Method for producing noble metal nanoparticles

By adsorbing noble metal ions onto yeast and using controlled reducing agents, the method effectively forms nanoparticles on the yeast surface, facilitating easy separation and reducing costs, addressing the challenge of internal nanoparticle formation in yeast cells.

JP2024140136AInactive Publication Date: 2024-10-10MITSUBISHI MATERIALS CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023051140
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing noble metal nanoparticles using yeast result in nanoparticles being predominantly formed inside the yeast cells, making separation difficult and costly due to the need for expensive enzyme treatment to break the cell wall.

Method used

A method involving the adsorption of noble metal ions onto the surface of yeast, followed by the addition of a reducing agent like hydroxylamine, ascorbic acid, or hydrogen peroxide at controlled pH and temperature to form nanoparticles on the yeast surface, allowing easy separation without enzyme treatment.

Benefits of technology

Enables efficient and cost-effective separation of noble metal nanoparticles from yeast, reducing the need for expensive enzyme-based cell wall destruction and ensuring nearly all nanoparticles are formed on the yeast surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140136000001_ABST
    Figure 2024140136000001_ABST
Patent Text Reader

Abstract

To provide a method for producing noble metal nanoparticles which is capable of efficiently separating noble metal nanoparticles created by using yeast from yeast at a low cost.SOLUTION: A method for producing noble metal nanoparticles has: a noble metal adsorption process in which yeast is added to solution containing noble metal ion, and the solution is stirred to allow a surface of the yeast to adsorb noble metal; and a nanoparticulation process in which reducing agent is added to the yeast on which noble metal has been adsorbed to create noble metal nanoparticles being particles of nanometer size of the noble metal on the surface of the yeast, where the reducing agent includes at least one kind of hydroxylamine, ascorbic acid, formic acid and hydrogen peroxide.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing precious metal nanoparticles, which comprises generating precious metal nanoparticles from a solution containing precious metal ions. [Background technology]

[0002] Noble metal nanoparticles, which are made by forming noble metals (Au, Ag, Pt, Pd, Rh, Ir, Ru, Os) into nano-sized particles, are increasingly being used in fields such as catalysts, biosensors, memory, medical materials, antibacterial materials, etc. Waste materials containing noble metals are attracting attention as a stable source of supply of such noble metal nanoparticles. For example, Patent Document 1 discloses a precious metal recovery method in which yeast is added to a waste-derived precious metal eluate to adsorb the precious metal, and then a reducing agent is added to the yeast with the adsorbed precious metal to produce precious metal nanoparticles. Furthermore, for example, Patent Documents 2 and 3 disclose a method for producing metal nanoparticles using microorganisms as a reaction field without using chemical reducing agents, which produces metal nanoparticles by utilizing the unique reducing action of microorganisms, known as biomineralization. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2023-004079 A [Patent Document 2] JP 2018-035413 A [Patent Document 3] JP 2017-020100 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, it has been confirmed that most of the precious metal nanoparticles produced in the methods for producing precious metal nanoparticles using yeast as disclosed in Patent Documents 1 to 3 are produced inside the yeast. That is, it is believed that precious metal ions are adsorbed on the surface of the yeast, and then the precious metal ions are taken into the cell wall of the yeast over time, and then reduction of the precious metal ions begins, producing precious metal nanoparticles inside the cell wall of the yeast.

[0005] When the precious metal nanoparticles are taken up inside the yeast, a process of breaking the yeast cell wall to separate the cell components from the precious metal nanoparticles is required when separating the precious metal nanoparticles from the yeast. However, when physically breaking the cell wall, the precious metal nanoparticles and the cell components are tightly bound and mixed together, making separation very difficult. On the other hand, when chemically breaking the cell wall, it is necessary to use expensive enzymes such as zymolyase for yeast, which increases the cost of separation.

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a method for producing precious metal nanoparticles that enables the precious metal nanoparticles produced using yeast to be separated from the yeast efficiently and at low cost. [Means for solving the problem]

[0007] In order to solve the above problems, a method for producing precious metal nanoparticles according to one embodiment of the present invention proposes the following means. (1) A method for producing precious metal nanoparticles according to aspect 1 of the present invention includes a precious metal adsorption step of adding yeast to a solution containing precious metal ions and stirring the solution to adsorb the precious metal onto the surface of the yeast, and a nanoparticle formation step of adding a reducing agent to the yeast to which the precious metal has been adsorbed to produce precious metal nanoparticles, which are nanometer-sized particles of the precious metal, on the surface of the yeast, wherein the reducing agent includes at least one of hydroxylamine, ascorbic acid, formic acid, and hydrogen peroxide.

