Plastic decomposing method

The use of crystalline metallosilicate in a subcritical or supercritical state with carbon dioxide or hydrocarbons addresses the limitations of existing plastic recycling methods, achieving high-yield production of valuable organic compounds like benzene, toluene, and xylene.

JP2024139166APending Publication Date: 2024-10-09MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023049985
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing methods for chemical recycling of plastics, such as pyrolysis and catalytic decomposition, face limitations in product selectivity and catalyst durability, particularly when producing chemicals for naphtha crackers, and the obtained products have limited uses due to high-temperature water constraints.

Method used

A method involving the use of crystalline metallosilicate, such as zeolite or gallosilicate, in a subcritical or supercritical state without hydroxyl groups, with a processing medium like carbon dioxide or hydrocarbons, to decompose plastics, maintaining crystallinity and suppressing uneven heating, thereby producing high-yield low-molecular organic substances.

Benefits of technology

This method efficiently produces low-molecular organic compounds like benzene, toluene, and xylene, enhancing the yield and selectivity of chemical products, while maintaining catalyst stability and reducing unwanted by-products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139166000001_ABST
    Figure 2024139166000001_ABST
Patent Text Reader

Abstract

To provide a plastic decomposing method which can efficiently obtain a useful low molecular organic matter containing a plastic as a raw material, specifically, to provide a plastic decomposing method which performs a decomposition reaction using a plastic as a raw material, and can obtain a decomposition matter, especially, a low molecular organic matter with a high yield, while maintaining crystallinity of crystalline metallosilicate and suppressing carbonization of the plastic.SOLUTION: A plastic decomposing method heats and decomposes a plastic, in the presence of a treatment medium having no crystalline metallosilicate and hydroxyl group in a subcritical or supercritical state.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for decomposing plastics. [Background technology]

[0002] Petroleum-based plastics have excellent workability, heat resistance, electrical conductivity, transparency, and chemical resistance. While plastic is used for a variety of purposes, the amount of plastic waste is increasing year by year worldwide. Plastics may contain a mixture of plastics with different properties and may be contaminated with foreign matter. Due to these factors, some plastics, such as PET bottles, are being recycled. Currently, most waste plastics are incinerated or landfilled after use, except for plastics. There is a demand for chemical recycling, which reuses waste as chemical raw materials. The methods of decomposition include pyrolysis, which involves thermal decomposition of plastics in an oxygen-free environment, and catalytic decomposition. One of these methods involves mixing plastic with a supercritical treatment medium. In recent years, the supercritical decomposition method, which uses a heat medium as a processing medium, has attracted attention. It directly penetrates the plastic and heats it up, so uneven heating of the plastic is suppressed and it is preferable. In Patent Document 1, polyolefin is used as a catalyst, and the production of heavy carbonaceous materials that are not easily generated can be reduced. This publication discloses a method for contacting and reacting with supercritical water in a reactor to convert the mixture into oil. In addition, Patent Document 2 discloses a method for treating organic substances such as plastics with a metal catalyst made of a hydrogen activating metal and A method for converting hydrogen into a gas containing hydrogen by contacting subcritical water or supercritical water in the presence of an oxidizing agent is disclosed. As shown. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 06-279762 [Patent Document 2] JP 2009-30071 A Summary of the Invention [Problem to be solved by the invention]

[0004] The products obtained in Patent Document 1 are mainly paraffins and olefins having carbon numbers of about 10 to 30. The direct use of the resulting products is limited to fuel and other uses. Even if it is used as a raw material for a naphtha cracker, the selectivity of the naphtha content of the resulting product is poor. There are some issues. The technology disclosed in Patent Document 2 produces light hydrocarbon gases such as hydrogen and methane as products. However, there is a problem that the light hydrocarbon gas obtained has limited uses. Since high-temperature water is used, the catalysts that can be used are limited to those that are water-resistant. In order to realize more economical chemical recycling of plastics, Directing carbon dioxide into high-demand chemicals and selectively directing carbon dioxide into components that are used as raw materials in naphtha crackers There is a need for efficient production of useful chemicals from plastics, including selective conversion. [Means for solving the problem]

[0005] As a result of intensive research aimed at solving the above problems, the present inventors have discovered a crystalline metallosilicate and The plastic is decomposed in the presence of a treatment medium that does not have a hydroxyl group and is in a subcritical or supercritical state. The present invention has been completed based on the finding that the above problems can be solved by using the above-mentioned method.

[0006] That is, the present invention relates to the following. [1] Crystalline metallosilicate and a treatment medium having no hydroxyl groups in a subcritical or supercritical state 2. A method for decomposing plastics, comprising heating a plastic in the presence of a chemical compound. [2] The heating temperature is 300°C or higher and 550°C or lower. How to disassemble a . [3] The crystalline metallosilicate includes a zeolite and / or a gallosilicate. A method for decomposing plastics as described in [1] or [2] above. [4] Any of the above [1] to [3], wherein the crystalline metallosilicate has an MFI structure. The method for decomposing the plastics described above. [5] The decomposition product obtained by the decomposition contains 45 wt% or more of organic matter having a carbon number of 2 to 12. The method for decomposing plastics according to any one of the above [1] to [4]. [6] The decomposition products obtained by the decomposition are at least one of the group consisting of benzene, toluene and xylene. The plastic according to any one of the above [1] to [5], which contains at least one of the above-mentioned How to disassemble the block. [7] The above [1] to [1], wherein the plastic contains polyethylene and / or polypropylene. [6] A method for decomposing plastics according to any one of the above. [8] The method according to any one of [1] to [7] above, wherein the treatment medium is carbon dioxide. How to break down a tic. Effect of the Invention

[0007] The present invention provides a useful low-temperature polymeric material using plastics such as polyethylene and polypropylene as raw materials. The objective of the present invention is to provide a method for decomposing plastics that can efficiently obtain molecular organic matter. Specifically, plastic is used as a raw material and a decomposition reaction is carried out to produce crystalline meta. While maintaining the crystallinity of the silicate, the carbonization of plastic is suppressed, and decomposition products, especially The present invention aims to provide a method for decomposing plastics that can efficiently obtain low molecular weight organic matter. can. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram showing a batch-type decomposition apparatus used in plastic decomposition according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing a semi-flow type decomposition device used in plastic decomposition according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing a reaction tube constituting a semi-flow type decomposition apparatus used in plastic decomposition according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following describes the embodiment of the present invention in detail. The present invention is not limited to these examples unless it exceeds the gist of the present invention. In addition, "~" indicates a range of values, and the values ​​before and after it are the lower and upper limits. This means to include as.

