Electrode, electrochemical element, device, mobile body, method for manufacturing electrode, and method for manufacturing electrochemical element
The electrode design with a 90% coverage insulating layer and branched flow paths addresses safety and permeability issues in electrochemical elements by preventing short circuits and enhancing electrolyte flow.
Patent Information
- Application Number
- JP2023045106
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional film separators in electrochemical elements, such as lithium ion batteries, have low heat resistance, leading to shrinkage or melting during short circuits, which can cause safety issues and reduce electrolyte permeability, affecting battery performance.
An electrode design with an insulating layer covering at least 90% of the electrode composite material layer, featuring a flow path that branches in multiple directions to enhance electrolyte permeability and prevent short circuits.
The design maintains safety by preventing short circuits and ensures excellent electrolyte permeability, improving battery performance and productivity.
Smart Images

Figure 2024134757000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode, an electrochemical element, a device, a moving body, a method for manufacturing an electrode, and a method for manufacturing an electrochemical element. [Background technology]
[0002] In recent years, as electrochemical elements have become higher in output and capacity, safety issues caused by stored energy have become an issue. In each electrode consisting of a positive electrode and a negative electrode used in a storage element such as a lithium-ion battery, an electrode mixture layer is formed on an electrode substrate such as a metal foil, and a lithium-ion-permeable separator is provided between the positive electrode and the negative electrode to prevent contact between the positive electrode and the negative electrode.
[0003] As such a separator, a film separator made of a thermoplastic resin is mainly used, but the film separator has a problem in that it has low heat resistance and is likely to shrink or melt due to heat generated when a short circuit occurs between the positive electrode and the negative electrode, thereby expanding the short circuit area. In view of this, an electric double layer capacitor separator has been disclosed that can suppress the occurrence of internal short circuits, is easy to handle even though it is thin, and is effective in reducing internal resistance. The electric double layer capacitor separator is made of electrically insulating ceramic powder particles bound with a binder that is resistant to an electrolyte and is integrally bonded to the surface of the positive electrode and / or negative electrode of the electric double layer capacitor, and has porosity that is continuous in the thickness direction (see, for example, Patent Document 1). Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide an electrode that is excellent in liquid permeability in the planar direction of the electrode while maintaining safety by forming an insulating layer on the surface of an electrode mixture layer. [Means for solving the problem]
[0005] The electrode of the present invention as a means for solving the above-mentioned problems is an electrode having an electrode substrate, an electrode mixture layer provided on the electrode substrate, and an insulating layer provided on the electrode mixture layer, wherein the insulating layer has an insulating portion covering the electrode mixture layer, and a flow path portion having a flow path that is connected in the planar direction of the electrode and branches in two or more directions, and the coverage rate of the electrode mixture layer by the insulating portion is 90% or more. Effect of the Invention
[0006] According to the present invention, it is possible to provide an electrode that is excellent in liquid permeability in the planar direction of the electrode while maintaining safety by forming an insulating layer on the surface of the electrode mixture layer. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of an electrode according to the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of the electrode of the present embodiment. [Figure 3A] FIG. 3A is a schematic diagram showing an example of a two-way branching flow path pattern in an insulating layer of an electrode according to this embodiment. [Figure 3B] FIG. 3B is a schematic diagram showing an example of a three-way branching flow path pattern in the insulating layer of the electrode of this embodiment. [Figure 3C] FIG. 3C is a schematic diagram showing another example of a flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 4A] FIG. 4A is a schematic diagram showing an example of a flow path pattern of an insulating layer in the electrode of this embodiment. [Figure 4B] FIG. 4B is a schematic diagram showing another example of a flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 4C] FIG. 4C is a schematic diagram showing another example of a flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 4D] FIG. 4D is a schematic diagram showing another example of a flow path pattern in the insulating layer of the electrode of this embodiment. [Figure 4E]FIG. 4E is a schematic diagram showing another example of the flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 4F] FIG. 4F is a schematic diagram showing another example of a flow path pattern in the insulating layer of the electrode of this embodiment. [Figure 4G] FIG. 4G is a schematic diagram showing another example of the flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 4H] FIG. 4H is a schematic diagram showing another example of the flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 5A] FIG. 5A is a schematic diagram showing another example of a flow path pattern of an insulating layer in the electrode of this embodiment. [Figure 5B] FIG. 5B is a schematic diagram showing another example of a flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 5C] FIG. 5C is a schematic diagram showing another example of a flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 5D] FIG. 5D is a schematic diagram showing another example of a flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 5E] FIG. 5E is a schematic diagram showing another example of the flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 5F] FIG. 5F is a schematic diagram showing another example of a flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 5G] FIG. 5G is a schematic diagram showing another example of the flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 5H] FIG. 5H is a schematic diagram showing another example of the flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 5I] FIG. 5I is a schematic diagram showing another example of a flow path pattern of the insulating layer in the electrode of this embodiment. [Figure 6A] FIG. 6A is a schematic diagram showing a flow path pattern of an insulating layer in the electrode of Comparative Example 1. FIG. [Figure 6B] FIG. 6B is a schematic diagram showing a flow path pattern of an insulating layer in the electrode of Comparative Example 2. [Figure 6C]FIG. 6C is a schematic diagram showing a flow path pattern of an insulating layer in the electrode of Comparative Example 3. [Figure 6D] FIG. 6D is a schematic diagram showing a flow path pattern of the insulating layer in the electrode of Comparative Example 4. [Figure 6E] FIG. 6E is a schematic diagram showing a flow path pattern of an insulating layer in the electrode of Comparative Example 5. [Figure 6F] FIG. 6F is a schematic diagram showing a flow path pattern of the insulating layer in the electrode of Comparative Example 6. [Figure 7] FIG. 7 is a schematic diagram showing an example of a method for producing an electrode according to this embodiment. [Figure 8] FIG. 8 is a schematic diagram showing another example of the electrode manufacturing apparatus of the present embodiment. [Figure 9] FIG. 9 is a schematic diagram showing an example of a method for producing an electrode according to this embodiment. [Figure 10] FIG. 10 is a schematic diagram showing an example of a modified example of the liquid ejection device. [Figure 11] FIG. 11 is a schematic diagram showing an example of a method for producing an electrode according to this embodiment. [Figure 12] FIG. 12 is a schematic diagram showing an example of a modified example of the liquid ejection device. [Figure 13] FIG. 13 is a cross-sectional view showing an example of the electrochemical device of this embodiment. [Figure 14] FIG. 14 is a schematic diagram showing an example of a moving body according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] (electrode) The electrode of the present invention has an electrode substrate, an electrode mixture layer provided on the electrode substrate, and an insulating layer provided on the electrode mixture layer, wherein the insulating layer has an insulating portion covering the electrode mixture layer, and a flow path portion having a flow path that is connected in the planar direction of the electrode and branches into two or more directions, and the coverage rate of the electrode mixture layer by the insulating portion is 90% or more.
[0009] The electrode of the present invention is an invention based on the fact that the present inventors have found the following problems in the conventional art. That is, in order to prevent short circuits between the positive and negative electrodes, it is desirable to cover the entire surface of the electrode mixture layer with an insulating layer, but in the electric double layer capacitor separator of the conventional technology, when an insulating layer is formed on the surface of the electrode mixture layer, insulating particles are filled into the gap between the electrode mixture layer and the film separator, so that the amount of electrolyte is reduced by the amount of insulating particles filled when the battery is assembled. In particular, in an electrode in which the gap is reduced by multi-layer lamination, the permeability of the electrolyte in the electrode plane direction is deteriorated during assembly of the battery, and there are problems in that the electrolyte does not reach all areas and air bubbles are trapped, thereby hindering ion permeation. Not only does the deterioration of the electrolyte permeability reduce productivity, but it also reduces battery performance.
[0010] <Insulating layer> The insulating layer has an insulating portion that covers the electrode mixture layer and a flow path portion that is connected in the planar direction of the electrode and has flow paths that branch into two or more directions, and the coverage rate of the electrode mixture layer by the insulating portion is 90% or more. The insulating portion covers 90% or more of the surface of the electrode mixture layer (coverage rate is 90% or more), thereby suppressing the occurrence of a short circuit between the positive electrode and the negative electrode. The flow path portion of the insulating layer communicates with the planar direction of the electrodes as a passage for the electrolyte, and the flow path portion is patterned in the insulating layer, thereby enabling the electrolyte to efficiently permeate between the electrode mixture layer and the separator. In addition, the flow path has branches in two or more directions, so that even if the flow path is blocked, the electrolyte can permeate by detouring, and therefore excellent liquid permeability can be exhibited even in a narrow flow path portion where the flow path is likely to be blocked.
[0011] 1, the electrode 10 has an electrode substrate 1, an electrode mixture layer 2 on the electrode substrate 1, and an insulating layer 3 on the electrode mixture layer 2. The insulating layer 3 has an insulating portion 3a that covers the electrode mixture layer 2, and a flow path portion 3b that communicates in the planar direction of the electrode 10 and has flow paths (or gaps) that branch in two or more directions. The coverage rate of the electrode mixture layer 2 by the insulating portion 3a is 90% or more. In one embodiment, as shown in Fig. 1, flow path portion 3b has an exposed surface of electrode mixture layer 2. In another embodiment, as shown in Fig. 2, flow path portion 3b has second insulating portion 3c on electrode mixture layer 2 in flow path portion 3b, and the thickness of second insulating portion 3c is smaller than the thickness of insulating portion 3a.
[0012] As shown in the schematic plan view of Fig. 3A, the insulating layer 3 has an insulating portion 3a that covers the electrode mixture layer 2, and a flow path portion 3b that communicates in the planar direction of the electrode 10 and has a flow path (or a gap) that branches in two directions. Alternatively, as shown in Fig. 3B, the insulating layer 3 may have a flow path portion 3b that has a flow path that branches in three directions. The flow channels having two-way branches, three-way branches, four-way branches, or five-way branches shown in FIG. 3C are all examples of the "flow channel branching into two or more directions" of the embodiment. Note that the flow path shown in FIG. 3C, which is blocked (not connected) or has no branching, does not correspond to the "flow path branching in two or more directions" of this embodiment, but the electrode of this embodiment may have such a flow path as long as it does not impede the effects of the present invention.
[0013] Suitable examples of the pattern formed from the insulating portion and the flow path portion include the patterns shown in FIGS. 4A to H and the patterns shown in FIGS. 5A to I. Here, Figures 4 to 6 are top views that show a schematic view of a portion of an electrode on which an insulating layer is formed, and in Figures 4 to 6, the white parts indicate the insulating parts, and the black parts indicate the flow path parts (or the exposed surface of the electrode mixture layer). Specifically, suitable patterns include combinations of shapes such as a triangle (Figure 4A), a diamond (Figure 4B), a honeycomb (Figure 4C), a scale (Figure 4D), a combination of circles and straight lines (Figure 4E), a vertical ladder shape (Figure 4F), a horizontal ladder shape (Figure 4G), a horizontal brick shape (or a horizontal rectangle, Figure 4H), an hemp leaf shape (Figure 5A), a cloisonne shape (Figure 5B), a herringbone shape (Figure 5C), a weight connection shape (Figure 5D), a brick masonry shape (or a vertical rectangle, Figure 5E), a basket weave shape (Figure 5F), a Moroccan shape (Figure 5G), a three-sided shape (Figure 5H), and a cypress fence shape (Figure 5I).
[0014] On the other hand, the patterns shown in FIGS. 6A to 6F are patterns used in Comparative Examples 1 to 6 in the examples described later, and all of them are modes in which the insulating layer in the electrode of this embodiment is not filled. Specifically, there are an embodiment without an insulating layer / uncoated (Figure 6A), an embodiment in which the insulating layer is fully coated and thus has no flow path (Figure 6B), an embodiment in which there are zigzag-shaped flow paths with no branches (Figure 6C), an embodiment in which the insulating portion has a random sea-island shape and has no communicating flow paths (Figure 6D), an embodiment in which the insulating portion has a lattice pattern and has no communicating flow paths (Figure 6E), and an embodiment in which the insulating portion has a checkerboard pattern and has no communicating flow paths (Figure 6F).
[0015] The insulating layer is not particularly limited and may be provided on either the positive electrode or the negative electrode, or may be provided on both the positive electrode and the negative electrode, depending on the purpose. In one embodiment, the electrode is preferably a positive electrode. That is, it is preferable that an insulating layer is provided on the positive electrode. When the positive electrode has a resin film separator made of, for example, polyolefin, etc., in contact with the positive electrode, the resin film separator gradually carbonizes due to charging of the battery, so that the charge gradually leaks from the resin film separator, leading to deterioration of the battery performance. When an insulating layer is provided on the positive electrode, it is preferable in terms of preventing carbonization of the resin film separator. In one embodiment, the electrode is preferably a negative electrode. That is, it is preferable that an insulating layer is provided on the negative electrode. When a positive electrode and a negative electrode having different sizes are stacked, a particularly strong pressure is applied to the outer peripheral end (edge) of the electrode, which may cause a short circuit inside the battery, resulting in a risk of fire. When the size of the negative electrode is larger than that of the positive electrode, it is preferable to provide an insulating layer on the negative electrode, since it reduces the generation of heat due to an internal short circuit and improves safety.
[0016] <<Insulation section>> The insulating portion is a coating film that covers the surface of the electrode mixture layer with an insulator, among the patterns formed on the insulating layer, and refers to a portion that is thicker than the flow path portion described below in the thickness direction of the insulating layer observed from a cross section in the electrode stacking direction.
[0017] [Insulation shape] From the viewpoint of passing the electrolyte uniformly through the entire electrode, the shape of the insulating part in the insulating layer is preferably a pattern in which insulating parts of the same shape are repeatedly arranged with a gap between them via a flow path part. Also, depending on the size of the electrode or the purpose of securing many inlets for the electrolyte, the insulating part may have a pattern in which insulating parts made of a combination of two or more shapes are repeatedly arranged with a gap between them via a flow path part. In addition, the end e of the insulating part is preferably rounded in order to disperse the pressure generated when stacking. If the corners of the insulating part are sharp, there is a risk that the adjacent flow path part will be blocked when the end e is damaged due to a load applied thereto by pressure.
