Copper ion removal method from aqueous nickel chloride solution and production method of aqueous nickel chloride solution
The method optimizes copper ion removal in nickel chloride solutions by using a two-stage cementation process with specific nickel chloride solutions and sulfide raw materials, efficiently reducing copper ions and maintaining chlorine leaching rates in the nickel hydrometallurgical process.
Patent Information
- Application Number
- JP2023058136
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
The existing nickel hydrometallurgical smelting process faces challenges in efficiently removing copper ions from aqueous nickel chloride solutions with high copper ion concentrations, leading to inefficiencies in the cementation process and potential deterioration of the chlorine leaching rate.
A method involving the optimized addition of two types of nickel chloride solutions with different divalent copper ion ratios, combined with a two-stage cementation process using sulfide raw materials, is employed to reduce and fix copper ions as sulfides, utilizing a copper ion removal apparatus with multiple reaction vessels.
This approach effectively reduces copper ions to monovalent form, enhancing the processing capacity and maintaining the chlorine leaching rate, allowing for higher copper concentrations and improved nickel yield without requiring additional equipment or reducing copper concentrations.
Smart Images

Figure 2024145681000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a technique for removing copper contained in an aqueous nickel chloride solution. More specifically, the present invention relates to a method for removing copper ions from an aqueous nickel chloride solution in, for example, a cementation step in a nickel hydrometallurgical process, and a method for producing an aqueous nickel chloride solution from which copper ions have been removed. [Background technology]
[0002] In the nickel hydrometallurgy process (hereinafter referred to as the "MCLE process"), the raw materials, nickel matte or nickel-cobalt mixed sulfide (MS: mixed sulfide), are leached with chlorine, and the resulting leachate (chlorine leachate) is purified to remove impurities, and then nickel and cobalt are recovered in the form of electrolytic nickel and electrolytic cobalt in an electrolytic process.
[0003] As shown in FIG. 1, the chlorine leaching solution obtained from the chlorine leaching process is subjected to removal of excess copper in the copper removal electrolysis process provided between the cementation process and the cementation process, and impurities such as iron and arsenic are removed in the iron removal process, and then the solution is sent to the cobalt solvent extraction process. In the cobalt solvent extraction process, nickel and cobalt are separated by solvent extraction to obtain a crude nickel chloride solution (NiCl2) and a crude cobalt chloride solution (CoCl2). The crude nickel chloride solution is further purified by removing impurities in the solution purification process and sent to the nickel electrolysis process. Then, in the nickel electrolysis process, electrolytic nickel is produced by electrolytic winning. Meanwhile, the crude cobalt chloride solution is also further purified by removing impurities in the solution purification process and sent to the cobalt electrolysis process, where electrolytic winning is produced.
[0004] The MCLE process includes a cementation step to remove copper ions, which are impurities contained in the chlorine leachate (copper-containing nickel chloride aqueous solution) obtained by chlorine leaching.
[0005] In the cementation process, nickel and cobalt are leached from nickel matte and MS (hereinafter, these may be collectively referred to as "nickel sulfide raw material") by utilizing the oxidizing power of divalent copper ions contained in the chlorine leachate, and copper ions and silver ions contained in the chlorine leachate are distributed to the solid side by utilizing the reducing power of nickel matte and MS, and are removed. In this cementation process, a reduction process in which MS is added to a copper-containing nickel chloride aqueous solution to reduce copper ions in the solution from divalent to monovalent, and a sulfurization process in which nickel matte is added to a slurry obtained by the reduction process to fix the reduced monovalent copper ions as copper sulfide are configured to be performed in a total of n tanks (n is an integer of 4 or more) connected in series (for example, Patent Document 1). By undergoing such treatment in the cementation process, the copper ion concentration in the process liquid after the reaction (cementation end liquid) is reduced to a low concentration of 0.10 g / L or less, more preferably 0.05 g / L or less.
[0006] The final cementation liquid, which has been separated into solid and liquid through the cementation process, is sent to the next process, the cobalt solvent extraction process. Meanwhile, the solid residue slurry (cementation residue slurry) is sent to the chlorine leaching process, where valuable metals are leached as much as possible by reaction with chlorine gas together with new raw materials.