[0010] <How to disassemble plastic> The method for decomposing plastics of the present invention comprises using a crystalline metallosilicate and a subcritical or supercritical The present invention is characterized in that plastics are decomposed to obtain organic matter in the presence of a treatment medium that does not have a hydroxyl group in the form of a water-soluble organic compound. It is a sign.

[0011] <Processing medium> A non-hydroxylic treatment medium in a subcritical or supercritical state (such as, but not limited to, Examples include supercritical carbon dioxide and supercritical hydrocarbons such as octane. By using the subcritical or supercritical liquid in the present invention, plastics can be decomposed efficiently. The advantages of using a treatment medium that does not have a hydroxyl group include the following: 1) Subcritical and supercritical fluids have low interfacial tension, low viscosity, and high diffusivity compared to liquids. This allows it to penetrate well into plastics with a wide variety of shapes and properties. 2) The kinetic viscosity of the material is smaller than that of gas or liquid, so even slight temperature differences can easily cause thermal convection. It is possible to heat the plastic evenly and prevent the formation of solids due to overheating. 3) Heat Since the conductivity of gas is higher than that of gas, exothermic reactions and adsorption occur in the micropores of crystalline metallosilicates. When a thermal reaction occurs, heat can be quickly applied or removed to stabilize the reaction temperature. 4) The solubility of crystalline metallosilicates in low polar organic matter is greater than that of gases. When a chemical reaction involving the generation of organic matter occurs on the surface of a solid catalyst such as Since it dissolves, it can suppress undesirable coking on the catalyst surface. 5) Crystallization When trivalent elements contained in hydrophilic metallosilicates are exposed to water or water-producing reaction sites at high temperatures, It is known that some of the hydroxyl groups are eliminated, resulting in a decrease in catalytic activity. If it is a processing medium, it can be operated stably.

[0012] In one embodiment, the following advantages are provided when the treatment medium is carbon dioxide: do. 1) Carbon dioxide is non-polar, so it can dissolve low-polarity organic matter well. 2) Carbon dioxide itself has low activity, so when water or alcohol is used as a treatment medium, Unlike conventional methods, the treatment medium itself reacts to inhibit the formation of undesirable oxygen-containing compounds. 3) Carbon dioxide vaporizes when the pressure and temperature are returned to normal, so the separation of the treatment medium is possible. Therefore, unlike when water is used as the treatment medium, wastewater treatment is not required. 4) Carbon dioxide and nitrogen are inexpensive inert treatment media. It has a larger heat capacity than other materials, making it excellent at heating plastics as a heat transfer medium. 5) Carbon dioxide is more effective as a preventive measure against gas explosions than nitrogen, making it safer. 6) The critical temperature of carbon dioxide is higher than that of nitrogen, so the energy required for storage is 7) The carbon dioxide produced during the decomposition of plastics is used as a processing medium. Light hydrocarbons such as methane and ethane become water and carbon dioxide when burned. By separating the water, it can be easily reused as a treatment medium.

[0013] In another embodiment, when the processing medium is a hydrocarbon, the following advantages are given: . 1) Hydrocarbons are contained in the products of decomposing plastics, so they can be easily removed by distillation, etc. It can be easily separated from the product and recycled as a processing medium. ) Hydrocarbons do not contain oxygen atoms, so unlike the use of water or alcohol as the treatment medium, Even if the treatment medium itself reacts, it will not produce undesirable oxygen-containing compounds. .

[0014] In addition, "supercritical carbon dioxide" means that the pressure is equal to or higher than the critical pressure of carbon dioxide. The critical pressure of carbon dioxide is 7.38 MPa and the critical temperature is 31.1°C. The pressure is equal to or greater than the critical pressure of carbon dioxide, and the temperature is slightly below the critical temperature. Carbon dioxide, or the pressure is slightly below the critical pressure of carbon dioxide and the temperature is above the critical temperature or less than the critical temperature and pressure. However, it refers to carbon dioxide in a state close to this.

[0015] In addition, the term "supercritical hydrocarbon" refers to a hydrocarbon in which the pressure is equal to or higher than the critical pressure and the temperature is This refers to a hydrocarbon in a state above its critical temperature. The critical pressure and critical temperature of a hydrocarbon are It depends on the type. Also, "subcritical hydrocarbons" are those that are heated at pressures above the critical pressure of the hydrocarbon. Hydrocarbons at or above the critical temperature and slightly below the critical temperature, or at pressures slightly below the critical temperature. or a hydrocarbon in a state where the pressure is less than the critical pressure of the hydrocarbon and the temperature is equal to or greater than the critical temperature of the hydrocarbon; Refers to hydrocarbons whose temperature is below the critical temperature and whose pressure is below but close to the critical pressure. vinegar.