[0018] [Coverage] The insulating layer covers the surface of the electrode mixture layer on the opposing electrode side, and the coverage (coverage ratio of the electrode mixture layer) is 90% or more in total. By covering 90% or more of the electrode mixture layer surface with the insulating layer, an excellent effect of preventing the occurrence of a short circuit is exhibited. In addition, since direct contact between the electrode mixture layer and the separator can be reduced, oxidation deterioration of the resin film separator in particular is suppressed, and the float characteristics are improved. The coverage is more preferably 92% or more, and even more preferably 95% or more.
[0019] The coverage can be calculated from an analysis image based on brightness and hue by observing the surface of the insulating layer with an optical microscope or a scanning electron microscope (SEM). Note that the image analysis may be performed by any method or condition that can distinguish between the covered portion and the uncovered portion of the insulating layer on the electrode mixture layer, and is not particularly limited and may be appropriately selected depending on the purpose. Other techniques that may be used include, for example, a component mapping technique using Fourier transform microscopic infrared spectroscopy (microscopic FT-IR) and analysis using elemental analysis by energy dispersive X-ray spectroscopy (EDS).
[0020] [Average thickness of insulation part] The average thickness of the insulating portion can be measured from a cross-sectional observation image of the electrode. An electrode (test piece) with an insulating layer cut into 5 mm squares was impregnated with a liquid that was vacuum-defoamed after mixing two-liquid epoxy resin (embedding epoxy resin type 53, manufactured by Sankei Co., Ltd.). The electrode impregnated with the epoxy resin was sandwiched between smooth polytetrafluoroethylene plates and cured in a thermostatic chamber at 40°C for 12 hours. After the epoxy resin was cured, the electrode was fixed on a glass plate with masking tape, and the blade of a 76 razor (manufactured by Nissin EM Co., Ltd.) was pressed vertically against the surface opposite the insulating layer to be observed for cross-section, to cut it. Furthermore, the cross-section of the cut sample was finished using a cross-section polisher (SM-09010, manufactured by JEOL Ltd.) under the conditions of an acceleration voltage of 5.0 kV, a beam current of 120 μA, and a processing time of 180 minutes. Using a scanning electron microscope (SEM) (Merlin, manufactured by Carl Zeiss Co., Ltd.), the cross section is photographed under the conditions of TLD, backscattered electron composition image, magnification 2500 times, WD 5.0 mm, acceleration voltage 2.0 kV, and field of view width 50.8 μm. The captured image is output as a TIFF image, and the image editing software GIMP 2.10.32 (GNU GPL) is used to calculate the area of the insulating part from the brightness difference of the image, and the thickness is calculated by dividing the area by the film thickness and the number of pixels in the vertical direction. The average value of the calculation results for three images with different viewing ranges is taken as the measured value.
[0021] The average thickness of the insulating portion is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 μm or more and 30 μm or less. The lower limit of the average thickness is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 4 μm or more, from the viewpoint of improving safety and liquid permeability of the flow path portion. The upper limit of the average thickness is preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less, because the gap between the positive electrode and the negative electrode becomes small, ion movement becomes easy, and the charging efficiency is improved, thereby suppressing side reactions and improving the float characteristics.
[0022] The insulating part is a porous structure that isolates the positive electrode and the negative electrode and ensures ionic conductivity between the positive electrode and the negative electrode. There are no particular limitations and the insulating part can be appropriately selected depending on the purpose. For example, the insulating part may be a porous structure formed from a composition containing insulating particles and a binder (first embodiment), or a porous resin obtained by polymerizing a liquid composition containing a polymerizable compound and a liquid (second embodiment).
[0023] [First embodiment: insulating part containing insulating particles] When the insulating part is a porous structure formed from a composition containing insulating particles and a binder, it is preferable that the porous structure has a porous structure in which a skeleton is formed by binding multiple insulating particles together with the binder.
[0024] -Insulating particles- The insulating particles are not particularly limited as long as they are highly electrically insulating particles, and can be appropriately selected depending on the purpose. Examples of the insulating particles include inorganic oxide particles and resin particles. These may be used alone or in combination of two or more. Among these, inorganic oxide particles are preferred from the viewpoints of the heat resistance of the insulating particles and the safety of the electrochemical device.
[0025] --Inorganic oxide particles-- The inorganic oxide particles are not particularly limited and can be appropriately selected depending on the purpose. Examples of the inorganic oxide particles include industrially synthesized or pulverized particles, ceramic particles, particles derived from mineral resources, and the like. Examples of inorganic oxide particles include aluminum oxide, titanium dioxide, barium titanate, zirconium dioxide, nickel oxide, manganese oxide, vanadium dioxide, silicon dioxide, cordierite, steatite, forsterite, mullite, zeolite, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of electrical resistance and stability, high-purity synthetic products are preferred, and it is more preferable to contain at least one of aluminum, silicon, and zirconium, with high-purity aluminum oxide (α-alumina) being even more preferred.
[0026] Commercially available aluminum oxide products include, for example, high purity alumina AKP series AKP-15, AKP-20, AKP-30, AKP-50, AKP-53, AKP-700, AKP-3000, AKP-G07, AKP-G15, etc. (all manufactured by Sumitomo Chemical Co., Ltd.); α-alumina Sumicorundum TM Series Sumicorundum TM Examples of such powders include AA-03, AA-04, AA-05, AA-07, AA-1.5, etc. (all manufactured by Sumitomo Chemical Co., Ltd.); alumina LS series LS-235, LS-235C, LS-711, LS-711C, LS-500, LS-250, etc. (all manufactured by Nippon Light Metal Co., Ltd.); plate-shaped alumina powder Seraph series SERATH00610, SERATH02025, etc. (all manufactured by Kinsei Matec Co., Ltd.); high-purity alumina Taimicron (TM) series TM-DA, TM-DAR, TM-5D, etc. (all manufactured by Taimei Chemical Industry Co., Ltd.); and the like.
[0027] Commercially available silicon dioxide products include, for example, AEROSIL fumed silica. TMSeries 50, 90G, 130, 200, 200V, 200CF, 200FAD, 300, 300CF, R972, R976, W7520, etc. (all manufactured by Nippon Aerosil Co., Ltd.); Spherical silica particles Sea Hoster TM KE series E10, E30, W10, W30, W50, P10, P30, P50, etc. (all manufactured by Nippon Shokubai Co., Ltd.); SYLOJET TM Series (GRACE DAVISON); Snowtex TM Series (manufactured by Nissan Chemical Co., Ltd.);
[0028] Commercially available zirconium oxide compounds include, for example, zirconia powder, Treceram TM Series 3YI-R, 3YLB, etc. (all manufactured by Toray Industries, Inc.), Zirconia nanoparticles Zircostar TM Series ZP-153, HR-101, etc. (all manufactured by Nippon Shokubai Co., Ltd.);
[0029] --Resin particles-- Suitable examples of the resin particles include thermosetting resins and thermoplastic resins having relatively high heat resistance and chemical resistance, such as melamine resins, unsaturated polyester resins, acrylic resins, and silicone-acrylic resins.
[0030] Commercially available resin particles include, for example, Optobeads, a composite spherical particle made of melamine resin and silica. TM Series 500S, 2000M, etc. (All of the above are manufactured by Nissan Chemical Co., Ltd.); Melamine / benzoguanamine resin fine particles Eposter TM Series SS, S, FS, S6, S12, etc. (all manufactured by Nippon Shokubai Co., Ltd.);
[0031] <Primary particle size> The primary particle diameter of the insulating particles means the average diameter of the primary particles (single particles) of the insulating particles. When the insulating particles are particles other than spherical, the longest part of the diameter of the particle (maximum diameter) is defined as the primary particle diameter, regardless of the aspect ratio. The average primary particle size of the insulating particles is preferably 500 nm or less. When the average primary particle diameter of the insulating particles is 500 nm or less, the pattern of the flow path portion can be precisely formed, improving the liquid permeability. In addition, when the electrode is a positive electrode, the thickness of the insulating portion becomes uniform, which is advantageous in improving the float characteristics. It is also preferable that the insulating particles have a uniform particle size and do not contain coarse particles, and that the insulating layer contains only insulating particles with a primary particle size of 1 μm or less. Specifically, the average primary particle diameter can be calculated from the average of the measured values of the diameter or the longest diameter of the primary particles by obtaining an image of the surface of the insulating part or of a cross section of the electrode processed in the same manner as in the measurement of the average thickness of the insulating part using a scanning electron microscope (Merlin, manufactured by Carl Zeiss K.K.).
[0032] -Binder- The binder is not particularly limited and can be appropriately selected depending on the purpose. Examples of the binder include acrylic resin, styrene-butadiene rubber resin, polyvinylidene fluoride, and polyvinylpyrrolidone.
[0033] -Dispersant- The composition for forming the insulating portion, which contains insulating particles and a binder, may further contain a dispersant in order to uniformly disperse the insulating particles in the solvent. Examples of the dispersant include a surfactant and a polymer compound having an adsorptive group. Commercially available dispersants include the fluorosurfactant Megafac. TM Series F173, F444, F470, etc. (all manufactured by DIC Corporation); High molecular weight dispersant Marialim TM Series AAB-0851, AFB-1521, AKM-0531, AWS-0851, HKM-50A, SC-0708A, SC-0505K, SC-1015F, etc. (all manufactured by NOF Corporation); Wetting and dispersing agent Disperser TM Series DISPERBYK-103, DISPERBYK-2000 (manufactured by BYK-Chemie);
[0034] The method for producing the composition for forming the insulating layer is not particularly limited, but it is preferable that the insulating particles are uniformly dispersed in the solvent. For example, the insulating particles are added to a solvent A, a dispersion is obtained using a dispersing machine, and then the obtained dispersion is diluted by adding a solvent B in which a binder and optionally a dispersing agent are dissolved. The solvent A and the solvent B may be the same solvent or different solvents.
[0035] Examples of the method for producing the dispersion include a method in which a solvent, insulating particles, and optionally a dispersant are preliminarily stirred, and then the mixture is dispersed in a dispersing machine. The dispersing machine is not particularly limited and can be appropriately selected depending on the purpose. Examples of the dispersing machine include a homomixer, a homogenizer, an ultrasonic dispersing machine, a ball mill, a bead mill, and a cavitation mill.
[0036] [Second embodiment: porous resin] The insulating portion may be a porous resin obtained by polymerizing a liquid composition containing a polymerizable compound and a liquid. Details of the polymerizable compound, the liquid, and the method for producing the porous resin will be described later in the method for producing an electrode of the present invention.
[0037] The porous resin as the insulating part is not particularly limited, but from the viewpoint of ensuring good permeability of liquids and gases, it is preferable that the porous resin has a three-dimensional branched network structure of the cured resin as a skeleton, and has a co-continuous structure (also called a monolith structure) in which a plurality of holes in the porous resin are continuously connected. That is, it is preferable that the porous resin has a large number of holes, and each hole has a connection with other holes around it and spreads three-dimensionally. By connecting the holes to each other, the infiltration of liquids and gases occurs sufficiently, and functions such as substance separation and reaction field can be efficiently expressed. Here, the "co-continuous structure" means a structure in which two or more substances or phases each have a continuous structure and do not form an interface, and in this embodiment, it means a structure in which both the resin phase and the pore phase are three-dimensional branched network continuous phases. Such structures can be formed, for example, by polymerizing the liquid composition by a polymerization induced phase separation method.
[0038] A method for confirming that the porous insulating layer has a bicontinuous structure and that the pores are interconnected can be, for example, a method for observing an image of a cross section of the porous insulating layer using a scanning electron microscope (SEM) or the like to confirm that the pores are interconnected. In addition, air permeability is one of the physical properties that can be obtained by interconnecting pores.
[0039] [Air permeability] The air permeability of the porous resin is preferably 1,000 sec / 100 mL or less, more preferably 500 sec / 100 mL or less, and even more preferably 300 sec / 100 mL or less. The air permeability is measured in accordance with JIS P8117, and can be measured, for example, by using a Gurley densometer (manufactured by Toyo Seiki Seisakusho, Ltd.). As an example, it may be determined that the pores are interconnected when the air permeability is 1,000 sec / 100 mL or less.
[0040] The cross-sectional shape of the pores of the porous resin may be various shapes and sizes, such as a substantially circular shape, a substantially elliptical shape, a substantially polygonal shape, etc. Here, the size of the pores refers to the length of the longest part in the cross-sectional shape. The size of the pores can be obtained from a cross-sectional photograph taken with a scanning electron microscope (SEM).
[0041] The size of the pores in the porous resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01 μm or more and 10 μm or less from the viewpoint of liquid or gas permeability. When the pore size is 0.1 μm or more and 10 μm or less, the liquid or gas can be sufficiently infiltrated into the porous structure, and functions such as material separation and reaction field can be efficiently exhibited. In addition, when the porous resin is used as an insulating layer of an electric storage element, when the pore size is 10 μm or less, short circuit between the positive electrode and the negative electrode due to lithium dendrites generated inside the electric storage element can be prevented, and safety is improved. The method for adjusting the pore size and porosity of the porous resin to fall within these ranges is not particularly limited, and examples thereof include a method of adjusting the content of the polymerizable compound in the liquid composition to fall within the above-mentioned range, a method of adjusting the content of the porogen in the liquid composition to fall within the above-mentioned range, and a method of adjusting the irradiation conditions of active energy rays.
[0042] <<Flow passage section>> The flow path portion has flow paths which communicate with each other in the planar direction of the electrodes and branch into two or more directions. Here, the flow path refers to a void portion of the pattern formed in the insulating layer, which has higher liquid permeability than the insulating portion and serves as a path for the electrolyte. In one embodiment, the flow path portion may have an exposed surface of the electrode mixture layer, and in another embodiment, the flow path portion may have a second insulating portion provided on the electrode mixture layer in the flow path portion, and the thickness of the second insulating portion may be smaller than the thickness of the insulating portion. In other words, the flow path portion may be a void portion where no insulating portion is formed (a portion where the coating film of the insulating portion is not coated), or may be a recessed portion where the coating amount of the second insulating portion is small, i.e., a portion that is thinner in the thickness direction than the insulating portion. Furthermore, the material of the second insulating portion may be the same as or different from the material of the insulating portion.