[0008] (2) A second aspect of the present invention is characterized in that in the method for producing precious metal nanoparticles according to the first aspect, the nanoparticle formation step is carried out within 48 hours after the completion of the precious metal adsorption step.

[0009] (3) Aspect 3 of the present invention is characterized in that, in the method for producing precious metal nanoparticles of aspect 1 or 2, the nanoparticle formation step comprises heating the yeast or the reducing agent having the precious metal adsorbed on its surface to a temperature in the range of 30°C or higher and lower than 100°C.

[0010] (4) A fourth aspect of the present invention is characterized in that, in the method for producing precious metal nanoparticles according to any one of the first to third aspects, the yeast includes one or more species of the genera Saccharomyces, Zygosaccharomyces, Schizosaccharomyces, and Debaryomyces.

[0011] (5) A fifth aspect of the present invention is characterized in that, in the method for producing precious metal nanoparticles according to any one of the first to fourth aspects, the precious metal includes one or more of gold, platinum, silver, palladium, rhodium, iridium, ruthenium, and osmium.

[0012] (6) A sixth aspect of the present invention is the method for producing precious metal nanoparticles according to any one of the first to fifth aspects, characterized in that the precious metal nanoparticles have an average particle diameter in the range of 1 nm or more and 100 nm or less.

[0013] (7) A seventh aspect of the present invention is the method for producing precious metal nanoparticles according to any one of the first to sixth aspects, characterized in that the nanoparticle formation step is carried out in an acidic condition of pH-3 to 4. Effect of the Invention

[0014] According to the present invention, it is possible to provide a method for producing precious metal nanoparticles, which enables precious metal nanoparticles produced using yeast to be separated from the yeast efficiently at low cost. [Brief description of the drawings]

[0015] [Figure 1] 1 is a flow chart showing a step-by-step method for producing precious metal nanoparticles according to an embodiment of the present invention. [Diagram 2] 1 is a TEM image showing the results of Example 1 of the present invention. [Diagram 3] 1 is a TEM image showing the results of Example 2 of the present invention. [Figure 4] 1 is a TEM image showing the results of Example 3 of the present invention. [Diagram 5] 1 is a TEM image showing the results of Example 4 of the present invention. [Figure 6] 1 is a TEM image showing the results of Comparative Example 1. [Figure 7] 4 is a TEM image showing the results of Comparative Example 2. [Figure 8] 1 is a TEM image showing the results of Comparative Example 3. [Figure 9] 1 is a TEM image showing the results of Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, a method for producing precious metal nanoparticles, which is one embodiment of the present invention, will be described with reference to the drawings. Note that the embodiment shown below is specifically described to better understand the gist of the invention, and does not limit the present invention unless otherwise specified.

[0017] FIG. 1 is a flow chart showing a step-by-step method for producing precious metal nanoparticles according to one embodiment of the present invention. In the method for producing precious metal nanoparticles of this embodiment, a series of procedures for separating and recovering precious metals from, for example, a circuit board of an electronic device (a material containing precious metals) and forming the recovered precious metals into nanoparticles will be described. The circuit board of an electronic device contains precious metals such as Au, Ag, etc. in the soldered portions and wiring. Note that the precious metals in this embodiment refer to the following eight elements: gold, platinum, silver, palladium, rhodium, iridium, ruthenium, and osmium.

[0018] In the method for producing precious metal nanoparticles of this embodiment, first, a solution containing precious metal ions (hereinafter referred to as a precious metal solution) is prepared. Such a precious metal solution can be obtained, for example, by treating a circuit board of an electronic device in which precious metals such as gold, silver, and platinum are used in soldering points and wiring with hydrochloric acid and hydrogen peroxide, and then dissolving it with aqua regia. In particular, by using recycled raw materials such as discarded circuit boards, the precious metal solution can be obtained at low cost.