[0016] <Decomposition products obtained by heating plastic> In the present invention, this refers to organic matter as a decomposition product obtained by heating plastic. The carbon number of is not particularly limited, but it contains 45 wt% or more of organic matter with a carbon number of 2 to 12. It is preferable that the content is 50 wt% or more, more preferably 60 wt% or more. There is no upper limit, and it may be 100 wt%. The organic substance having 2 to 12 carbon atoms (hereinafter, sometimes referred to as a low molecular weight organic substance) is: Saturated aliphatic hydrocarbons, unsaturated aliphatic hydrocarbons, and aromatic hydrocarbons with carbon numbers from 2 to 12 Hydrocarbons having carbon numbers within the above range are in high demand as chemical raw materials. The decomposition products obtained are not particularly limited as long as they fall within the above definition, but may include, for example, For example, ethane, propane, butane, pentane, hexane, heptane, octane, nonane, deca Saturated aliphatic hydrocarbons such as cyclopentane, cyclohexane, undecane, and dodecane; , cycloheptane, cyclooctane, cyclononane, cyclodecane, cycloundecane, Saturated aliphatic hydrocarbons with cyclic structures such as cyclododecane; ethylene, propylene, butene pentene, hexene, heptene, octene, nonene, decene, undecene, dodecene Unsaturated aliphatic hydrocarbons such as benzene, toluene, xylene, trimethylbenzene, ethylene Aromatic hydrocarbons such as ethylbenzene, ethyltoluene, and triethylbenzene. The above hydrocarbons may also have branches or functional groups. The decomposition products of the present invention are benzene, toluene and xylene, which are in high demand as raw materials for chemical products. It is preferable that the content of at least one of the group consisting of the above is 1 wt % or more, and more preferably 3 wt % or more. It is more preferable that the content of these is 5 wt%, and it is even more preferable that the content of these is 5 wt%. It's fine.

[0017] <Raw materials> The plastics used as raw materials in the present invention are those that can achieve the effects of the present invention. There is no particular limitation as long as the polymer is a polyethylene, polypropylene, polybutene, polybutadiene, etc. Polyolefins such as poly(4-methyl-1-pentene); polystyrene, polymethacrylate Methyl acrylate, polyvinyl chloride, polyvinyl alcohol, polyvinyl acetate, polyacrylo Nitrile, ethylene vinyl alcohol copolymer resin and other addition polymerization polymers; polycarbonate Polyethylene terephthalate, polyamide, polyimide, polyurethane, polyether Polycondensation polymers such as polyether ether ketone and polyether ether ketone are also included. These plastics may be copolymerized. These plastics may also be mixed. The form of the material may be a molded product such as a film or a tube. Among these plastics, polyolefins are the most popular from the viewpoint of increasing the yield of low molecular weight organic matter. and / or polystyrene is preferably included.

[0018] The content of polyolefin and / or polystyrene is not particularly limited, but low molecular weight organic matter In view of the high yield of polyolefin and / or polystyrene in the plastic, It is preferable that the composition contains 30 wt% or more of phosphate, more preferably 50 wt% or more of phosphate, and 70 It is more preferable that the content of the polyolefin is at least 5% by weight. and / or polystyrene. Among polyolefins, polyethylene and other polyolefins are the most widely discharged as industrial and household waste. and polypropylene, and for the same reason, polystyrene. That is, it contains one of polyethylene, polypropylene, and polystyrene. It may be any two or all of polyethylene, polypropylene, and polystyrene. may also include

[0019] <Crystalline metallosilicate> The crystalline metallosilicate of the present invention is used as a catalyst. is not particularly limited, and examples thereof include zeolite, galloaluminosilicate, gallosilicate, boroaluminosilicate, and the like. Silicate, titanosilicate, vanadosilicate, aluminoferrisilicate, ferri Among them, zeolite and gauss are preferable because of their high catalytic activity. Examples of the silicate include aluminosilicate, gallosilicate, and borosilicate. More preferably, Zeolites and gallosilicates are examples.

[0020] <Structure of crystalline metallosilicate> The skeletal structure of the crystalline metallosilicate used in the present invention is not particularly limited, and may be any of the crystalline metallosilicates listed in the International Zeon Index. International Zeolite Association (IZA) Hereafter, this will be referred to as "IZA".) For example, LTA structure, FAU structure, MFI structure, MWW structure, BEA structure, C Among them, MFI structure and M Examples of the structure include a WW structure and a CHA structure, and more preferably, an MFI structure.

[0021] <Shape of crystalline metallosilicate> The crystalline metallosilicate may be used as a catalyst as it is in the reaction, or may be used as an inert catalyst in the reaction. The material may be shaped using a material or binder, or may be mixed with these and used in the reaction. By forming the catalyst into a shape, the strength and abrasion resistance of the catalyst can be improved. Examples of the material include, but are not limited to, alumina and clay.

[0022] <Composition of crystalline metallosilicate> Crystalline metallosilicates SiO2 / M2O3 (where M is Al, Ga, B, Ti, V, Fe, and other trivalent elements may be used alone or in combination. The molar ratio may be such that the lower limit is 5 or more in order to provide the catalyst with sufficient durability. The upper limit is preferably 2000 or less, and more preferably 10 or more. It is more preferable that the SiO2 / M2O3 molar ratio is equal to or less than the above upper limit. , improving the decomposition rate of plastic.

[0023] <Cation species of crystalline metallosilicate> The ion exchange sites in the crystalline metallosilicate framework used in the present invention are usually proto There are cations such as proton and ammonium, which are called proton type and ammonium type, respectively. In the present invention, either the proton type or the ammonium type may be used, but the proton type is preferred. The ammonium type may be calcined to form a proton type. Some of the elements in the periodic table are Na and K in group Ia, Mg and Ca in group IIa, and IIIb in group IIIb. B, Al, Ga, transition elements Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, It may be replaced with a metal element such as Mo. Among them, B, which has high catalytic activity, Ga, Fe, Co, Ni, Cu, and Zn are preferred, and B, Ga, and Zn are more preferred. These elements may be used alone or in combination. Examples of the method include liquid phase ion exchange and solid phase ion exchange.

[0024] <Supporting on crystalline metallosilicate> In addition, using crystalline metallosilicates as supports, we have been able to detect Na and K in Group Ia of the periodic table, and Zn in Group II of the periodic table. Mg and Ca in group a, B, Al, Ga in group IIIb of the periodic table, and Ti, V, Cr, and M in the transition elements Metal elements such as n, Fe, Co, Ni, Cu, Zn, and Mo may be supported. Since the catalytic activity is high, B, Ga, Fe, Co, Ni, Cu, and Zn are preferred. More preferably, a and Zn are preferable. These elements may be used alone or in combination. In the case of supporting metals, the impregnation method, the ion exchange method, the deposition precipitation method, the pore Filling method, incipient-wetness method, spray application method, etc. In addition, physical mixing and coprecipitation methods are also used. Among them, the impregnation method and The ion exchange method is preferred because it is simple and has a low process load. In the case of egg shell, the metal distribution is uniform by utilizing the difference in the adsorption speed of the supported metal. It may be made into egg white type, egg yolk type, or egg yolk type.