[0043] As described above, the flow path section has flow paths that communicate in the planar direction of the electrodes and branch in two or more directions. The flow paths have branches (branched paths) that branch in two or more directions on their paths, and have a shape in which one or more combinations of branches in two or more directions are repeatedly arranged, for example, as shown in Figures 3A to 3C. By making the flow path portion substantially straight and / or substantially curved when viewed from the Z direction (thickness direction), it is possible to make the coverage rate by the insulating portion 90% or more, as described above.
[0044] "The flow path portion communicates in the planar direction of the electrodes" means that the void portion forming the flow path communicates from one side surface of the insulating layer at the electrode end to the other side surface of the insulating layer in the planar direction (electrode stacking direction). The "other side surface" may be an opposing side surface to the "one side surface," an adjacent side surface, or a plurality of opposing and adjacent side surfaces. Furthermore, for example, when the insulating layer is formed in a circular shape, this means that the void portion that forms a flow path in the planar direction (electrode stacking direction) is connected from a specific point on the circumference to a different point on the circumference that is different from the specific point.
[0045] Among these, the flow path portion preferably communicates from the side surface of the insulating layer where the electrolyte is injected to another side surface opposite the side surface during an electrolyte injection step performed when fabricating the electrode into an electrochemical element, i.e., communicates in the planar direction (electrode lamination direction) from the inlet side to the outlet side of the electrolyte at the electrode end. For example, in the case of a laminated electrochemical element in which rectangular electrodes are laminated, if a flow path portion communicates from the electrolyte injection side of the insulating layer at the electrode end to the other side opposite to said side, the electrolyte can easily spread inside the laminated electrodes, improving the permeability of the electrolyte. Also, in the case of a wound electrochemical element in which a strip-shaped electrode is wound, if the flow path portion communicates in a direction perpendicular to the winding, i.e., from the electrolyte injection side of the insulating layer to the other side opposite to said side, the permeability of the electrolyte can be improved as in the case of a laminated electrochemical element.
[0046] The shortest path of the flow path communicating with a pair of opposing side surfaces of the insulating layer is not particularly limited and may be appropriately selected depending on the purpose, but it is preferably short and more preferably straight. The length of the shortest path is preferably 2 times or less, more preferably 1.75 times or less, even more preferably 1.5 times or less, and particularly preferably 1.2 times or less, the distance between a pair of opposing side surfaces of the insulating layer, and it is most preferable that the length is the same as the distance, i.e., the flow path is a straight line that linearly connects the shortest distance between the pair of side surfaces.
[0047] The flow path section has at least one branch path in two or more directions in addition to one flow path (for example, in the inflow direction of the electrolyte) in a flow path that communicates in the planar direction of the electrodes. By having the flow path branch in two or more directions, even if the flow path is blocked, the electrolyte can bypass and penetrate. By forming a pattern of such flow paths branching in two or more directions in the insulating layer, the electrolyte is uniformly distributed between the electrode mixture layer and the insulating layer, and excellent electrolyte permeability in the electrode plane direction is exhibited. Therefore, even if the flow path is blocked due to the falling off of the active material or the falling off of the material constituting the insulating part, good liquid permeability can be exhibited.
[0048] The number of branches is 2 or more, and more preferably 3 or more. By having 3 or more branches, in addition to providing good liquid permeability as described above, for example, the force applied to the insulating part during a pressing step performed in forming an electrode or manufacturing an electrochemical element can be dispersed in multiple directions, resulting in an electrode with high strength. In addition, it is preferable that two or more branch paths branching from one flow path are formed so as to join again at a point other than the branch point. With such a configuration, even if the flow path is blocked, the electrolyte can be uniformly distributed over the entire electrode, and excellent electrolyte permeability in the electrode plane direction can be achieved.
[0049] The frequency of the flow path portions can be appropriately selected depending on the size of the electrode and the pattern shape, but it is preferable that one or more branch points appear per 10 mm of the shortest path in the direction of electrolyte flow (the direction connecting the electrolyte injection side and the electrolyte outflow side), more preferably two or more, and even more preferably three or more. If the coverage rate by the insulating portion is within a range of 90% or more, the electrolyte can be more easily distributed as the frequency of the flow path portions increases, thereby improving the liquid permeability.
[0050] The width of the flow path is preferably uniform, and is preferably 0.1 mm or more and 2.0 mm or less, more preferably 0.2 mm or more and 1.5 mm or less, and even more preferably 0.3 mm or more and 1.0 mm or less. When the width of the flow path is 0.1 mm or more, clogging of the flow path is unlikely to occur, improving the liquid permeability, and when it is 2.0 mm or less, exposure of the active material is reduced, improving the insulation properties. In addition, the width of the flow path is preferably 50% or less of the maximum length of the insulating part. If the width is greater than half of the maximum length of the insulating part, it becomes difficult to obtain a sufficient coverage rate of the electrode mixture layer on the insulating part. Here, the "maximum length of the insulating part" means the maximum length of the two-dimensional shape of one shape pattern of the insulating part surrounded by the flow path when viewed in a plan view.
[0051] In addition, the flow path portion may have a second insulating portion provided on the electrode mixture layer in the flow path portion, and the thickness of the second insulating portion may be smaller than the thickness of the insulating portion. When providing the flow path portion in the insulating layer, the pattern of the flow path portion may be formed in such a way that a difference in film thickness is created between the insulating portion and the flow path portion. The flow passage portion has a second insulating portion, which improves the float characteristic. The material of the second insulating portion may be the same as or different from the material of the insulating portion. The average thickness of the second insulating part is smaller than that of the insulating part, and is preferably smaller than the average thickness of the insulating part by 2 μm to 20 μm. If the difference in the average thickness of the second insulating part from the average thickness of the insulating part is 2 μm or more, a space is secured in the flow path part, improving the permeability of the electrolyte, and if it is 20 μm or less, the gap between the positive electrode and the negative electrode becomes small, ion migration becomes easy, and the battery characteristics are improved.
[0052] The cross-sectional shape of the flow path (void) in a cross section on a plane perpendicular to the longitudinal direction of the flow path is preferably a rectangle, an open-topped trapezoid, or an open-topped sector. In these shapes, the area of the insulating part in contact with the electrode mixture layer is large, and damage to the insulating part can be prevented during a pressing process performed in, for example, forming an electrode or manufacturing an electrochemical element, and therefore, the broken insulating part can be prevented from blocking the flow path.
[0053] When the flow path portion has a second insulating portion, the difference between the skeletal density of the porous structure of the second insulating portion in the flow path portion and the skeletal density of the porous structure of the insulating portion is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less. When the difference is 20% or less, the lithium ion permeability of the flow path portion is not impaired when the electrochemical element is formed, and the battery characteristics are improved. The skeletal density of the porous structure of the second insulating part and the insulating part can be determined by observing the cross section of the insulating layer and analyzing the image using a scanning electron microscope (Merlin, manufactured by Carl Zeiss Co., Ltd.) in particular. The cross section of the insulating layer is photographed in the same manner as for the average thickness of the insulating part, the photographed image is output as a TIFF image, and the proportion of the skeletal part of the insulating layer is calculated as the skeletal density from the brightness of the image of the resin skeletal part and the void part using image editing software GIMP 2.10.32 (GNU GPL). In addition, a range is selected on the GIMP operation screen so that the insulating layer is included in the thickness direction, and a histogram is created by brightness, and for example, the brightness in 256 gradations is set to 70 (threshold value), and the ratio of the number of pixels with brightness corresponding to the skeleton is calculated as a percentage. Similarly, the average value of the calculation results for five images with different viewing ranges is taken as the measured value of the skeleton density.
[0054] <Electrodes (first electrode, second electrode)> The electrode includes an electrode substrate, an electrode mixture layer, and an insulating layer. The negative electrode and positive electrode are collectively referred to as "electrodes", the negative electrode substrate (negative electrode substrate) and the positive electrode substrate (positive electrode substrate) are collectively referred to as the "electrode substrate", and the negative electrode mixture layer and positive electrode mixture layer are collectively referred to as the "electrode mixture layer". Moreover, when the first electrode is a negative electrode, the second electrode refers to a positive electrode, and when the first electrode is a positive electrode, the second electrode refers to a negative electrode.
[0055] <Electrode base> The electrode substrate is not particularly limited as long as it is a substrate having flatness and electrical conductivity, and can be appropriately selected depending on the purpose. The shape of the electrode substrate is not particularly limited and can be appropriately selected depending on the purpose. However, a plate or foil shape is preferable because it allows not only the electrode active material to be applied to both the front and back surfaces to form an electrode, but also the battery capacity to be increased by stacking multiple electrodes. From the viewpoint of electrical conductivity, the surface of the electrode substrate is preferably made of metals, such as nickel, aluminum, copper, titanium, etc., etched foils in which these metals are etched to form fine holes, perforated electrode substrates used in lithium ion capacitors, etc. In addition to the above, a conductive or semiconductor thin film formed on a flat substrate such as glass or plastic, or a thin conductive electrode film deposited by vapor deposition can be used.
[0056] <Electrode composite layer> The electrode mixture layer contains an active material, and may further contain other components, such as a binder, a conductive assistant, a dispersant, a dispersion medium, a non-aqueous electrolyte, a solid electrolyte, or a gel electrolyte, as necessary.
[0057] -Active material- As the active material, a positive electrode active material or a negative electrode active material can be used. The positive electrode active material or the negative electrode active material may be used alone or in combination of two or more kinds.
[0058] The positive electrode active material is not particularly limited as long as it is a material capable of reversibly absorbing and releasing alkali metal ions, and an alkali metal-containing transition metal compound can be used. Examples of the alkali metal-containing transition metal compound include lithium-containing transition metal compounds such as composite oxides containing lithium and one or more elements selected from the group consisting of cobalt, manganese, nickel, chromium, iron, and vanadium. Examples of the lithium-containing transition metal compound include lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide. As the alkali metal-containing transition metal compound, a polyanion-based compound having an XO4 tetrahedron (X=P, S, As, Mo, W, Si, etc.) in the crystal structure can also be used. Among these, lithium-containing transition metal phosphate compounds such as lithium iron phosphate and lithium vanadium phosphate are preferred in terms of cycle characteristics, and lithium vanadium phosphate is particularly preferred in terms of lithium diffusion coefficient and output characteristics. From the viewpoint of electronic conductivity, the polyanion-based compound is preferably composited by coating the surface with a conductive assistant such as a carbon material.
[0059] Examples of sodium-containing transition metal compounds include NaMO2-type oxides, sodium chromite (NaCrO2), sodium ferrate (NaFeO2), sodium nickelate (NaNiO2), sodium cobaltate (NaCoO2), sodium manganate (NaMnO2), and sodium vanadate (NaVO2). A part of M may be substituted with a metal element other than M and Na, for example, at least one selected from the group consisting of Cr, Ni, Fe, Co, Mn, V, Ti, and Al. In addition, as a sodium-containing metal oxide, NaF e PO4F, NaVPO4F, NaCoPO4, NaNiPO4, NaMnPO4, NaMn 1.5 Ni 0.5 O4, or Na2V2(PO4)3, etc. can also be used.
[0060] The negative electrode active material may be a material capable of absorbing and desorbing metals that form alloys with alkali metal ions such as Li ions or Na ions, etc. Examples of such materials include composite oxides of transition metals and Li, metal oxides, alloy materials, inorganic compounds such as transition metal sulfides, carbon materials, organic compounds, Li metal, and Na metal.
[0061] The composite oxides include LiMnO2, LiMn2O4, and lithium titanate (Li4Ti5O 12 , Li2Ti3O7), Lithium manganese titanate (LiMg 1 / 2 Ti3 / 2 O4), lithium cobalt titanate (LiCo 1 / 2 Ti 3 / 2 O4), Lithium Zinc Titanate (LiZn 1 / 2 Ti 3 / 2 O4), lithium iron titanate (LiFeTiO4), lithium chromium titanate (LiCrTiO4), lithium strontium titanate (Li2SrTi6O 14 ), or lithium barium titanate (Li2BaTi6O 14 ) etc.
[0062] The sodium composite oxide includes sodium titanate, for example, Na2Ti3O7 or Na4Ti5O 12 A part of Ti or Na in sodium titanate may be substituted with another element, for example, at least one selected from the group consisting of Ni, Co, Mn, Fe, Al, and Cr.
[0063] Examples of metal oxides include TiO2, Nb2TiO7, WO3, MoO2, MnO2, V2O5, SiO2, SiO, and SnO2.
[0064] Examples of alloy materials include Al, Si, Sn, Ge, Pb, As, and Sb. Examples of transition metal sulfides include FeS and TiS. Examples of carbon materials include graphite, non-graphitizable carbon, and easily graphitizable carbon. The inorganic compound may be a compound in which the transition metal of the above composite oxide is replaced with a different element.
[0065] -Binder- The binder can be added when the dispersant or electrolyte material is not sufficient to bond the positive electrode materials together or the negative electrode materials together, or to bond the positive electrode materials or the negative electrode materials to the electrically conductive layer, to ensure the binding force. There are no particular limitations on the binder as long as it can provide binding force, but from the viewpoint of inkjet ejection properties, a compound that does not increase viscosity is preferable. The binder can be a method of polymerizing a monomer compound after application, or a method of using polymer particles. In addition, a polymer compound that can be dispersed in a dispersion medium can be used as a material that does not increase the viscosity of the liquid composition. Furthermore, when a polymer compound that can be dissolved in a dispersion medium is used, the liquid composition in which the polymer compound is dissolved in the dispersion medium only needs to have a viscosity that allows it to be ejected from a liquid ejection head.
[0066] Examples of using a monomer compound include a method of applying a dispersion liquid containing a compound having a polymerizable moiety and a polymerization initiator or catalyst, in which the compound having a polymerizable moiety is dissolved, followed by heating; and a method of irradiating with non-ionizing radiation, ionizing radiation, or infrared radiation. In a compound having a polymerizable site, the polymerizable site may be one in the molecule, or may be polyfunctional. Note that a polyfunctional polymerizable compound means a compound having two or more polymerizable groups. There is no particular limitation on the polyfunctional polymerizable compound, so long as it can be polymerized by heating or irradiation with non-ionizing radiation, ionizing radiation, or infrared radiation. Examples of the polyfunctional polymerizable compound include acrylate resins, methacrylate resins, urethane acrylate resins, vinyl ester resins, unsaturated polyesters, epoxy resins, oxetane resins, vinyl ethers, and resins utilizing ene-thiol reactions, etc. Among these, from the viewpoint of productivity, acrylate resins, methacrylate resins, urethane acrylate resins, and vinyl ester resins are preferred.