[0007] At this time, the copper ions in the chlorine leaching solution obtained by chlorine leaching function as an ion carrier that absorbs chlorine gas (for example, Patent Document 2), so the higher the copper grade in the residue slurry and the copper ion concentration in the chlorine leaching solution, the more favorable the chlorine leaching reaction becomes. However, since the chlorine leaching solution is the starting solution for the reaction in the cementation process, if the copper ion concentration is high, problems such as those described below will occur.
[0008] Here, the cementation process is composed of a first cementation process in which a sulfide raw material A containing nickel sulfide is added to a copper-containing nickel chloride aqueous solution, which is a chlorine leachate obtained by chlorine leaching, to reduce the divalent copper ions in the nickel chloride aqueous solution to monovalent copper ions, and a second cementation process in which a sulfide raw material B containing nickel disulfide is added to a first slurry obtained in the first cementation process, to fix the monovalent copper ions contained in the first slurry as sulfides.
[0009] The reducing power of the sulfide raw material A added in the first cementation step is weaker than that of the sulfide raw material B added in the second cementation step. Therefore, it can only reduce divalent copper ions to monovalent copper ions. A certain reaction time is required to reduce divalent copper ions to monovalent copper ions. If the reaction time cannot be secured, the reaction in the second cementation step will be carried out with some divalent copper ions remaining. However, in such a case, there is a problem that the amount of sulfide raw material B required for sulfidation fixation of copper ions must be increased in the second cementation step.
[0010] Therefore, it is desirable to reduce as many divalent copper ions as possible to monovalent copper ions in the first cementation step. However, in order to achieve this, the only options are to extend the reaction time or to reduce the copper ion concentration in the nickel chloride aqueous solution. In the former case, the degree of freedom in adjustment is extremely low, and capital investment such as the addition of reaction tanks is required. In the latter case, although this can be achieved by reducing the copper concentration in the nickel chloride aqueous solution used in the cementation reaction, there is a problem in that reducing the copper concentration leads to a deterioration in the leaching rate in the chlorine leaching step as described above. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2017-155281 A [Patent Document 2] JP 2012-026027 A Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention has been proposed in view of the above circumstances, and has an object to provide a method capable of efficiently removing copper ions from an aqueous nickel chloride solution even when the aqueous nickel chloride solution has a high copper ion concentration. [Means for solving the problem]
[0013] As a result of extensive investigations, the inventors have found that the above-mentioned problems can be solved by optimizing the addition positions of two types of aqueous solutions having different divalent copper ion ratios as the nickel chloride aqueous solutions in the cementation treatment of an aqueous nickel chloride solution containing copper ions, subjecting the aqueous nickel chloride solution with a higher divalent copper ion ratio to a reduction treatment, and adding an aqueous nickel chloride solution with a lower divalent copper ion ratio to the aqueous nickel chloride solution with a higher divalent copper ion ratio, and subjecting the resulting solution to a sulfurization treatment, thereby completing the present invention.
[0014] (1) The first invention of the present invention is a method for removing copper ions from an aqueous nickel chloride solution containing copper ions, comprising a first cementation step of adding a sulfide raw material A containing nickel sulfide to the aqueous nickel chloride solution to reduce divalent copper ions in the aqueous nickel chloride solution to monovalent copper ions, and a second cementation step of adding a sulfide raw material B containing nickel disulfide to a first slurry obtained in the first cementation step to fix the monovalent copper ions contained in the first slurry as sulfides, and performing a cementation treatment to obtain the aqueous nickel chloride solution to be treated, the aqueous nickel chloride solution having a copper ion concentration of 20 to 80 g / L, a ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ +Cu + )) is 60 to 100%, and the copper ion concentration is 1 to 20 g / L and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu2+ +Cu + and a nickel chloride aqueous solution b having a nickel chloride concentration of 0 to 40%. In the first cementation step, the nickel chloride aqueous solution a is used as the nickel chloride aqueous solution for treatment, and in the second cementation step, in addition to the nickel chloride aqueous solution a, the nickel chloride aqueous solution b is further added and used for treatment.
