Preparation device of silicon carbide crystal

By using the two-phase separation reaction between gaseous elemental carbon and molten silicon source in the preparation of silicon carbide crystals, the microtubule defects and heterocrystal problems are solved, and the preparation of high-quality silicon carbide crystals is achieved, which improves the reaction efficiency and crystal purity.

CN222100200UActive Publication Date: 2024-12-03XIAMEN FUNANO NEW MATERIAL TECH COMPANY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420524117.9
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-03-18
Publication Date
2024-12-03
Estimated Expiration
2034-03-18

AI Technical Summary

Technical Problem

In the existing silicon carbide crystal preparation technology, microtube defects lead to device breakdown failure, and the unavoidable heterogeneous crystal problems during the growth process of liquid phase epitaxial method affect crystal quality.

Method used

Use gaseous elemental carbon as the carbon source to separate two phases from the molten silicon source. The gaseous elemental carbon enters the growth chamber through the valve assembly, and reacts with the silicon source to generate silicon carbide crystals to ensure sufficient carbon source in the growth chamber and maintain uniform carbon. Concentration and reaction conditions to avoid the introduction of impurities.

Benefits of technology

The reaction rate and utilization rate of carbon source and silicon source are improved, high-quality silicon carbide crystals are obtained, growth temperature and impurity pollution are reduced, and graphitization is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222100200U_ABST
    Figure CN222100200U_ABST
Patent Text Reader

Abstract

The utility model relates to a silicon carbide crystal preparation device which comprises a carbon source bin, a growth bin and a seed crystal shaft, the carbon source bin and the growth bin are communicated with each other, the seed crystal shaft extends into the growth bin, and a valve assembly is arranged on a transmission channel between the carbon source bin and the growth bin and is in transmission connection with a driving component. The valve assembly is controlled by the driving part to conduct opening and closing actions, and the carbon source bin and the growth bin are sleeved with a first induction heating coil and a second induction heating coil which are used for induction heating respectively. The preparation device disclosed by the utility model can be used for conveying sufficient gaseous elemental carbon to the growth bin, ensuring that sufficient carbon sources always exist in the growth bin, and enabling raw materials in the growth bin to always keep the same carbon concentration, so that solution components in the growth bin are kept uniform, the reaction rate and the utilization rate of the carbon sources and silicon sources are improved, and the production cost is reduced. And finally obtaining high-quality silicon carbide crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of silicon carbide crystal preparation, in particular to a device for preparing silicon carbide crystal. Background Art

[0002] Silicon carbide (SiC) is the third generation of half-wide bandgap semiconductor materials after silicon, germanium, gallium arsenide, etc. It has obvious advantages in bandgap width, thermal conductivity, critical breakdown field strength, saturated electron drift rate, etc. The bandgap widths of 4H-SiC and 6H-SiC are 3.26eV and 3.08eV respectively. The bandgap of 3C-SiC is the narrowest, and its bandgap width is also around 2.39eV. The bandgap width of SiC is 2-3 times that of Si, the thermal conductivity is 2.6-3.3 times that of Si, the critical breakdown field strength is 7-13 times that of Si, and the saturated electron drift rate is 2-2.7 times that of Si. The use of wide bandgap materials can greatly increase the operating temperature of the device. The maximum operating temperature of power devices using SiC substrates may exceed 600℃. Higher critical breakdown field strength can reduce the size of the device, so that the device can be miniaturized while eliminating a large number of heat sinks and reducing energy consumption. Higher saturated electron drift rate can increase the switching speed of the device and reduce switching losses. Therefore, compared with Si, SiC is more suitable for manufacturing high-temperature, high-frequency, and high-power power devices.