[0067] Examples of materials that make up the polymer particles include polyvinylidene fluoride, acrylic resin, polyamide compounds, polyimide compounds, polyamideimide, ethylene-propylene-butadiene rubber (EPBR), styrene-butadiene copolymer, nitrile butadiene rubber (HNBR), isoprene rubber, polyisobutene, polyethylene glycol (PEO), polymethyl methacrylic acid (PMMA), polyethylene vinyl acetate (PEVA), polyethylene, polypropylene, polyurethane, nylon, polytetrafluoroethylene, polyphenylene sulfide, polyethylene terephthalate, and polybutylene terephthalate.
[0068] Examples of polymer compounds include polyamide compounds, polyimide compounds, polyamideimide, ethylene-propylene-butadiene rubber (EPBR), styrene-butadiene rubber (SBR), nitrile butadiene rubber (NBR), isoprene rubber, polyisobutene, polyethylene glycol (PEO), polymethyl methacrylic acid (PMMA), and polyethylene vinyl acetate (PEVA).
[0069] The mass ratio of the binder to the active material is preferably 10% or less, more preferably 5% or less. When the mass ratio of the binder to the active material is 10% or less, the binding strength during electrode formation is improved without impairing the ejection properties.
[0070] -Conductive additive- The conductive assistant may be previously compounded with the active material, or may be added when the dispersion liquid is prepared. As the conductive assistant, for example, conductive carbon black formed by a furnace method, an acetylene method, a gasification method, or the like, as well as carbon materials such as carbon nanofibers, carbon nanotubes, graphene, or graphite particles can be used. As the conductive assistant other than the carbon material, for example, metal particles such as aluminum or metal fibers can be used. The mass ratio of the conductive assistant to the active material is preferably 10% by mass or less, and more preferably 8% by mass or less. When the mass ratio of the conductive assistant to the active material is 10% by mass or less, the stability of the dispersion is improved.
[0071] -Dispersant- The dispersant is not particularly limited as long as it is capable of improving the dispersibility of the active material, polymer particles, or conductive assistant in the dispersion medium. Examples of the dispersant include polymer types such as polycarboxylic acid, naphthalenesulfonic acid-formalin condensation, polyethylene glycol, polycarboxylic acid partial alkyl ester, polyether, and polyalkylene polyamine; surfactant types such as alkylsulfonic acid, quaternary ammonium, higher alcohol alkylene oxide, polyhydric alcohol ester, and alkyl polyamine; and inorganic types such as polyphosphate.
[0072] (Electrode manufacturing method and electrode manufacturing device) The method for manufacturing an electrode of the present invention includes an insulating layer formation step of applying a liquid composition containing an insulating material onto an electrode mixture layer in a substrate having an electrode base and an electrode mixture layer provided on the electrode base, thereby forming an insulating layer having an insulating portion and a flow path portion. The insulating portion covers the electrode mixture layer, the coverage rate of the electrode mixture layer by the insulating portion is 90% or more, and the flow path portion has flow paths that are connected in the planar direction of the electrodes and branch into two or more directions. The electrode manufacturing apparatus of the present invention has a container that contains a liquid composition containing an insulating material, and an insulating layer forming means for applying a liquid composition containing an insulating material onto an electrode mixture layer in a substrate having an electrode base on which an electrode mixture layer is provided, thereby forming an insulating layer having an insulating portion and a flow path portion. The method for producing an electrode of the present invention includes an insulating layer forming step, preferably includes an electrode mixture layer forming step, and further includes other steps as necessary. The electrode manufacturing apparatus of the present invention has an insulating layer forming means, and preferably has an electrode mixture layer forming means, and further has other means as necessary.
[0073] <Containment Container> The storage vessel includes a liquid composition containing an insulating material and a container, and the liquid composition is stored in the container. Examples of containers include glass bottles, plastic containers, plastic bottles, stainless steel bottles, one-gallon cans, drums, and the like.
[0074] <Electrode mixture layer forming step and electrode mixture layer forming means> The electrode mixture layer forming step is a step of forming an electrode mixture layer on an electrode substrate, and can be suitably carried out by an electrode mixture layer forming means. The electrode mixture layer forming means is a means for forming an electrode mixture layer on an electrode substrate. The electrode mixture layer can be formed by applying a liquid composition for forming an electrode mixture layer onto an electrode substrate using the liquid composition for forming an electrode mixture layer.
[0075] -Liquid composition for forming electrode mixture layer- The liquid composition contains an active material and a dispersion medium, and further contains other components such as a conductive assistant and a dispersant, if necessary. These components can be appropriately selected from the items explained in the electrode mixture layer of the electrode of the present invention.
[0076] As a method for applying the liquid composition, for example, a comma coater method, a die coater method, a curtain coating method, a spray coating method, a liquid ejection method (inkjet method, IJ method), etc. can be used depending on the purpose.
[0077] After the liquid composition is applied, a heat treatment may be performed to dry the solvent. The heating method is not particularly limited, and examples thereof include a method of heating the coated surface with a resistance heater, an infrared heater, a fan heater, etc., and a method of drying from the back side of the coated surface with a hot plate, a drum heater, etc. From the viewpoint of uniformly heating and drying the coated surface, a resistance heater, an infrared heater, or a fan heater that can dry the coated surface without contacting it is preferred. These heating mechanisms may be used alone or in combination of two or more.
[0078] The heating temperature is not particularly limited, but is preferably 70° C. or higher and 150° C. or lower from the viewpoint of protecting the active material of the electrode substrate and the electrode mixture layer.
[0079] The average thickness of the negative electrode mixture layer is preferably 10 μm to 450 μm, and more preferably 20 μm to 100 μm. When the average thickness of the negative electrode mixture layer is 10 μm or more, the energy density of the electrochemical device is improved, and when it is 450 μm or less, the load characteristics of the electrochemical device are improved.
[0080] The average thickness of the positive electrode mixture layer is preferably 10 μm to 300 μm, and more preferably 40 μm to 150 μm. When the average thickness of the positive electrode mixture layer is 20 μm or more, the energy density of the electrochemical device is improved, and when it is 300 μm or less, the load characteristics of the electrochemical device are improved.
[0081] An electrode mixture layer and an insulating layer may be formed on both sides of the positive electrode substrate and / or the negative electrode substrate. In order to increase the charge / discharge capacity of the electrode element, the electrodes may be laminated in multiple layers or may be wound and stacked. There is no particular limit to the number of layers of positive electrodes or negative electrodes, and they may be increased as necessary.
[0082] <Insulating layer forming step and insulating layer forming means> The insulating layer forming step is a step of applying a liquid composition containing an insulating material onto an electrode mixture layer in a substrate having an electrode base on which an electrode mixture layer is provided, to form an insulating layer having an insulating portion and a flow path portion, and can be suitably performed by an insulating layer forming means. The insulating layer forming means is a means for applying a liquid composition containing an insulating material onto an electrode mixture layer in a substrate having an electrode base and an electrode mixture layer provided on the electrode base, thereby forming an insulating layer having an insulating portion and a flow path portion. The insulating portion covers the electrode mixture layer, the coverage rate of the electrode mixture layer by the insulating portion is 90% or more, and the flow path portion has flow paths that are connected in the planar direction of the electrodes and branch into two or more directions.
[0083] The liquid composition may be a composition containing insulating particles and a binder, as described in the insulating portion of the electrode, or a liquid composition containing a polymerizable compound and a liquid, and either of these can be suitably applied. Here, the insulating particles and the porous resin formed by polymerizing the polymerizable compound each function as an insulating material.
[0084] [First embodiment: liquid composition containing insulating particles and binder] When the liquid composition contains insulating particles and a binder, an example of a method for forming an insulating layer includes a method in which a composition containing insulating particles and a binder is applied onto an electrode mixture layer and then dried.
[0085] The method for applying the liquid composition is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include an inkjet method, a screen printing method, a gravure printing method, an offset printing method, etc. Among these, the inkjet method is preferred in that it is possible to form a high-density coating pattern on the electrode mixture layer in a non-contact and on-demand manner, and it is easy to adjust the film thickness by the coating amount.
[0086] After applying the liquid composition for the insulating layer, a heating treatment may be performed to dry the solvent. The heating method is not particularly limited, and may be appropriately selected from the same heating methods as those described in the electrode mixture layer forming step.
[0087] The heating temperature is not particularly limited, but is preferably 70° C. or higher and 150° C. or lower. A heating temperature of 70° C. or higher is preferable because the strength of the insulating layer increases by heating, and a heating temperature of 150° C. or lower is preferable because bubbles due to bumping on the surface of the insulating layer can be prevented.
[0088] [Second embodiment: liquid composition containing a polymerizable compound and a liquid] In the case where the liquid composition contains a polymerizable compound and a liquid, the insulating layer and the porous resin as the insulating portion can be formed by a porous resin manufacturing method including an application step and a polymerization step, as described below.
[0089] The method for producing a porous resin includes an application step of applying a liquid composition containing a polymerizable compound and a liquid, and a polymerization step of polymerizing the applied liquid composition layer to form a porous resin, and may further include other steps, such as a removal step of removing the liquid from the porous resin, after the polymerization step, as necessary.
[0090] - Application process - The application step is a step of applying a liquid composition onto the electrode mixture layer. The applied liquid composition preferably forms a liquid composition layer, which is a liquid film of the liquid composition, on the electrode mixture layer.
[0091] The application step is not particularly limited as long as it can apply the liquid composition, and can be appropriately selected according to the purpose. For example, any printing device can be used according to various printing methods such as spin coating, casting, microgravure coating, gravure coating, bar coating, roll coating, wire bar coating, dip coating, slit coating, capillary coating, spray coating, nozzle coating, gravure printing, screen printing, flexographic printing, offset printing, reverse printing, and inkjet printing. Among these, inkjet printing is preferred. This allows the resin layer to be formed accurately in the required area.
[0092] -Liquid composition- The liquid composition is a liquid composition for forming a porous resin, and contains a polymerizable compound and a liquid, and further contains other components such as a polymerization initiator, as necessary. It is preferable that the light transmittance at a wavelength of 550 nm measured while stirring the liquid composition is 30% or more, and the increase rate of the haze value in a haze measurement element prepared by polymerizing the liquid composition is 1.0% or more. The liquid composition forms a porous resin having a resin skeleton by polymerization. Here, "the liquid composition forms a porous resin" refers not only to the case where a porous resin is formed in the liquid composition, but also to the case where a precursor of the porous resin (e.g., the skeletal part of the porous resin) is formed in the liquid composition, and the porous resin is formed in a subsequent process (e.g., a heating process, etc.).
[0093] --Polymerizable compound-- The polymerizable compound forms a resin by polymerization, and forms a porous resin depending on the composition and characteristics of the liquid composition. The polymerizable compound is not particularly limited as long as it forms a polymer (resin) by polymerization, and any known polymerizable compound can be appropriately selected depending on the purpose, but it is preferable that the polymerizable compound has at least one radically polymerizable functional group.
[0094] Suitable examples of the polymerizable compound include radical polymerizable compounds such as monofunctional, bifunctional, trifunctional or higher functional radical polymerizable monomers and oligomers; functional monomers and oligomers having a functional group other than the polymerizable functional group. Among these, bifunctional or higher functional radical polymerizable compounds are preferred. The polymerizable group of the polymerizable compound is preferably at least one of a (meth)acryloyl group and a vinyl group, and more preferably a (meth)acryloyl group. The polymerizable compound is preferably polymerizable by energy irradiation, and more preferably polymerizable by heat or light.
[0095] The resin formed from the polymerizable compound is preferably a resin having a mesh-like structure formed by application of active energy rays (for example, by irradiation with light or heating), etc. Suitable examples thereof include acrylate resins, methacrylate resins, urethane acrylate resins, vinyl ester resins, unsaturated polyester resins, epoxy resins, oxetane resins, vinyl ether resins, and resins formed by ene-thiol reactions. Among these, acrylate resins, methacrylate resins, and urethane acrylate resins, which are resins formed from polymerizable compounds having a (meth)acryloyl group, are more preferred because they can be easily used to form a structure by utilizing highly reactive radical polymerization, and from the viewpoint of productivity, vinyl ester resins, which are resins formed from polymerizable compounds having a vinyl group, are more preferred. These may be used alone or in combination of two or more. When using two or more, the combination of polymerizable compounds is not particularly limited and can be appropriately selected according to the purpose, but for example, in order to impart flexibility, it is preferable to mix other resins with urethane acrylate resin as the main component. Note that a polymerizable compound having at least one of an acryloyl group and a methacryloyl group is referred to as a polymerizable compound having a (meth)acryloyl group.
[0096] The active energy ray is not particularly limited as long as it can provide the energy required for the polymerization reaction of the polymerizable compound in the liquid composition, and can be appropriately selected according to the purpose, and examples thereof include ultraviolet rays, electron beams, α rays, β rays, γ rays, and X-rays. Among these, ultraviolet rays are preferred. In particular, when a high-energy light source is used, the polymerization reaction can be promoted without using a polymerization initiator.
[0097] Examples of the monofunctional radical polymerizable compound include 2-(2-ethoxyethoxy)ethyl acrylate, methoxypolyethylene glycol monoacrylate, methoxypolyethylene glycol monomethacrylate, phenoxypolyethylene glycol acrylate, 2-acryloyloxyethyl succinate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, tetrahydrofurfuryl acrylate, 2-ethylhexyl carbitol acrylate, 3-methoxybutyl acrylate, benzyl acrylate, cyclohexyl acrylate, isoamyl acrylate, isobutyl acrylate, methoxytriethylene glycol acrylate, phenoxytetraethylene glycol acrylate, cetyl acrylate, isostearyl acrylate, stearyl acrylate, and styrene monomer. These may be used alone or in combination of two or more.
[0098] Examples of the bifunctional radical polymerizable compound include 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, neopentyl glycol diacrylate, EO-modified bisphenol A diacrylate, EO-modified bisphenol F diacrylate, neopentyl glycol diacrylate, tricyclodecane dimethanol diacrylate, etc. These may be used alone or in combination of two or more.