[0025] <Heating temperature> The temperature in the reactor when the plastic is heated and decomposed is within the range in which the effect of the present invention can be obtained. Although there are no particular limitations on the temperature, it is preferable that the temperature is in the range of 300° C. or higher and 550° C. or lower. If the temperature inside the reactor is 300°C or higher, the decomposition reaction of plastics will proceed sufficiently. From this viewpoint, the temperature in the reactor is preferably 350° C. or higher, more preferably 400° C. or higher. It is more preferable that the temperature is 425° C. or higher, and particularly preferable that the temperature is 425° C. or higher. In order to maintain a high yield of organic matter having a carbon number of 2 or more, the reaction temperature is preferably 500° C. or less. It is preferable that the heating temperature is 475° C. or lower, and more preferable that the heating temperature is 475° C. or lower.

[0026] <Reaction pressure> The reaction pressure when decomposing plastics is not particularly limited as long as the effect of the present invention is achieved. However, if the treatment medium is carbon dioxide, the pressure range is 5.0 MPa to 50 MPa. When the decomposition pressure is 5.0 MPa or more, the density of carbon dioxide is 1.0 times that of normal pressure. Since the amount of plastic decomposition products increases tenfold, the decomposition products can be dissolved effectively. The pressure is more preferably 5.5 MPa or more, and even more preferably 6.0 MPa or more. Preferred.

[0027] <Response time> The reaction time when decomposing plastics in a batch decomposition device is as follows: The time period is not particularly limited, but is preferably 1 minute to 300 minutes, more preferably 2 minutes to 150 minutes, The reaction time is more preferably in the range of 3 minutes to 100 minutes, particularly preferably in the range of 5 minutes to 60 minutes. Within this range, excessive cracking and recombination are suppressed, and a high oil yield is maintained. When decomposing plastics using a flow-through or semi-flow-through decomposition device, the crystalline metallosilicic acid The reaction time can be determined arbitrarily depending on the amount of the cate and the target product obtained by decomposition.

[0028] <Hydrogenation> In the decomposition reaction of the plastic of the present invention, hydrogen or a substance capable of donating hydrogen may be added. By introducing a hydrogen donor, the products of the cracking reaction can be continuously hydrogenated. In this case, subcritical and supercritical fluids can dissolve hydrogen in any ratio and also dissolve it in a decomposed form. Since there is no phase separation between the solution and hydrogen gas and a homogeneous phase is formed, a high reaction rate can be achieved. There are no particular limitations on the hydrogen donating substance, so long as it is a substance that can donate hydrogen. For example, water; alcohols such as methanol and ethanol; carbons such as hexane and octane; Hydrogen hydride; polycyclic hydrocarbons such as tetralin and dihydroanthracene. When adding substances with hydroxyl groups such as water or alcohol, the upper limit of the amount of the solvent is The amount of the catalyst added is preferably 5 wt % based on the total weight of the catalyst. The activity of the talosilicate is maintained.

[0029] <Auxiliary Agents> In the plastic decomposition reaction of the present invention, in order to enhance the intermolecular interaction between the product and the treatment medium, To achieve this, one or more auxiliary agents may be added. The auxiliary agents are generally polar substances. As for the substance, any substance that has the effect of enhancing the intermolecular interaction between the product and the processing medium can be used. Examples include, but are not limited to, water; alcohols such as methanol, ethanol, and propanol; Ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone Acetic acid, formic acid, and other carboxylic acids; methyl acetate, ethyl acetate, propyl acetate, and butyl acetate , ethyl formate, and other esters; diethyl ether, diisopropyl ether, tetrahydrofuran Ethers such as methyl tert-butyl ether, acetonitrile, acrylonitrile, nitriles such as nitrile; amines such as ethylenediamine, pyridine, and the like. When adding substances with hydroxyl groups such as water or alcohol, the upper limit of the amount to be added is the amount of the solvent. The amount of the solvent is preferably 5 wt %. By keeping the amount of the solvent below the upper limit, the crystallinity is improved. The activity of the metallosilicate is maintained.

[0030] <Device> Next, we will explain the method of decomposing plastics using a plastic decomposition device. is not limited to this. FIG. 1 shows a batch-type decomposition apparatus used for decomposing plastics according to one embodiment of the present invention. FIG 2 is a schematic diagram showing a semi-flow evaporator used in plastic decomposition according to one embodiment of the present invention. 3 is a schematic diagram showing a conventional decomposition device according to one embodiment of the present invention. FIG. 10 is a schematic diagram showing a reaction tube constituting a semi-flow type decomposition apparatus used in the Nitrogen gas cylinder, 10b is a carbon dioxide cylinder, 11a, 11b, 11c, and 11d are valves 12 is a high pressure pump, 13 is a pressure gauge, and 14 is a solid such as resin or crystalline metallosilicate. A metal mesh filter to prevent the outflow of materials downstream, 15 is a high-pressure vessel, and 16 is a heat A temperature controller with a coupler, 17 is an electric furnace, 18 is a cooler, 19 is a gas bag, 2 1a is a nitrogen gas cylinder, 21b is a carbon dioxide cylinder, 22a, 22b, and 22c are valves, 23 is a high pressure pump, 24 is a pressure gauge, 25 is a preheating tube, 26 is a check valve, 27 is a reaction tube, 28 is A temperature controller equipped with a thermocouple, 29 is an electric furnace, 30 is a cooler, 31 is a back pressure valve, 32 is a cooling trap bottle, 33 is a wet gas meter, 34 is a gas bag, and 41 is a thermocouple insertion hole. The reaction tube 41 has openings on three sides so that the reaction can be performed. The reaction tube 42 is a reaction tube for resins and crystalline metallosilicates. 43 is a metal mesh filter to prevent solids from flowing downstream, and 44 is a solid plastic filter. The gear-shaped partition plate is provided to prevent direct contact between the quartz and the crystalline metallosilicate. It is a metal rod.