[0015] (2) A second aspect of the present invention is a method for removing copper ions from an aqueous nickel chloride solution, comprising the steps of: performing the cementation treatment using a copper ion removal apparatus having a total of n reaction tanks (n is an integer of 4 or more) connected in series; supplying the nickel chloride aqueous solution a and charging the sulfide raw material A to a first-stage reaction tank located at the most upstream in the copper ion removal apparatus; charging the sulfide raw material B to a final-stage (n-th) reaction tank located at the most downstream and an (n-1)-th reaction tank located one stage before the final-stage reaction tank; and supplying the nickel chloride aqueous solution b to a central reaction tank (when n is an even number, the (n / 2+1)-th reaction tank).
[0016] (3) A third aspect of the present invention is a method for removing copper ions from an aqueous nickel chloride solution according to the first or second aspect of the present invention, wherein the sulfide raw material A is a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material, and the sulfide raw material B is nickel matte produced by a pyrometallurgical method for nickel.
[0017] (4) A fourth invention of the present invention is a method for removing copper ions from an aqueous nickel chloride solution according to any one of the first to third inventions, further comprising a copper removal electrolysis step of recovering copper powder by electrowinning and obtaining an electrolytic waste liquid using a part of the first slurry obtained through the first cementation step as an initial liquid, and in the cementation treatment, the electrolytic waste liquid obtained from the copper removal electrolysis step is used as the aqueous nickel chloride solution b.
[0018] (5) A fifth aspect of the present invention is a method for obtaining an aqueous nickel chloride solution from a raw material containing nickel, the method comprising: a chlorine leaching step of blowing chlorine gas into a nickel-containing material slurry to perform chlorine leaching to obtain a chlorine leachate and a chlorine leach residue; and a cementation step of performing the cementation treatment for performing the copper ion removal method according to claim 1 on the aqueous nickel chloride solution containing copper ions, which is the chlorine leachate, to obtain the aqueous nickel chloride solution from which the copper ions have been removed. The slurry produced in the cementation step is subjected to solid-liquid separation to obtain a cementation residue, and the slurry of the cementation residue (residue slurry) is transferred to the chlorine leaching step. In the chlorine leaching step, chlorine leaching is performed by blowing chlorine gas into the nickel-containing material slurry containing the residue slurry. This is a method for producing an aqueous nickel chloride solution.
[0019] (6) A sixth aspect of the present invention is a method for producing an aqueous nickel chloride solution according to the fifth aspect of the present invention, further comprising a copper removal electrolysis step of recovering copper powder by electrowinning and obtaining an electrolytic waste liquid using a part of the first slurry obtained through a first cementation step in the cementation step as an initial liquid, wherein the aqueous nickel chloride solution a to be supplied to the cementation step is the chlorine leachate obtained from the chlorine leaching step, and the aqueous nickel chloride solution b is the electrolytic waste liquid obtained from the copper removal electrolysis step.
[0020] (7) A seventh aspect of the present invention is a method for producing an aqueous nickel chloride solution according to the fifth or sixth aspect of the present invention, wherein the copper concentration of the chlorine leachate to be subjected to the cementation step is adjusted so that the redox potential (based on a silver / silver chloride electrode) of the second slurry obtained through the second cementation step is controlled to be not less than -100 mV and less than 0 mV. Effect of the Invention
[0021] According to the present invention, there can be provided a method capable of efficiently removing copper ions from an aqueous nickel chloride solution even when the aqueous nickel chloride solution has a high copper ion concentration. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a process diagram showing a schematic flow of a nickel hydrometallurgical process (MCLE process). [Diagram 2] FIG. 2 is a process diagram showing an example of a cementation process flow. [Diagram 3] FIG. 1 is a schematic diagram showing an example of the configuration of a copper ion removal device. [Figure 4] FIG. 1 is a process diagram illustrating the flow of the MCLE process for producing electrolytic nickel from raw nickel sulfide. [Diagram 5] FIG. 2 is a graph showing the relationship between the copper ion concentration in the starting treatment liquid (chlorine leachate which is a copper-containing nickel chloride aqueous solution) in the cementation step and the nickel grade in the chlorine leach residue obtained from the chlorine leach step. [Figure 6] FIG. 2 is a graph showing the results of the treatment in Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, a specific embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail with reference to the drawings. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention.