[0003] Currently, commercialized SiC substrates are obtained through the physical vapor transport (PVT) method. The substrates contain a large number of defects, especially micropipe defects, which can lead to breakdown failure of the device. With the high power and high frequency of power devices, the demand for producing high-quality SiC substrates is becoming more and more urgent. The liquid phase epitaxy (LPE) method is an ideal method for growing high-quality SiC crystals because its growth process is in a near-equilibrium state, especially it can eliminate the micropipe defects that are difficult to avoid during the growth process of the PVT method. The existing LPE method for growing silicon carbide crystals is to melt silicon in a high-purity graphite crucible by heating to form a solution of carbon in silicon, and then extend the graphite shaft with a seed crystal attached to the head into the solution for growth.

[0004] Under high temperature conditions, molten silicon will volatilize. When vapor silicon encounters a cold object, it will condense into silicon powder particles. If silicon vapor encounters graphite parts or graphite insulation materials, it will react with carbon to generate tiny silicon carbide particles. At the top of the graphite crucible, the temperature is relatively low, and the volatilization of silicon vapor will generate small silicon carbide particles at the top of the graphite crucible. Some of these particles will adhere to the graphite crucible, and some will fall back into the crucible with the disturbance of the atmosphere. When the phenomenon of falling into the crucible occurs, impure crystals will be formed in the solution. As the solution flows, the growing single crystal will be mixed with polycrystals, making the entire crystal unusable. Utility Model Content

[0005] In view of the deficiencies in the prior art, the utility model provides a device for preparing silicon carbide crystals, creatively adopts gaseous elemental carbon as a carbon source, performs two-phase separation with a molten silicon source, heats the carbon source (fullerene) and sublimates it into gaseous elemental carbon, and after the concentration of the gaseous elemental carbon reaches a certain level, opens the valve assembly, and the gaseous elemental carbon enters the growth chamber, and the seed crystal shaft with the seed crystal attached to the head is extended into the silicon source, and the gaseous elemental carbon is fully reacted with the heated and molten silicon source to gradually generate silicon carbide crystals on the seed crystal.

[0006] The preparation device can be used to transport sufficient gaseous elemental carbon to the growth chamber, ensuring that there is always sufficient carbon source in the growth chamber, so that the raw materials in the growth chamber always maintain the same carbon concentration, thereby maintaining the uniformity of the solution components in the growth chamber, improving the reaction rate and utilization rate of the carbon source and silicon source, and ultimately obtaining high-quality silicon carbide crystals.

[0007] In order to achieve the above object, the utility model is realized by the following technical solutions:

[0008] A device for preparing silicon carbide crystals comprises a carbon source bin and a growth bin which are interconnected and a seed crystal shaft extending into the growth bin. A valve assembly is provided on a transmission channel between the carbon source bin and the growth bin. The valve assembly is transmission-connected to a driving component. The driving component controls the valve assembly to perform a switching action. A first induction heating coil and a second induction heating coil for induction heating are respectively provided on the outside of the carbon source bin and the growth bin.

[0009] Furthermore, the valve assembly includes a valve movable block and a valve static block that cooperate with each other. The driving component includes a driving motor and a driving shaft driven by the driving motor. The driving shaft is connected to the valve movable block. The driving shaft drives the valve movable block to rotate relative to the valve static block to switch the switching state of the valve assembly.

[0010] Furthermore, the exterior of the carbon source silo and the growth silo is coated with a heat-insulating layer.

[0011] Furthermore, a guide plate is provided in the growth chamber.

[0012] The above technical solution has the following advantages or beneficial effects:

[0013] In the preparation device of silicon carbide crystals described in the utility model, sufficient gaseous elemental carbon can be transported to the growth chamber by the preparation device, ensuring that there is always sufficient carbon source in the growth chamber, so that the raw materials in the growth chamber always maintain the same carbon concentration, thereby maintaining uniformity of the solution components in the growth chamber, improving the reaction rate and utilization rate of the carbon source and the silicon source, and finally obtaining high-quality silicon carbide crystals. Using gaseous elemental carbon as the carbon source requires a lower temperature. On the one hand, no additives need to be added to avoid the introduction of impurities; on the other hand, the heating temperature will not be too high, not exceeding 2000°C, to avoid the occurrence of graphitization. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a schematic structural diagram of a device for preparing silicon carbide crystals according to an embodiment of the utility model.