[0031] <Reaction form> In the plastic decomposition reaction of the present invention, the reaction type is not particularly limited. For example, It can be carried out in any manner, such as batch, flow, or semi-flow. The stick decomposition reaction may be a single-stage reaction or a multi-stage reaction. In the case of a multi-stage reaction, Although not limited to this, the carbon number is reduced by mixing the plastic with a treatment medium in a subcritical or supercritical state. The process involves roughly decomposing organic matter into 10 to 40 parts, and using a subcritical or supercritical treatment medium with heterogeneous The process may further comprise the step of decomposing the polycondensation polymer by a catalyst. You can use them together or interchangeably. The plastic to be supplied may be in a solid state or may be pre-heated and melted. It is preferable that the material is melted to suppress temperature changes and pulsations in the raw material supply. The method of melting the cellulose is not particularly limited, but it is possible to provide a melting layer or an extruder in the preceding stage of the reaction process, It is preferable to maintain the temperature at a predetermined level before supplying the mixture to the reaction step. The use of an extruder is particularly advantageous in terms of feeding the plastic in the presence of a processing medium at a given temperature. I wish. The batch type has the following two advantages: 1) Plastics can be treated with a simple device configuration. 2) The solid residues accumulated in the device can be easily removed. In the case of the flow-through and semi-flow-through systems, the length of time that the supplied plastic comes into contact with the crystalline metallosilicate is The retention time can be strictly controlled, so that the products are gradually decomposed or decarbonized. This can suppress undesirable reactions such as EXAMPLES

[0032] The present invention will be described in more detail in the following examples and comparative examples. is not limited by.

[0033] <Preparation of crystalline metallosilicate> <Preparation Example 1> MFI-structured NH4-type gallium silicate powder (manufactured by N.E. Chemcat, SiO 6.0 g of 1,2-Ga2O3 (molar ratio = 30, volume average diameter = 8.4 μm) was placed in a glass firing tube. After drying for 3 hours at 200℃ under an air flow of 200mL / min, it was heated to 500℃ for 1 hour. The temperature was raised over a period of 100°C, and then the temperature was kept at 500°C for 4 hours. The temperature was then lowered to room temperature, and the MFI structure was formed. H-type gallium silicate powder (hereinafter also referred to as H-GaSi powder) was used.

[0034] <Preparation Example 2> MFI structure NH4 type zeolite powder (manufactured by N.E. Chemcat, SiO2 / Al 3.0 g of 2O3 (molar ratio = 30, volume average diameter = 5.4 μm) was placed in a glass firing tube, After drying at 120℃ for 7 hours under air flow of 200mL / min, it was heated to 500℃ for 1 hour. The temperature was raised to 500°C and held at that temperature for 4 hours, after which the temperature was lowered to room temperature and the H-type zeolite with MFI structure was formed. The powder was called H-ZSM-5 powder (hereinafter also referred to as H-ZSM-5 powder).

[0035] <Preparation Example 3> Gallium(III) nitrate n-hydrate (Fujifilm Wako Pure Chemical Industries, product number 072-02701 1.72 g of ethyl acetate was added to 11 g of deionized water and completely dissolved. MFI-structured H-type zeolite molded body in a car (Tosoh, product number HSZ-840HOD 1A) 10g was dropped and then lightly mixed to make a homogeneous state. It was soaked for 1.5 hours. After that, the beaker was placed on a hot stirrer set at 110°C and dried for 3 hours. The dried product was placed in a glass sintering tube and heated for 100 minutes under an air flow of 200 mL / min. After drying at ℃ for 7 hours, the temperature was raised to 500℃ over 2 hours and then held at 500℃ for 4 hours. After that, the temperature was lowered to room temperature to obtain a zeolite molded product with an MFI structure supporting 5 wt% of gallium element. (Hereinafter, this will be referred to as Ga / ZSM-5 compact).

[0036] [Example 1] The batch type plastic decomposition device shown in Figure 1 was used. The vessel 15 has an inner diameter of 30 mm, a depth of 80 mm, a capacity of approximately 56 mL, a maximum operating temperature of 500°C, and A stationary Inconel vessel with a high operating pressure of 50 MPa was used. The cooling pipes from 1c onwards were removed and a gas bag 19 was connected. The empty pressure vessel was weighed, and the weight was recorded as the empty pressure vessel weight. The raw material, low-density polyethylene (hereinafter referred to as LDPE) (Sigma-Aldric 6 g of H-GaSi powder (manufactured by H-GaSb, product number 428043) and 0.3 g of H-GaSi powder obtained in Preparation Example 1 were placed in a pressure vessel. The pressure vessel 15 containing the raw material and the crystalline metallosilicate was weighed. The value was the weight of the pressure vessel before treatment. After confirming that there was no gas in the tank, the pressure was slowly released. The tank was pressurized to 1 MPa with carbon dioxide, and the pressure was released to normal. After repeating the operation of restoring pressure three times, gently circulate gas through the container at normal pressure for about 30 seconds to check the inside The atmosphere was replaced, all valves were closed, and the container was placed in an electric furnace 17. The temperature is raised to the specified temperature (450°C) at a rate of 4°C per minute, and carbon dioxide is introduced just before the specified temperature. The pressure was increased and the specified conditions (decomposition temperature: 450°C, decomposition pressure: 30MPa) were reached. After the holding time was completed, the power supply to the electric furnace 17 was turned off. Then, the container was removed from the electric furnace 17 and cooled by blowing air. When the temperature inside the container became 40° C. or lower, the valve 1 was closed. 1c was slowly opened, and the entire amount of gas was collected in the gas bag 19 and weighed. The pressure vessel 15 was weighed, and the weight was recorded as the weight of the pressure vessel after treatment. The vessel was opened and the liquid was collected. The sample was removed and weighed. The recovered sample was a crystalline metallosilicate and liquid. The gas was analyzed by GC-FID under the following conditions. Check the peaks showing the components, and make sure that all peaks showing components with carbon numbers of 13 or more are below the detection limit. Therefore, the amount of low molecular weight organic matter contained in the gas obtained from the reaction was calculated using the following method. The recovered liquid was analyzed by GC-FID and thermogravimetric differential calorimetry under the following conditions. The results of the GC-FID showed that benzene, toluene, and The total yield of benzene and xylene was 11.3 wt%. As a result of TG-DTA analysis, a DTA curve with a downward convex and broad shape was shown from around 38°C to around 600°C, confirming that the obtained recovered liquid was a multi-component system. Therefore, the low molecular weight organic substances contained in the recovered liquid were calculated by the following method. The total amount of low molecular weight organic substances in the gas and liquid was taken as the amount of low molecular weight organic substances generated. As a result, the amount of low molecular weight organic substances generated was 4.56 g, and the ratio to the raw material LD PE was 76 wt%.

