Silver removal method from aqueous nickel chloride solution
The method addresses the challenge of stabilizing copper and silver removal in the MCLE process by employing controlled redox potential in two cementation steps, ensuring low silver concentrations and high-quality electrolytic nickel production.
Patent Information
- Application Number
- JP2023058135
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
The MCLE process struggles to stably reduce copper and silver concentrations in the final cementation solution due to varying impurity loads from different raw material sources, making it difficult to achieve target concentrations.
A method involving two cementation steps with controlled redox potential, using sulfide raw materials to reduce copper ions and fix them as sulfides, and adjusting the oxidation-reduction potential of the second slurry to a specific range to efficiently remove silver from the nickel chloride solution.
This method effectively reduces silver concentration to below 0.05 mg/L, preventing contamination of electrolytic nickel and enhancing the quality of the final product.
Smart Images

Figure 2024145680000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a technique for removing silver contained in an aqueous nickel chloride solution, and more particularly to a method for removing silver from an aqueous nickel chloride solution in a cementation step of a nickel hydrometallurgical process. [Background technology]
[0002] In the nickel hydrometallurgy process (hereinafter referred to as the "MCLE process"), the raw materials, nickel matte and nickel-cobalt mixed sulfide (MS: mixed sulfide), are leached with chlorine, and the resulting leachate (chlorine leachate) is purified to remove impurities, and then nickel and cobalt are recovered in the form of electrolytic nickel and electrolytic cobalt in an electrolytic process.
[0003] As shown in FIG. 1, the chlorine leaching solution obtained from the chlorine leaching process is subjected to removal of excess copper in the copper removal electrolysis process provided between the cementation process and the cementation process, and impurities such as iron and arsenic are removed in the iron removal process, and then the solution is sent to the cobalt solvent extraction process. In the cobalt solvent extraction process, nickel and cobalt are separated by solvent extraction to obtain a crude nickel chloride solution (NiCl2) and a crude cobalt chloride solution (CoCl2). The crude nickel chloride solution is further purified by removing impurities in the solution purification process and sent to the nickel electrolysis process. Then, in the nickel electrolysis process, electrolytic nickel is produced by electrolytic winning. Meanwhile, the crude cobalt chloride solution is also further purified by removing impurities in the solution purification process and sent to the cobalt electrolysis process, where electrolytic winning is produced.
[0004] The MCLE process includes a cementation step to remove copper ions, which are impurities contained in the chlorine leachate (copper-containing nickel chloride aqueous solution) obtained by chlorine leaching.
[0005] In the cementation process, nickel and cobalt are leached from nickel matte and MS (hereinafter, these may be collectively referred to as "nickel sulfide raw material") by utilizing the oxidizing power of divalent copper ions contained in the chlorine leachate, and copper ions and silver ions contained in the chlorine leachate are distributed to the solid side by utilizing the reducing power of nickel matte and MS, and are removed. In this cementation process, a reduction process in which MS is added to a copper-containing nickel chloride aqueous solution to reduce copper ions in the solution from divalent to monovalent, and a sulfurization process in which nickel matte is added to a slurry obtained by the reduction process to fix the reduced monovalent copper ions as copper sulfide are configured to be performed in a total of n tanks (n is an integer of 4 or more) connected in series (for example, Patent Document 1). By undergoing such treatment in the cementation process, the copper ion concentration in the process liquid after the reaction (cementation end liquid) is reduced to a low concentration of 0.10 g / L or less, more preferably 0.05 g / L or less.
[0006] However, nickel sulfide raw materials to be treated in the MCLE process are processed using raw materials from various sources, and depending on the raw material processing composition, the load of various impurities may increase. This may also increase the amount of copper and silver to be removed. Therefore, it was sometimes difficult to stably reduce the copper and silver concentrations in the resulting cementation end solution to the target value. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2017-155281 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been proposed in view of the above circumstances, and has an object to provide a method for efficiently removing silver ions from an aqueous nickel chloride solution. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, they have found that silver can be efficiently removed by subjecting an aqueous nickel chloride solution containing copper and silver impurities to a cementation treatment consisting of a first cementation step in which copper ions are reduced from divalent to monovalent and a second cementation step in which the reduced monovalent copper ions are immobilized as sulfides, and controlling the oxidation-reduction potential of the slurry (second slurry) obtained through the second cementation step to fall within a specific range, thereby completing the present invention.