[0024] ≪1. Method for removing copper ions from nickel chloride solution≫ The method for removing copper ions according to the present embodiment is a method for removing copper ions from an aqueous nickel chloride solution containing the copper ions.
[0025] For example, an example of the nickel chloride aqueous solution to be treated is a copper-containing nickel chloride aqueous solution (chlorine leachate) obtained by chlorine leaching of raw nickel sulfide in a nickel hydrometallurgical smelting process (MCLE process).The copper ion removal method can be applied to the treatment in the cementation step in the MCLE process.
[0026] 2 is a process diagram showing an example of the flow of cementation treatment for carrying out this method. Specifically, this method includes a first cementation step S21 in which a sulfide raw material A containing nickel sulfide is added to a copper-containing nickel chloride aqueous solution to reduce divalent copper ions in the nickel chloride aqueous solution to monovalent copper ions, and a second cementation step S22 in which a sulfide raw material B containing trinickel disulfide is added to a first slurry obtained in the first cementation step S21 to fix the monovalent copper ions contained in the first slurry as sulfides.
[0027] Here, the treatment in the first cementation step S21 is also referred to as a “reduction treatment,” and the treatment in the second cementation step S22 is also referred to as a “sulfurization treatment.” An overview of each of the first cementation step S21 and the second cementation step S22 will be described below.
[0028] [About the cementation process] (First cementation process S21) First, in the first cementation step S21, a sulfide raw material A containing nickel sulfide (NiS) is added to the copper-containing nickel chloride aqueous solution (chlorine leachate) to be treated, thereby reducing the copper ions in the aqueous solution. As the sulfide raw material A, a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material can be used.
[0029] In the first cementation step S21, it is presumed that a reduction reaction of copper ions occurs, for example, as shown in the following formulas [1] and [2]. 4NiS+2Cu 2+→ Ni 2+ +Ni3S4+2Cu + [1] NiS+2Cu + → Ni 2+ +Cu2S [2]
[0030] As shown in formula [1] above, in the reduction treatment in the first cementation step S21, a sulfide raw material A containing nickel sulfide is added to the nickel chloride aqueous solution, and the nickel sulfide reduces the divalent copper ions in the aqueous solution to monovalent copper ions. The copper ions thus reduced are fixed as copper sulfides by the sulfide raw material B added in the next step, the second cementation step S22.
[0031] The temperature conditions for the reduction treatment in the first cementation step S21 are not particularly limited, and may be in the range of about 80 to 110°C, and is preferably in the range of 80 to 90°C.
[0032] (Second cementation process S22) Next, in the second cementation step S22, a sulfide raw material B containing trinickel disulfide (nickel subsulfide, Ni3S2) is added to the first slurry obtained through the first cementation step S21, and the monovalent copper ions in the slurry are precipitated and removed as copper sulfide. As the sulfide raw material B, nickel matte produced by a nickel dry smelting method can be used. The nickel matte contains trinickel disulfide and nickel metal.
[0033] In the second cementation step S22, for example, sulfurization reactions represented by the following formulas [3] to [5] are presumed to occur. Note that the following reaction formulas are reaction formulas when nickel matte is used as the sulfide raw material B. Ni+Cu 2+ →Ni 2+ +Cu + [3] Ni3S4+6Cu + →3Ni 2+ +S+3Cu2S [4] Ni3S2+6Cu + +S→3Ni 2+ +3Cu2S [5]
[0034] As shown in the above formulas [3] to [5], the trinickel disulfide (Ni3S2) and nickel metal (Ni) contained in the added nickel matte cause a reaction (sulfurization treatment) in which monovalent copper ions are precipitated and removed as solids. As a result, the copper ions contained in the copper-containing nickel chloride aqueous solution are fixed and removed mainly as copper sulfide.
[0035] In the second cementation step S22, a chlorine leaching residue may be added as a sulfur source to more efficiently immobilize the monovalent copper ions as sulfides. The chlorine leaching residue is a residue remaining in the solid phase in the chlorine leaching step S1 in the MCLE process, and its main component is sulfur. By adding this as a sulfur source, the monovalent copper ions can be immobilized as copper sulfide together with the nickel matte.
