Anionically modified microfibril cellulose
Anion-modified microfibrillar cellulose with controlled fiber distribution provides enhanced uniformity and performance by balancing micron and nanoscale fibers, improving dispersion stability and thixotropy, and addressing the challenges of cellulose nanofiber use and cost.
Patent Information
- Application Number
- JP2023044417
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Cellulose nanofibers are difficult to use due to their fine size, leading to issues such as slipping through wires and poor paper strength, and are expensive to manufacture, while existing microfibrillar cellulose lacks controlled fiber distribution, affecting uniformity and performance.
Anion-modified microfibrillar cellulose with controlled fiber distribution, characterized by specific phase difference, fiber width, and length-weighted fiber length distribution, is produced through mechanical fibrillation and anionic modification, ensuring a balanced mixture of micron and nanoscale fibers.
The anion-modified microfibrillar cellulose exhibits superior uniformity, dispersion stability, thixotropy, and viscosity, with improved fiber yield and strength, addressing the limitations of conventional microfibrillar cellulose.
Smart Images

Figure 2024134220000001
Abstract
Description
[Technical field]
[0001] The present invention relates to anionically modified microfibril cellulose. [Background technology]
[0002] It is known that when an anionic group such as a carboxyl group or a carboxymethyl group is introduced into a cellulose molecular chain and mechanically treated (defibrated), it can be converted into a cellulose nanofiber having a nanoscale fiber width of less than 500 nm on average. In particular, cellulose nanofibers with a fiber diameter of about 4 nm correspond to single microfibrils, which are the basic units of cellulose bundles in plant cell walls. Such cellulose nanofibers have high thixotropy and water retention and can be used in various fields, but since they are very fine, they may be difficult to use depending on the application. For example, when cellulose nanofibers are used as a papermaking additive, if the amount is small, problems such as poor yield due to easy slipping through the wire and difficulty in obtaining strong paper may occur. In addition, cellulose nanofibers are expensive to manufacture. In response to this, the applicant has provided fibrillated chemically modified cellulose fibers that are less defibrated than cellulose nanofibers (Patent Document 1).
[0003] Meanwhile, a method that uses optical phase difference distribution analysis has been proposed recently as a system for objectively quantitatively evaluating the degree of defibration of wood pulp raw materials (Non-Patent Document 1). This system injects an aqueous suspension of defibrated pulp into a quartz flow channel with a given cross section, and maps and images the optical phase difference of the defibrated pulp suspension. The average phase difference and its variation (standard deviation) at the observation angle of the phase difference image directly and quantitatively reflect the degree of defibration. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2020 / 195671 [Non-patent literature]
[0005] [Non-Patent Document 1] K. Uetani, etc., "Direct determination of the degree of fibrillation of wood pulps by distribution analysis of pixel-resolved optical retardation", Carbohydrate Polymers, 254, 117460, December 1, 2020 Summary of the Invention [Problem to be solved by the invention]
[0006] The objective of the present invention is to provide microfibril cellulose having novel characteristics in a fibrillated chemically modified cellulose fiber (microfibril cellulose) that is less defibrated than cellulose nanofiber. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors produced an anion-modified microfibril cellulose in which the average phase difference and its variation (standard deviation) obtained by optical phase difference distribution analysis are within a specific range, and the average fiber width and the ratio of fibers in the range of 0 to 0.2 mm in the length-weighted fiber length distribution are within a specific range. Since microfibril cellulose has a low degree of defibration, it is in a state in which fibers of various sizes, from micron-order fibers to fibers close to nanofibers, are mixed, and such a mixed state of fibers could not be expressed by a conventional method of directly deriving dimensional information of fibers. In contrast, it was found that the degree of defibration can be derived based on the degree of such a mixed state of fibers (fiber distribution) by using the average phase difference and its variation (standard deviation) obtained by optical phase difference distribution analysis. Taking into account this fiber distribution, the anion-modified microfibril cellulose obtained in the present invention has a low ratio of fibers that are close to unfibrillated, contains a large amount of fibers that have been finely refined to the submicron level, and has little variation in fiber size. It has been found that this anion-modified microfibril cellulose has superior uniformity, dispersion stability, expression of thixotropy, and viscosity compared to conventional microfibril cellulose in which the fiber distribution has not been adjusted, and has been completed based on this discovery.
[0008] The present invention includes, but is not limited to, the following: [1] Anion-modified microfibril cellulose satisfying the following conditions (A) to (C): (A) The average phase difference obtained from a phase difference map image acquired at a wavelength of 543 nm using a two-dimensional birefringence evaluation system microscope is 10.0 nm or less, and the variation (standard deviation) of the average phase difference is 15.0 nm or less. (B) the average fiber width is in the range of 1.0 to 28.0 μm; and (C) In the length-weighted fiber length distribution, the ratio of fibers in the range of 0 to 0.2 mm is 80.0% or more. [2] The anion-modified microfibril cellulose according to [1], having an average retardation of 8.0 nm or less. [3] The anion-modified microfibril cellulose according to [1] or [2], having an average retardation of 2.0 nm or more. [4] The anion-modified microfibril cellulose according to [1] or [2], having an average retardation of 3.0 nm or more. [5] The anion-modified microfibril cellulose according to any one of [1] to [4], which has a transmittance of light with a wavelength of 660 nm of 60.0% or less when dispersed in water at a solid content concentration of 1% by mass. [6] (D) An anion-modified microfibril cellulose according to any one of [1] to [5], further satisfying the following: (D) The cryl value is in the range of more than 2.0 and less than 4.0. [7] (E) The anion-modified microfibril cellulose according to any one of [1] to [5], further satisfying that the cryl value is in the range of 2.0 or less. [8] An aqueous dispersion comprising the anion-modified microfibril cellulose according to any one of [1] to [7]. Effect of the Invention
[0009] The anion-modified microfibril cellulose of the present invention is characterized in that it contains a small proportion of fibers close to unfibrillated, contains a large amount of fibers that have been refined to the submicron level, and has little variation in fiber size. Such anion-modified microfibril cellulose is superior in uniformity, dispersion stability, expression of thixotropy, exertion of viscosity, etc., compared to conventional microfibril cellulose in which such fiber distribution has not been adjusted. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Anion-modified microfibril cellulose> Anion-modified microfibril cellulose (hereinafter, "microfibril cellulose" will be referred to as "MFC") is a fiber obtained by moderately beating or defibrating anion-modified cellulose fiber (hereinafter, "anion-modified cellulose") using a refiner or the like to fibrillate it. Anion-modified MFC includes various fibers of different sizes, such as fibers with cellulose microfibril fluff on the surface and fibers defibrated to a fiber width of the submicron order due to moderate beating or defibration. Anion-modified MFC includes fibers with a fiber width of the micron order, unlike anion-modified cellulose nanofibers (hereinafter, "cellulose nanofibers" will be referred to as "CNF") that are highly defibrated to a nanoscale fiber width (for example, an average fiber width of less than 1 μm). In addition, anion-modified MFC has characteristics such as being easier to defibrate, having high water retention, and having high thixotropy due to the anion-modification, compared to non-anion-modified MFC.