[0015] Figure 2 It is a schematic structural diagram of a valve assembly in an open state according to an embodiment of the utility model.

[0016] Figure 3 It is a schematic structural diagram of the valve assembly in a closed state according to an embodiment of the utility model.

[0017] Description of labels:

[0018] 1. Carbon source silo, 2. Carbon source, 3. Growth chamber, 4. Silicon source, 5. Seed crystal shaft, 6. Seed crystal, 7. Guide plate, 8. Insulation layer, 9. Valve moving block, 10. Valve static block, 11. First induction heating coil, 12. Second induction heating coil, 13. Drive shaft, 14. Drive motor. DETAILED DESCRIPTION

[0019] The utility model is further described below in conjunction with the accompanying drawings and embodiments.

[0020] In the description of the present invention, it should be understood that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., indicating directions or positional relationships, are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.

[0021] As attached Figure 1 To Attachment Figure 3As shown, this embodiment provides a device for preparing silicon carbide crystals, including a carbon source silo 1 and a growth silo 3 which are interconnected and a seed crystal shaft 5 extending into the growth silo 3. A valve assembly is provided on the transmission channel between the carbon source silo 1 and the growth silo 3. The valve assembly is transmission-connected to a driving component, and the driving component controls the valve assembly to perform switching actions. The outside of the carbon source silo 1 and the growth silo 3 are respectively provided with a first induction heating coil 11 and a second induction heating coil 12 for induction heating.

[0022] Please refer to the attached Figure 1 To Attachment Figure 3 In one preferred embodiment, the valve assembly includes a valve movable block 9 and a valve static block 10 that cooperate with each other, and the driving component includes a driving motor 14 and a driving shaft 13 driven by the driving motor 14. The driving shaft 13 is connected to the valve movable block 9, and the driving shaft 13 drives the valve movable block 9 to rotate relative to the valve static block 10 to switch the switching state of the valve assembly.

[0023] Please refer to the attached Figure 1 To Attachment Figure 3 In one preferred embodiment, the carbon source silo 1 and the growth silo 3 are coated with a heat preservation layer 8. The heat preservation layer 8 is used to ensure the temperature stability of the carbon source silo 1 and the growth silo 3.

[0024] Please refer to the attached Figure 1 To Attachment Figure 3 In one preferred embodiment, a guide plate 7 is provided in the growth chamber 3, through which the gaseous elemental carbon can be preferentially transferred to the interior of the silicon source to directly react with the silicon source.

[0025] The utility model also provides a method for preparing silicon carbide crystals by liquid phase epitaxy, wherein a carbon source 2 is placed in a carbon source silo 1, a silicon source 4 is placed in a growth silo 3, a seed crystal 6 is attached to one end of a seed crystal axis 5 and extends into the growth silo 3, the carbon source silo 1 is heated to allow the carbon source 2 to sublime to generate gaseous elemental carbon, the growth silo 3 is heated to allow the silicon source 4 to form a molten state, the gaseous elemental carbon is transferred to the growth silo 3 to react with the molten silicon source 4 to form a growth solution with a supersaturated zone, and the seed crystal axis 5 is moved to control the seed crystal 6 to be immersed in the supersaturated zone of the growth solution for crystal growth.

[0026] Preferably, a method for preparing silicon carbide crystal by liquid phase epitaxy comprises the following steps:

[0027] S1, providing a preparation device for silicon carbide crystals, the preparation device for silicon carbide crystals comprising a carbon source silo 1 and a growth silo 3 which are interconnected and a seed crystal shaft 5 extending into the growth silo 3, a valve assembly being provided on the transmission channel between the carbon source silo 1 and the growth silo 3, the time and amount of gaseous elemental carbon entering the growth silo being controlled by the valve assembly, the carbon source 2 being loaded into the carbon source silo 1, the silicon source 4 being placed in the growth silo 3, the seed crystal 6 being attached to one end of the seed crystal shaft 5 extending into the interior of the growth silo 3, and the seed crystal being just immersed in the silicon source, and the height of the seed crystal shaft being adjusted according to the actual reaction process;