[0019] Yeast is added to the precious metal solution thus obtained and stirred, and the precious metal ions contained in the precious metal solution are adsorbed onto the surface of the yeast (precious metal adsorption step S1). In the precious metal adsorption step S1, yeast is added to the precious metal solution and stirred. In this precious metal adsorption step S1, the yeast comes into contact with the precious metal ions contained in the precious metal solution, and the precious metal ions are adsorbed onto the surface of the yeast.

[0020] The amount of yeast added in the precious metal adsorption step S1 may be in the range of 0.004 to 39 times the mass of the precious metal contained in the precious metal solution. The mass of the precious metal contained in the precious metal solution may be measured in advance using an ICP optical emission spectrometer, an absorptiometer, or the like.

[0021] The yeast used in the precious metal adsorption step S1 may be any yeast capable of adsorbing precious metal ions. Examples of yeasts that can be used in this embodiment include yeasts of the genus Saccharomyces, Torulopsis, Zygosaccharomyces, Schizosaccharomyces, Pichia, Yarrowia, Hansenula, Kluyveromyces, Debaryomyces, Geotrichum, Wickerhamia, Fellomyces, and Sporobolomyces. Among these, yeasts of the genus Saccharomyces, Zygosaccharomyces, Schizosaccharomyces, and Debaryomyces are particularly preferred.

[0022] Yeasts of the genus Saccharomyces are representative of budding yeasts, and may be, for example, S. bayanus, S. boulardii, S. bulderi, S. cariocanus, S. cariocus, S. cerevisiae, S. chevalieri, S. dairenensis, S. ellipsoideus, S. florentinus, S. kluyveri, S. martiniae, S. monacensis, S. norbensis, S. paradoxus, S. pastorianus, S. spencerorum, S. turicensis, S. unisporus, S. uvarum, or S. zonatus.

[0023] The genus Zygosaccharomyces is a salt-tolerant yeast, and is isolated from miso and soy sauce, and may be, for example, Z. rouxii. The genus Schizosaccharomyces is a fission yeast, and may be, for example, S. cryophilus, S. japonicus, S. octosporus, or S. pombe. Another preferred yeast is Debaryomyces hansenii, deposited under the accession number NITE BP-01780 (Patent Microorganism Deposit Center, National Institute of Technology and Evaluation, Room 122, 2-5-8 Kazusa Kamatari, Kisarazu City, Chiba Prefecture, Japan).

[0024] The yeast used in the precious metal adsorption step S1 may be a live yeast, or may be a dead yeast as long as it can exert the function of reducing precious metal ions.

[0025] There are no particular limitations on the pH or temperature of the liquid obtained by adding yeast to the precious metal solution. For example, the pH may be from -3 to 7, which is strongly acidic to neutral. The temperature is 10°C or higher and 45°C or lower, and preferably 20°C or higher and 35°C or lower.

[0026] The time for performing the precious metal adsorption step S1 may be, for example, within a range of 4 hours or less as the time for stirring after adding yeast to the precious metal solution. If the stirring time exceeds 4 hours, there is a concern that the precious metal ions contained in the precious metal solution may penetrate into the yeast.

[0027] Next, the yeast-added precious metal solution is subjected to solid-liquid separation by filtration or the like, and the solid phase (yeast with precious metal ions attached to its surface) is washed with ion-exchanged water or pure water. For example, washing is preferably performed about three times by changing the washing water.

[0028] Then, a reducing agent is added to the yeast (solid phase) having precious metal ions attached to its surface after solid-liquid separation to produce precious metal nanoparticles (nanoparticle formation step S2). The reducing agent used in the nanoparticle formation step S2 includes at least one of hydroxylamine (NH2OH), L-ascorbic acid, formic acid (CH2O2), and hydrogen peroxide (H2O2).

[0029] Hydroxylamine is a chemically unstable crystalline form and is therefore used in the form of an aqueous solution. Furthermore, the formic acid may have a concentration of 90% by mass or more, or may be in the form of an aqueous solution.

[0030] In this embodiment, an aqueous solution of hydroxylamine hydrochloride is used as the reducing agent in the nanoparticle formation step S2.