[0011] <Anion modification> When producing the anion-modified MFC of the present invention, first, the raw cellulose fiber is anion-modified to obtain anion-modified cellulose. The types of anion modification include, but are not limited to, oxidation (also called carboxylation) in which a carboxyl group is introduced into the cellulose chain, carboxyalkylation in which a carboxyalkyl group such as a carboxymethyl group (hereinafter, "carboxymethyl" is referred to as "CM") is ether-bonded to the cellulose chain, and phosphoric acid esterification in which a phosphoric acid group is introduced into the cellulose chain. Among them, oxidation (carboxylation) and carboxyalkylation are more preferable.
[0012] Anion-modified cellulose may take a form in which an anion group such as a carboxyl group, a CM group, or a phosphate group has a metal ion such as a sodium ion or a potassium ion as a counter ion (this form is called "salt-type anion-modified cellulose"). In this specification, anion-modified cellulose also includes salt-type anion-modified cellulose. Furthermore, anion-modified MFC also includes salt-type anion-modified MFC. In contrast to salt-type anion-modified cellulose, when the anion group has a proton as a counter ion, it is called "hydrogen-type anion-modified cellulose".
[0013] The anion-modified cellulose used in producing the anion-modified MFC of the present invention maintains at least a part of the fibrous shape of cellulose even when dispersed in water. That is, when an aqueous dispersion of anion-modified cellulose is observed with an electron microscope or the like, a fibrous substance can be observed, and when measured by X-ray diffraction, a peak of cellulose type I crystals can be observed.
[0014] The cellulose as a raw material for obtaining anion-modified cellulose is not particularly limited, and examples thereof include those derived from plants, animals (e.g., ascidians), algae, and microorganisms (e.g., acetic acid bacteria (Acetobacter)). Examples of those derived from plants include wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, and pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), softwood dissolving pulp, hardwood dissolving pulp, recycled pulp, waste paper, etc.). In addition, cellulose powder obtained by pulverizing the above-mentioned cellulose raw material may be used. As the cellulose raw material, any one or a combination of these may be used, but cellulose fibers derived from plants or microorganisms are preferred, cellulose fibers derived from plants are more preferred, and wood-based pulp is even more preferred.
[0015] In order to obtain an anion-modified cellulose having a peak of cellulose type I crystallinity, it is preferable to use cellulose having a high crystallinity of cellulose type I as a raw material. The crystallinity of the cellulose raw material is preferably 70% or more, more preferably 80% or more. The method for measuring the crystallinity of cellulose type I will be described later.
[0016] <Anion modification-oxidation> An example of anion modification is oxidation (carboxylation) in which a carboxyl group is introduced into a cellulose chain. In this specification, carboxylated cellulose is referred to as "oxidized cellulose." As the oxidized cellulose, commercially available products may be used, or it may be produced by oxidizing the above-mentioned cellulose raw material by a known method. The amount of carboxyl groups is preferably 0.1 to 2.5 mmol / g, more preferably 0.6 mmol / g to 2.5 mmol / g, and even more preferably 1.0 mmol / g to 2.0 mmol / g, based on the bone dry mass of the oxidized cellulose.
[0017] The amount of carboxyl groups in oxidized cellulose can be measured by the following method: 60 ml of a 0.5% by mass slurry (aqueous dispersion) of oxidized cellulose is prepared, and a 0.1 M aqueous hydrochloric acid solution is added to adjust the pH to 2.5. A 0.05 N aqueous sodium hydroxide solution is then added dropwise and the electrical conductivity is measured until the pH reaches 11. The electrical conductivity is calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual: Amount of carboxyl groups [mmol / g oxidized cellulose] = a [ml] × 0.05 / mass of oxidized cellulose [g].
[0018] The amount of carboxyl groups in the oxidized cellulose before fibrillation is usually the same as the amount of carboxyl groups in the oxidized cellulose after fibrillation (oxidized MFC). One example of the oxidation method is a method in which the cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, and mixtures thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the cellulose surface, resulting in the formation of aldehyde groups and carboxyl groups (-COOH) or carboxylate groups (-COO - The concentration of the cellulose raw material during the reaction is not particularly limited, but is preferably 5% by mass or less.
[0019] The term "N-oxyl compound" refers to a compound capable of generating nitroxy radicals. Any compound that can promote the target oxidation reaction can be used as the N-oxyl compound. Examples include 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO). The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing the cellulose raw material. For example, 0.01 to 10 mmol is preferable, 0.01 to 1 mmol is more preferable, and 0.05 to 0.5 mmol is even more preferable, per 1 g of bone-dry cellulose raw material. In addition, the amount is preferably about 0.1 to 4 mmol / L relative to the reaction system.
[0020] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can dissociate and ionize in water. Also, iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone-dry cellulose raw material.
[0021] The oxidizing agent may be a known one, such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxide, peroxide, etc. Among them, sodium hypochlorite is preferable because it is inexpensive and has a low environmental impact. The appropriate amount of the oxidizing agent to be used is, for example, preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, further preferably 1 to 25 mmol, and most preferably 3 to 10 mmol, per 1 g of bone-dry cellulose raw material. Also, for example, 1 to 40 mol is preferable per 1 mol of the N-oxyl compound.
[0022] The oxidation process of the cellulose raw material can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4 to 40°C, or may be room temperature of about 15 to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose chain, and a decrease in the pH of the reaction solution is observed. In order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably about 10 to 11. The reaction medium is preferably water, because it is easy to handle and does not easily cause side reactions. The reaction time in the oxidation reaction can be appropriately set according to the degree of progress of the oxidation, and is usually 0.5 to 6 hours, for example, about 0.5 to 4 hours.
[0023] The oxidation reaction may also be carried out in two stages. For example, the oxidized cellulose obtained by filtration after completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, allowing efficient oxidation without reaction inhibition by table salt produced as a by-product in the first-stage reaction.
