Electrolyte solution and electrochemical anticorrosion method

The use of specific electrolyte solutions with organic acid salts and alkyl sulfonates in an electrochemical method addresses ASR and chloride-induced corrosion in reinforced concrete, ensuring structural durability by reducing alkali ion concentration and chloride migration.

JP2024140668APending Publication Date: 2024-10-10DENKA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023051933
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing electrochemical methods for repairing reinforced concrete structures face issues with alkali-silica reaction (ASR) due to the accumulation of alkali metal ions at the cathode, leading to concrete expansion and reduced durability.

Method used

An electrolyte solution containing organic acid salts of carboxylates and alkyl sulfonates with 3 or less carbon atoms, preferably with alkaline earth metals, is used in conjunction with an electrochemical method to suppress ASR and chloride migration, maintaining a pH of 6.5 to 12.0 and concentration of 3 to 20% by mass, with direct current applied between external and internal electrodes.

Benefits of technology

The method effectively suppresses ASR and chloride-induced corrosion, maintaining concrete durability by reducing alkali ion concentration and chloride migration, thereby preventing concrete expansion and enhancing structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140668000001_ABST
    Figure 2024140668000001_ABST
Patent Text Reader

Abstract

To provide an electrolyte solution for use in an electrochemical anticorrosion method capable of preventing salt damage and ASR, and also to provide an electrochemical anticorrosion method.SOLUTION: The present invention provides an electrolyte solution for use in an electrochemical anticorrosion method. The electrolyte solution comprises at least one organic acid salt selected from carboxylates with 3 or fewer carbon atoms and alkyl sulfonates with 3 or fewer carbon atoms.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolyte solution and an electrochemical corrosion protection method. [Background technology]

[0002] Conventionally, reinforced concrete has generally been used for the construction of civil engineering structures such as roads and railways, specifically bridge substructures, bridge girders, underground structures such as tunnels, semi-underground structures, culverts, etc. This reinforced concrete is widely used as a structural material because it is possible to create a composite structure that has both compressive strength and tensile strength by combining concrete, which has high compressive strength performance, with reinforcing bars, which have high tensile strength performance. Structures using this reinforced concrete are known as PC structures, and there are many concrete structures in which PC steel materials (PC steel wires, PC steel bars, PC steel strands, etc.) are placed within the concrete.

[0003] By the way, if there is a large amount of chloride ions around steel materials such as reinforcing bars and prestressing steel in concrete, so-called salt damage occurs. In the case of concrete structures in coastal areas, salt damage occurs when seawater splashes onto the concrete surface, and the chloride ions penetrate the concrete due to the adsorption phenomenon of concrete or the concentration gradient, and reach the reinforcing bars. The chloride ions destroy the passive film of the reinforcing bars, causing corrosion. Furthermore, in past concrete structures, sea sand was sometimes used as fine aggregate, and in such cases, due to insufficient management, the chloride ions were not sufficiently removed, resulting in the presence of a large amount of chloride ions in the concrete, which resulted in the destruction of the passive film of the reinforcing bars and the start of corrosion. In addition, salt damage can also occur due to chloride-based antifreeze agents used in road management. As the above-mentioned deterioration phenomenon of reinforced concrete progresses, the durability of the composite structure will be significantly reduced.

[0004] Non-destructive electrochemical repair methods for deteriorated reinforced concrete have been proposed and implemented. For example, Patent Document 1 proposes an electrochemical treatment method for reinforced concrete in which an external electrode is provided on one side of a plate-like body, an electrode unit panel in which the entire area where the external electrode is provided is covered with an electrolyte solution retaining material is arranged side by side on the concrete surface to be treated, a reinforcing bar embedded in the concrete serves as an internal electrode, and a direct current is passed between the external and internal electrodes to cause chloride ions in the concrete to migrate to the external electrode side and be removed. As solutes of the electrolyte solution used in this electrochemical treatment method, carbonates, nitrates, nitrites, sulfates, borates, and hydroxides and chlorides of lithium, sodium, and potassium, as well as magnesium and calcium, are described. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6586000 Summary of the Invention [Problem to be solved by the invention]

[0006] By carrying out repairs using electrochemical methods such as the method disclosed in Patent Document 1, desalination of concrete structures can be carried out non-destructively and efficiently. However, in the electrochemical method, alkali metal ions such as sodium contained in concrete are attracted to the cathode in the concrete and accumulate around the reinforcing bars (steel materials) which are the cathode, which may initiate the alkali-silica reaction (hereinafter referred to as "ASR"). When ASR starts, the highly reactive silica inside the concrete reacts with the alkali to produce an alkali silicate gel, which absorbs water and expands, causing cracks in the concrete structure and reducing its durability.