[0031] The nanoparticle forming step S2 is preferably started within 48 hours after the completion of the previous precious metal adsorption step S1. It is more preferable to start within 24 hours. If the nanoparticle forming step S2 is started more than 48 hours after the completion of the precious metal adsorption step S1, there is a concern that too many precious metal ions will be taken into the yeast. In addition, there is a concern that the precious metal ions will be reduced by the reducing properties of the yeast itself, resulting in the generation of coarse particles of precious metals with particle sizes larger than nano size.

[0032] In the nanoparticle forming step S2, a reducing agent is added to the yeast having precious metal ions attached to its surface, and then the mixture is stirred for, for example, 2 hours or less. If the stirring is continued for more than 2 hours, the reduction of the precious metal ions will not proceed any further, and there is a concern that the precious metal precipitated by reduction will become coarse particles of precious metal with a particle size larger than nano size.

[0033] In the nanoparticle forming step S2, the liquid temperature of the yeast having the precious metal adsorbed on its surface and the reducing agent is preferably in the range of 30° C. or higher and lower than 100° C. By setting the temperature in the nanoparticle forming step S2 in the range of 30° C. or higher and lower than 100° C., the precious metal ions can be efficiently reduced without lowering the reducing ability of the reducing agent and without boiling the reducing agent. The pH of the liquid in the nanoparticle forming step S2 may be acidic, and may be, for example, strongly acidic to weakly acidic, from -3 to 4.

[0034] In this way, precious metal nanoparticles having an average particle size in the range of 1 nm to 100 nm are reduced and generated on the surface of the yeast that has been subjected to the nanoparticle formation step S2. Almost all of these precious metal nanoparticles are formed on the surface of the yeast, and almost none are generated inside the yeast.

[0035] Thereafter, the yeast with precious metal nanoparticles formed on its surface and the reducing agent are subjected to solid-liquid separation by filtration or the like, and then ion-exchanged water or pure water is added to the solid phase (yeast with precious metal nanoparticles formed on its surface) and stirred, whereby the yeast and the precious metal nanoparticles can be easily separated.

[0036] As described above, in the method for producing precious metal nanoparticles of the embodiment, a reducing agent containing at least one of hydroxylamine, ascorbic acid, formic acid, and hydrogen peroxide is added to yeast having adsorbed precious metal ions to reduce the precious metal ions, so that the precious metal is selectively reduced and produced on the surface of the yeast, and is hardly produced inside the yeast.

[0037] This makes it possible to separate the yeast from the generated precious metal nanoparticles by a simple method such as stirring and washing the yeast after the precious metal reduction. Therefore, there is no need for a costly and laborious separation process, such as decomposing the yeast cell wall using expensive enzymes and extracting the precious metal generated inside the enzyme, as in the conventional method. Therefore, it becomes possible to efficiently recover precious metal nanoparticles from a precious metal solution at low cost using enzymes.

[0038] Although the embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope of the invention and its equivalents as described in the claims, as well as in the scope and spirit of the invention. EXAMPLES

[0039] The effect of the present invention was verified. (Example 1 of the present invention) As a precious metal solution, an aqueous solution of chloroauric acid (concentration: 1.88 mM / L) was prepared. In addition, yeast was dispersed in water to prepare a yeast suspension (yeast species: Saccharomyces cerevisiae), concentration: 3.0 × 10 8 Then, 1.3 mL of the yeast suspension was added to 40 mL of the precious metal solution and stirred at room temperature (25°C) for 2 hours to adsorb gold ions onto the yeast surface (precious metal adsorption step).

[0040] After this, the mixture was centrifuged for 5 minutes in a centrifuge to separate the precipitate (yeast with gold ions adsorbed). Then, this precipitate A was washed three times by adding ultrapure water and centrifuging it to separate the precipitate A. After that, the washed precipitate A was dispersed in 100 mL of ultrapure water to obtain a dispersion A of yeast with gold ions adsorbed on its surface.

[0041] Then, within 1 hour after the precious metal adsorption step was completed, 20 mL of the yeast dispersion A described above and 40 mL of a hydroxylamine hydrochloride aqueous solution (concentration: 5% by mass) as a reducing agent were added to 340 mL of ultrapure water, and the liquid temperature was kept at 80° C. and stirred for 1 hour (nanoparticle formation step). Note that the liquid pH after the addition of the hydroxylamine hydrochloride aqueous solution was 3.4 (pH 4.9 before the addition).