[0024] Another example of the oxidation method is a method in which the cellulose raw material is oxidized by contacting it with an ozone-containing gas. This oxidation reaction oxidizes at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring, and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 to 250 g / m 3 It is preferable that the thickness is 50 to 220 g / m 3It is more preferable that the ozone is added to the cellulose raw material in an amount of 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solid content of the cellulose raw material. The ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is not particularly limited, but is about 1 to 360 minutes, and is preferably about 30 to 360 minutes. When the ozone treatment conditions are within these ranges, the cellulose raw material can be prevented from being excessively oxidized and decomposed, and the yield of oxidized cellulose is good. After the ozone treatment, an oxidizing agent may be used to perform a post-oxidation treatment. The oxidizing agent used in the post-oxidation treatment is not particularly limited, but examples thereof include chlorine-based compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, these oxidizing agents are dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and the cellulose raw material is immersed in the solution to perform the post-oxidation treatment.
[0025] The amount of carboxyl groups in the oxidized cellulose can be adjusted by controlling the reaction conditions, such as the amount of the oxidizing agent added and the reaction time. <Anion modification - Carboxyalkylation> An example of anion modification is carboxyalkylation, in which a carboxyalkyl group such as a CM group is ether-bonded to a cellulose chain. In this specification, carboxyalkylated cellulose is called "carboxyalkylated cellulose". Carboxymethylated cellulose is called "CM-cellulose". As the carboxyalkylated cellulose, commercially available products may be used, or the cellulose raw material may be produced by carboxyalkylating the above-mentioned cellulose raw material by a known method. The degree of carboxyalkyl substitution per anhydrous glucose unit of cellulose is preferably 0.01 to 0.50. The upper limit is preferably 0.40 or less. If the degree of carboxyalkyl substitution exceeds 0.50, dissolution in water occurs easily, and the fiber form cannot be maintained in water. In order to obtain the effect of carboxyalkylation, it is necessary to have a certain degree of substitution. For example, if the degree of substitution is less than 0.02, depending on the application, the advantage of introducing a carboxyalkyl group may not be obtained. Therefore, the degree of carboxyalkyl substitution is preferably 0.02 or more, more preferably 0.05 or more, more preferably 0.10 or more, more preferably 0.15 or more, more preferably 0.20 or more, and even more preferably 0.25 or more. The degree of carboxyalkyl substitution can be adjusted by controlling the amount of the carboxyalkylating agent to be reacted, the amount of the mercerizing agent, the composition ratio of water to the organic solvent, and the like.
[0026] In this specification, anhydroglucose unit means each anhydroglucose (glucose residue) constituting cellulose. In addition, the degree of carboxyalkyl substitution (also called the degree of etherification) indicates the ratio of hydroxyl groups in the glucose residues constituting cellulose that are substituted with carboxyalkyl ethers (the number of carboxyalkyl ethers per glucose residue). The degree of carboxyalkyl substitution is sometimes abbreviated as DS.
[0027] The method for determining the degree of carboxyalkyl substitution is as follows: Weigh out approximately 2.0 g of the sample and place it in a 300 mL Erlenmeyer flask with a stopper. Add 100 mL of nitric acid methanol (a solution of 100 mL of concentrated nitric acid added to 1000 mL of methanol) and shake for 3 hours to convert the salt-type carboxyalkylated cellulose to hydrogen-type carboxyalkylated cellulose. Weigh out 1.5 to 2.0 g of hydrogen-type carboxyalkylated cellulose (absolutely dry) and place it in a 300 mL Erlenmeyer flask with a stopper. Moisten with 15 mL of 80% methanol, add 100 mL of 0.1 N-NaOH, and shake at room temperature for 3 hours. Using phenolphthalein as an indicator, back-titrate the excess NaOH with 0.1 N-H2SO4, and calculate the degree of carboxyalkyl substitution (DS) using the following formula. A = [(100 × F'-0.1N-H2SO4 (mL) × F) × 0.1] / (bone-dry mass of hydrogen-type carboxyalkylated cellulose (g)) Degree of carboxyalkyl substitution (DS) = 0.162 x A / (1-0.058 x A) F': Factor of 0.1N-H2SO4 F: Factor of 0.1N NaOH.
[0028] The DS of the carboxyalkylated cellulose before fibrillation and the DS of the carboxyalkylated cellulose after fibrillation (carboxyalkylated MFC) are usually the same.
[0029] As an example of a method for producing carboxyalkylated cellulose, an example for producing carboxyalkylated cellulose will be described below. First, the cellulose raw material is mixed with a solvent and a mercerizing agent, and the cellulose raw material is mercerized at a reaction temperature of 0 to 70° C., preferably 10 to 60° C., for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Next, the mercerizing agent is added in an amount of 0.05 to 10.0 times the moles per glucose residue, and mercerization is performed at a reaction temperature of 30 to 90° C., preferably 40 to 80° C., for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.
[0030] As the solvent, 3 to 20 times by mass of water or an organic solvent or a mixture thereof can be used. Examples of the organic solvent include, but are not limited to, alcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, isobutanol, and tertiary butanol, ketones such as acetone, diethyl ketone, and methyl ethyl ketone, as well as dioxane, diethyl ether, benzene, and dichloromethane. Among these, monohydric alcohols having 1 to 4 carbon atoms are preferred because of their excellent compatibility with water, and monohydric alcohols having 1 to 3 carbon atoms are more preferred. As the mercerizing agent, it is preferred to use 0.5 to 20 times by mole of an alkali metal hydroxide per anhydrous glucose residue of the cellulose raw material, specifically sodium hydroxide or potassium hydroxide. Examples of the mercerizing agent include monochloroacetic acid, sodium monochloroacetate, methyl monochloroacetate, ethyl monochloroacetate, and isopropyl monochloroacetate. Among these, monochloroacetic acid or sodium monochloroacetate is preferred in terms of the ease of availability of the raw material. The amount of the CM agent used is not particularly limited, but is preferably added in the range of 0.5 to 1.5 mol per anhydrous glucose unit of cellulose. The lower limit of the above range is more preferably 0.6 mol or more, and even more preferably 0.7 mol or more, and the upper limit is more preferably 1.3 mol or less, and even more preferably 1.1 mol or less. The CM agent may be added to the reactor as, for example, a 5 to 80 mass % and more preferably a 30 to 60 mass % aqueous solution, but is not limited thereto, or may be added in a powder state without being dissolved in a solvent such as water.