[0010] (1) A first aspect of the present invention is a method for removing silver from an aqueous nickel chloride solution containing copper and silver, comprising: a first cementation step of adding a sulfide raw material A containing nickel sulfide to the aqueous nickel chloride solution to reduce divalent copper ions in the aqueous nickel chloride solution to monovalent copper ions; and a second cementation step of adding a sulfide raw material B containing trinickel disulfide to a first slurry obtained in the first cementation step to fix the monovalent copper ions contained in the first slurry as sulfides, wherein the oxidation-reduction potential (based on a silver / silver chloride electrode) of the second slurry obtained in the second cementation step is controlled to be −100 mV or more and less than 0 mV.
[0011] (2) A second aspect of the present invention is a method for removing silver from an aqueous nickel chloride solution, wherein, in the first aspect of the invention, the redox potential of the second slurry (based on a silver / silver chloride electrode) is controlled to be −50 mV or more and less than 0 mV.
[0012] (3) A third aspect of the present invention is a method for removing silver from an aqueous nickel chloride solution according to the first or second aspect of the present invention, wherein a copper concentration in the aqueous nickel chloride solution is adjusted to control an oxidation-reduction potential of the second slurry.
[0013] (4) A fourth aspect of the present invention is the method for removing silver from an aqueous nickel chloride solution according to the third aspect of the present invention, wherein a copper concentration of the aqueous nickel chloride solution is adjusted to a range of 10 g / L to 50 g / L to control an oxidation-reduction potential of the second slurry.
[0014] (5) A fifth aspect of the present invention is a method for removing silver from an aqueous nickel chloride solution according to any one of the first to fourth aspects of the present invention, wherein the sulfide raw material A is a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material, and the sulfide raw material B is nickel matte produced by a pyrometallurgical method for nickel. Effect of the Invention
[0015] According to the present invention, a method for efficiently removing silver ions from an aqueous nickel chloride solution can be provided. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a process diagram showing a schematic flow of a nickel hydrometallurgical process (MCLE process). [Diagram 2] FIG. 1 is a flow chart showing a detailed flow of the MCLE process, and is an example of a process for producing electrolytic nickel. [Diagram 3] FIG. 2 is a process diagram showing the processing flow in the cementation process S2. [Figure 4] 1 is a graph showing the relationship between the oxidation-reduction potential (based on a silver / silver chloride electrode) of the second slurry obtained in the second cementation step S22 and the copper ion concentration and silver ion concentration in the final cementation solution. [Diagram 5] 1 is a graph showing the relationship between the oxidation-reduction potential (based on a silver / silver chloride electrode) of the second slurry obtained from the second cementation step S22 and the amount of nickel matte slurry added in the second cementation step S22. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, a specific embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail with reference to the drawings. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention.
[0018] ≪1. How to remove silver from nickel chloride solution≫ The method for removing silver according to the present embodiment is a method for removing silver from an aqueous nickel chloride solution containing copper and silver. For example, the aqueous nickel chloride solution may be a copper-containing aqueous nickel chloride solution (chlorine leachate) obtained by chlorine leaching of raw nickel sulfide in a nickel hydrometallurgy process (MCLE process).
[0019] Specifically, this method includes a first cementation step in which a sulfide raw material A containing nickel sulfide is added to an aqueous nickel chloride solution to reduce divalent copper ions in the aqueous nickel chloride solution to monovalent copper ions, and a second cementation step in which a sulfide raw material B containing trinickel disulfide is added to a first slurry obtained in the first cementation step to fix the monovalent copper ions contained in the first slurry as sulfides.
[0020] For example, sulfide raw material A may be a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material, and sulfide raw material B may be nickel matte produced by a nickel pyrometallurgical process.
[0021] The silver removal method according to this embodiment is characterized in that the redox potential (based on a silver / silver chloride electrode) of the second slurry obtained in the second cementation process is controlled to be within a specific range.
[0022] According to such a method, silver, which is an impurity, can be efficiently removed from the nickel chloride aqueous solution. By subjecting the nickel chloride aqueous solution (final cementation solution) obtained by applying such a removal method to the manufacturing process of electrolytic nickel, the silver content in the aqueous solution is effectively reduced, and therefore contamination of electrolytic nickel by silver can be extremely effectively prevented.