[0042] After this, the mixture was centrifuged for 5 minutes in a centrifuge to separate the precipitate (yeast with gold nanoparticles formed on its surface). Then, this precipitate B was washed three times by adding ultrapure water and centrifuging it to separate the precipitate B. After that, the washed precipitate B was dispersed in 100 mL of ultrapure water to obtain a dispersion B of yeast with gold nanoparticles formed on its surface.

[0043] A TEM image of the yeast dispersion B obtained as described above is shown in FIG. As shown in Figure 2, it was confirmed that the gold nanoparticles (black dots) were only attached to the surface of the yeast, and no gold nanoparticles were produced inside the yeast. This confirmed that gold nanoparticles were produced in the yeast contained in yeast dispersion B.

[0044] (Example 2 of the present invention) The procedure was the same as in Example 1 of the present invention, except that 40 mL of a formic acid aqueous solution (concentration: 5% by mass) was added as a reducing agent, and the liquid temperature was kept at 80°C and stirred for 1 hour. The pH after addition of the formic acid aqueous solution (reducing agent) was 2.38. Figure 3 shows a TEM image of the yeast dispersion obtained in the above manner. As shown in Figure 3, it was confirmed that gold nanoparticles (black dots) were formed only on the surface of the yeast and attached thereto, and that no gold nanoparticles were formed inside the yeast.

[0045] (Example 3 of the present invention) The procedure was the same as in Example 1 of the present invention, except that 40 mL of an aqueous hydrogen peroxide solution (concentration: 5% by mass) was added as a reducing agent, and the liquid temperature was kept at 80°C and stirred for 1 hour. The pH after addition of the aqueous hydrogen peroxide solution (reducing agent) was 3.77. Figure 4 shows a TEM image of the yeast dispersion obtained in the above manner. As shown in Figure 4, it was confirmed that gold nanoparticles (black dots) were formed only on the surface of the yeast and attached thereto, and that no gold nanoparticles were formed inside the yeast.

[0046] (Example 4 of the present invention) The procedure was the same as in Example 1 of the present invention, except that 40 mL of an aqueous ascorbic acid solution (concentration: 5% by mass) was added as a reducing agent, and the liquid temperature was kept at 80°C and stirred for 1 hour. The pH after addition of the aqueous ascorbic acid solution (reducing agent) was 2.87. A TEM image of the yeast dispersion obtained in the above manner is shown in FIG. 5. It was confirmed from FIG. 5 that gold nanoparticles (black dots) formed only on the surface of the yeast and were attached thereto, and that no gold nanoparticles were formed inside the yeast.

[0047] Comparative Example 1 The procedure was the same as in Example 1 of the present invention, except that 40 mL of an aqueous sodium ascorbate solution (concentration: 5% by mass) was added as a reducing agent, and the liquid temperature was kept at 80°C and stirred for 1 hour. The pH after addition of the aqueous ascorbic acid solution (reducing agent) was 6.65. A TEM image of the yeast dispersion obtained as described above is shown in FIG. 6. As shown in FIG. 6, since no gold nanoparticles were generated on the surface of the yeast and the contrast inside the yeast was high, it is believed that gold nanoparticles were generated and aggregated inside the yeast.

[0048] Comparative Example 2 The procedure was the same as in Example 1 of the present invention, except that 40 mL of an aqueous solution of sodium borohydride (concentration: 5% by mass) was added as a reducing agent, and the liquid temperature was kept at room temperature (25°C) and stirred for 1 hour. The pH after the addition of the aqueous solution of sodium borohydride (reducing agent) was 10.3. The TEM image of the yeast dispersion obtained in the above manner (Comparative Example 2) is shown in FIG.

[0049] According to FIG. 7, since no gold nanoparticles were generated on the surface of the yeast and the contrast inside the yeast was high, it is believed that gold nanoparticles were generated and aggregated inside the yeast.

[0050] Comparative Example 3 The procedure was the same as in Example 1 of the present invention, except that 40 mL of an aqueous sodium formate solution (concentration: 5% by mass) was added as a reducing agent, and the liquid temperature was kept at 80° C. and stirred for 1 hour. The pH after the addition of the aqueous sodium formate solution (reducing agent) was 7.6. A cross-sectional TEM image of yeast cells in the yeast dispersion thus obtained (Comparative Example 3) is shown in FIG.