[0031] When monochloroacetic acid or sodium monochloroacetate is used as the CM agent, the molar ratio of the mercerizing agent to the CM agent (mercerizing agent / CM agent) is generally set to 0.90 to 2.45. This is because if it is less than 0.90, the CM reaction may be insufficient, and unreacted monochloroacetic acid or sodium monochloroacetate may remain and be wasted, and if it exceeds 2.45, a side reaction between the excess mercerizing agent and monochloroacetic acid or sodium monochloroacetate may proceed, resulting in the production of an alkali metal glycolate, which may be uneconomical.
[0032] When CM is performed on a cellulose raw material, there are usually a method in which both mercerization and CM are performed in a solvent mainly composed of water (aqueous medium method) and a method in which both mercerization and CM are performed in a mixed solvent of water and an organic solvent (solvent method), but in the present invention, a solvent mainly composed of water may be used for mercerization and a mixed solvent of an organic solvent and water may be used for CM. By doing so, it is possible to economically obtain CM-modified cellulose in which CM groups are introduced uniformly, not locally, even when the crystallinity of the cellulose is maintained at 50% or more.
[0033] A solvent that mainly uses water (a solvent that is mainly made of water) refers to a solvent that contains water at a ratio of more than 50% by mass. The amount of water in the solvent that is mainly made of water is preferably 55% by mass or more, more preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more. Particularly preferably, the solvent that is mainly made of water is 100% by mass (i.e., water). The higher the amount of water during mercerization, the more advantageously the CM group is introduced more uniformly into the cellulose. As the solvent other than water in the solvent that is mainly made of water (used in a mixture with water), the organic solvents described above can be used. The amount of the organic solvent in the solvent that is mainly made of water is preferably 45% by mass or less, more preferably 40% by mass or less, more preferably 30% by mass or less, more preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and more preferably 0% by mass.
[0034] It is preferable to add an organic solvent or an aqueous solution of an organic solvent to the reactor simultaneously with the addition of the CM agent, or before or immediately after the addition of the CM agent, or to reduce the amount of organic solvent other than water used in the mercerization treatment by reducing pressure or the like to form a mixed solvent of water and an organic solvent, and to allow the CM reaction to proceed in this mixed solvent of water and an organic solvent. The timing of adding or reducing the organic solvent may be any time between the end of the mercerization reaction and just after the addition of the CM agent, and is not particularly limited, but is preferably within 30 minutes before or after the addition of the CM agent, for example.
[0035] The ratio of the organic solvent in the mixed solvent during CMization is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 45% by mass or more, and particularly preferably 50% by mass or more, based on the total of water and organic solvent. The higher the ratio of the organic solvent, the more uniform the CM group substitution is, and the more stable the quality of the obtained CM-modified cellulose is. There is no upper limit to the ratio of the organic solvent, and it may be, for example, 99% by mass or less. In consideration of the cost of the organic solvent to be added, it is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0036] The reaction medium for CM (a mixed solvent of water and an organic solvent, etc., not containing cellulose) preferably has a lower proportion of water (in other words, a higher proportion of organic solvent) than the reaction medium for mercerization. By satisfying this range, the crystallinity of the resulting CM-cellulose is easily maintained. In addition, when the reaction medium for CM has a lower proportion of water (a higher proportion of organic solvent) than the reaction medium for mercerization, there is also an advantage that when transferring from the mercerization reaction to the CM reaction, a mixed solvent for the CM reaction can be formed by the simple means of adding a desired amount of organic solvent to the reaction system after the mercerization reaction is completed.
[0037] <Anion modification - phosphate esterification> An example of anionic modification is phosphorylation, which introduces a phosphate group into a cellulose chain. In this specification, phosphorylated cellulose is referred to as "phosphated cellulose". As the phosphated cellulose, commercially available products may be used, or it may be produced by phosphorylating the above-mentioned cellulose raw material by a known method. The degree of phosphate substitution per glucose unit of the phosphated cellulose is preferably 0.001 or more and less than 0.40. The degree of phosphate substitution in the phosphated cellulose before fibrillation is usually the same as the degree of phosphate substitution in the phosphated cellulose after fibrillation (phosphated MFC).
[0038] Examples of the method of phosphate esterification include a method of mixing a powder or an aqueous solution of a compound having a phosphoric acid group with a cellulose raw material, and a method of adding an aqueous solution of a compound having a phosphoric acid group to a slurry of a cellulose raw material. Examples of the compound having a phosphoric acid group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium phosphite, potassium phosphite, sodium hypophosphite, potassium hypophosphite, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. Phosphate groups can be introduced into the cellulose raw material by using one or more of these in combination. Among these, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are preferred from the viewpoints of high efficiency of phosphoric acid group introduction and easy industrial application. Sodium dihydrogen phosphate and disodium hydrogen phosphate are particularly preferred. In addition, it is desirable to use the compound having a phosphoric acid group as an aqueous solution, since the reaction can proceed uniformly and the efficiency of phosphoric acid group introduction is high. The pH of the aqueous solution of the compound having a phosphate group is preferably 7 or less since this increases the efficiency of introducing the phosphate group, but is preferably 3 to 7 from the viewpoint of suppressing hydrolysis of the fibers.
[0039] Specific examples of methods for producing cellulose phosphate include the following. A compound having a phosphate group is added to a suspension of a cellulose raw material having a solid content concentration of 0.1 to 10% by mass while stirring to introduce phosphate groups into the cellulose. When the cellulose raw material is taken as 100 parts by mass, the amount of the compound having a phosphate group added is preferably 0.2 to 500 parts by mass, more preferably 1 to 400 parts by mass, in terms of phosphorus element amount.
[0040] After the obtained suspension of cellulose phosphate is dehydrated, from the viewpoint of suppressing hydrolysis of cellulose, it is preferably heat-treated at 100 to 170° C. Furthermore, it is preferable to heat at 130° C. or less, preferably 110° C. or less while water is contained during the heat treatment, and to heat at 100 to 170° C. after the water is removed.
[0041] <Fibrillation> For example, the anion-modified cellulose obtained by the above method can be appropriately beaten or defibrated to obtain fibrillated anion-modified cellulose (anion-modified microfibrillary cellulose, anion-modified MFC). The beating or defibration in the fibrillation is preferably performed in a wet state (i.e., in the form of a dispersion in which water or the like is used as a dispersion medium) using an apparatus such as a disk-type, conical-type, or cylindrical-type refiner, a high-speed defibrator, a shear-type mixer, a colloid mill, a high-pressure jet disperser, a cavitation, a beater, a PFI mill, a kneader, or a disperser, but is not particularly limited to these apparatuses, and any apparatus that imparts mechanical defibration force in a wet state may be used.
