifically as follows.
[0008] A tape comprises a first pressure-sensitive adhesive layer, a foamed resin layer, a second pressure-sensitive adhesive layer, a first release layer, a substrate layer and a second release layer which are adjacent to each other from top to bottom, characterized in that a logo printing layer is provided on a surface of the second release layer adjacent to the substrate layer, and the surface area of the logo printing layer accounts for 5 to 30% of the surface area of the substrate layer.
[0009] Among them, the thickness of the first pressure-sensitive adhesive layer is 15 to 100 μm, the thickness of the foamed resin layer is 100 to 400 μm, the thickness of the second pressure-sensitive adhesive layer is 15 to 100 μm, the thickness of the first release layer is 0.2 to 2 μm, the thickness of the substrate layer is 5 to 100 μm, and the thickness of the second release layer is 0.2 to 2 μm.
[0010] Wherein, the logo on the logo printing layer is one of NITTO, Nitto, NITTO TAPE or Nitto tape.
[0011] The foamed resin layer contains a foamed resin having pores with a height of 150 μm or less and lengths of 500 μm or less in the MD and TD directions, respectively.
[0012] Wherein, the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are acrylic adhesive layers.
[0013] Wherein, the foamed resin layer comprises one of polyurethane foamed resin, polyester foamed resin, phenolic foamed resin and polyolefin foamed resin.
[0014] Wherein, the first release layer and the second release layer are silicone resin release layers.
[0015] Wherein, the substrate layer is a polyimide film, a polyester film, a polynaphthyl ester film, a polyamide film or a polyolefin film.
[0016] The logo protrusion thickness of the logo printing layer is 0.2-0.8 μm, and the depression thickness of the first pressure-sensitive adhesive layer at the position corresponding to the logo in the logo printing layer is 0.2-0.8 μm.
[0017] Effect of utility model
[0018] The adhesive tape of the utility model can be kept adhered to the predetermined sticking position of the adherend, is easy to remove after use, does not cause residual adhesive pollution to the adherend, and has a clear product mark. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic cross-sectional view of an adhesive tape according to an embodiment of the present utility model.
[0020] Figure 2 This is a scanning electron microscope (SEM) photograph of the foamed resin layer.
[0021] Description of Reference Numerals
[0022] 1. First pressure-sensitive adhesive layer
[0023] 2 Foam resin layer
[0024] 3 Second pressure-sensitive adhesive layer
[0025] 4 First release layer
[0026] 5. Substrate layer
[0027] 6 Second release layer
[0028] 7 Logo printing layer
[0029] 100 Tape DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0031] like Figure 1As shown, the adhesive tape 100 of the utility model includes a first pressure-sensitive adhesive layer 1, a foamed resin layer 2, a second pressure-sensitive adhesive layer 3, a first release layer 4, a substrate layer 5 and a second release layer 6 which are adjacent to each other from top to bottom, wherein a logo printing layer 7 is provided on a surface of the second release layer 6 adjacent to the substrate layer 5, and the surface area of the logo printing layer 7 accounts for 5 to 30% of the surface area of the substrate layer 5, preferably 10 to 20%, and more preferably 12 to 18%.
[0032] The thickness of the first pressure-sensitive adhesive layer 1 is 15-100 μm, preferably 25-75 μm, the thickness of the foamed resin layer 2 is 100-400 μm, preferably 150-300 μm, the thickness of the second pressure-sensitive adhesive layer 3 is 15-100 μm, preferably 25-75 μm, the thickness of the first release layer 4 is 0.2-2 μm, the thickness of the substrate layer 5 is 5-100 μm, preferably 35-75 μm, and the thickness of the second release layer 6 is 0.2-2 μm, preferably 0.2-1 μm. As a test method for the thickness of each layer, various known layer thickness test methods can be used, such as a scanning electron microscope (SEM) with a magnification of hundreds to tens of thousands of times.
[0033] In the present invention, the logo on the logo printing layer 7 is one of NITTO, Nitto, NITTO TAPE or Nittotape.
[0034] The foamed resin layer 2 contains a foamed resin having a hole with a height of 150 μm or less (preferably 120 μm or less) and a length of 500 μm or less (preferably 300 μm or less) in the MD and TD directions. There is no particular restriction on the foamed resin contained in the foamed resin layer, which can be one of a polyurethane foamed resin, a polyester foamed resin, a phenolic foamed resin, and a polyolefin foamed resin. The foamed resin layer 2 can be subjected to a conventional surface treatment, such as a conventional corona treatment, an ionizing radiation treatment, a sodium-naphthalene treatment, etc.
[0035] The first pressure-sensitive adhesive layer 1 and the second pressure-sensitive adhesive layer 3 are acrylic adhesive layers.
[0036] The first release layer 4 and the second release layer 6 are silicone release layers. The release layers can also be subjected to conventional electrostatic treatment.
[0037] The type of the substrate layer 5 is not particularly limited, and may be a polyimide film, a polyester film, a polynaphthyl ester film, a polyamide film, or a polyolefin film.
[0038] The logo protrusion thickness of the logo printing layer 7 is 0.2-0.8 μm. Since the second release layer 6 and the logo printing layer 7 are correspondingly stacked with the first pressure-sensitive adhesive layer 1 when the tape is rolled up, the depression thickness of the first pressure-sensitive adhesive layer 1 corresponding to the logo in the logo printing layer 7 is 0.2-0.8 μm.