[0023] ≪2. Example of application to electrolytic nickel manufacturing process≫ The silver removal method according to the present embodiment will be described more specifically below based on a specific example in which it is applied to a process for producing electrolytic nickel.
[0024] FIG. 2 is a process diagram showing an example of a manufacturing process of electrolytic nickel. As shown in FIG. 2, the manufacturing process of electrolytic nickel includes a chlorine leaching step S1 in which metals such as nickel are chlorine leached from nickel sulfide as a raw material to produce a copper-containing nickel chloride aqueous solution, which is a chlorine leaching solution; a cementation step S2 in which copper ions are immobilized and removed from the obtained copper-containing nickel chloride aqueous solution; a liquid purification step S3 in which impurities such as heavy metals other than nickel are removed from the cementation end solution; and an electrolysis step S4 in which electrolytic nickel is obtained by electrowinning from the high-purity nickel chloride aqueous solution obtained through the liquid purification step S3. Although FIG. 1 and FIG. 2 are different in notation, both are flow diagrams of an electrolytic nickel manufacturing process (MCLE process), and all of the "iron removal step", "cobalt solvent extraction step", and "liquid purification step" in FIG. 1 are included in the "liquid purification step S3" in FIG. 2. In addition, the "copper removal electrolysis step" shown in FIG. 1 is omitted in FIG. 2.
[0025] [Chlorine leaching process] In the chlorine leaching step S1, nickel sulfide such as nickel matte produced by a nickel dry smelting method is used as a raw material, and metals such as nickel are leached with chlorine. Specifically, nickel in the nickel sulfide is leached by chlorine gas recovered in the electrolysis step S4 together with the cementation residue after the cementation step S2 described below, to generate a copper-containing nickel chloride aqueous solution as a chlorine leachate. The nickel sulfide raw material is, for example, repulped and slurried with the nickel chloride aqueous solution (electrolysis waste liquid) obtained in the electrolysis step S4.
[0026] In the chlorine leaching step S1, for example, reactions shown in the following formulas [1] to [3] occur. Cl2+2Cu + → 2Cl - +2Cu 2+ [1] NiS+2Cu 2+ → Ni 2+ +S 0 +2Cu + [2] Cu2S+2Cu 2+ → 4Cu + +S 0 [3]
[0027] That is, in the chlorine leaching step S1, when the raw nickel sulfide is delivered, metal components such as nickel sulfide (NiS) and copper sulfide (Cu2S) contained in the nickel sulfide are oxidized and leached by "divalent copper ions" oxidized by chlorine gas. This produces a chlorine leaching solution, a nickel chloride aqueous solution containing copper ions (copper-containing nickel chloride aqueous solution). As shown in formulas [1] to [3], it is estimated that oxidative leaching using divalent copper ions as electron carriers is performed in the chlorine leaching step S1. In addition, NiS in formula [2] represents the main component of MS, and Cu2S in formula [3] represents the main component of cementation residue.
[0028] The copper-containing nickel chloride aqueous solution produced in the chlorine leaching step S1 is treated in the next cementation step S2, where the copper ions contained in the aqueous solution are immobilized and removed. Meanwhile, in the chlorine leaching step S1, the chlorine leaching residue, mainly composed of sulfur, remains in the solid phase.
[0029] [Cementation process] In the cementation step S2, copper ions are immobilized and removed from the copper-containing nickel chloride aqueous solution, which is the chlorine leaching solution produced in the chlorine leaching step S1.
[0030] The copper-containing nickel chloride aqueous solution contains copper ions as described above, and also contains silver ions derived from the nickel sulfide raw material and the cementation residue that was subjected to the chlorine leaching treatment together with the nickel sulfide raw material. This copper-containing nickel chloride aqueous solution is an aqueous solution containing copper and silver. In the smelting process of electrolytic nickel, the copper and silver contained in the high-purity nickel chloride aqueous solution that is the subject of nickel electrowinning become impurities that directly contaminate the electrolytic nickel obtained by electrowinning. Therefore, by effectively removing copper and silver from the nickel chloride aqueous solution, high-quality electrolytic nickel can be produced.
[0031] Here, copper can be removed by the subsequent solution purification step S3, which includes treatments such as solvent extraction and oxidation neutralization. On the other hand, silver remaining in the cementation end solution is difficult to extract with amine extractants such as TNOA, despite forming a stable chloro complex ion. Therefore, silver remaining in the cementation end solution is likely to be mixed into electrolytic nickel without being sufficiently removed in the subsequent solution purification step S3.