[0042] When fibrillation is performed by a wet method, a dispersion of anion-modified cellulose is prepared. The solid content concentration in the dispersion of anion-modified cellulose to be subjected to fibrillation is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more. The upper limit of the concentration is preferably 40% by mass or less, more preferably 30% by mass or less, more preferably 10% by mass or less, and even more preferably 8% by mass or less. The dispersion medium is preferably water.
[0043] The pH of the dispersion of anion-modified cellulose to be fibrillated is preferably 7.0 or less, more preferably 6.0 or less, and even more preferably 5.0 or less. There is no particular lower limit for the pH, and it is usually 2.0 or more, preferably 3.0 or more, and more preferably 3.5 or more. The pH can be adjusted by adding an acid such as hydrochloric acid to the dispersion.
[0044] Before preparing a dispersion for fibrillation, the anion-modified cellulose obtained by the above method may be dried and pulverized in advance. The dry-pulverized anion-modified cellulose may then be dispersed in a dispersion medium and subjected to fibrillation (wet). The apparatus used for dry-pulverizing the raw material is not particularly limited, and examples thereof include impact mills such as hammer mills and pin mills, media mills such as ball mills and tower mills, and jet mills.
[0045] As described later, the fibrillation is performed in such a range that, in the obtained MFC, (A) the average phase difference obtained from a phase difference map image obtained at a wavelength of 543 nm with a two-dimensional birefringence evaluation system microscope is 10.0 nm or less, the variation (standard deviation) of the average phase difference is 15.0 nm or less, (B) the average fiber width is within the range of 1.0 to 28.0 μm, and (C) the fiber ratio in the range of 0 to 0.2 mm in the length-weighted fiber length distribution is 80.0% or more. In order to obtain such an anion-modified MFC, it is preferable to adjust the concentration and processing flow rate during fibrillation, and further to adjust the processing speed (solid kg / min). The processing flow rate is preferably 10 to 1000 L / min, more preferably 50 to 600 L / min, and even more preferably 80 to 400 L / min. In the case of beating treatment with a refiner, 80 to 280 L / min is more preferable, and in the case of treatment with a high-speed fiberizer such as a top finer, 150 to 400 L / min is more preferable. The treatment speed is preferably 0.2 to 20 kg / min solid, more preferably 0.5 to 15 kg / min solid, and further preferably 1.0 to 10 kg / min solid.
[0046] <Average phase difference and its standard deviation> The anion-modified MFC of the present invention has an average phase difference (hereinafter simply referred to as "average phase difference") obtained from a phase difference map image acquired at a wavelength of 543 nm by a two-dimensional birefringence evaluation system microscope of 10.0 nm or less. More preferably, it is 8.0 nm or less. The lower limit is not particularly limited, but is preferably 2.0 nm or more, and more preferably 3.0 nm or more. In addition, the anion-modified MFC of the present invention has a standard deviation of a phase difference distribution obtained from a phase difference map image acquired at a wavelength of 543 nm by a two-dimensional birefringence evaluation system microscope of 15.0 nm or less. More preferably, it is 12.0 nm or less, and even more preferably, it is 10.0 nm or less. This average phase difference and its standard deviation are indicators of the degree of cellulose defibration, as explained in Non-Patent Document 1. By performing fibrillation to such an extent that the average phase difference and its standard deviation are within this range, a characteristic of having an appropriate balance of fibers in the submicron region in which fibrillation has progressed can be obtained. Therefore, compared to conventional MFCs in which the fiber distribution is not adjusted, it has superior uniformity, dispersion stability, thixotropy, and viscosity.
[0047] In the present invention, the average phase difference can be measured by the following method: Using ion-exchanged water, prepare a 0.2% by mass aqueous dispersion of anion-modified MFC while stirring at 3000 rpm for 1 minute. A quartz channel with an internal channel cross-sectional dimension of 1 mm x 1 mm is horizontally placed on the observation stage of a two-dimensional birefringence evaluation system microscope (product name: WPA-micro, manufactured by Photonic Lattice), and the prepared aqueous dispersion is poured into the quartz channel with a syringe to fill it. After obtaining a baseline at the quartz glass part outside the channel, the observation field is returned so that the channel is in the center, and a 2x, 5x, or 20x objective lens is selected as necessary, and a phase difference map image is obtained at a wavelength of 543 nm. From the obtained phase difference map image, the average phase difference and standard deviation are obtained using WPA-View analysis software (version 2.4.9.5, manufactured by Photonic Lattice). Note that five or more phase difference map images are obtained at each magnification for each sample, and the average phase difference and standard deviation are obtained for the five or more images, and their average values are obtained as the average phase difference and standard deviation of the corresponding sample.
[0048] <Average fiber width> The anion-modified MFC of the present invention has an average fiber width of 1.0 to 28.0 μm. More preferably, it is 2.0 to 26.0 μm, and even more preferably, it is 4.0 to 24.0 μm. By performing moderate fibrillation to such an extent that the average fiber width falls within this range, an MFC is obtained that contains a small proportion of fibers close to unfibrillated and a large amount of fibers that have been finely refined to the submicron level. Such an MFC is excellent in expressing thixotropy and exerting viscosity.
[0049] In the present invention, the average fiber width can be measured in the following manner: 300mL of the aqueous dispersion diluted to 0.1g of anion-modified MFC solids was subjected to an image analysis type fiber analyzer (product name: L&W Fiber Tester Plus, manufactured by ABB) and measurements were performed for 300 seconds to determine the length-weighted fiber width (n=2). Note that the measurement was performed after setting the Max value of Fines Limit to 0 and the Min value of Length class1 to 0 on the Sample type screen that determines the measurement conditions.
[0050] <Fiber ratio in the 0~0.2mm length range> In the anion-modified MFC of the present invention, the fiber ratio in the range of 0 to 0.2 mm in the length-weighted fiber length distribution (hereinafter simply referred to as "fiber ratio" or "fiber ratio of 0 to 0.2 mm length") is 80.0% or more. More preferably, it is 85.0% or more, and further preferably, it is 90.0% or more. There is no particular upper limit, and it is 100.0% or less. By adjusting the fibrillation to such an extent that the above fiber ratio falls within this range, the effects of the present invention can be appropriately obtained.