[0036] (Solid-liquid separation step S23) The second slurry obtained through the sulfurization treatment in the second cementation step S22 is composed of a cementation residue containing sulfide of sulfurized copper and a final cementation liquid which is an aqueous nickel chloride solution from which copper has been removed. Therefore, by subjecting the second slurry to a solid-liquid separation treatment (solid-liquid separation step S23), the final cementation liquid and the cementation residue can be separated and recovered.
[0037] [About the nickel chloride aqueous solution used as the starting solution for treatment] In the method according to the present embodiment, the nickel chloride aqueous solution to be subjected to the cementation treatment (to be treated) has a copper ion concentration of 20 to 80 g / L, and the ratio of divalent copper ions (Cu 2+ / (Cu 2+ +Cu + )) is 60-100%, and "nickel chloride aqueous solution a" has a copper ion concentration of 1-20g / L and the ratio of divalent copper ions (Cu2+ / (Cu 2+ +Cu + )) is 0 to 40%. Two types of nickel chloride aqueous solutions, "nickel chloride aqueous solution b" and "nickel chloride aqueous solution c" with nickel chloride content of 0 to 40% are added separately to the optimal positions.
[0038] Specifically, in the first cementation step S21, a "nickel chloride aqueous solution a" is used as the nickel chloride aqueous solution for treatment, and in the second cementation step S22, in addition to the nickel chloride aqueous solution a, a "nickel chloride aqueous solution b" is further added and then subjected to treatment.
[0039] The "aqueous nickel chloride solution a" is not particularly limited, but for example, a chlorine leachate obtained through the chlorine leach step S1 in a nickel hydrometallurgical process (MCLE process) can be used.
[0040] The method according to the present embodiment may further include a copper removal electrolysis step in which copper powder is recovered by electrowinning using a part of the first slurry obtained through the first cementation step S21 as a starting solution, and an electrolysis waste liquid is obtained. In this case, the electrolysis waste liquid (copper removal electrolysis waste liquid) obtained from the copper removal electrolysis step may be used as the "nickel chloride aqueous solution b".
[0041] Table 1 below shows an example of the liquid composition of the "chlorine leaching solution" used as the "nickel chloride aqueous solution a" and the "decopper electrolysis waste liquid" used as the "nickel chloride aqueous solution b".
[0042] [Table 1]
[0043] As shown in the composition example in Table 1, the chlorine leaching solution (nickel chloride aqueous solution a) has high nickel and copper concentrations, and is also at a relatively high temperature. In addition, due to its high oxidation-reduction potential (ORP), almost all of the copper ions in the solution exist in the form of divalent copper ions. On the other hand, the copper removal electrolysis waste solution (nickel chloride aqueous solution b) has low nickel and copper concentrations, and is also at a relatively low temperature. In addition, due to its low ORP, almost all of the copper ions in the solution exist in the form of monovalent copper ions.
[0044] Therefore, even if the decoppering electrolysis waste liquid (nickel chloride aqueous solution b) is subjected to treatment in the first cementation step S21, it hardly reacts with the sulfide raw material A. When performing treatment in the first cementation step S21, if the nickel chloride aqueous solution to be treated contains an aqueous solution with a high ratio of monovalent copper ions, such as nickel chloride aqueous solution b, the divalent copper ions in the chlorine leachate (nickel chloride aqueous solution a) are diluted with the monovalent copper ions, decreasing the ratio of divalent copper ions, and the efficiency of reduction of divalent copper ions to monovalent copper ions by the sulfide raw material A decreases.
[0045] Therefore, in the method according to the present embodiment, as described above, in the first cementation step S21, the "nickel chloride aqueous solution a" is used as the nickel chloride aqueous solution for treatment, and in the second cementation step S22, in addition to the nickel chloride aqueous solution a, the "nickel chloride aqueous solution b" is further added and used for treatment.
[0046] According to this method, divalent copper ions contained in the nickel chloride aqueous solution to be treated (nickel chloride aqueous solution a) can be efficiently reduced to monovalent copper ions in the first cementation step S21, and the monovalent copper ions can be fixed as sulfides in the second cementation step S22, thereby effectively removing the copper ions from the nickel chloride aqueous solution.