[0032] Fig. 3 is a process diagram showing the flow of treatment in the cementation step S2. As shown in Fig. 3, the cementation step S2 includes a first cementation step (reduction step) S21 in which a sulfide raw material A containing nickel sulfide is added to a copper-containing nickel chloride aqueous solution to reduce copper ions in the aqueous solution, a second cementation step (sulfurization step) S22 in which a sulfide raw material B containing trinickel disulfide is added to a first slurry obtained through the first cementation step S21 to fix the copper ions as sulfides, and a solid-liquid separation step S23 in which the obtained second slurry is separated into solid and liquid.
[0033] The final cementation solution obtained through the cementation step S2 consisting of the above-mentioned steps (S21 to S23) is sent to a solution purification step S3, where impurities such as iron and zinc are removed. Meanwhile, the cementation residue containing sulfides such as copper sulfide immobilized in the cementation step S2 is sent again to the chlorine leaching step S1, where it is subjected to chlorine leaching treatment together with new nickel sulfide raw material.
[0034] (First cementation process) First, in the first cementation step S21, a sulfide raw material A containing nickel sulfide (NiS) is added to the copper-containing nickel chloride aqueous solution (chlorine leachate) generated in the chlorine leaching step S1 to reduce the copper ions in the aqueous solution. As the sulfide raw material A, a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material can be used.
[0035] Specifically, in the first cementation step S21, it is presumed that a reduction reaction of copper ions occurs, for example, as shown in the following formulas [4] and [5]. 4NiS+2Cu 2+ → Ni 2+ +Ni3S4+2Cu + [4] NiS+2Cu + → Ni 2+ +Cu2S [5]
[0036] As shown in formula [4] above, in the reduction treatment in the first cementation step S21, a sulfide raw material A containing nickel sulfide is added to the copper-containing nickel chloride aqueous solution, and the nickel sulfide reduces the divalent copper ions in the aqueous solution to monovalent copper ions. The copper ions thus reduced are fixed as copper sulfides by the sulfide raw material B added in the next step, the second cementation step S22.
[0037] That is, in the cementation step S2, the reducing power of nickel sulfide is maximized in the first cementation step S21 to reduce copper ions, and copper sulfide is formed in the second cementation step S22. This makes it possible to more efficiently form copper sulfide, which is an immobilized product of copper ions, and to effectively remove copper ions while reducing the amount of sulfide raw material B added in the second cementation step S22.
[0038] The temperature conditions for the reduction treatment in the first cementation step S21 are not particularly limited, and may be in the range of about 80°C to 110°C, and preferably in the range of 80°C to 90°C. By setting the temperature condition at 80°C or higher, the reduction reaction of the copper ions in the copper-containing nickel chloride aqueous solution can be efficiently advanced, and the immobilization efficiency of the copper ions in the second cementation step S22 described below can be improved. If the temperature condition is set to be higher than 110°C, the reduction efficiency of the copper ions is improved, but there is a possibility that efficient operation cannot be performed due to the equipment costs due to heat-resistant specifications and the operating costs due to the increased amount of steam.
[0039] The nickel sulfide contained in the added sulfide raw material A has low reactivity as a sulfurizing agent, and it is difficult to remove copper ions from the copper-containing nickel chloride aqueous solution to a low concentration. However, it can also cause a small amount of reaction to fix monovalent copper ions as copper sulfide (Cu2S) as shown in the above formula [5]. Therefore, by adding the sulfide raw material A containing nickel sulfide, it is possible to fix the ions as copper sulfide in the first cementation step S21, making it possible to perform an efficient copper removal process.
[0040] (Second cementation process) Next, in the second cementation step S22, a sulfide raw material B containing trinickel disulfide (nickel subsulfide, Ni3S2) is added to the first slurry obtained through the first cementation step S21, and the monovalent copper ions in the slurry are precipitated and removed as copper sulfide. Nickel matte produced by a nickel dry smelting method can be used as the sulfide raw material B. The nickel matte contains trinickel disulfide and nickel metal.