[0007] In view of the above, an object of the present invention is to provide an electrolyte solution used in an electrochemical corrosion protection method that can suppress salt damage and ASR, and an electrochemical corrosion protection method. [Means for solving the problem]

[0008] As a result of intensive research to solve the above problems, the present inventors have come up with the following invention and found that the above problems can be solved. [1] An electrolyte solution used in an electrochemical corrosion protection method, the electrolyte solution comprising at least one organic acid salt selected from the group consisting of a carboxylate having 3 or less carbon atoms and an alkylsulfonate having 3 or less carbon atoms. [2] The electrolyte solution according to [1], wherein the organic acid salt contains an alkaline earth metal. [3] The electrolyte solution according to [1] or [2], having a pH of 6.5 to 12.0. [4] The electrolyte solution according to any one of [1] to [3], wherein the concentration of the electrolyte is 3 to 20 mass %. [5] An electrochemical corrosion protection method for reinforced concrete, in which an electrode installed on the surface side of the concrete is designated as an external electrode, a reinforcing bar buried inside the concrete is designated as an internal electrode, the internal electrode, an electrolyte solution retention material retaining the electrolyte solution described in any one of [1] to [4], and the external electrode are arranged in this order, and a direct current is passed between the external electrode and the internal electrode. Effect of the Invention

[0009] According to the present invention, it is possible to provide an electrolyte solution used in an electrochemical corrosion protection method capable of suppressing salt damage and ASR, and an electrochemical corrosion protection method. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a partial cross-sectional view showing an example of an electrochemical corrosion protection system used to implement an electrochemical corrosion protection method according to an embodiment of the present invention. [Diagram 2]FIG. 1 is a cross-sectional view of the side surface for explaining a test method in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Electrolyte solution] The electrolyte solution of the present invention is an electrolyte solution used in an electrochemical corrosion protection method, and contains at least one organic acid salt of a carboxylate having 3 or less carbon atoms and an alkylsulfonate having 3 or less carbon atoms as an electrolyte.

[0012] (Carboxylic acids with 3 or less carbon atoms) The electrolyte contained in the electrolyte solution of the present invention may be a carboxylate having 3 or less carbon atoms. Examples of the carboxylate having 3 or less carbon atoms include salts of formic acid, acetic acid, and propionic acid. Among these, propionate is preferred from the viewpoint of suppressing the expansion of ASR.

[0013] The carboxylate having 3 or less carbon atoms preferably contains an alkaline earth metal. Examples of the alkaline earth metal include Be, Mg, Ca, Sr, Ba, and Ra. Among them, Ca is preferred from the viewpoint of suppressing the expansion of ASR. Therefore, calcium propionate is preferred as the carboxylate having 3 or less carbon atoms.

[0014] (Alkyl sulfonate salts with 3 or less carbon atoms) As the electrolyte contained in the electrolyte solution of the present invention, an alkylsulfonate having 3 or less carbon atoms can be used. As the alkylsulfonate having 3 or less carbon atoms, salts of methanesulfonic acid, ethanesulfonic acid, 1-propanesulfonic acid, and 2-propanesulfonic acid can be used. Among them, ethanesulfonate is preferable from the viewpoint of suppressing the expansion of ASR.

[0015] In addition, the alkylsulfonate having 3 or less carbon atoms preferably contains an alkaline earth metal, similar to the carboxylate having 3 or less carbon atoms. Examples of the alkaline earth metal include Be, Mg, Ca, Sr, Ba, and Ra, and among these, Ca is preferred from the viewpoint of suppressing the expansion of ASR. Therefore, calcium ethanesulfonate is preferred as the alkylsulfonate having 3 or less carbon atoms.

[0016] The electrolyte solution of the present invention can suppress salt damage and ASR in concrete. Although the reason for this is not clear, it is presumed to be as follows. For example, calcium propionate has a relatively high solubility and a large ionic radius of propionate ion that is not fixed to a double salt with a hydrate. When such calcium propionate is added to water, in the early stage of hydration, OH - The counter ion in equilibrium changes from the highly soluble NaOH to the less soluble Ca(OH)2, so the OH in the electrolyte solution - In addition, calcium propionate has a large ionic radius of propionate ion, and is difficult to fix to hydrate, so it can remain in the liquid phase for a long time, and OH - Therefore, calcium propionate can maintain the effect of decreasing the concentration of OH from the early stage of hydration. - Since the reduction in concentration can be maintained for a long period of time, it is assumed that this has the effect of suppressing expansion due to ASR.