[0051] In the present invention, the fiber ratio can be measured by the following method: 300 mL of an aqueous dispersion diluted to 0.1 g of anion-modified MFC solids was fed into an image analysis type fiber analyzer (product name: L&W Fiber Tester Plus, manufactured by ABB) and measurements were taken for 300 seconds, and the fiber ratio in the range of 0 to 0.2 mm was calculated from L1 (displayed as the fiber ratio of 0 to 0.1 mm length multiplied by 100) and L2 (displayed as the fiber ratio of 0.1 to 0.2 mm length multiplied by 100). Note that the measurement was performed after setting the Max value of Fines Limit to 0 and the Min value of Length class 1 to 0 on the Sample type screen that defines the measurement conditions.
[0052] <Transparency> The anion-modified MFC of the present invention, when dispersed in water with a solid content concentration of 1% by mass, preferably has a transmittance (hereinafter referred to as "transparency") of light with a wavelength of 660 nm of 60.0% or less, more preferably 50.0% or less, and even more preferably 45.0% or less. There is no particular lower limit and it may be 0.0% or more. When the transparency is in this range, the degree of fibrillation is appropriate and the effects of the present invention are easily obtained. In the present invention, the transparency can be measured by the following method: An aqueous dispersion of anion-modified MFC (solid content concentration: 1% by mass) is prepared, and the transmittance of light with a wavelength of 660 nm is measured using a UV-VIS spectrophotometer UV-1800 (Shimadzu Corporation) with a square cell with an optical path length of 10 mm.
[0053] <Krill value> The krill value is a relative numerical value representing the amount of fibers (krill) on the order of submicrons, and is a value measured by the following method. When the anion-modified MFC of the present invention has a krill value in the range of more than 2.0 and less than 4.0, it is preferable from the viewpoint of excellent thixotropy since it contains many fibers in the submicron range. Also, when the krill value is in the range of 0.0 or more and 2.0 or less, it is preferable from the viewpoint of low viscosity and excellent workability. In the present invention, the krill value can be measured by the following method: 300 mL of an aqueous dispersion containing 0.1 g of anion-modified MFC in solid content was prepared, and the dispersion was subjected to an image analysis type fiber analyzer (product name: L&W Fiber Tester Plus, manufactured by ABB) and measurements were performed for 300 seconds, and the resulting crill value was used.
[0054] <Other> The anion-modified MFC of the present invention preferably has a BET specific surface area of 100 m 2 / g or more, more preferably 110m 2 / g or more. When the BET specific surface area is large, the degree of fibrillation is appropriate, and the effects of the present invention are easily obtained. The BET specific surface area can be measured by the following method with reference to the nitrogen gas adsorption method (JIS Z 8830): (1) Approximately 2% by mass of anion-modified MFC slurry (dispersion medium: water) was separated and placed in a centrifuge container so that the solid content was approximately 0.1 g, and 100 mL of ethanol was added. (2) Add a stirrer and stir at 500 rpm for at least 30 minutes. (3) Remove the stirrer and sediment the anion-modified MFC in a centrifuge at 7,000 G for 30 minutes at 30°C. (4) Remove the supernatant while trying to avoid removing as much of the anion-modified MFC as possible. (5) Add 100 mL of ethanol, add a stir bar, stir under conditions (2), centrifuge under conditions (3), and remove the supernatant under conditions (4); repeat this process three times. (6) The solvent in (5) is changed from ethanol to t-butanol, and the stirring, centrifugation, and removal of the supernatant are repeated three times in the same manner as in (5) at room temperature above the melting point of t-butanol. (7) After the final solvent removal, add 30 mL of t-butanol, mix gently, then transfer to a recovery flask and freeze in an ice bath. (8) Chill in the freezer for at least 30 minutes. (9) Place in a freeze-dryer and freeze-dry for 3 days. (10) Measure the BET specific surface area (pretreatment conditions: under nitrogen flow at 105°C for 2 hours, relative pressure of 0.01 to 0.30, sample amount of approximately 30 mg).
[0055] The degree of crystallinity of the cellulose in the anion-modified MFC of the present invention is preferably 50% or more, more preferably 60% or more, for crystalline type I. The crystallinity of the cellulose can be controlled by the degree of anion modification. The upper limit of the degree of crystallinity of cellulose type I is not particularly limited. In reality, the upper limit is thought to be about 90%.
[0056] The method for measuring the crystallinity of cellulose type I of anion-modified MFC is as follows: The sample is placed in a glass cell and measured using an X-ray diffraction measuring device (product name: LabX XRD-6000, manufactured by Shimadzu Corporation). The degree of crystallinity is calculated using the method of Segal et al., and is calculated from the diffraction intensity of the 002 plane at 2θ = 22.6° and the diffraction intensity of the amorphous part at 2θ = 18.5° using the diffraction intensity of the X-ray diffraction pattern at 2θ = 10° to 30° as the baseline, according to the following formula.
[0057] Xc = (I002c - Ia) / I002c x 100 Xc = Crystallinity of cellulose type I (%) I002c: 2θ=22.6°, diffraction intensity of 002 plane Ia: 2θ=18.5°, diffraction intensity of the amorphous part.
[0058] The anion-modified MFC of the present invention, when used in water as a dispersion medium, generally takes the form of a translucent to white gel, cream, or paste with a solids concentration of about 1% by mass or more. The anion-modified MFC may be in the form of a dispersion obtained after production, but may be dried or redispersed in water as necessary. The drying method is not particularly limited, and known methods such as freeze drying, spray drying, tray drying, drum drying, belt drying, thin spreading on a glass plate or the like and drying, fluidized bed drying, microwave drying, and heated fan type reduced pressure drying can be used. After drying, the MFC may be pulverized with a cutter mill, hammer mill, pin mill, jet mill, or the like as necessary. The method of redispersion in water is also not particularly limited, and known dispersing devices can be used.
[0059] <Application> The anion-modified MFC of the present invention is superior in dispersibility, expression of thixotropy, and exertion of viscosity, etc., compared with conventional MFC in which the fiber state is not adjusted, and is therefore expected to easily exert the desired effects with the addition of a small amount when used in various applications. In addition, since the degree of defibration is not too strong and an appropriate fiber diameter in the submicron region is maintained, it is considered that it can be used particularly optimally in applications requiring fiber strength or applications requiring high fiber yield. However, it may also be used in other applications. The fields in which anion-modified MFC is used are not limited, and it is believed that it can be used as a thickener, gelling agent, paste, food additive, excipient, paint additive, adhesive additive, papermaking additive, abrasive, rubber / plastic compounding material, water retention agent, shape retention agent, muddy water regulator, filter aid, overflow prevention agent, etc. in various fields in which additives are generally used, such as food, feed, cosmetics, medicine, papermaking, various chemical products, paints, sprays, pesticides, civil engineering, construction, electronic materials, flame retardants, household goods, adhesives, cleaning agents, fragrances, lubricating compositions, etc.