[0047] Moreover, the most effective means for reducing as many divalent copper ions as possible to monovalent copper ions in the first cementation step S21 is to extend the reaction time, i.e., the residence time in the reaction tank. Therefore, by not subjecting the copper removal electrolytic waste liquid (nickel chloride aqueous solution b) to treatment in the first cementation step S21 or adding it further downstream of the first cementation step S21, the treatment flow rate in the first cementation step S21 is reduced, and the residence time of the nickel chloride aqueous solution (nickel chloride aqueous solution a) is extended accordingly. This allows the divalent copper ions contained in the nickel chloride aqueous solution (nickel chloride aqueous solution a) to be treated in the first cementation step S21 to be efficiently reduced to monovalent copper ions.
[0048] By subjecting the nickel chloride aqueous solution (final cementation solution) obtained by applying such a removal method to the manufacturing process of electrolytic nickel, the content of copper ions in the aqueous solution is effectively reduced, making it possible to obtain highly pure electrolytic nickel.
[0049] In addition, when a chlorine leachate obtained through the chlorine leaching step S1 in a nickel hydrometallurgy process (MCLE process) is used as the nickel chloride aqueous solution to be treated (nickel chloride aqueous solution a), copper ions can be effectively removed without taking measures such as lowering the copper ion concentration of the nickel chloride aqueous solution. Therefore, when considering the circulation cycle of the nickel hydrometallurgy process, it is possible to effectively prevent a situation in which the copper ions functioning as ion carriers for chlorine gas absorption become insufficient, resulting in a deterioration in the chlorine leaching rate in the chlorine leaching step S1.
[0050] Furthermore, since copper ions can be efficiently removed, the copper concentration of the chlorine leaching solution can be intentionally increased to improve the leaching rate in the chlorine leaching step S1, i.e., the nickel recovery rate.
[0051] Furthermore, an increase in the reduction treatment capacity in the first cementation step S21 means an increase in the treatment capacity of the sulfide raw material A containing nickel sulfide, making it possible to treat a larger amount of raw material.
[0052] (About nickel chloride solution a) The nickel chloride aqueous solution a is the starting solution for the cementation treatment. As described above, the nickel chloride aqueous solution a has a copper ion concentration of 20 to 80 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ +Cu + )) is 60 to 100%. The temperature is not particularly limited, and a temperature of about 70 to 100° C. can be used.
[0053] As such an aqueous nickel chloride solution a, a chlorine leachate obtained through the chlorine leach step S1 in a nickel hydrometallurgical process (MCLE process) can be used.
[0054] The chlorine leaching step S1 in the MCLE process is briefly described below. In the chlorine leaching step S1, nickel sulfide such as nickel matte produced by a nickel dry smelting method is used as a raw material, and metals such as nickel are leached with chlorine gas together with the cementation residue after the cementation step to generate a copper-containing nickel chloride aqueous solution as a chlorine leachate.
[0055] In the chlorine leaching step S1, for example, reactions shown in the following formulas [6] to [8] occur. Cl2+2Cu + → 2Cl - +2Cu 2+ [6] NiS+2Cu 2+ → Ni 2+ +S 0 +2Cu + [7] Cu2S+2Cu 2+ → 4Cu + +S 0 [8]
[0056] That is, in the chlorine leaching step S1, when the raw nickel sulfide is delivered, the metal components contained in the nickel sulfide, such as nickel sulfide (NiS) and copper sulfide (Cu2S), are oxidized and leached by "divalent copper ions" oxidized by chlorine gas. This produces a nickel chloride aqueous solution containing copper ions (copper-containing nickel chloride aqueous solution), which is the chlorine leaching solution. As shown in formula [6], it is estimated that oxidative leaching using divalent copper ions as electron carriers is carried out in the chlorine leaching step S1. In addition, NiS in formula [7] represents the main component of MS, and Cu2S in formula [8] represents the main component of cementation residue.
[0057] (About nickel chloride aqueous solution b) The nickel chloride aqueous solution b is the starting solution for the cementation treatment, similar to the nickel chloride aqueous solution a. As described above, the nickel chloride aqueous solution b has a copper ion concentration of 1 to 20 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ +Cu + )) is 0 to 40%. That is, the nickel chloride aqueous solution b is an aqueous solution having a smaller content of divalent copper ions than the nickel chloride aqueous solution a, in other words, a larger content of monovalent copper ions.