[0017] [ka]

[0018] In the above, an example is described in which calcium propionate is used as the electrolyte, but it is presumed that similar effects can be achieved with carboxylates having 3 or less carbon atoms and alkylsulfonates having 3 or less carbon atoms.

[0019] The electrolyte solution is prepared by dissolving the electrolyte in a solvent, preferably water. The pH of the electrolyte solution is preferably 6.5 to 12.0, more preferably 7.0 to 11.8, and even more preferably 7.5 to 11.5. By setting the pH within the above range, it is possible to suppress an increase in voltage, remove chlorine from the electrolyte solution, and suppress the expansion rate.

[0020] The electrolyte concentration is preferably 3% by mass or more and 20% by mass or less, more preferably 5% by mass or more and 18% by mass or less, and even more preferably 8% by mass or more and 15% by mass or less. By setting the electrolyte concentration within the above range, the pH can be set to 6.5 or more and 12.0 or less. In addition, the voltage rise can be suppressed, chlorine can be removed from the electrolyte solution, and the expansion rate can be suppressed.

[0021] [Electrochemical corrosion prevention method] In the electrochemical corrosion protection method of the present invention, an electrode placed on the surface side of the concrete is designated as the external electrode, a reinforcing bar buried inside the concrete is designated as the internal electrode, the internal electrode, an electrolyte solution holding material holding the above-described electrolyte solution, and an external electrode are arranged in this order, and a direct current is passed between the external electrode and the internal electrode.

[0022] The electrochemical corrosion protection method of the present invention uses a direct current to destroy, for example, chloride ions (Cl - ) can be removed by causing it to migrate to an external electrode (desalinization method), or an alkaline electrolyte solution can be electrically penetrated into the rebar inside the concrete to restore the alkalinity of neutralized concrete (re-alkalinization method). In addition, because corrosion of rebar progresses through an electrochemical reaction, by continuously passing a direct current through the rebar, the corrosion reaction of the rebar can be electrochemically suppressed, thereby improving the durability of the concrete structure (electrochemical protection method). Also, by electrophoresis of the electrolyte ions present in the electrolyte solution to the rebar (cathode) side, and depositing inorganic electrodeposits in the cracks and on the concrete surface, it is possible to seal cracks that have occurred in the concrete and densify the concrete surface (electrochemical deposition method).

[0023] Furthermore, according to the electrochemical corrosion protection method of the present invention, an electrolyte solution is used that contains, as an electrolyte, at least one organic acid salt of a carboxylate having 3 or less carbon atoms and / or an alkylsulfonate having 3 or less carbon atoms. This makes it possible to suppress expansion due to ASR and to suppress deterioration of concrete due to the occurrence of cracks.

[0024] In addition, the electrochemical corrosion prevention method can eliminate chloride ions (Cl - ) is removed by migrating to the external electrode, so the pH is reduced by implementing electrochemical corrosion protection methods. The pH of the electrolyte solution during the electrochemical corrosion protection method is preferably in the range of 6.5 to 12.0, which is the pH of the electrolyte solution described above, and more preferably 7.0 or more. More preferably, the pH is 11.8 or less, and even more preferably, 7.5 to 11.5. Since the pH of the electrolyte solution changes due to the electrochemical corrosion protection method, it is preferable to carry out the treatment while adjusting the pH to within the above range. When the pH of the electrolyte solution becomes low, the pH can be adjusted by preparing a new electrolyte solution to replace the low electrolyte solution. When the pH becomes high, the pH can be adjusted by diluting with water, for example.

[0025] [Electrochemical corrosion protection system] Next, a system used for carrying out the electrochemical corrosion protection method of the present invention will be described. Fig. 1 is a partial cross-sectional view showing an example of an electrochemical corrosion protection system used in the electrochemical corrosion protection method. The electrochemical corrosion protection system shown in Fig. 1 is an electrochemical corrosion protection system for reinforced concrete in which an electrode installed on the surface side of concrete 10 is an external electrode 20, a reinforcing bar (not shown) embedded inside the concrete 10 is an internal electrode, the internal electrode, an electrolyte retention material 22 retaining an electrolyte solution, the external electrode 20, and a protective substrate 24 are arranged in this order, and a direct current is passed between the external electrode 20 and the internal electrode.