[0060] Examples of food products include, but are not limited to, water retention agents, shape retention agents, viscosity regulators, emulsion stabilizers, dispersion stabilizers, etc. Examples of foods that can be used include, but are not limited to, beverages (cocoa, juices containing fiber and fruit pulp, shiruko, amazake, lactic acid bacteria drinks, fruit milk, etc.), soups (corn soup, ramen soup, miso soup, consommé, etc.), sauces, dressings, ketchup, mayonnaise, jams, yogurt, whipped cream, dried foods (dried processed foods, instant ramen, pasta noodles, etc.), gluten-free pasta, ice cream, monaka, sherbet, polyjuice, confectioneries (gummy candies, soft candies, jellies, cookies, etc.), meringues, bread, gluten-free bread, fillings, pancakes, pastes, edible films, etc.
[0061] When added to food, the amount added can be appropriately selected depending on the expected effect, but for example, it is preferably 0.1 to 20 mass % relative to the total mass of the food, more preferably 0.5 to 15 mass %, and even more preferably 0.5 to 10 mass %.
[0062] For pharmaceutical purposes, the composition can be used, for example and without limitation, as a water retention imparting agent, shape retention imparting agent, viscosity modifier, emulsion stabilizer, dispersion stabilizer, etc. For pharmaceutical purposes, the composition can be used, for example and without limitation, as a tablet, ointment, bandage, cataplasm, hand cream, toothpaste, etc.
[0063] When added to a pharmaceutical product, the amount added can be appropriately selected depending on the expected effect, but for example, the amount is preferably 0.1 to 30 mass%, more preferably 0.5 to 20 mass%, and even more preferably 0.5 to 10 mass%, relative to the total mass of the pharmaceutical product.
[0064] For cosmetics, for example, but not limited to, it can be used as a water retention imparting agent, shape retention imparting agent, viscosity adjusting agent, emulsion stabilizer, dispersion stabilizer, etc. For cosmetics that can be used, for example, but not limited to, face powder, foundation, scrub face wash, pack, face wash foam, face wash cream, hair mousse, shampoo, soap, lotion, hair color, hair bleach, mascara, eyeliner, nail, antiperspirant, etc.
[0065] The amount added to a cosmetic product can be appropriately selected depending on the expected effect, but is preferably 0.1 to 30 mass %, more preferably 0.5 to 20 mass %, and even more preferably 0.5 to 10 mass %, relative to the total mass of the cosmetic product.
[0066] For feed, for example, but not limited to, it can be used as a water retention imparting agent, a shape retention imparting agent, a viscosity adjusting agent, an emulsion stabilizer, a dispersion stabilizer, etc. For feed, for example, but not limited to, moist pellets, expansion pellets, milk substitutes for cows, etc. can be used.
[0067] The amount added to feed can be appropriately selected depending on the expected effect, but is preferably 0.1 to 20 mass%, more preferably 0.5 to 15 mass%, and even more preferably 0.5 to 10 mass%, based on the total mass of the feed.
[0068] Examples of papermaking agents include, but are not limited to, water retention agents, shape retention agents, viscosity regulators, emulsion stabilizers, and dispersion stabilizers. They can also be used as papermaking chemicals, such as surface sizing agents, retention improvers, paper strength agents, coating agents, and bulky paper additives.
[0069] When used as a papermaking chemical, the amount added can be appropriately selected depending on the expected effect, but for example, it is preferably 0.1 to 30 mass % relative to the total mass of the papermaking chemical, more preferably 0.5 to 20 mass %, and even more preferably 0.5 to 10 mass %.
[0070] Examples of paints that can be used include, but are not limited to, water retention agents, shape retention agents, viscosity adjusters, emulsion stabilizers, dispersion stabilizers, etc. Examples of paints that can be used include, but are not limited to, matte paints, architectural paints, and automotive paints.
[0071] The amount added to the paint can be appropriately selected depending on the expected effect, but is preferably 0.1 to 30 mass %, more preferably 0.5 to 20 mass %, and even more preferably 0.5 to 10 mass %, based on the total mass of the paint. EXAMPLES
[0072] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. Unless otherwise specified, parts and % indicate parts by mass and % by mass.
[0073] Example 1 5.00 g (bone dry) of bleached unbeaten kraft pulp (brightness 85%) derived from coniferous trees was added to 500 mL of an aqueous solution containing 39 mg (0.05 mmol per 1 g of bone dry cellulose) of TEMPO (Sigma Aldrich) and 514 mg (1.0 mmol per 1 g of bone dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.5 mmol / g, and the oxidation reaction was started at room temperature. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The mixture after the reaction was filtered through a glass filter to separate the pulp, and the pulp was thoroughly washed with water to obtain oxidized pulp (carboxylated cellulose). The pulp yield was 90%, the time required for the oxidation reaction was 90 minutes, and the amount of carboxyl groups was 1.4 mmol / g.
[0074] The oxidized pulp obtained in the above process was adjusted to 2.5% (w / v) with water and treated 10 times in a cavitation jet device at 7MPa with the treatment concentration and treatment flow rate adjusted to the above ranges to obtain oxidized MFC. The physical properties of the obtained oxidized MFC are shown in Table 1.
[0075] Example 2 40 kg (bone-dry) of bleached unbeaten kraft pulp (whiteness 85%: manufactured by Nippon Paper Industries Co., Ltd.) derived from conifers was added to 4000 L of an aqueous solution containing 312 g (0.05 mmol per 1 g of bone-dry cellulose) of TEMPO (manufactured by Sigma Aldrich) and 4112 g (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.5 mmol / g, and the oxidation reaction was started at room temperature. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. After adding hydrochloric acid to the reaction mixture to adjust the pH to 2, the pulp was thoroughly washed by repeatedly dehydrating and diluting with water, and finally an oxidized pulp was obtained until the pulp solids concentration reached 20% by mass. The pulp yield was 90% and the carboxyl group content was 1.41 mmol / g.
[0076] The obtained oxidized pulp was dispersed in tap water, sodium hydroxide was added, and the mixture was stirred to obtain an aqueous dispersion of oxidized pulp having a pH of 7.7 and a solid content of 1.1% by mass. 3000 kg of the obtained aqueous dispersion of oxidized pulp was refined in a monoflow type double disc refiner (AWN20 manufactured by Aikawa Iron Works Co., Ltd.) by adjusting the blade height, blade width, clearance, etc. appropriately so as to prevent mechanical contact, and the treatment concentration and treatment flow rate were adjusted to the aforementioned range while performing partial circulation under a circulation rate of 77%, and the oxidized pulp was beaten to produce oxidized MFC. The physical properties of the obtained oxidized MFC are shown in Table 1.