[0037] <GC-FID Analysis> Apparatus: GC-2014 Shimadzu Corporation Column: DB-5 Agilent Technology (60 m, 0.25 mm, 1.0 μm) Column temperature condition: Hold at 40°C for 3 minutes, heat from 40°C to 325°C at 10°C / min and then hold at 325°C for 5 minutes Flow rate: 1 mL / min Detection: FID Sample injection volume (liquid): 1 μL Sample injection volume (gas): 1 mL

[0038] <tg-dta> Equipment: Hitachi High-Tech Science STA300 Sample container: SiO2 Filled sample amount: 10mg Temperature conditions: 30°C to 600°C after 30 minutes at room temperature Heat up at 10℃ / min Atmosphere: Nitrogen 200mL / min

[0039] <Calculation of the amount of low molecular weight organic matter contained in gas> Amount of low molecular weight organic matter contained in gas = (Weight of pressure vessel before treatment) - (Weight of pressure vessel after treatment) (amount of methane detected by GC-FID) / (total organic matter detected by GC-FID) (Quantity of items) <Calculation of the amount of low molecular weight organic matter contained in liquid> A standard sample of dodecane, which has the highest carbon number among low-molecular-weight organic substances (Tokyo Chemical Industry Co., Ltd., product number S0284) was analyzed by TG-DTA and found to have a distillation temperature of 140°C. The proportion of low molecular weight organic matter in the collected liquid was analyzed by TG-DTA. The weight loss rate from room temperature to 140°C was calculated. Amount of low molecular weight organic matter contained in the liquid = {(weight of pressure vessel after treatment) - (weight of empty pressure vessel)} - (weight of crystalline metallosilicate added) × (weight obtained by analysis with a thermogravimetric differential thermal analyzer) (percentage of low molecular weight organic matter removed)

[0040] [Example 2] In Example 1, the reaction temperature was 425° C., the decomposition pressure was 10 MPa, and the reaction time was 60 minutes. The reaction was carried out in the same manner as in Example 1, except that the above-mentioned reaction was carried out in the same manner as in Example 1. The metallosilicate was a liquid. Analysis in the same manner as in Example 1 revealed that benzene, The total yield of toluene and xylene was 41.6 wt%. The amount of low-molecular-weight organic substances generated was calculated to be 4.98 g, and the ratio to LDPE as the raw material was 83 wt%. The ratio was 83 wt%.

[0041] [Comparative Example 1] In Comparative Example 1, the reaction was carried out in the same manner as in Example 1, except that the crystalline metallosilicate was not charged into the pressure vessel 15. The recovered product was a liquid. When analyzed by the same method as in Example 1, the total yield of benzene, toluene, and xylene was 0.58 wt%. The total yield of benzene, toluene, and xylene was 0.58 wt%. Also, when calculating the amount of low-molecular-weight organic substances generated by the same method as in Example 1, it was 2.4 g, and the ratio to LDPE as the raw material was 40 wt%. The ratio to LDPE as the raw material was 40 wt%.

[0042] [Example 3] In Example 3, the reaction was carried out in the same manner as in Example 1, except that the reaction time was set to 120 minutes. The recovered product was the same as in Example 1, i.e., crystalline metallosilicate and a liquid. The crystalline metallosilicate recovered under the following conditions was analyzed by XRD. As a result, it was confirmed that it had the same peak shape as the unused crystalline metallosilicate. Also, when evaluating the crystallinity of the crystalline metallosilicate under the following conditions, it was 100%. The crystalline metallosilicate recovered under the following conditions was analyzed by XRD. As a result, it was confirmed that it had the same peak shape as the unused crystalline metallosilicate. Also, when evaluating the crystallinity of the crystalline metallosilicate under the following conditions, it was 100%. When evaluating the crystallinity of the crystalline metallosilicate under the following conditions, it was 100%.

[0043] [XRD Analysis] Apparatus: PANalytical X‘Pert Pro MPD X-ray source: Cu K α Scanning range: 5° to 50°

[0044] [Crystallinity of Crystalline Metallosilicate] Crystallinity of crystalline metallosilicate = 100×(peak area of crystalline part) / {(peak area of crystalline part)+(area of amorphous part)} The crystallinity of the crystalline metallosilicate = 100×(peak area of the crystalline part) / {(peak area of the crystalline part)+(area of the amorphous part)}