[0041] Specifically, in the second cementation step S22, for example, sulfurization reactions represented by the following formulas [6] to [8] are presumed to occur. Note that the following reaction formulas are reaction formulas when nickel matte is used as the sulfide raw material B. Ni+2Cu + →Ni 2+ +Cu...[6] Ni3S4+6Cu + →3Ni 2+ +S+3Cu2S [7] Ni3S2+6Cu + +S→3Ni 2+ +3Cu2S [8]
[0042] That is, in the second cementation step S22, as shown in the above formulas [6] to [8], a reaction occurs in which the monovalent copper ions are precipitated and removed as a solid by the trinickel disulfide (Ni3S2) and nickel metal (Ni) contained in the added nickel matte. As a result, the copper ions contained in the copper-containing nickel chloride aqueous solution are fixed mainly as copper sulfide and removed.
[0043] In this way, nickel matte as sulfide raw material B reduces monovalent copper ions to metallic copper and copper sulfide by utilizing the reducing power of the main forms of trinickel disulfide and nickel metal. The nickel itself in the nickel matte is leached into nickel ions by the oxidizing power of the monovalent copper ions. The nickel matte also serves as a sulfur source for immobilizing the reduced monovalent copper ions, and reacts with the monovalent copper ions to produce copper sulfide.
[0044] In the second cementation step S22, the chlorine leaching residue may be added as a sulfur source in order to more efficiently immobilize the monovalent copper ions as sulfides. The chlorine leaching residue is the residue remaining in the solid phase in the chlorine leaching step S1, and its main component is sulfur. By adding this as a sulfur source, the monovalent copper ions can be immobilized as sulfides such as copper sulfide together with the nickel matte. This makes it possible to more efficiently reduce the copper concentration in the copper-containing nickel chloride aqueous solution to a low concentration range.
[0045] The copper sulfide immobilized in the second cementation step S22 is separated and removed as a cementation residue in a solid-liquid separation step S23 described below, and is returned to the chlorine leaching step S1.
[0046] Here, the method according to the present embodiment is characterized in that the oxidation-reduction potential (ORP) (based on a silver / silver chloride electrode) of the second slurry obtained through the second cementation step S22 is controlled to be within a specific range. Specifically, the ORP of the second slurry is controlled to be -100 mV or more and less than 0 mV. More preferably, the ORP is controlled to be -50 mV or more and less than 0 mV.
[0047] Fig. 4 is a graph showing the relationship between the ORP (based on silver / silver chloride electrode) of the second slurry and the copper ion concentration and silver ion concentration in the final cementation liquid (aqueous nickel chloride solution after the cementation step S2). As a result of the study by the present inventors, as shown in the graph of Fig. 4, there is a correlation between the ORP of the second slurry and the silver ion concentration in the final cementation liquid, and in particular, it was found that the silver ion concentration in the final cementation liquid can be effectively reduced by the ORP of the second slurry being less than 0 mV.
[0048] In this way, by controlling and treating the ORP of the obtained second slurry to be within the above-mentioned specific range, it is possible to efficiently remove the impurity silver from the copper-containing nickel chloride aqueous solution (chlorine leachate), and obtain a solution with an effectively reduced silver concentration. The impurity silver is distributed to the cementation residue together with the copper fixed as sulfide through the second cementation step S22, and is sent to the chlorine leaching step S1.
[0049] There is no particular limitation on the method for controlling the ORP of the second slurry. Specifically, for example, the ORP can be controlled by adjusting the copper concentration of the aqueous nickel chloride solution to be subjected to the cementation step S2, that is, the copper-containing aqueous nickel chloride solution which is the chlorine leaching solution obtained from the chlorine leaching step S1. For example, the copper concentration of the aqueous copper chloride solution is adjusted to a range of 10 g / L to 70 g / L. Then, the aqueous copper chloride solution with the adjusted copper concentration is subjected to the cementation step S2, and the above-mentioned reduction treatment (first cementation step S21) and sulfurization treatment (second cementation step S22) are performed, whereby the ORP of the obtained second slurry can be controlled to a range of -100 mV or more and less than 0 mV.
[0050] In controlling the ORP of the second slurry to be within a specific range, the higher the copper concentration of the copper-containing nickel chloride aqueous solution, the greater the amount of sulfide raw material B (e.g., nickel matte) added in the second cementation step S22. For this reason, from the viewpoint of adjusting the copper concentration of the copper-containing nickel chloride aqueous solution so that the ORP of the second slurry is controlled within the above-mentioned range, and suppressing the amount of sulfide raw material B added (used amount) to perform more efficient treatment, it is more preferable that the copper concentration of the copper-containing nickel chloride aqueous solution be in the range of 10 g / L to 50 g / L.