[0099] Examples of the trifunctional or higher radical polymerizable compound include trimethylolpropane triacrylate (TMPTA), trimethylolpropane trimethacrylate, EO-modified trimethylolpropane triacrylate, PO-modified trimethylolpropane triacrylate, caprolactone-modified trimethylolpropane triacrylate, HPA-modified trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate (PETTA), glycerol triacrylate, ECH-modified glycerol triacrylate, EO-modified glycerol triacrylate, PO-modified glycerol triacrylate, and trimethylolpropane triacrylate. Examples of the acrylates include thi(acryloxyethyl)isocyanurate, dipentaerythritol hexaacrylate (DPHA), caprolactone-modified dipentaerythritol hexaacrylate, dipentaerythritol hydroxypentaacrylate, alkyl-modified dipentaerythritol pentaacrylate, alkyl-modified dipentaerythritol tetraacrylate, alkyl-modified dipentaerythritol triacrylate, dimethylolpropane tetraacrylate (DTMPTA), pentaerythritol ethoxy tetraacrylate, EO-modified phosphoric acid triacrylate, and 2,2,5,5-tetrahydroxymethylcyclopentanone tetraacrylate. These may be used alone or in combination of two or more.
[0100] The content of the polymerizable compound is preferably from 5.0% by mass to 70.0% by mass, more preferably from 10.0% by mass to 50.0% by mass, and even more preferably from 20.0% by mass to 40.0% by mass, based on the total amount of the liquid composition. When the content is 70.0% by mass or less, the size of the pores in the resulting porous body is not too small, such as a few nm or less, and the porous body has an appropriate porosity, which is preferable because it can suppress the tendency for liquids and gases to become less likely to penetrate. Also, when the content is 5.0% by mass or more, the three-dimensional network structure of the resin is sufficiently formed, a sufficient porous structure is obtained, and the strength of the resulting porous structure also tends to be improved, which is preferable.
[0101] --liquid-- The liquid contains a porogen and, if necessary, further contains other liquids other than the porogen. The porogen is a liquid that is compatible with the polymerizable compound and becomes incompatible with the polymer (resin) (causes phase separation) during the polymerization of the polymerizable compound in the liquid composition. By including a porogen in the liquid composition, a porous resin is formed when the polymerizable compound is polymerized. In addition, it is preferable that the porogen can dissolve a compound (a polymerization initiator described later) that generates a radical or an acid by light or heat. The liquid or porogen may be used alone or in combination of two or more kinds. In this embodiment, the liquid is not polymerizable.
[0102] The boiling point of one type of porogen alone or two or more types of porogen in combination is preferably 50°C to 250°C, more preferably 70°C to 200°C, and even more preferably 120°C to 190°C at normal pressure. By having a boiling point of 50°C or more, vaporization of the porogen at around room temperature is suppressed, making the liquid composition easy to handle and making it easy to control the content of the porogen in the liquid composition. In addition, by having a boiling point of 250°C or less, the time required for the process of removing the porogen after polymerization is shortened, improving the productivity of the porous resin. In addition, since the amount of porogen remaining inside the porous resin can be suppressed, the quality is improved when the porous resin is used as a functional layer such as a material separation layer that separates substances or a reaction layer as a reaction field.
[0103] Examples of the porogen include ethylene glycols such as diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisopropyl ether, and dipropylene glycol monomethyl ether; esters such as γ-butyrolactone and propylene carbonate; and amides such as N,N-dimethylacetamide. In addition, liquids with relatively large molecular weights such as methyl tetradecanoate, methyl decanoate, methyl myristate, and tetradecane can also be used. In addition, liquids such as acetone, 2-ethylhexanol, and 1-bromonaphthalene can also be used.
[0104] It should be noted that not all of the above-listed liquids are porogens. As described above, a porogen is a liquid that is compatible with a polymerizable compound and is incompatible with (subjects to phase separation from) a polymerized product (resin) produced in the course of polymerization of the polymerizable compound in a liquid composition. In other words, whether or not a liquid corresponds to a porogen is determined by its relationship with the polymerizable compound and the polymerized product (resin formed by polymerization of the polymerizable compound). In addition, since the liquid composition only needs to contain at least one type of porogen having the above-mentioned specific relationship with the polymerizable compound, the range of material selection when preparing the liquid composition is broadened, and the liquid composition can be easily designed. By broadening the range of material selection when preparing the liquid composition, the range of response is broadened when there are characteristics required for the liquid composition from a viewpoint other than the formation of a porous structure. For example, when the liquid composition is discharged by the inkjet method, the liquid composition is required to have discharge stability and the like from a viewpoint other than the formation of a porous structure, and the wide range of material selection makes it easy to design the liquid composition.
[0105] The content of the liquid or porogen is preferably from 30.0% by mass to 95.0% by mass, more preferably from 50.0% by mass to 90.0% by mass, and even more preferably from 60.0% by mass to 80.0% by mass, based on the total amount of the liquid composition. When the content of the liquid or porogen is 30.0% by mass or more, the size of the pores in the resulting porous body is not too small, such as several nm or less, and the porous body has an appropriate porosity, which is preferable because it is possible to suppress the tendency for liquid or gas to penetrate less easily. Also, when the content of the liquid or porogen is 95.0% by mass or less, the three-dimensional network structure of the resin is sufficiently formed, a porous structure is sufficiently obtained, and the strength of the resulting porous structure also tends to be improved, which is preferable.
[0106] The mass ratio of the polymerizable compound content to the porogen content in the liquid composition (polymerizable compound:porogen) is preferably from 1.0:0.4 to 1.0:19.0, more preferably from 1.0:1.0 to 1.0:9.0, and even more preferably from 1.0:1.5 to 1.0:4.0.
[0107] --Other ingredients-- ---Polymerization initiator--- The liquid composition may contain other components, such as a polymerization initiator. The polymerization initiator is a material capable of generating active species such as radicals and cations by energy such as light and heat, and initiating polymerization of a polymerizable compound. Examples of the polymerization initiator include known radical polymerization initiators, cationic polymerization initiators, and base generators. These may be used alone or in combination of two or more. Among these, photoradical polymerization initiators are preferred.
[0108] The photoradical polymerization initiator is not particularly limited, and a known photoradical generator can be appropriately selected depending on the purpose. Examples of the photoradical polymerization initiator include Michler's ketone and benzophenone, known under the trade names Irgacure and Darocur, and acetophenone derivatives. Specific examples of the compounds include α-hydroxy-acetophenone, α-aminoacetophenone, 4-aroyl-1,3-dioxolane, benzil ketal, 2,2-diethoxyacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, benzophenone, 2-chlorobenzophenone, pp'-dichlorobenzophenone, pp'-bisdiethylaminobenzophenone, Michler's ketone, benzil, benzoin, benzil dimethyl ketal, tetramethylthiuram monosulfide, thioxanthone, and 2-chlorothioxanthone. benzoin peroxide, di-tert-butyl peroxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, methyl benzoyl formate, benzoin isopropyl ether, benzoin methyl ether, benzoin ethyl ether, benzoin ether, benzoin isobutyl ether, benzoin n-butyl ether, benzoin Zoin n-propyl, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 1-hydroxy-cyclohexyl-phenyl-ketone, 2,2-dimethoxy-1,2-diphenylethan-1-one, bis(η5-2,4-cyclopentadiene-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-methyl-1[4-(methylthio) )phenyl]-2-morpholinopropan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Darocur 1173), bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one monoacylphosphine oxide, bisacylphosphine oxide; titanocene, fluorescene, anthraquinone, thioxanthone; xanthone, lophine dimer, trihalomethyl compounds;Examples include dihalomethyl compounds, active ester compounds, and organic boron compounds.
[0109] Furthermore, a photocrosslinking radical generator such as a bisazide compound may be simultaneously contained. When polymerization is performed by heat alone, a thermal polymerization initiator such as azobisisobutyronitrile (AIBN), which is a typical radical generator, can be used.
[0110] The content of the polymerization initiator is preferably from 0.05% by mass to 10.0% by mass, and more preferably from 0.5% by mass to 5.0% by mass, based on the total mass of the polymerizable compounds being 100.0% by mass, in terms of obtaining a sufficient curing rate.
[0111] The liquid composition may be a non-dispersed composition that does not contain a dispersion in the liquid composition, or a dispersed composition that contains a dispersion in the liquid composition, but is preferably a non-dispersed composition.
[0112] [Polymerization-induced phase separation] Porous resins are formed by polymerization-induced phase separation. Polymerization-induced phase separation refers to a state in which the polymerizable compound and porogen are compatible, but the polymer (resin) that is generated during the polymerization process of the polymerizable compound and the porogen are not compatible (phase separation occurs). Although there are other methods for obtaining porous bodies by phase separation, the polymerization-induced phase separation method can form a porous body with a network structure, which is expected to be highly resistant to chemicals and heat. In addition, compared to other methods, it has the advantage of a shorter process time and easier surface modification.
[0113] Next, a process for forming a porous resin using polymerization-induced phase separation by a liquid composition containing a polymerizable compound will be described. The polymerizable compound undergoes a polymerization reaction by light irradiation or the like to form a resin. During this process, the solubility of the porogen in the growing resin decreases, and phase separation occurs between the resin and the porogen. Finally, the resin forms a porous structure having a co-continuous structure due to the resin skeleton, with the porogen filling the pores. When this is dried, the porogen is removed, and a porous resin having a co-continuous structure of a three-dimensional network structure remains. Therefore, in order to form a porous resin with an appropriate porosity, the compatibility of the porogen with the polymerizable compound and the compatibility of the porogen with the resin formed by polymerization of the polymerizable compound are examined.
[0114] [Light transmittance] The liquid composition has a light transmittance of 30% or more at a wavelength of 550 nm, measured while being stirred. The compatibility between the porogen and the polymerizable compound can be judged by the light transmittance. When the light transmittance is 30% or more, it is determined that the liquid contains porogen and that the polymerizable compound and the porogen are in a compatible state, and when the light transmittance is less than 30%, it is determined that the polymerizable compound and the liquid are in an incompatible state.
[0115] Specifically, the light transmittance can be measured by the following method. First, the liquid composition is poured into a quartz cell, and while stirring with a stirrer at 300 rpm, the transmittance of the liquid composition to light (visible light) at a wavelength of 550 nm is measured under the following conditions. Quartz cell: Special microcell with screw cap (product number: 42016, manufactured by Mitrica Co., Ltd.) ·Transmittance measurement device: Ocean Optics USB4000 ·Stirring speed: 300rpm ·Measurement wavelength: 550nm Reference: Obtained by measuring the light transmittance at a wavelength of 550 nm when the quartz cell is filled with air (transmittance: 100%)
[0116] [Haze value increase rate] The increase rate of the haze value in a haze measuring element prepared by polymerizing the liquid composition is 1.0% or more. The compatibility between the porogen and the resin formed by polymerization of the polymerizable compound can be judged by the rate of increase in the haze value. When the increase in the haze value is 1.0% or more, it is determined that the liquid contains porogen and the resin and the porogen are incompatible with each other, and when the increase in the haze value is less than 1.0%, it is determined that the resin and the liquid are compatible with each other. The haze value in the haze measuring element increases as the compatibility between the porogen and the resin formed by polymerization of the polymerizable compound decreases, and decreases as the compatibility increases. Also, the higher the haze value, the easier it is for the resin formed by polymerization of the polymerizable compound to form a porous structure.
[0117] Specifically, the rate of increase in haze value is the rate of increase in haze value before and after polymerization of a haze measurement element having an average thickness of 100 μm prepared by polymerizing the liquid composition, and can be measured by the following method. - Fabrication of haze measurement element - First, resin particles as a gap agent are uniformly dispersed on a non-alkali glass substrate by spin coating. Then, the substrate coated with the gap agent is bonded to a non-alkali glass substrate not coated with the gap agent, with the surfaces coated with the gap agent sandwiched between them. Next, a liquid composition is filled between the bonded substrates by utilizing capillary action to prepare a "pre-UV haze measurement element". Next, the pre-UV haze measurement element is irradiated with UV light to harden the liquid composition. Finally, the periphery of the substrate is sealed with a sealant to prepare a "haze measurement element". The size of the gap agent (average particle diameter 100 μm) corresponds to the average thickness of the haze measurement element. The various conditions during preparation are shown below. Non-alkali glass substrate: Nippon Electric Glass Co., Ltd., 40 mm, t=0.7 mm, OA-10G Gap agent: Sekisui Chemical Co., Ltd., resin microparticle Micropearl GS-L100, average particle size 100 μm Spin coating conditions: Dispersion drop amount 150 μL, rotation speed 1000 rpm, rotation time 30 s Filled liquid composition volume: 160μL UV irradiation conditions: UV-LED is used as the light source, light source wavelength is 365 nm, irradiation intensity is 30 mW / cm 2 , irradiation time 20s Sealant: TB3035B (Three Bond)
[0118] - Haze value (cloudiness) measurement - Next, the haze value (cloudiness) is measured using the prepared haze measurement element before UV irradiation and the haze measurement element. The measured value in the haze measurement element before UV irradiation is set as a reference (haze value 0), and the increase rate of the measured value (haze value) in the haze measurement element relative to the measured value in the haze measurement element before UV irradiation is calculated. The equipment used for the measurements is shown below. Haze measuring device: Haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0119] [Method of producing liquid composition] The method for producing the liquid composition is not particularly limited and can be appropriately selected depending on the purpose. However, it is preferable to produce the liquid composition through a step of dissolving a polymerization initiator in a polymerizable compound, a step of further dissolving a porogen and other components, and a step of stirring to obtain a homogeneous solution.
[0120] [Viscosity of liquid composition] From the viewpoint of workability when applying the liquid composition, the viscosity of the liquid composition is preferably from 1.0 mPa·s to 150.0 mPa·s, more preferably from 1.0 mPa·s to 30.0 mPa·s, and particularly preferably from 1.0 mPa·s to 25.0 mPa·s at 25° C. By having a viscosity of from 1.0 mPa·s to 30.0 mPa·s, good ejection properties can be obtained even when the liquid composition is applied to an inkjet method. Here, the viscosity can be measured, for example, using a viscometer (device name: RE-550L, manufactured by Toki Sangyo Co., Ltd.).
[0121] -Polymerization process- The polymerization step is a step of polymerizing the liquid composition layer to form a porous resin. The polymerization method is not particularly limited and can be appropriately selected depending on the purpose as long as it can impart energy necessary to proceed with the polymerization reaction of the polymerizable compound. Examples of the polymerization method include irradiation with light such as ultraviolet rays, electron beams, α rays, β rays, γ rays, X-rays, and infrared rays; and heating.