[0045] [Comparative Example 2] The plastic decomposition device used was the same as that used in Example 1. LDPE (mentioned above) 6 g, 0.3 g of the H-ZSM-5 powder obtained in Preparation Example 2, and 20 g of water previously bubbled with nitrogen The nitrogen gas cylinder 10a was pressurized to its maximum pressure to ensure there was no leakage. After confirming that the pressure was high, the pressure was slowly released. Pressurize the tank with nitrogen to 1 MPa, then release the pressure and return it to normal pressure. After repeating this three times, gas was gently passed through the container at normal pressure for about 30 seconds to replace the internal atmosphere. All valves were closed, and the container was placed in an electric furnace 17. The temperature was increased to the desired value at a rate of 4°C per minute. The temperature was raised to 450°C and then held for a specified time (120 minutes) after reaching the specified temperature. After completion of the heating, the power supply to the electric furnace 17 was turned off, and the container was removed from the electric furnace 17 and cooled by blowing air. When the internal temperature drops below 40°C, slowly open valve 11c and transfer all the gas into gas bag 19. The container was opened and the sample was taken out. The recovered material was crystalline metallosilicate and liquid. The liquid had a two-phase structure of water and oil. XRD analysis of the talosilicate revealed that crystalline metallosilicates were formed at temperatures between 20° and 30°. A halo pattern was observed, which was believed to be due to the amorphous portion of the crystal. The degree of crystallinity of the crystalline metallosilicate was evaluated by the method described above and found to be 54%.

[0046] [Comparative Example 3] In Comparative Example 2, the crystalline metallosilicate used was the H-GaSi powder obtained in Preparation Example 1. The reaction was carried out in the same manner as in Comparative Example 2, except that the amount of the reaction mixture was 0.3 g. The liquid had a two-phase structure with crystalline metallosilicate as well. XRD analysis of the crystalline metallosilicate revealed that the crystalline metallosilicate was formed at an angle of 20° to 30°. A halo pattern was observed, which was believed to be due to the amorphous portion of the silicate. The degree of crystallinity of the crystalline metallosilicate was evaluated by the same method as in 3 and was found to be 68%. .

[0047] [Example 4] As a plastic decomposition device, a semi-flow type decomposition device as shown in Figure 2 was used. 41 is as shown in Figure 3, with an inner diameter of 7.3 mm, a length of 248 mm, and a capacity of approximately 10 mL. The Inconel tube with a maximum operating temperature of 450°C and a maximum operating pressure of 30MPa was used. The metal rod 43 has an outer diameter of 2 mm and a length of 220 mm. The gear-shaped partition plate is 1 It is attached at 72 mm, and its shape is 7 mm in tip diameter and 1.3 mm in pitch. . The reaction tube 41 was charged with the raw material polypropylene (Sigma-Aldrich, product number 182 After adding 2.5 g of 389), a metal rod 43 equipped with a partition plate was inserted into the reaction tube 41. 0.9 g of the Ga / ZSM-5 compact obtained in Preparation Example 3 was placed into the opposite side of the reaction tube 41. 41 is connected to the device, and the nitrogen gas cylinder 21a is pressurized to a maximum pressure of 10 MPa or more to prevent pressure leakage. After confirming that there was no gas, the pressure was slowly released. The pressure was increased to 1 MPa using carbon dioxide cylinder 21b. After repeating the depressurization and returning to normal pressure three times, carbon dioxide was gently pumped into the device at normal pressure for about 3 minutes. The internal atmosphere was replaced by flowing for 0 seconds. After the inside of the apparatus was replaced with carbon dioxide, the inlet valve 22b and the back pressure valve 31 were closed. The reaction tube 27 and the reaction tube 25 were placed in an electric furnace 29, and the temperature was increased at a rate of 10° C. per minute. As the temperature began to rise, valve 22b was opened to introduce carbon dioxide into the device at a rate of 0. The flow rate of the high pressure pump 23 was appropriately adjusted so that the pressure could be increased at a rate of 25 MPa. When the specified conditions (decomposition temperature: 430°C, decomposition pressure: 10MPa) are reached, high-pressure pump 2 Set the flow rate of 3 to 2.5 mL / min, and slowly open the back pressure valve 31 to maintain a predetermined pressure. The reaction was started when carbon dioxide was discharged from the back pressure valve 31, and the reaction was continued for a predetermined time. (Retention time: 60 minutes) The discharged liquid was collected in a trap bottle 32 and the gas was collected in a gas bag 34. After the retention was completed, the flow was stopped and the back pressure valve 31 was closed. 7 was taken out of the electric furnace 29 and cooled by blowing air. When the temperature inside the reaction tube became 40° C. or lower, the back pressure valve was closed. Fully open valve 31 to release the residual pressure in the device and trap any gas or liquid remaining in the device. The collected liquid was collected in the bottle 32 and the gas bag 34. After the pressure in the apparatus returned to normal, the collected liquid was collected in the trap bottle 32 and the gas bag 34. The box 34 was removed from the apparatus and weighed. The reaction tube 27 was removed from the apparatus and the contents were collected. The contents were only crystalline metallosilicate. The resin was carbonized on the wall of the reaction tube. No solid matter that would have formed was observed by visual inspection. The collected gas was analyzed by GC-FID and the collected gas was analyzed by the method described above. The weight of the gas and liquid collected was 1.88 kg of gas and liquid hydrocarbons. g. The yield of gas and liquid hydrocarbons recovered by the following method was calculated. , 75.2wt%.

[0048] <Gas and liquid hydrocarbon yield> Yield of gas and liquid hydrocarbons = 100 x (weight of gas and liquid hydrocarbons recovered) / (weight of polypropylene charged into the reaction tube)