[0039] As a method for forming each layer, any appropriate method may be adopted, and examples thereof include roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, knife coating, and micro-gap coating printing.
[0040] In the present invention, the materials contained in each layer are all materials of known types.
[0041] The following examples are merely illustrative and are not intended to limit the present invention.
[0042] Example 1
[0043] A foamed resin film having a thickness of 200 μm (manufactured by Sekisui Chemical Co., Ltd., wherein the foamed resin has pores with a height of 120 μm or less and lengths in the MD and TD directions of 300 μm or less, respectively) was subjected to double-sided corona treatment.
[0044] An acrylic adhesive layer was coated on both sides of the treated foamed resin film to form a first pressure-sensitive adhesive layer with a thickness of 35 μm and a second pressure-sensitive adhesive layer with a thickness of 35 μm, respectively.
[0045] A polyethylene terephthalate (PET) resin film with a thickness of 75 μm is subjected to corona treatment on both sides, and a logo printing layer with a NITTO logo is printed on one side. After printing, the area occupied by the five letters is 15% of the surface of the polyethylene terephthalate (PET) resin film, and the thickness of the raised logo is 0.4-0.5 μm. Then, a second silicone resin layer (thickness 0.3 μm) is coated on the logo printing layer, and the logo printing layer forms a 0.4-0.5 μm raised NITTO logo on the surface of the second silicone resin layer. Then, a first silicone resin layer (thickness 0.5 μm) is coated on the other side of the polyethylene terephthalate (PET) resin film, and then the first silicone resin layer is attached to the second pressure-sensitive adhesive layer, and rolled up to form an adhesive tape, and a 0.4-0.5 μm recessed NITTO logo is formed on the surface of the first pressure-sensitive adhesive layer.
[0046] Example 2
[0047] A foamed resin film having a thickness of 300 μm (manufactured by Sekisui Chemical Co., Ltd., wherein the foamed resin has pores with a height of 120 μm or less and lengths in the MD and TD directions of 300 μm or less each) was subjected to double-sided corona treatment.
[0048] An acrylic adhesive layer was coated on both sides of the treated foamed resin film to form a first pressure-sensitive adhesive layer with a thickness of 35 μm and a second pressure-sensitive adhesive layer with a thickness of 35 μm, respectively.
[0049] A polyethylene terephthalate (PET) resin film with a thickness of 50 μm is subjected to corona treatment on both sides, and a logo printing layer with a NITTO logo is printed on one side. After printing, the area occupied by the five letters is 15% of the surface of the polyethylene terephthalate (PET) resin film, and the thickness of the raised logo is 0.3-0.4 μm. Then, a second silicone resin layer (thickness 0.3 μm) is coated on the logo printing layer, and the logo printing layer forms a 0.3-0.4 μm raised NITTO logo on the surface of the second silicone resin layer. Then, a first silicone resin layer (thickness 0.5 μm) is coated on the other side of the polyethylene terephthalate (PET) resin film, and then the first silicone resin layer is attached to the second pressure-sensitive adhesive layer, and rolled up to form an adhesive tape, and a 0.3-0.4 μm recessed NITTO logo is formed on the surface of the first pressure-sensitive adhesive layer.
Claims
1. An adhesive tape comprising a first pressure-sensitive adhesive layer, a foamed resin layer, a second pressure-sensitive adhesive layer, a first release layer, a substrate layer and a second release layer, which are adjacent to each other from top to bottom, characterized in that: A logo printing layer is disposed on a surface of the second release layer adjacent to the substrate layer, and a surface area of the logo printing layer accounts for 5 to 30% of a surface area of the substrate layer.
2. The adhesive tape according to claim 1, characterized in that The thickness of the first pressure-sensitive adhesive layer is 15 to 100 μm, the thickness of the foamed resin layer is 100 to 400 μm, the thickness of the second pressure-sensitive adhesive layer is 15 to 100 μm, the thickness of the first release layer is 0.2 to 2 μm, the thickness of the substrate layer is 5 to 100 μm, and the thickness of the second release layer is 0.2 to 2 μm.
3. The adhesive tape according to claim 1 or 2, characterized in that: The foamed resin layer contains a foamed resin having pores with a height of 150 μm or less and lengths in the MD and TD directions of 500 μm or less, respectively.
4. The adhesive tape according to claim 1 or 2, characterized in that: The first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are acrylic adhesive layers.
5. The adhesive tape according to claim 1 or 2, characterized in that: The foamed resin layer includes one of polyurethane foamed resin, polyester foamed resin, phenolic foamed resin and polyolefin foamed resin.
6. The adhesive tape according to claim 1 or 2, characterized in that: The first release layer and the second release layer are silicone release layers.
7. The adhesive tape according to claim 1 or 2, characterized in that: The substrate layer is a polyimide film, a polyester film, a polynaphthyl ester film, a polyamide film or a polyolefin film.
8. The adhesive tape according to claim 1 or 2, characterized in that: The logo protrusion thickness of the logo printing layer is 0.2-0.8 μm, and the depression thickness of the first pressure-sensitive adhesive layer at a position corresponding to the logo in the logo printing layer is 0.2-0.8 μm.