[0051] FIG. 8 clearly shows that gold nanoparticles are not produced on the surface of the yeast, but are produced inside the cell wall and in the protoplasm of the yeast.

[0052] Comparative Example 4 As a precious metal solution, 40 mL of an aqueous solution of chloroauric acid (concentration: 100 ppm) was prepared. Then, yeast (yeast species: Saccharomyces cerevisiae) was added in an amount 20 times the mass of gold contained in the aqueous solution of chloroauric acid, and the mixture was stirred for 10 minutes to allow gold ions to be adsorbed onto the surface of the yeast.

[0053] After that, the mixture was centrifuged for 5 minutes using a centrifuge to separate the precipitate (yeast adsorbing gold ions). Ultrapure water was added to the precipitate C, and the mixture was centrifuged, followed by washing to separate the precipitate C, which was repeated three times to obtain yeast adsorbing gold ions (Comparative Example 3). After that, the yeast (Comparative Example 3) was left to stand in the air for 9 days at room temperature (25°C) without adding a reducing agent. An SEM image of the yeast obtained in this manner (Comparative Example 4) is shown in FIG. 9.

[0054] According to Figure 9, when the yeast was left to stand for a long period of time, gold particles were precipitated on the surface of the yeast due to the reducing action of the yeast's own secretions, but the precipitated gold particles were larger than nano-sized and were aggregated triangular or hexagonal plate-like gold particles. Therefore, it was confirmed that gold nanoparticles cannot be formed from gold ions by the reducing action of the yeast itself. [Industrial Applicability]

[0055] The method for producing precious metal nanoparticles of the present invention can separate the produced precious metal nanoparticles from the yeast when recovering the precious metal from the precious metal solution using yeast, without destroying the cell wall of the yeast using expensive materials such as enzymes. This makes it possible to produce precious metal nanoparticles, which are increasingly being used in fields such as catalysts, biosensors, memories, medical materials, and antibacterial materials, at low cost using waste circuit boards containing precious metals as raw materials. Therefore, the method has industrial applicability.

Claims

1. A precious metal adsorption step of adding yeast to a solution containing precious metal ions and stirring the solution to adsorb precious metals onto the surface of the yeast; A nanoparticle forming process in which a reducing agent is added to the yeast to which the precious metal is adsorbed, to generate precious metal nanoparticles, which are nanometer-sized particles of the precious metal, on the surface of the yeast, The method for producing precious metal nanoparticles, wherein the reducing agent contains at least one of hydroxylamine, ascorbic acid, formic acid, and hydrogen peroxide.

2. 2. The method for producing precious metal nanoparticles according to claim 1, wherein the nanoparticle formation step is carried out within 48 hours after the completion of the precious metal adsorption step.

3. 3. The method for producing precious metal nanoparticles according to claim 1, wherein the nanoparticle formation step comprises heating the yeast or the reducing agent having the precious metal adsorbed on its surface to a temperature in the range of 30°C or higher and lower than 100°C.

4. 3. The method for producing precious metal nanoparticles according to claim 1, wherein the yeast includes one or more of the genera Saccharomyces, Zygosaccharomyces, Schizosaccharomyces, and Debaryomyces.

5. 3. The method for producing precious metal nanoparticles according to claim 1, wherein the precious metal includes one or more of gold, platinum, silver, palladium, rhodium, iridium, ruthenium, and osmium.

6. 3. The method for producing precious metal nanoparticles according to claim 1, wherein the precious metal nanoparticles have an average particle size in the range of 1 nm or more and 100 nm or less.

7. 3. The method for producing precious metal nanoparticles according to claim 1, wherein the nanoparticle formation step is carried out under an acidic condition of pH -3 to 4.

Citation Information

Patent Citations

  • High-performance wrench

    CN107893194A

  • Method for producing gold nanorod

    JP2009270128A

  • Method for recovering noble metal

    JP2023004079A

  • Bag for metal recovery, package boody for metal recovery and method for recovering metal

    JP2017020100A

  • Noble metal recovery method

    JP2018035413A