[0122] -Removal process- The removing step is a step of removing the liquid from the porous resin after the polymerization step. The method for removing the liquid is not particularly limited, and examples thereof include a method for removing the liquid from the porous resin by heating. In this case, heating under reduced pressure is preferable because it can further promote the removal of the liquid and suppress the liquid from remaining in the porous resin.
[0123] <Other processes> Other steps in the manufacturing method of the electrode are not particularly limited as long as they do not impair the effects of the present invention and can be appropriately selected depending on the purpose. For example, there can be mentioned a cutting step of cutting the electrode to a desired size by punching or the like.
[0124] [Embodiment in which an insulating layer is formed by directly applying a liquid composition to a substrate] FIG. 7 is a schematic diagram showing an example of an electrode manufacturing apparatus for implementing the electrode manufacturing method of this embodiment. The electrode manufacturing apparatus 500 in Fig. 7 is an apparatus for manufacturing an insulating layer using the liquid composition described above. The electrode manufacturing apparatus 500 includes a printing section 100 that performs an application process for applying the liquid composition onto a printing substrate 34 to form a liquid composition layer, and a heating section 200 as necessary. The electrode manufacturing apparatus 500 includes a transport section 35 that transports the printing substrate 34, and the transport section 35 transports the printing substrate 34 at a preset speed in the order of the printing section 100 and, as necessary, the heating section 200. The printing substrate 4 is an electrode mixture layer provided on an electrode substrate.
[0125] -Printing Department 100- The printing unit 10 includes an optional printing device 31a corresponding to an inkjet printing method, which is an application means for realizing an application step of applying a liquid composition for forming an insulating layer on a printing substrate 34, a storage container 31b for storing the liquid composition, and a supply tube 31c for supplying the liquid composition stored in the storage container 31b to the printing device 31a. The storage container 31b stores the liquid composition 37, and the printing unit 100 ejects the liquid composition 37 from the printing device 31a and applies the liquid composition 37 onto the printing substrate 34 to form a thin film of the liquid composition layer. The storage container 31b may be integrated with the electrode manufacturing device, or may be removable from the electrode manufacturing device. Alternatively, the storage container 31b may be a container used for adding to a storage container integrated with the electrode manufacturing device or a storage container removable from the electrode manufacturing device. The storage container 31b and the supply tube 31c can be arbitrarily selected as long as they can stably store and supply the liquid composition 7.
[0126] -Heating section 200- As shown in Fig. 7, the heating section 200 has a heating device 33a, and performs a liquid removal step in which the liquid composition layer formed by the printing section 100 is heated by the heating device 33a to dry and remove the remaining liquid. This allows the formation of an insulating layer. The heating section 200 may perform liquid removal under reduced pressure. The heating device 33a is not particularly limited and can be appropriately selected depending on the purpose. For example, a substrate heater, an IR heater, a hot air heater, or a combination of these can be used. The heating temperature and time can be appropriately selected depending on the boiling point of the liquid contained in the liquid composition layer and the thickness of the formed film.
[0127] FIG. 8 is a schematic diagram showing another example of an electrode manufacturing apparatus (liquid ejection apparatus) for implementing the electrode manufacturing method of the present embodiment. The liquid ejection device 300 ′ is capable of circulating the liquid composition through the liquid ejection head 306 , the tank 307 , and the tube 308 by controlling the pump 3101 and the valves 311 and 312 . In addition, the liquid ejection device 300' is provided with an external tank 313, and when the liquid composition in the tank 307 decreases, it is possible to supply the liquid composition from the external tank 313 to the tank 307 by controlling the pump 3101 and the valves 311, 312, and 314. By using the electrode manufacturing device, it is possible to eject a liquid composition onto a target object.
[0128] FIG. 9 shows an example of a method for manufacturing the electrode of this embodiment. The method for producing an electrode 210 having a porous resin provided on a substrate includes a step of sequentially discharging the liquid composition 12A onto a substrate 211 using a liquid discharger 300'. First, an elongated substrate 211 is prepared. Then, the substrate 211 is wound around a cylindrical core, and set on a feed roller 304 and a take-up roller 305 so that the side on which the porous resin 212 is formed faces upward in FIG. 9. Here, the feed roller 304 and the take-up roller 305 rotate counterclockwise, and the substrate 211 is transported from right to left in FIG. 9. Then, droplets of the liquid composition 12A are ejected from a liquid ejection head 306 installed above the substrate 211 between the feed roller 304 and the take-up roller 305, in the same manner as in FIG. 8, onto the substrate 211 that is being transported sequentially.
[0129] A plurality of liquid ejection heads 306 may be installed in a direction substantially parallel to or substantially perpendicular to the transport direction of the substrate 211. Next, the substrate 211 onto which the droplets of the liquid composition 12A have been ejected is transported to a heating mechanism 309 by a delivery roller 304 and a take-up roller 305. As a result, a porous resin 212 is formed, and an electrode 210 having a porous resin provided on the substrate is obtained. Thereafter, the electrode 210 having the polymer electrolyte provided thereon is cut to a desired size by punching or the like.
[0130] The heating mechanism 309 may be installed either above or below the base material 211, or a plurality of heating mechanisms may be installed. The heating mechanism 309 is not particularly limited as long as it does not directly contact the liquid composition 12A, and examples thereof include a resistance heater, an infrared heater, a fan heater, etc. A plurality of heating mechanisms 309 may be installed. Also, a UV curing device for polymerization may be installed.
[0131] In addition, the liquid composition 12A discharged onto the substrate 211 is preferably heated, and may be heated by a stage or by a heating mechanism other than the stage. The heating mechanism may be installed either above or below the electrode substrate 11, or multiple heating mechanisms may be installed. The heating temperature is not particularly limited. The liquid composition 12A is dried by heating to form an insulating layer.
[0132] As shown in FIG. 10, the tank 307 may be supplied with ink from tanks 313A and 313B connected to the tanks 307A and 307B, and the liquid ejection head 306 may have a plurality of heads 306A and 306B.
[0133] [Embodiment in which an electrode is formed by indirectly applying a liquid composition to a substrate] Figures 11 and 12 are configuration diagrams showing an example of a printing unit that employs an inkjet method and a transfer method as an application means in an electrode manufacturing apparatus of this embodiment, and Figure 6 is a configuration diagram showing a printing unit that uses a drum-shaped intermediate transfer body, and Figure 7 is a configuration diagram showing a printing unit that uses an endless belt-shaped intermediate transfer body. The printing unit 400' shown in FIG. 11 is an inkjet printer that transfers a liquid composition layer or an insulating layer onto a substrate via an intermediate transfer body 4001, thereby forming an insulating layer on the substrate.
[0134] The printing section 400 ′ includes an inkjet section 420 , a transfer drum 4000 , a pretreatment unit 4002 , an absorption unit 4003 , a heating unit 4004 and a cleaning unit 4005 . The inkjet unit 420 includes a head module 422 that holds a plurality of heads 401. The heads 401 eject a liquid composition onto an intermediate transfer body 4001 supported by a transfer drum 4000, and form a liquid composition layer on the intermediate transfer body 4001. Each head 401 is a line head, and nozzles are arranged in a range that covers the width of a recording area of a substrate of the maximum size that can be used. The head 401 has a nozzle surface on its lower surface on which nozzles are formed, and the nozzle surface faces the surface of the intermediate transfer body 4001 via a minute gap. In the case of this embodiment, the intermediate transfer body 4001 is configured to circulate on a circular orbit, so the plurality of heads 401 are arranged radially.
[0135] The transfer drum 4000 faces the impression cylinder 621 and forms a transfer nip. The pretreatment unit 4002 applies, for example, a reaction liquid for increasing the viscosity of the liquid composition onto the intermediate transfer body 4001 before the liquid composition is discharged by the head 401. The absorption unit 4003 absorbs liquid components from the liquid composition layer on the intermediate transfer body 4001 before transfer. The heating unit 4004 heats the ink layer on the intermediate transfer body 4001 before transfer. By heating the liquid composition layer, it is dried to form an insulating layer. In addition, the organic solvent is removed, improving the transferability to the substrate. The cleaning unit 4005 cleans the intermediate transfer body 4001 after transfer and removes foreign matter such as ink and dust remaining on the intermediate transfer body 4001. The outer peripheral surface of the impression cylinder 621 is in pressure contact with the intermediate transfer body 4001, and the liquid composition layer and the insulating layer on the intermediate transfer body 4001 are transferred to the substrate when the substrate passes through the transfer nip between the impression cylinder 621 and the intermediate transfer body 4001. The impression cylinder 621 may be configured to have at least one gripping mechanism for holding the leading end of the substrate on its outer peripheral surface.
[0136] The printing unit 400 ″ shown in FIG. 12 is an inkjet printer that transfers a liquid composition layer or an insulating layer onto a substrate via an intermediate transfer belt 4006 to form an insulating layer on the substrate. The printing unit 400'' ejects droplets of the liquid composition from a plurality of heads 401 provided in the inkjet unit 420 to form a liquid composition layer on the outer circumferential surface of the intermediate transfer belt 4006. The liquid composition layer formed on the intermediate transfer belt 4006 is heated by a heating unit 4007 and dried to form an insulating layer, which becomes a film on the intermediate transfer belt 4006.
[0137] The insulating layer formed as a film on the intermediate transfer belt 4006 is transferred to the substrate in the transfer nip portion where the intermediate transfer belt 4006 faces the transfer roller 622. The surface of the intermediate transfer belt 4006 after transfer is cleaned by the cleaning roller 4008. The intermediate transfer belt 4006 is stretched over a drive roller 4009a, an opposing roller 4009b, multiple (four in this example) shape maintaining rollers 4009c, 4009d, 4009e, and 4009f, and multiple (four in this example) support rollers 4009g, and moves in the direction of the arrow in the figure. The support roller 4009g, which is provided opposite the head 401, maintains the tension state of the intermediate transfer belt 4006 when ink droplets are ejected from the head 401.
[0138] (Electrochemical element) The electrochemical device of the present invention has the above-mentioned electrode of the present invention, and preferably also has an electrolyte (also referred to as an "electrolytic solution"), a separator, and an exterior. The electrochemical element may include a positive electrode, a negative electrode, an electrolyte, a separator, and an exterior. The electrochemical element uses the electrode of the present invention as at least one of the positive electrode and the negative electrode.
[0139] <Electrolyte> As the electrolyte, an aqueous electrolyte solution or a non-aqueous electrolyte can be used.
[0140] -Aqueous electrolyte solution- The electrolyte aqueous solution is an aqueous solution in which an electrolyte salt is dissolved in water. Examples of the electrolyte salt that can be used include sodium hydroxide, potassium hydroxide, sodium chloride, potassium chloride, ammonium chloride, zinc chloride, zinc acetate, zinc bromide, zinc iodide, zinc tartrate, and zinc perchlorate.
[0141] -Non-aqueous electrolyte- As the non-aqueous electrolyte, a non-aqueous electrolytic solution can be used.
[0142] --Nonaqueous electrolyte-- The non-aqueous electrolyte is an electrolyte in which an electrolyte salt is dissolved in a non-aqueous solvent.
[0143] --Non-aqueous solvent-- The non-aqueous solvent is not particularly limited, and for example, an aprotic organic solvent is preferably used. As the aprotic organic solvent, a carbonate-based organic solvent such as a chain carbonate or a cyclic carbonate can be used. Among these, a chain carbonate is preferred because it has a high dissolving power for electrolyte salts. In addition, the aprotic organic solvent preferably has a low viscosity.
[0144] Examples of the chain carbonate include dimethyl carbonate (DMC), diethyl carbonate (DEC), and methyl ethyl carbonate (EMC).
[0145] The content of the chain carbonate in the non-aqueous solvent is preferably 50% by mass or more. When the content of the chain carbonate in the non-aqueous solvent is 50% by mass or more, the content of the cyclic substance is small even if the cyclic substance (e.g., cyclic carbonate, cyclic ester) has a high relative dielectric constant in the non-aqueous solvent other than the chain carbonate. Therefore, even if a non-aqueous electrolyte solution with a high concentration of 2M or more is prepared, the viscosity of the non-aqueous electrolyte solution is low, and the non-aqueous electrolyte solution is absorbed into the electrode and ions are diffused well.
[0146] Examples of cyclic carbonates include propylene carbonate (PC), ethylene carbonate (EC), butylene carbonate (BC), and vinylene carbonate (VC).
[0147] As non-aqueous solvents other than carbonate-based organic solvents, for example, ester-based organic solvents such as cyclic esters and chain esters, and ether-based organic solvents such as cyclic ethers and chain ethers can be used.
[0148] Examples of cyclic esters include γ-butyrolactone (γBL), 2-methyl-γ-butyrolactone, acetyl-γ-butyrolactone, γ-valerolactone, etc. Examples of chain esters include alkyl propionate esters, dialkyl malonate esters, alkyl acetate esters (e.g., methyl acetate (MA), ethyl acetate), alkyl formate esters (e.g., methyl formate (MF), ethyl formate), etc.
[0149] Examples of cyclic ethers include tetrahydrofuran, alkyltetrahydrofuran, alkoxytetrahydrofuran, dialkoxytetrahydrofuran, 1,3-dioxolane, alkyl-1,3-dioxolane, and 1,4-dioxolane.
[0150] Examples of the chain ether include 1,2-dimethoxyethane (DME), diethyl ether, ethylene glycol dialkyl ether, diethylene glycol dialkyl ether, triethylene glycol dialkyl ether, and tetraethylene glycol dialkyl ether.
[0151] -Electrolyte salt- There are no particular limitations on the electrolyte salt, so long as it has high ion conductivity and is soluble in a non-aqueous solvent.
[0152] The electrolyte salt preferably contains a halogen atom. Examples of the cation constituting the electrolyte salt include lithium ions. Examples of the anion constituting the electrolyte salt include BF4 - , PF6 - , AsF6 - , CF3SO3 - , (CF3SO2)2N - , (C2F5SO2)2N - etc.
[0153] The lithium salt is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include lithium hexafluorophosphate (LiPF6), lithium borofluoride (LiBF4), lithium arsenic hexafluoride (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethylsulfonyl)imide (LiN(CF3SO2)2), lithium bis(pentafluoroethylsulfonyl)imide (LiN(C2F5SO2)2), etc. Among these, LiPF6 is preferred from the viewpoint of ion conductivity, and LiBF4 is preferred from the viewpoint of stability.