[0051] It is also possible to control the copper concentration of the copper-containing nickel chloride aqueous solution by increasing the ORP of the second slurry, and to increase the copper concentration of the copper-containing nickel chloride aqueous solution by decreasing the ORP of the second slurry. When the copper concentration of the copper-containing nickel chloride aqueous solution is less than 10 g / L, the chlorine leaching reaction becomes insufficient because of the oxidation leaching using copper ions as a medium in the chlorine leaching step S1, and nickel, copper, etc. in the nickel sulfide cannot be sufficiently leached. When the copper concentration of the copper-containing nickel chloride aqueous solution exceeds 50 g / L, the amount of sulfide raw material B added increases as described above, and the sulfurization reaction in the second cementation step S22 becomes unstable, and the concentrations of copper and silver in the cementation final solution may increase.
[0052] The copper concentration of the copper-containing nickel chloride aqueous solution, which is the chlorine leachate, can be adjusted, for example, by extracting copper powder by copper electrowinning in the copper removal step, when the copper concentration is to be reduced. Specifically, first, a part of the first slurry is extracted, and the solid content is removed by a solid-liquid separator, and then the nickel electrolytic waste liquid is mixed and the copper concentration is adjusted to obtain a copper removal electrolytic feed solution. Then, the copper removal electrolytic feed solution is supplied to an electrolytic cell, and copper is electrolytically extracted as copper powder by an electrolytic extraction method using an insoluble anode. In the MCLE process, copper, which is an impurity input from the nickel sulfide raw material, is intentionally concentrated and circulated to be used as an oxidation leaching medium. Therefore, the copper concentration of the copper-containing nickel chloride aqueous solution can be adjusted by the balance between the copper input from the raw material and the copper powder that is removed. For this reason, the copper concentration of the chlorine leachate can be adjusted by adjusting the amount of copper powder that is removed by adjusting the current and number of cells for copper removal electrolysis.
[0053] The ORP of the second slurry can also be controlled by adjusting the amount of sulfide raw material B added in the treatment in the second cementation step S22. Fig. 5 is a graph showing the relationship between the ORP of the second slurry (based on a silver / silver chloride electrode) and the amount of sulfide raw material B (nickel matte) added in the second cementation step S22. As shown in the graph in Fig. 5, it can be seen that the ORP of the resulting second slurry can be controlled to less than 0 mV by adding the nickel matte slurry in the treatment in the second cementation step S22 at a rate of about 200 L / min.
[0054] As shown in Fig. 5, the ORP of the second slurry decreases as the amount of sulfide raw material B added increases. From this, by controlling the ORP of the second slurry preferably within a range of -50 mV or more and less than 0 mV, it is possible to efficiently remove silver from the nickel chloride aqueous solution and obtain a cementation final solution in which the silver concentration is effectively reduced, and it is also possible to reduce the amount of sulfide raw material B added (used amount) in the treatment in the second cementation step S22, thereby making it possible to perform a more efficient treatment. Note that the values on the vertical axis of Fig. 5 are merely relative values, and are values when the treatment flow rate in the second cementation step S22 is 1000 to 2000 L / min and the slurry concentration of the nickel matte slurry is 300 to 350 g / L.
[0055] The ORP of the second slurry can be measured, for example, by continuously monitoring it using an oxidation-reduction potentiometer provided in the reaction tank. In this manner, by monitoring the ORP of the slurry, which is the reaction liquid, appropriate and accurate control is possible.
[0056] The temperature conditions for the sulfurization treatment in the second cementation step S22 are not particularly limited, but are preferably in the range of about 60° C. to 100° C. If the temperature conditions are less than 60° C., the immobilization reaction of the copper ions may not proceed sufficiently, and the monovalent copper ions may not be effectively converted into sulfides. On the other hand, if the temperature conditions are higher than 100° C., the cost of cooling after the reaction is high, which is not preferable.