[0077] Example 3 The oxidized pulp obtained in the same manner as in Example 2 was dispersed in ion-exchanged water to obtain an aqueous dispersion of oxidized pulp having a solid content concentration of 4.95 mass %.
[0078] To the aqueous dispersion, 0.6 g of 5% sodium hydroxide solution and 0.14 g of 35% hydrogen peroxide solution were added per 1 g of bone-dry oxidized pulp, and then thoroughly stirred. After stirring, the mixture was left to stand for 30 minutes to obtain hydrogen peroxide-treated oxidized pulp. 72 L of the obtained aqueous dispersion of hydrogen peroxide-treated oxidized pulp was circulated for 29 minutes using a 14-inch lab refiner (manufactured by Aikawa Iron Works Co., Ltd.) with the treatment concentration and treatment flow rate adjusted to the aforementioned ranges, to prepare oxidized MFC. The physical properties of the obtained oxidized MFC are shown in Table 1.
[0079] Example 4 The oxidized pulp obtained in the same manner as in Example 2 was dispersed in ion-exchanged water, sodium hydroxide was added, and the mixture was stirred to obtain an aqueous dispersion of oxidized pulp having a pH of 8.6 and a solids concentration of 2.0% by mass.
[0080] The resulting oxidized pulp aqueous dispersion (80 L) was circulated for 16 minutes using a 14-inch lab refiner (manufactured by Aikawa Iron Works Co., Ltd.) with the treatment concentration and treatment flow rate adjusted to the aforementioned ranges to prepare an oxidized MFC. The physical properties of the resulting oxidized MFC are shown in Table 1.
[0081] Example 5 In a twin-shaft kneader adjusted to a rotation speed of 100 rpm, 130 parts of water and 20 parts of sodium hydroxide dissolved in 100 parts of water were added, and 100 parts of hardwood pulp (LBKP, manufactured by Nippon Paper Industries Co., Ltd.) was added in terms of dry mass when dried at 100 ° C for 60 minutes. The mixture was stirred and mixed at 30 ° C for 90 minutes to prepare a mercerized cellulose raw material. Further, 250 parts of isopropanol (IPA) and 60 parts of sodium monochloroacetate were added while stirring, and after stirring for 30 minutes, the mixture was heated to 70 ° C and subjected to a mercury conversion reaction for 90 minutes. The concentration of IPA in the reaction medium during the mercury conversion reaction was 55%. After the reaction was completed, the mixture was neutralized with acetic acid to obtain mercury conversion cellulose (sodium salt) with a CM substitution degree of 0.34 and a crystallinity of cellulose I type of 65%.
[0082] The obtained carboxymethyl cellulose was dispersed in ion-exchanged water, sodium hydroxide was added thereto, and the mixture was stirred to obtain an aqueous dispersion of carboxymethyl cellulose having a pH of 7.5 and a solid content of 4.0% by mass.
[0083] The resulting aqueous dispersion of carboxymethyl cellulose (72 L) was circulated for 12 minutes using a B-50 Topfiner (manufactured by Aikawa Iron Works Co., Ltd.) with the treatment concentration and treatment flow rate adjusted to the aforementioned ranges to prepare a carboxymethyl cellulose MFC. The physical properties of the resulting carboxymethyl cellulose MFC are shown in Table 1.
[0084] Comparative Example 1 The oxidized pulp obtained in the same manner as in Example 1 was dispersed in ion-exchanged water, and sodium hydroxide was added and stirred to obtain an aqueous dispersion of oxidized pulp with a pH of 8.8 and a solid content of 4.72% by mass. The physical properties of the obtained oxidized pulp are shown in Table 1.
[0085] Comparative Example 2 80 L of the oxidized pulp aqueous dispersion obtained in Comparative Example 1 was circulated for 14 minutes using a 14-inch lab refiner (manufactured by Aikawa Iron Works Co., Ltd.) to prepare an oxidized MFC. The physical properties of the obtained oxidized MFC are shown in Table 1.
[0086] [Table 1]
[0087] The present invention provides an anion-modified MFC having: (A) an average phase difference obtained from a phase difference map image acquired at a wavelength of 543 nm using a two-dimensional birefringence evaluation system microscope of 10.0 nm or less, and a variation (standard deviation) in the average phase difference of 15.0 nm or less; (B) an average fiber width in the range of 1.0 to 28.0 μm; and (C) a fiber ratio in the range of 0 to 0.2 mm in the length-weighted fiber length distribution of 80.0% or more.
Claims
1. Anion-modified microfibril cellulose satisfying the following conditions (A) to (C): (A) The average phase difference obtained from a phase difference map image acquired at a wavelength of 543 nm using a two-dimensional birefringence evaluation system microscope is 10.0 nm or less, and the variation (standard deviation) of the average phase difference is 15.0 nm or less; (B) the average fiber width is in the range of 1.0 to 28.0 μm; and (C) The ratio of fibers in the range of 0 to 0.2 mm in the length-weighted fiber length distribution is 80.0% or more.
2. The anion-modified microfibril cellulose according to claim 1, having an average retardation of 8.0 nm or less.
3. The anion-modified microfibril cellulose according to claim 1 or 2, having an average retardation of 2.0 nm or more.
4. The anion-modified microfibril cellulose according to claim 1 or 2, having an average retardation of 3.0 nm or more.
5. 3. The anion-modified microfibril cellulose according to claim 1 or 2, which has a transmittance of 60.0% or less for light having a wavelength of 660 nm when dispersed in water at a solid content concentration of 1% by mass.
6. (D) the krill value is in the range of more than 2.0 and less than 4.0; The anionically modified microfibril cellulose according to claim 1 or 2, further satisfying the above.
7. (E) the krill value is in the range of 2.0 or less; The anionically modified microfibril cellulose according to claim 1 or 2, further satisfying the above.
8. An aqueous dispersion comprising the anionically modified microfibril cellulose according to claim 1 or 2.
Citation Information
Patent Citations
Paper comprising chemically-modified and fibrillated cellulose fiber-containing clear coating layer
JP2021161599A
Method for producing chemically modified microfibril cellulose fiber
JP2022051300A
Method for producing chemically modified microfibril cellulose fiber
JP2022111469A
Production method for chemically-modified microfibril cellulose fibers
WO2021054274A1
Method for manufacturing modified cellulose microfibrils
WO2021112195A1