[0026] As shown in FIG. 1, an electrolyte retaining material 22 holding an electrolyte solution, an external electrode 20, and a protective substrate 24 are arranged in this order to form an electrode unit panel 26, which is fixed, for example, by a plurality of crosspieces 30 on the outside of the protective substrate 24. In addition, a water supply hose 34 serving as an electrolyte supply pipe is provided and fixed between the two crosspieces 30. An electrolyte supply port (not shown) is provided at an arbitrary position of the water supply hose 34. In addition, a recovery pipe (not shown) having an electrolyte recovery port for recovering the electrolyte from the water supply hose 34 is also provided as appropriate. That is, the electrolyte solution is continuously or intermittently supplied to the electrolyte retention material from the electrolyte supply port of the water supply hose 34, and the electrolyte is then recovered by the recovery pipe (not shown).

[0027] In other words, it is preferable that the system has an electrolyte supply port provided at an arbitrary location and an electrolyte recovery port provided, and the electrolyte is continuously or intermittently supplied to the electrolyte retention material from the electrolyte supply port and the electrolyte is recovered from the electrolyte solution recovery port. With such a configuration, a stable supply of electrolyte is possible, and the effect of the system can be more easily exhibited.

[0028] The electrodes constituting the external electrodes are preferably made of titanium round bars, because they have excellent corrosion resistance and can be reused, and more preferably have their surfaces baked with iridium. The round bars preferably have a diameter of about 2 to 5 mm. Ordinary steel bars plated with titanium, titanium alloy, platinum, or the like may also be used.

[0029] The electrolyte solution holding material 22 may be a nonwoven fabric made of a hydrophilic material, a nonwoven fabric that has been treated to be hydrophilic, or a felt. The nonwoven fabric made of hydrophilic materials is a nonwoven fabric made from raw materials that have hydrophilic properties such as regenerated fibers such as rayon and cupra, and natural fibers such as cotton. A hydrophilically treated nonwoven fabric is a nonwoven fabric made from synthetic fibers such as olefins (such as polyethylene or polypropylene), polyesters, or polyamides, and is made hydrophilic by applying capillary action to the synthetic fibers, which are made to swell or become porous by a method such as polymerizing the synthetic fibers in the presence of a compound having a hydrophilic group (such as an oxidation product of polyethylene glycol) during the synthetic fiber manufacturing process, or by treating the synthetic fibers with a metal salt (such as stannous chloride), partially dissolving the surface to make it porous, and then depositing a metal hydroxide. Felt is made by compressing wool or other animal fibers into a sheet form.

[0030] The external electrode 20 and the reinforcing bar (internal electrode) embedded in the concrete are each connected to an electrode cable, allowing current to flow between the electrodes.

[0031] In the above state, a direct current (preferably 0.5 A / m per concrete surface area) is applied between the external electrode and the reinforcing bar (internal electrode) embedded in the concrete. 2 More preferably, 0.7 to 1.5 A / m 2 ) while supplying the electrolyte solution to the electrolyte supply pipe continuously or intermittently (intermittently).

[0032] Here, from the viewpoint of efficiently electropermeating the electrolyte into the concrete and removing the chloride ions inside the concrete by causing them to migrate to the external electrode side, it is preferable that the electrolyte solution be supplied intermittently. EXAMPLES

[0033] The present invention will be described in more detail below using examples and comparative examples. However, the present invention is not limited to the following examples and comparative examples as long as it does not deviate from the gist of the present invention.

[0034] <Experimental Example 1> Cylindrical specimens with a diameter of 100 mm and a length of 400 mm were prepared using concrete with the composition shown in Table 1 below and reinforcing bars with a diameter of 13 mm. The concrete was mixed with a Cl content of approximately 5 kg / m3 in order to confirm the elution of chlorine in each experiment. 3 The reagent NaCl was added so that the concrete was sealed and cured for 28 days before being used in the test.

[0035] [Table 1]

[0036] 2, in the electrical current test, a cylindrical specimen 46 was placed in a container 44 containing an electrolyte solution 42, and a titanium mesh 48 was further placed around the cylindrical specimen 46. A reinforcing bar 50 was used as an internal electrode, and the titanium mesh 48 was used as an external electrode, so that a direct current could be passed between them.

[0037] As an example, the electrolyte solution was prepared using calcium propionate and calcium ethanesulfonate to have the concentrations shown in Table 2. As a comparative example, calcium carbonate and lithium carbonate were used to have the concentrations shown in Table 2.