[0028] S2, evacuating the interior of the silicon carbide crystal preparation device through a vacuum system, then introducing an inert gas into the interior of the silicon carbide crystal preparation device and maintaining it in a negative pressure state, heating the carbon source silo 1 to sublime the carbon source 2 to produce gaseous elemental carbon, the carbon source 2 is heated and sublimated in the carbon source silo 1 for 0.1 to 2 hours, and while heating the carbon source silo 1, the growth silo 3 is heated to form a molten state of the silicon source 4;

[0029] S3, after the gaseous elemental carbon fills the entire carbon source bin 1 and the temperature of the growth bin 3 is stable, the valve assembly is opened, and the gaseous elemental carbon is transmitted to the growth bin 3 through the transmission channel to react with the molten silicon source 4 to form a growth solution with a supersaturated zone, and then the seed crystal 6 is controlled to be immersed in the supersaturated zone of the growth solution by moving the seed crystal axis 5 to grow crystals, and the reaction is maintained for 48 to 200 hours;

[0030] S4, after the crystal growth is completely completed, the silicon carbide crystal preparation device is cooled down, and an inert gas is filled into the growth chamber 3 of the silicon carbide crystal preparation device to normal pressure, and the growth chamber 3 is opened to obtain the silicon carbide crystal.

[0031] Preferably, the heating temperature of the carbon source bin 1 is 450-900°C, and the heating temperature of the growth bin 3 is 1100-1900°C.

[0032] Preferably, in step S2, the carbon source silo 1 is heated to 450-900° C. within 0.5 h;

[0033] More preferably, in step S2, the carbon source silo 1 is heated to 720-760° C. within 0.5 h.

[0034] Preferably, in step S2, the growth chamber 3 is heated to 1100-1900° C. within 1 hour;

[0035] More preferably, in step S2, the growth chamber 3 is heated to 1600-1800° C. within 1 hour.

[0036] Preferably, the carbon source 2 is fullerene; the number of carbon atoms of the fullerene is 20-560, preferably one or more of C60, C70, C76, C78, ​​C80 and C84.

[0037] Preferably, the inert gas is helium or argon with a purity of >99.99%.

[0038] As described above, the embodiments are only used to illustrate the technical solutions of the utility model, rather than to limit it. Although the utility model has been described in detail with reference to the aforementioned embodiments, ordinary technicians in the field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein with equivalents. These modifications or replacements do not make the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the utility model. Therefore, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the protection scope of the utility model.

Claims

1. A device for preparing silicon carbide crystals, Features: The invention comprises a carbon source silo (1) and a growth silo (3) which are interconnected, and a seed crystal shaft (5) which extends into the growth silo (3). A valve assembly is provided on the transmission channel between the carbon source silo (1) and the growth silo (3). The valve assembly is in transmission connection with a driving component. The driving component controls the valve assembly to perform a switching action. The carbon source silo (1) and the growth silo (3) are respectively provided with a first induction heating coil (11) and a second induction heating coil (12) for induction heating on the outside.

2. The device for preparing silicon carbide crystal according to claim 1, Features: The valve assembly comprises a valve movable block (9) and a valve stationary block (10) which cooperate with each other, and a driving component comprises a driving motor (14) and a driving shaft (13) driven by the driving motor (14). The driving shaft (13) is connected to the valve movable block (9), and the driving shaft (13) drives the valve movable block (9) to rotate relative to the valve stationary block (10) to switch the on / off state of the valve assembly.

3. The device for preparing silicon carbide crystal according to claim 1, Features: The exterior of the carbon source silo (1) and the growth silo (3) is coated with a heat-insulating layer (8).

4. The device for preparing silicon carbide crystal according to claim 1, Features: A flow guide plate (7) is provided in the growth chamber (3).