[0154] The electrolyte salts may be used alone or in combination of two or more.
[0155] The concentration of the electrolyte salt in the nonaqueous electrolytic solution can be appropriately selected depending on the purpose, but when the nonaqueous electrochemical device is of a swing type, the concentration is preferably 1 mol / L to 2 mol / L, and when the nonaqueous electrochemical device is of a reserve type, the concentration is preferably 2 mol / L to 4 mol / L.
[0156] <separator> The separator is provided between the electrodes to prevent a short circuit between the positive and negative electrodes.
[0157] The separator is not particularly limited and can be appropriately selected from sheets or films having ion permeable voids according to the purpose, and examples thereof include paper such as kraft paper, vinylon-mixed paper, and synthetic pulp-mixed paper; polyolefin nonwoven fabrics such as cellophane, polyethylene graft membrane, and polypropylene melt-blown nonwoven fabric; polyamide nonwoven fabrics, glass fiber nonwoven fabrics, and micropore membranes. These may be used alone or in combination of two or more. The separator may have a single layer structure or a composite structure.
[0158] The size of the separator is not limited as long as it prevents a short circuit between the positive and negative electrodes and can be used in an electrochemical element, and the separator may cover the periphery of the electrodes as well as between the electrodes, if necessary.
[0159] <Exterior> The exterior packaging is not particularly limited as long as it can seal the electrodes, the electrolyte, and the separator or the solid electrolyte or the gel electrolyte, and any known exterior packaging can be appropriately selected depending on the purpose.
[0160] The electrochemical element can be produced, for example, by stacking a positive electrode and a negative electrode with a separator between them, rolling or folding the stack as necessary according to the shape of the battery, placing the stack in a battery container, injecting an electrolyte into the battery container, and sealing the container.
[0161] The shape of the electrochemical element is not particularly limited, and examples thereof include a laminate type, a cylinder type in which a sheet electrode and a separator are spirally wound, a cylinder type having an inside-out structure in which a pellet electrode and a separator are combined, and a coin type in which a pellet electrode and a separator are laminated.
[0162] FIG. 13 shows an example of an electrochemical device according to this embodiment. The electrochemical element 60 is a liquid-based electrochemical element in which an electrolyte layer 51 is formed by injecting an electrolyte aqueous solution or a non-aqueous electrolyte into the electrode element 40, and the electrode element 40 is sealed with an exterior 52. In the electrochemical element 60, the lead wires 41 and 42 are led out to the outside of the exterior 52.
[0163] In the electrode element 40, a negative electrode 15 and a positive electrode 25 are laminated with a separator 30 interposed therebetween. Here, the positive electrode 25 is laminated on both sides of the negative electrode 15. In addition, a lead wire 41 is connected to the negative electrode substrate 11, and a lead wire 42 is connected to the positive electrode substrate 21. In the case of a solid electrochemical element, the separator 30 may be replaced with a solid electrolyte or a gel electrolyte.
[0164] In negative electrode 15, negative electrode mixture layers 12 are formed on both sides of negative electrode substrate 11, and insulating layers 13 are formed on each of negative electrode mixture layers 12. The positive electrode 25 has a positive electrode substrate 21 and a positive electrode mixture layer 22 formed on both sides of the substrate 21 . Although not shown, an insulating layer may be formed on positive electrode mixture layer 22 . There is no particular limit to the number of stacked negative electrodes 15 and positive electrodes 25 of the electrode element 40. Furthermore, the number of negative electrodes 15 and the number of positive electrodes 25 of the electrode element 40 may be the same or different.
[0165] (device) The device of the present invention comprises the above-mentioned electrode of the present invention, and further comprises other members as necessary. The device is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include mobile objects such as vehicles, smartphones, notebook computers, pen-input personal computers, mobile personal computers, electronic book players, mobile phones, mobile fax machines, mobile copiers, mobile printers, headphone stereos, video movie machines, liquid crystal televisions, handy cleaners, portable CDs, mini discs, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power sources, motors, lighting equipment, toys, game machines, clocks, strobes, cameras, and other electric equipment. Among these, vehicles and electric equipment are particularly preferred. Examples of the mobile body include ordinary automobiles, large special purpose automobiles, small special purpose automobiles, trucks, large motorcycles, ordinary motorcycles, and the like.
[0166] [Mobile object] 13 shows an example of a mobile body equipped with an all-solid-state battery that is an electrochemical element of the present invention. Mobile body 70 is, for example, an electric vehicle. Mobile body 70 includes a motor 71, an electrochemical element 72, and wheels 73 that are an example of a means of transportation. Electrochemical element 72 is the electrochemical element of the present invention described above. Electrochemical element 72 drives motor 71 by supplying power to motor 71. Driven motor 71 can drive wheels 73, and as a result, mobile body 70 can move. According to the above-mentioned configuration, short-circuiting between the positive and negative electrodes is prevented, and the vehicle is driven by electric power from an electrochemical element having excellent battery characteristics, so that the vehicle can be moved safely and efficiently. The moving body 70 is not limited to an electric vehicle, but may be a PHEV or HEV, or a locomotive or motorcycle that can run using a diesel engine and an electrochemical device in combination. The moving body may also be a transport robot used in a factory or the like that can run using only an electrochemical device or a combination of an engine and an electrochemical device. The moving body may also be an object that does not move in its entirety, but only a part of it, such as an assembly robot that is arranged on a factory production line and whose arms, etc., can operate using only an electrochemical device or a combination of an engine and an electrochemical device.
[0167] (Electrochemical element manufacturing method and electrochemical element manufacturing apparatus) The method for manufacturing an electrochemical element of the present invention includes an electrode manufacturing step of manufacturing an electrode laminate by the above-mentioned method for manufacturing an electrode laminate of the present invention, and an element fabrication step of manufacturing an electrochemical element using the electrode laminate, and may further include other steps as necessary. The electrochemical element manufacturing apparatus of the present invention has an electrode manufacturing section that manufactures an electrode laminate using the above-mentioned electrode laminate manufacturing apparatus of the present invention, and an element production section that manufactures an electrochemical element using the electrode laminate, and may further have other means as necessary.
[0168] <Electrode manufacturing process and electrode manufacturing department> The electrode manufacturing process includes the insulating layer forming step explained in the above-mentioned method for manufacturing an electrode laminate of the present invention, and further includes other steps such as an electrode mixture layer forming step and an electrode processing step, as necessary. The electrode manufacturing section has the insulating layer forming means explained in the above-mentioned electrode laminate manufacturing apparatus of the present invention, and further has other means such as an electrode mixture layer forming means and an electrode processing means, if necessary. The electrode manufacturing process and the electrode manufacturing unit can manufacture an electrode having an electrode substrate, an electrode mixture layer provided on the electrode substrate, and an insulating layer provided on the electrode mixture layer.
[0169] <Device Fabrication Process and Device Fabrication Department> The device fabrication step is a step of manufacturing an electrochemical device using the electrode laminate. The device production section is a means for producing an electrochemical device using the electrode laminate. The method for producing an electrochemical element using the electrode laminate is not particularly limited, and a publicly known method for producing an electrochemical element can be appropriately selected depending on the purpose. For example, there is a method in which a storage element is produced by at least one of providing a counter electrode, winding or stacking, and housing in a container. The element fabrication step does not need to include all steps of element fabrication, and may include only a part of the steps.
[0170] <Electrode processing process and electrode processing section> The electrode processing unit is a means for processing the electrode on which the resin layer is formed downstream of the application unit. The electrode processing unit may perform at least one of cutting, folding, and lamination. The laminated electrode processing unit can, for example, cut the laminated electrode on which the resin layer is formed to prepare a laminate of laminated electrodes. The electrode processing unit can wind or stack the laminated electrode on which the resin layer is formed. The electrode processing section has, for example, an electrode processing device, and cuts, folds, stacks, or winds the laminated electrode on which the porous resin layer is formed, according to the desired battery form. The electrode processing step performed by the electrode processing unit is, for example, a step of processing a laminated electrode on which a resin layer has been formed downstream of the application step. The electrode processing step may include at least one of a cutting step, a folding step, and a bonding step. EXAMPLES
[0171] Examples of the present invention will be described below, but the present invention is not limited to these examples. In addition, "parts" and "%" respectively indicate "parts by mass" and "% by mass" based on mass unless otherwise specified.
[0172] Example 1 <Preparation of negative electrode> A two-roll direct coater was used to coat both sides of a copper foil (thickness: 20 μm) as a negative electrode substrate with a slurry for a negative electrode composite layer obtained by kneading 50 parts of a negative electrode active material (SCMGTM-XR-s, manufactured by Resonac Co., Ltd.), 45 parts of water, and 5 parts of polyvinylidene fluoride (Solef 5130, manufactured by Solvay Co., Ltd.), and then the slurry was dried to form a negative electrode composite layer. Then, a load of 10,000 kg was applied to the negative electrode composite layer with a roller having a diameter of 250 mm using an air-hydro type 10t roll press device, and a negative electrode with a thickness of 50 μm on one side (total thickness 120 μm) was produced.
[0173] <Preparation of positive electrode> A two-roll direct coat type comma coater was used to coat both sides of an aluminum foil (thickness: 20 μm) as a positive electrode substrate with a slurry for a positive electrode mixture layer obtained by kneading 50 parts of a positive electrode active material (lithium nickel oxide 503H, manufactured by JFE Mineral Co., Ltd.), 45 parts of N-methylpyrrolidone, and 5 parts of polyvinylidene fluoride (Solef 5130, manufactured by Solvay Co., Ltd.), and then the slurry was dried to form a positive electrode mixture layer. Then, an air-hydro type 10t roll press device was used to apply a load of 10,000 kg to the positive electrode mixture layer with a roller having a diameter of 250 mm, and a positive electrode with a thickness of 50 μm on one side (total thickness 120 μm) was produced.
[0174] <Preparation of Liquid Composition for Insulating Layer> In a glass container, add 38.8 parts of ethyl lactate and a polymer dispersant (Marialim TM While stirring a mixture of 0.8 parts of alumina powder (Sumicorundum SC-0708A, manufactured by NOF Corp.), TM AA-03, manufactured by Sumitomo Chemical Co., Ltd.) was added. After thorough stirring, zirconia beads (particle size: 5 mm, YTZ TM To the mixture was added 80 parts of ruthenium oxide (IKA ROLLER series, manufactured by Tosoh Corporation), and the mixture was subjected to a dispersion treatment for 72 hours in a ball mill (IKA ROLLER 10, manufactured by IKA Corporation) to obtain an alumina dispersion. In a separate glass container, add polyoxyethylene polyoxypropylene glycol (Epoxy TM A base liquid was prepared by adding 0.4 parts of 740 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), 10 parts of ethyl lactate, and 10.5 parts of hexylene glycol. The alumina dispersion was gradually added to the obtained base liquid while stirring, and after sufficient stirring, coarse particles were removed using a membrane filter with a pore size of 5 μm, thereby obtaining a liquid composition for an insulating layer.
[0175] The average primary particle diameters of the alumina powder and resin particles used were measured using a scanning electron microscope (Merlin, manufactured by Carl Zeiss KK), and the results were as follows. Sumicorundum TM AA-03 (Sumitomo Chemical Co., Ltd.): 240 nm Sumicorundum TMAA-07 (Sumitomo Chemical Co., Ltd.): 600 nm ·Eposter TM S6 (manufactured by Nippon Shokubai Co., Ltd.): 400 nm
[0176] <Formation of insulating layer and preparation of electrodes> Using a liquid ejection device (EV2500, Ricoh Co., Ltd.) and a liquid ejection head (MH5421F, Ricoh Co., Ltd.), the liquid composition for insulating layer was ejected onto one electrode mixture layer of the positive electrode to form the insulating layer pattern shown in FIG. 4A. The insulating layer pattern was scaled to the size shown in the figure and the width of the flow path was adjusted to achieve the desired coverage. Note that the flow path was left uncoated. The positive electrode coated with the liquid composition for insulating layer was dried by heating with hot air at 120°C for 5 minutes to form an insulating layer. An insulating layer was also formed on the opposite side, i.e., the other electrode mixture layer of the positive electrode, under the same conditions. Furthermore, the positive electrode was dried by heating in a vacuum oven at 150°C for 12 hours to obtain a positive electrode provided with an insulating layer as the electrode of Example 1. In the obtained electrode of Example 1, the coverage of the electrode mixture layer by the insulating portion was 92%, the average thickness of each insulating layer formed on both sides of the positive electrode was 5 μm, and the width of the flow path was 0.5 mm.
[0177] <Production of lithium-ion secondary battery> The positive electrode was cut to a size of 47 mm long x 27 mm wide (excluding the lead wire), and the negative electrode was cut to a size of 50 mm long x 30 mm wide (excluding the lead wire). A 16 μm thick polyethylene separator (SETELA TM Three positive electrodes and four negative electrodes were alternately stacked with intervening electrodes (series F20BHE, manufactured by Toray Industries, Inc., length 53 mm × width 33 mm) to obtain a stacked electrode element.
[0178] Next, the obtained laminated electrode element was sandwiched between laminate sheets of aluminum exterior, and the periphery was sealed with a laminator leaving an opening about 50 mm wide to form a bag-shaped exterior. As a non-aqueous electrolyte, an electrolyte solution was used in which lithium hexafluorophosphate (LiPF6) was dissolved as an electrolyte salt to a concentration of 1.5 mol / L in a mixed solvent of ethylene carbonate: dimethyl carbonate: ethyl methyl carbonate (1:1:1, volume ratio). The electrolyte solution was injected into the laminate sheet of the exterior from the upper opening, and then the opening was sealed with a degassing sealer. At this time, the electrolyte solution was first filled in the lower part of the exterior, and then the electrolyte solution was sucked into the opening side by degassing and passed through, so that the lower side (the side opposite the opening) became the electrolyte solution injection side in the insulating layer, and the upper side (the opening side) became the electrolyte solution outflow side. In this way, the electrolyte solution was passed through the laminated electrode element and sealed to obtain a lithium ion secondary battery as the electrochemical element of Example 1.
[0179] <Evaluation> The liquid permeability of the obtained electrode of Example 1, as well as the safety and float characteristics of the electrochemical device, were evaluated by the following procedures. The results are shown in Table 1.