[0057] (solid-liquid separation process) Next, in the solid-liquid separation step S23, the second slurry obtained through the second cementation step S22 is subjected to a solid-liquid separation treatment. By the solid-liquid separation in the solid-liquid separation step S23, the cementation residues such as copper sulfide generated in the second cementation step S22 are separated and removed, and a cementation end solution is obtained which is an aqueous nickel chloride solution in which the copper concentration is reduced to a low concentration of 0.05 g / L or less and the silver concentration is reduced to a low concentration of 0.05 mg / L or less.
[0058] The solid-liquid separation method is not particularly limited, and may be performed by a well-known method such as a centrifuge or a filter press, and can efficiently separate and remove precipitates such as copper sulfide, which is a cementation residue.
[0059] [Liquid purification process] In the solution purification step S3, impurities such as heavy metals other than nickel are removed from the final cementation solution (aqueous nickel chloride solution from which copper and silver have been removed) obtained by solid-liquid separation, thereby obtaining a high-purity aqueous nickel chloride solution for electrowinning.
[0060] The liquid purification step S3 mainly includes a deironization step, a decobaltization step, a deleading step, and a dezincification step. In these steps, for example, an oxidation neutralization method using chlorine gas as an oxidizing agent and nickel carbonate as an alkaline agent can be used to remove impurities from the cementation end solution. The oxidation neutralization method utilizes the property that heavy metals such as cobalt and iron, when they become highly oxidized ions, tend to become hydroxides in a low pH range, and is a method that is widely used in the liquid purification step of wet smelting and in the treatment of wastewater containing heavy metals.
[0061] Specifically, in the iron removal step in the liquid purification step S3, impurities are removed, for example, by the reaction of the following formula [9]. 2Fe 2+ +Cl2+3NiCO3+3H2O→ 2Fe(OH)3+3Ni 2+ +2Cl - +3CO2···[9]
[0062] As shown in the above formula [9], in the iron removal step in the solution purification step S3, hydroxide precipitates of impurity elements such as iron to be removed are formed from the cementation end solution, thereby obtaining an aqueous nickel chloride solution from which impurities have been removed.
[0063] In general, the chemicals used in the oxidation neutralization method include hypochlorous acid, oxygen, air, and the like as the oxidizing agent, in addition to chlorine gas. Also, hydroxides such as caustic soda, ammonia, and the like as the alkaline agent can be used in addition to nickel carbonate. These chemicals are used in combinations suited to the process conditions, but in the nickel hydrometallurgy process, it is preferable to use chlorine gas as the oxidizing agent and nickel carbonate as the alkaline agent. For example, chlorine gas is a strong oxidizing agent that is generated in the process and is easy to use. Also, the reason for using nickel carbonate as the alkaline agent is that it can control the ion concentrations of nickel, sodium, sulfate, and the like throughout the process, and has excellent reactivity during oxidation neutralization.
[0064] Furthermore, in the liquid purification step S3, the treatment steps are combined in the most efficient order according to the impurity composition of the treatment liquid (final cementation liquid). For example, the iron removal step is performed by the above-mentioned oxidation neutralization method, the cobalt removal step is performed by the solvent extraction method, the lead removal step is performed by the oxidation neutralization method under changed conditions, and the zinc removal step is performed by the ion exchange method.
[0065] [Electrolysis process] In the electrolysis step S4, electrolytic nickel is obtained by electrowinning from the high-purity aqueous nickel chloride solution purified through the above-mentioned solution purification step S3.
[0066] Specifically, in the electrolysis step S4, the reactions shown in the following formulas
[10] and
[11] occur at the cathode and the anode, respectively. (cathode side) Ni 2+ +2e - → Ni 0
[10] (anode side) 2Cl - → Cl2↑+2e -
[11]
[0067] That is, on the cathode side, nickel ions in the high-purity nickel chloride aqueous solution are precipitated as metal (electronic nickel) as shown in the above formula
[10] . On the anode side, chloride ions in the high-purity nickel chloride aqueous solution are generated as chlorine gas as shown in the above formula
[11] . The generated chlorine gas is used, for example, as recovered chlorine gas in the leaching process in the chlorine leaching step S1.