[0038] The DC power supply used a constant current method (a constant current value was applied), the voltage required to apply a specified current was measured, and the change in voltage over time was recorded and saved using a data logger. The current applied to the concrete was 1A / m per surface area of ​​the concrete. 2 It was decided.

[0039] Evaluation method Voltage (V): After a certain number of days had passed since the start of current flow, the potential difference between the anode and cathode was measured with a tester, and was recorded and stored with a data logger while current was being passed. Cl concentration: After a certain number of days had passed since the start of current application, about 5 ml of the electrolyte solution was sampled and the Cl concentration was measured using a potentiometric titrator and a chloride ion selective electrode. Accelerated expansion rate: Measured according to JCI-S-011-2017 Expansion rate measurement method for core samples of concrete structures. The accelerated expansion rate was measured after passing electricity through the concrete for 28 days, and then 100 and 300 days after the end of the electricity passage. The results are shown in Table 2.

[0040] [Table 2]

[0041] It was confirmed that in Test Nos. 1-1 and 1-2, which used calcium propionate and calcium ethanesulfonate as the electrolyte, a current could be passed at a lower voltage than in Test Nos. 1-3 and 1-4, which used potassium carbonate and lithium carbonate. In addition, the Cl concentration in the electrolyte solution after 14 days was higher in Test Nos. 1-1 and 1-2 than in Test Nos. 1-3 and 1-4, indicating that the chloride ions (Cl - It was confirmed that more of the ions were removed by migrating to the titanium mesh 48 side. Furthermore, in comparison with Test No. 1-3, it was confirmed that Test Nos. 1-1 and 1-2 were able to suppress the expansion rate and thus inhibit ASR.

[0042] (Test Example 2) The electrolyte solutions used were calcium propionate and calcium ethanesulfonate, and tests were performed by changing the pH and electrolyte concentration. The results are shown in Table 3.

[0043] [Table 3]

[0044] As shown in Table 3, in both examples using calcium propionate and calcium ethanesulfonate as the electrolyte, it was confirmed that the Cl concentration dissolved in the electrolyte solution could be increased and the expansion rate could be suppressed by increasing the pH and electrolyte concentration. In addition, although the voltage during current application increases by increasing the pH and electrolyte concentration, this is at a level that does not pose a problem in practical use. In this way, by increasing the pH and electrolyte concentration, the Cl removal rate can be increased and the expansion rate of the concrete can be suppressed. However, in order to suppress the voltage when a current is passed through the electrolyte, it is preferable to adjust the pH and concentration within a predetermined range. [Industrial Applicability]

[0045] INDUSTRIAL APPLICABILITY The present invention relates to an electrolyte solution and an electrochemical corrosion protection method that can be used for reinforced concrete having reinforcing bars inside, and can be suitably used for civil engineering construction structures such as roads and railways. [Explanation of symbols]

[0046] 10. Concrete 20 External electrode 22 Electrolyte retention material 24 Protection Board 26 Electrode unit panel 30 Crosspiece 34 Water supply hose 42 Electrolyte solution 44 Container 46 Cylindrical specimen 48 Titanium Mesh 50 Steel Bar

Claims

1. An electrolyte solution used in an electrochemical corrosion protection method, An electrolyte solution comprising at least one organic acid salt selected from the group consisting of a carboxylate having 3 or less carbon atoms and an alkylsulfonate having 3 or less carbon atoms as an electrolyte.

2. The electrolyte solution of claim 1 , wherein the organic acid salt comprises an alkaline earth metal.

3. 3. The electrolyte solution according to claim 1, wherein the pH is from 6.5 to 12.

0.

4. 3. The electrolyte solution according to claim 1, wherein the concentration of the electrolyte is 3 to 20 mass %.

5. 3. An electrochemical corrosion protection method for reinforced concrete, comprising the steps of: an electrode installed on the surface side of the concrete as an external electrode; a reinforcing bar buried inside the concrete as an internal electrode; arranging the internal electrode, an electrolyte solution retention material that retains the electrolyte solution according to claim 1 or 2, and the external electrode in this order; and passing a direct current between the external electrode and the internal electrode.

Citation Information

Patent Citations

  • Backfill for electric anticorrosion, and electric anticorrosion structure of concrete construction

    JP2015120950A

  • Method for suppressing alkali aggregate reaction in cement hardened body

    JP2021066610A

  • Electrochemical treatment method for reinforced concrete and electrode unit panel therefor

    JP6586000B2