[0180] <<Evaluation of electrode permeability>> The electrode (positive electrode) on which the insulating layer was formed was sandwiched between two glass slides, and the long side of the glass slide was sealed with polyimide tape while pressure was applied. 1 g of solvent was placed in a stainless steel petri dish with an inner diameter of 50 mm, and one of the short sides of the glass slide sandwiching the electrode was vertically immersed in the solvent. The test solvent used was a mixed solvent of ethylene carbonate: dimethyl carbonate: ethyl methyl carbonate (1:1:1, volume ratio) used in the electrolyte of the electrochemical element. The moment of immersion in the solvent was set as 0 seconds, and the height of the center of the part where the solvent had penetrated into the insulating layer was measured 60 seconds later. Measurements were performed three times, and the average value was calculated as the penetration height, and the liquid permeability was evaluated according to the following criteria. A was the best result, and C was the acceptable range. -Evaluation criteria- A: Penetration height is 12mm or more B: Penetration height is 10 mm or more and less than 12 mm C: Penetration height is 8 mm or more and less than 10 mm D: Penetration height is less than 8 mm
[0181] <<Safety assessment of electrochemical devices>> [Initial capacity measurement] The positive electrode lead wire and the negative electrode lead wire of the electrochemical element were connected to a charge / discharge tester (manufactured by Hokuto Denko Corporation), and the device was charged at a constant current and constant voltage with a maximum voltage of 4.2 V and a current rate of 0.2 C for 5 hours. After the charging was completed, the device was left to stand in a thermostatic chamber at 40° C. for 5 days. The device was then discharged at a constant current and constant voltage of 0.2 C to 2.5 V. The device was then charged at a constant current and constant voltage of 4.2 V and a current rate of 0.2 C for 5 hours, and after a 10-minute break, was discharged at a constant current and constant voltage of 0.2 C to 2.5 V. The discharge capacity at this time was taken as the initial capacity.
[0182] [Safety assessment] A nail penetration test was conducted to evaluate the safety of an electrochemical element having a battery with an insulating layer formed thereon. The positive and negative electrode leads of the electrochemical element (non-aqueous electrolyte storage element) for which the initial capacity had been measured were connected to a charge / discharge test device, and constant current and constant voltage charging was performed at a maximum voltage of 4.2V and a current rate of 1C for 3 hours, with the charge depth set to 100% (full charge). Next, an iron nail with a diameter of 4.5 mm was pierced horizontally to the direction in which the electrodes were stacked, intentionally shorting the non-aqueous electrolyte storage element, and the state of the element was observed, and safety was evaluated according to the following criteria. A was an excellent result, and a rating up to A was within the acceptable range. -Evaluation criteria- A: No ignition of electrochemical element due to nail insertion D: An electrochemical element caught fire due to a nail being inserted.
[0183] <<Evaluation of Float Characteristics of Electrochemical Devices>> The leakage current caused by oxidation degradation of the separator was evaluated by float characteristics. The positive and negative electrode leads of the electrochemical element (non-aqueous electrolyte storage element) for which the initial capacity was measured were connected to a charge / discharge test device, and the element was charged in a thermostatic chamber at 60°C with a maximum voltage of 4.2V and a current rate of 0.2C for 5 hours until it was fully charged. After a 10-minute break, the element was continued to be charged at a current rate of 0.2C. The current flowing during this process was measured, and the time it took for the integrated electric capacity to reach the specified value of 50mAh was measured, and the float characteristics were evaluated according to the following criteria. A was the best result, and C was considered to be within the acceptable range. -Evaluation criteria- A: It takes more than 200 hours to reach the specified value. B: Time to reach the specified value is between 175 hours and 200 hours C: Time to reach the specified value is between 150 and 175 hours D: Time to reach the specified value is less than 150 hours
[0184] (Examples 2 to 5) Electrodes and electrochemical elements of Examples 2 to 5 were produced and evaluated in the same manner as in Example 1, except that the coating pattern of the insulating part in Example 1 was replaced with the combination in Table 1. The results are shown in Table 1.
[0185] Example 6 An electrode and an electrochemical element of Example 6 were produced and evaluated in the same manner as in Example 1, except that the coverage rate of the insulating portion was set to 90% by reducing the image while fixing the flow path width in Example 1. The results are shown in Table 1.
[0186] (Examples 7 to 9) Electrodes and electrochemical elements of Examples 7 to 9 were produced and evaluated in the same manner as in Example 1, except that the coating pattern of the insulating part in Example 1 was replaced with the combination in Table 1. The results are shown in Table 1.
[0187] (Examples 10 to 15) The electrodes and electrochemical elements of Examples 10 to 15 were produced and evaluated in the same manner as in Example 1, except that the coating pattern and coverage of the insulating part were not changed and the scale of the width of the flow path part was adjusted to the size in Table 1. The results are shown in Table 1.
[0188] Example 16 In Example 1, the alumina powder used in the liquid composition for the insulating layer was Sumicorundum. TM Except for replacing the electrode with AA-07 (manufactured by Sumitomo Chemical Co., Ltd.), an electrode and an electrochemical element of Example 16 were produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0189] (Examples 17 to 20) The electrodes and electrochemical elements of Examples 17 to 20 were produced and evaluated in the same manner as in Example 1, except that in Example 1, the amount of inkjet coating was adjusted and pattern coating was performed so that the insulating part had a film thickness as shown in Table 1. The results are shown in Table 1.
[0190] Example 21 In Example 1, the alumina powder used in the liquid composition for the insulating layer was mixed with resin particles (eposters). TM An electrode and an electrochemical element of Example 21 were produced and evaluated in the same manner as in Example 1, except that the electrode was replaced with S6 manufactured by Nippon Shokubai Co., Ltd. The results are shown in Table 1.
[0191] (Examples 22 to 26) An electrode and an electrochemical element of Example 21 were produced and evaluated in the same manner as in Example 1, except that the step of forming an insulating layer in Example 1 was changed to a step of forming two insulating layers in two separate steps as follows. The results are shown in Table 1. The liquid composition for insulating layer was discharged onto one electrode mixture layer of the positive electrode to form a first insulating layer with a coverage of 100% and an average thickness of 1 μm. Next, a second insulating layer was formed on the first insulating layer by adjusting the amount of inkjet coating so that the total thickness of the first and second insulating layers would be the thickness of the insulating part shown in Table 1, and pattern coating of the insulating layer liquid composition was performed. The part where the second insulating part was formed on the first insulating layer by pattern coating (thick part) corresponds to insulating part 3a in Figure 2, and the part where only the first insulating layer was formed and the second insulating part was not formed corresponds to second insulating part 3c in Figure 2.
[0192] (Comparative Examples 1 to 3) Electrodes and electrochemical elements of Comparative Examples 1 to 3 were produced and evaluated in the same manner as in Example 1, except that the coating pattern of the insulating portion in Example 1 was replaced with the combination in Table 2. The results are shown in Table 2.
[0193] Comparative Example 4 An electrode and an electrochemical element of Comparative Example 4 were prepared and evaluated in the same manner as in Example 1, except that in the coating of the insulating part, uncoated parts having a randomly shaped sea-island structure were provided by an error diffusion method. The results are shown in Table 2. The sea-island structure shown in FIG. 6D corresponds to a configuration in which the sea portion is an insulating portion, the island portion is an uncoated portion of the insulating portion (exposed portion of the electrode substrate), and the insulating layer does not have a communicating flow path.
[0194] (Comparative Examples 5 to 6) Electrodes and electrochemical elements of Comparative Examples 5 and 6 were produced and evaluated in the same manner as in Example 1, except that the coating pattern of the insulating part in Example 1 was replaced with the combination in Table 2. The results are shown in Table 2.
[0195] Comparative Example 7 An electrode and an electrochemical element of Comparative Example 7 were prepared and evaluated in the same manner as in Example 1, except that the coverage rate of the insulating portion was set to 80% by reducing the image while fixing the flow path width in Example 1. The results are shown in Table 2.
[0196] [Table 1]
[0197] [Table 2]
[0198] For example, aspects of the present invention are as follows. <1> An electrode substrate; an electrode mixture layer provided on the electrode substrate; an insulating layer provided on the electrode mixture layer, The insulating layer is An insulating portion that covers the electrode mixture layer; A flow path portion having a flow path that is connected in a planar direction of the electrode and branches into two or more directions, The electrode is characterized in that the insulating portion covers 90% or more of the electrode mixture layer. <2> The flow path portion has an exposed surface of the electrode mixture layer. <1> 2 is an electrode according to the above. <3> The electrode mixture layer is provided on the flow path portion. The thickness of the second insulating portion is smaller than the thickness of the insulating portion. <1> 2 is an electrode according to the above. <4> The positive electrode <1> from <3> The electrode according to any one of the preceding claims. <5> The flow path communicates from a side surface of the insulating layer on which an electrolyte solution is injected to another side surface opposite the side surface. <1> from <4> The electrode according to any one of the preceding claims. <6> The shortest path of the flow path communicating with a pair of opposing side surfaces of the insulating layer is a straight line. <1> from <5> The electrode according to any one of the preceding claims. <7> The width of the flow path is 0.1 mm or more and 2.0 mm or less. <1> from <6> 13. The electrode according to any one of claims 1 to 12. <8> The insulating portion has an average thickness of 1 μm or more and 30 μm or less. <1> from <7> The electrode according to any one of the preceding claims. <9> the insulating portion includes insulating particles, The insulating particles have an average primary particle size of 500 nm or less. <1> from <8> The electrode according to any one of the preceding claims. <10> the insulating portion contains inorganic oxide particles, The inorganic oxide particles contain at least one of aluminum, silicon, and zirconium. <1> from <9> The electrode according to any one of the preceding claims. <11> The above <1> from <10> 1. An electrochemical device comprising the electrode according to claim 1. <12> The above <11> A device comprising the electrochemical element according to claim 1. <13> The above <11> A mobile object is characterized by having the electrochemical element described above. <14> A method for producing an electrode, comprising: applying a liquid composition containing an insulating material onto an electrode mixture layer of a substrate having an electrode base and an electrode mixture layer provided thereon, to form an insulating layer having an insulating portion and a flow path portion, the insulating portion covers the electrode mixture layer, and the coverage rate of the electrode mixture layer by the insulating portion is 90% or more; The method for manufacturing an electrode is characterized in that the flow path portion has flow paths that communicate in a planar direction of the electrode and branch into two or more directions. <15> The above <14> an electrode manufacturing process for manufacturing an electrode by the electrode manufacturing method according to the present invention; and a device forming step of manufacturing an electrochemical device using the electrode.
[0199] The above <1> from <10> The electrode according to any one of the preceding claims. <11> The electrochemical element according to <12> The device according to <13> The moving body according to <14> The method for producing the electrode according to the present invention <15> According to the method for producing an electrochemical element described above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]
[0200] 1: Electrode base 2: Electrode composite layer 3: Insulating layer 3a: Insulation part 3b: Channel section 3c: Second insulating part 10: Electrode 11: Negative electrode substrate 12: Negative electrode composite layer 13: Insulating layer 15: Electrode (negative electrode) 21: Positive electrode substrate 22: Positive electrode mixture layer 25: Electrode (positive electrode) 30: Separator 40: Electrode element 60: Electrochemical element 70: Mobile 100:Printing Department 200: Heating part 500: Electrode manufacturing equipment [Prior art documents] [Patent documents]
[0201] [Patent Document 1] JP 2000-277386 A
Claims
1. An electrode substrate; an electrode mixture layer provided on the electrode substrate; an insulating layer provided on the electrode mixture layer, The insulating layer is An insulating portion that covers the electrode mixture layer; A flow path portion having a flow path that is connected in a planar direction of the electrode and branches in two or more directions, An electrode, characterized in that the insulating portion covers 90% or more of the electrode mixture layer.
2. The electrode according to claim 1 , wherein the flow path portion has an exposed surface of the electrode mixture layer.
3. The electrode according to claim 1 , further comprising a second insulating portion provided on the electrode mixture layer in the flow path portion, the second insulating portion having a thickness smaller than that of the insulating portion.
4. 3. The electrode according to claim 1, which is a positive electrode.
5. 3. The electrode according to claim 1, wherein the flow path communicates from a side surface of the insulating layer on which an electrolyte is injected to another side surface opposite the side surface.
6. 3. The electrode according to claim 1, wherein the shortest path of the flow path communicating with a pair of opposing side surfaces of the insulating layer is a straight line.
7. 3. The electrode according to claim 1, wherein the width of the flow path is 0.1 mm or more and 2.0 mm or less.
8. 3. The electrode according to claim 1, wherein the insulating portion has an average thickness of 1 μm or more and 30 μm or less.
9. the insulating portion includes insulating particles, 3. The electrode according to claim 1, wherein the insulating particles have an average primary particle size of 500 nm or less.
10. the insulating portion contains inorganic oxide particles, 3. The electrode according to claim 1, wherein the inorganic oxide particles contain at least one of aluminum, silicon, and zirconium.
11. An electrochemical device comprising the electrode according to claim 1 or 2.
12. A device comprising the electrochemical element according to claim 11.
13. A moving object comprising the electrochemical device according to claim 11.
14. A method for producing an electrode, comprising: an insulating layer forming step of applying a liquid composition containing an insulating material onto an electrode mixture layer of a substrate having an electrode base and forming an insulating layer having an insulating portion and a flow path portion, the insulating portion covers the electrode mixture layer, and a coverage rate of the electrode mixture layer by the insulating portion is 90% or more; The method for manufacturing an electrode, wherein the flow path portion has flow paths that communicate with each other in a planar direction of the electrode and branch into two or more directions.
15. An electrode manufacturing process for manufacturing an electrode by the electrode manufacturing method according to claim 14; and producing an electrochemical element by using the electrode.
Citation Information
Patent Citations
Electrode plate of lithium ion secondary battery, and lithium ion secondary battery as well as manufacturing method of the same
JP2005174792A
Manufacturing method of electrode body
JP2018133299A
Electrode and manufacturing method therefor, electrode element, nonaqueous electrolyte power storage element
JP2019110110A
Electrode and manufacturing method thereof, and electrochemical element
JP2021082511A
Non-aqueous electrolyte secondary battery electrode and non-aqueous electrolyte secondary battery
WO2020184502A1