[0049] [Comparative Example 4] The same plastic decomposition device as in Example 4 was used. The reaction tube 41 was charged with polypropylene (Sigma-Aldrich, product number 18 After adding 2.5 g of 2389), a metal rod 43 equipped with a partition plate was inserted into the reaction tube 41. 0.9 g of the Ga / ZSM-5 compact obtained in Preparation Example 3 was placed into the opposite side of the reaction tube 41. The pipe 41 is connected to the device, and the nitrogen gas cylinder 21a is pressurized to a maximum pressure of 10 MPa or more to prevent pressure leakage. After confirming that there was no leakage, the pressure was slowly released. Pressurize the tank to 1MPa with nitrogen, release the pressure, and return to normal pressure. After repeating the returning operation three times, nitrogen was gently passed through the device at normal pressure for about 30 seconds to adjust the internal atmosphere. I replaced my mind. After replacing the inside of the apparatus with nitrogen, the inlet valve 22a and the back pressure valve 31 were closed. The reaction tube 27 was then placed in an electric furnace 29, and heating was started at a rate of 10° C. per minute. When the predetermined condition (decomposition temperature: 430° C.) was reached, the back pressure valve 31 was slowly opened. After valve 31 is fully opened, valve 22a is opened to allow nitrogen to flow, and this point is regarded as the start of the reaction. After holding for a specified time (holding time: 60 minutes), the discharged liquid is collected in a trap bottle 32 and the gas is collected in a gas bubbler 33. After the retention was completed, the flow was stopped and the back pressure valve 31 was closed. The reaction tube 27 and the reaction tube 5 were taken out of the electric furnace 29 and cooled by blowing air. When this happens, the back pressure valve 31 is fully opened to release the residual pressure in the device, and the gas and The liquid was also collected in the trap bottle 32 and the gas bag 34. After the pressure in the apparatus returned to normal pressure, The flask 32 and the gas bag 34 were removed from the apparatus and weighed. The reaction tube 27 was removed from the apparatus. The contents were collected. In addition to the crystalline metallosilicate, the contents contained resin on the wall of the reaction tube. The solid matter that seemed to have been carbonized was visually observed. The collected gas was analyzed by GC-FID and the collected gas was analyzed by GC-FID. The weight of the gas and liquid was measured and the amount of gas and liquid hydrocarbons was 0.90 g. The yields of gas and liquid hydrocarbons recovered in the same manner as in Example 4 were also determined. The result was 36.0 wt%.

[0050] [Table 1]

[0051] As is clear from the results in Table 1, poly(H-GaSi) synthesis was achieved using supercritical carbon dioxide in the presence of H-GaSi. In the decomposition reaction of ethylene, the product was larger than that without the addition of crystalline metallosilicate. The yields of low molecular weight organic compounds, benzene, toluene, and xylene in the reaction were improved. It became clear that the product ratio could be controlled by changing the temperature, reaction pressure, and reaction time. I did.

[0052] [Table 2]

[0053] As is clear from the results in Table 2, when supercritical carbon dioxide was selected as the treatment medium, In the case of the treatment medium, the crystallinity of the crystalline metallosilicate was maintained at 100% even after the reaction. When supercritical water is selected as the medium, the crystallinity of the crystalline metallosilicate after the reaction is has decreased.

[0054] [Table 3]

[0055] As is clear from the results in Table 3, when supercritical carbon dioxide was selected as the treatment medium, In this case, the generation of solid matter on the reaction tube wall is suppressed compared to when nitrogen gas is selected. This resulted in higher yields of gas and liquid hydrocarbons. [Industrial Applicability]

[0056] According to the plastic decomposition method of the present invention, useful plastics are decomposed using used plastics as raw materials. The crystalline metallosilane used as the catalyst in this process is The crystallinity of the crystalline structure is not reduced by the processing medium, so the yield is high in continuous production. In addition, the use of a subcritical or supercritical treatment medium can contribute to the improvement of the stability of the treatment. When carbon dioxide is used, the reactivity of the treatment medium is low, and therefore it is easy to recycle the treatment medium. As described above, the method for decomposing plastics of the present invention is capable of extracting low molecular weight substances from used plastics. It is a technology that can produce organic matter and enable chemical recycling, and has industrial value. The value is great, and the technology is also extremely effective in terms of environmental conservation. [Explanation of symbols]

[0057] 10a: Nitrogen gas cylinder 10b; Carbon dioxide cylinder 11a, 11b, 11c, 11d; valves 12;High pressure pump 13. Pressure gauge 14;Metal mesh filter 15. High pressure vessel 16;Temperature controller with thermocouple 17; Electric furnace 18;Cooler 19; Gas bag 21a; Nitrogen gas cylinder 21b; Carbon dioxide cylinder 22a, 22b, 22c; Valves 23;High pressure pump 24; Pressure gauge 25; Preheating tube 26; Check valve 27; Reaction tube 28;Temperature controller with thermocouple 29; Electric furnace 30;Cooler 31; Back pressure valve 32; Cooling trap bottle 33;Wet gas meter 34; Gas bag 41: Reaction tube 42; Metal mesh filter 43: Metal rod with gear-shaped partitions ​​

Claims

1. The presence of crystalline metallosilicates and non-hydroxylic processing media in the sub- or supercritical state 2. A method for decomposing plastics, comprising heating plastics under the conditions described above and decomposing the plastics.

2. The method of claim 1, wherein the heating temperature is 300° C. or more and 550° C. or less. How to solve it.

3. The crystalline metallosilicate comprises a zeolite and / or a gallosilicate.

3. The method for decomposing plastics according to claim 1 or 2.

4. The plastic according to claim 1 or 2, wherein the crystalline metallosilicate has an MFI structure. How to disassemble the block.

5. The decomposition product obtained by the decomposition contains 45 wt % or more of organic matter having a carbon number of 2 to 12. The method for decomposing plastics according to claim 1 or 2.

6. The decomposition product obtained by the decomposition is at least one of the group consisting of benzene, toluene and xylene. The method for decomposing plastics according to claim 1 or 2, further comprising the step of:

7. 3. The method according to claim 1 or 2, wherein the plastic comprises polyethylene and / or polypropylene. A method for decomposing the plastic described above.

8. The method for decomposing plastics according to claim 1 or 2, wherein the treatment medium is carbon dioxide.

Citation Information

Patent Citations

  • Electroconductive resin composition, method for manufacturing same and molded article obtained therefrom

    CN110325595A

  • A method for converting hydrocarbon materials into a fluid hydrocarbon product containing p-xylene.

    JP2015519377A

  • Method For Purification of Depolymerized Polymers Using Supercritical Fluid Extraction

    US20200087479A1

  • Method for gasifying organic substance

    JP2009030071A

  • JP279762A