[0068] According to the method of the present embodiment, as described above, the impurity silver can be efficiently and effectively removed from the nickel chloride aqueous solution in the cementation step S2. Therefore, in the electrolysis step S4, electrowinning is performed based on the high-purity nickel chloride aqueous solution in which the silver concentration is effectively reduced, so that electrolytic nickel free from silver contamination can be obtained. In addition, since silver is a relatively expensive metal, the loss can be recovered. EXAMPLES
[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0070] [Examples and Comparative Examples] In the MCLE process (see Figure 2), the chlorine leaching solution (copper-containing nickel chloride aqueous solution) obtained through the chlorine leaching step (S1) was subjected to a cementation step S2 consisting of a first cementation step (S21) and a second cementation step (S22) to obtain a nickel chloride aqueous solution from which copper has been removed (cementation end solution).
[0071] Specifically, in the first cementation step (S21), nickel-cobalt mixed sulfide was added to a copper-containing nickel chloride aqueous solution to perform a reduction treatment for reducing the divalent copper ions in the aqueous solution to monovalent copper ions, thereby obtaining a first slurry, and in the second cementation step (S22), nickel matte was added to the first slurry to perform a sulfurization treatment for immobilizing the monovalent copper ions as sulfides, thereby obtaining a second slurry.
[0072] In Examples 1 and 2 and Comparative Example 1, the copper concentration of the copper-containing nickel chloride aqueous solution subjected to the cementation step S2 was adjusted to control the oxidation-reduction potential (ORP) (based on a silver / silver chloride electrode) of the second slurry obtained through the sulfurization treatment in the second cementation step (S22), as shown in Table 1 below.
[0073] After the above treatment, the second slurry was subjected to solid-liquid separation to obtain a final reaction liquid (final cementation liquid), which was used to measure the concentrations of copper and silver impurities. The amount of nickel matte added in the treatment in the second cementation step (S22) was also measured. The results of these measurements are shown in Table 1 below.
[0074] [Table 1]
[0075] As shown in Table 1, in Examples 1 and 2, the ORP of the second slurry obtained through the treatment in the cementation step was controlled to be less than 0 mV, so that the copper concentration and silver concentration of the final reaction liquid (final cementation liquid) were both below the target concentration. In Example 2, the amount of nickel matte used in the treatment in the second cementation step was slightly increased. This is thought to be because the copper concentration of the nickel chloride aqueous solution subjected to the cementation step was higher than that in Example 1.
[0076] On the other hand, in Comparative Example 1, although the copper concentration of the final reaction solution (final cementation solution) was reduced to the target concentration, the impurity silver could not be removed efficiently, and the copper concentration was not reduced to the target concentration. This is believed to be because the ORP of the second slurry was a value exceeding 0 mV.
Claims
1. A method for removing silver from an aqueous nickel chloride solution containing copper and silver, comprising the steps of: a first cementation step of adding a sulfide raw material A containing nickel sulfide to the nickel chloride aqueous solution and reducing divalent copper ions in the nickel chloride aqueous solution to monovalent copper ions; A second cementation step of adding a sulfide raw material B containing trinickel disulfide to the first slurry obtained in the first cementation step, and immobilizing the monovalent copper ions contained in the first slurry as sulfides; The oxidation-reduction potential (based on a silver / silver chloride electrode) of the second slurry obtained in the second cementation step is controlled to be −100 mV or more and less than 0 mV. Method for removing silver from aqueous nickel chloride solution.
2. The oxidation-reduction potential of the second slurry (based on a silver / silver chloride electrode) is controlled to be −50 mV or more and less than 0 mV. The method for removing silver from an aqueous nickel chloride solution according to claim 1.
3. The oxidation-reduction potential of the second slurry is controlled by adjusting the copper concentration of the nickel chloride aqueous solution. The method for removing silver from an aqueous nickel chloride solution according to claim 1.
4. The copper concentration of the nickel chloride aqueous solution is adjusted to a range of 10 g / L to 50 g / L to control the oxidation-reduction potential of the second slurry. The method for removing silver from an aqueous nickel chloride solution according to claim 3.
5. The sulfide raw material A is a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material, The sulfide raw material B is nickel matte produced by a nickel dry smelting method.
5. The method for removing silver from an aqueous nickel chloride solution according to claim 1.
Citation Information
Patent Citations
Chlorination refining method for high-iron low-nickel sulphonium
CN107385233A
Nickel refining method
JP2003082421A
Method for recovering silver in hydrometallurgical copper refining process
JP2008115429A
Method for removing copper ions from copper-containing nickel chloride solution, and method for producing electrolytic nickel
JP2012026027A
Method for removing copper ion of aqueous nickel chloride solution and apparatus for removal treatment of copper ion