[0058] The temperature of the aqueous nickel chloride solution b is not particularly limited, and may be about 40 to 60°C.
[0059] As such an aqueous nickel chloride solution b, a copper removal electrolysis waste solution obtained through a copper removal electrolysis step in a nickel hydrometallurgical refining process (MCLE process) can be used.
[0060] The copper removal electrolysis process in the MCLE process is briefly described below. In the MCLE process, which produces electrolytic nickel from nickel chloride solution, copper derived from the raw material (nickel sulfide) is circulated in the process system while maintaining a certain concentration. Copper plays an important role as a leaching agent for efficiently and stably leaching nickel in the raw material during the chlorine leaching process (chlorine leaching process S1). In the MCLE process, the copper contained in the raw material is stored in the process system, and a large amount of copper is circulated as the chlorine leaching solution and cementation residue. On the other hand, in order to maintain an appropriate amount of copper circulating in the system, it is necessary to extract an amount of copper from the system that corresponds to the amount of copper newly supplied from the raw material. Therefore, in the MCLE process, a process (copper removal electrolysis process) is performed to remove part of the copper circulating in the system by electrowinning.
[0061] In the copper removal electrolytic treatment, a part of the first slurry obtained through the first cementation step S21 in the cementation step S2 is used as a starting solution, and copper powder is recovered by electrowinning and an electrolytic waste solution is obtained. As the electrolytic feed solution, a solution obtained by removing solids from the first slurry through solid-liquid separation (final reaction solution of the treatment in the first cementation step S21) is preferably used. Specifically, in the copper removal electrolytic treatment, the electrolytic feed solution is supplied to an electrolytic cell equipped with an electrode pair consisting of a positive electrode and a negative electrode, and electrolytic treatment is performed. As a result of this electrolytic treatment, dendritic copper powder is precipitated on the surface of the negative electrode, and chlorine gas is generated at the positive electrode.
[0062] On the other hand, after the copper removal electrolytic treatment, a solution from which copper has been separated, recovered and removed (copper removal electrolytic waste liquid) is obtained. As described above, this copper removal electrolytic waste liquid is the end-of-reaction solution from the treatment (reduction treatment) in the first cementation step S21, that is, the solution after electrolysis to recover copper powder from a solution containing a large amount of monovalent copper ions. Therefore, the copper removal electrolytic waste liquid is a solution with a relatively low copper ion concentration and a small ratio of divalent copper ions.
[0063] [About the copper ion removal device] Now, the cementation process consisting of the first cementation process S21 and the second cementation process S22 can be carried out using a copper ion removal apparatus equipped with a total of n reaction tanks (n is an integer of 4 or more) connected in series.
[0064] In such a cementation process using a copper ion removal apparatus in which n reaction tanks are connected in series, a first cementation process S21 (reduction process) is carried out in the first reaction tank located most upstream to the n-2th reaction tank located two tanks before the final reaction tank, and a second cementation process S22 (sulfurization process) is carried out in the final (nth) reaction tank located most downstream from the n-1th reaction tank located one tank before the final reaction tank.
[0065] In the method according to the present embodiment, an aqueous nickel chloride solution a is supplied to the first-stage reaction tank located at the most upstream position, and a sulfide raw material A containing nickel sulfide is also charged therein. A sulfide raw material B containing trinickel disulfide is charged to the final-stage (n-th) reaction tank located at the most downstream position, and the (n-1)-th reaction tank located one stage before the final-stage reaction tank. An aqueous nickel chloride solution b is supplied to the reaction tank located in the center (however, when n is an even number, the (n / 2+1)-th reaction tank).
[0066] In other words, in the method according to the present embodiment, the supply inlets of the aqueous nickel chloride solutions a and b, which have different compositions, are changed so that the aqueous nickel chloride solution a (with a divalent copper ion ratio of 60 to 100%) can be supplied to the reduction treatment in the first cementation step S21, and the aqueous nickel chloride solution b (with a divalent copper ion ratio of 0 to 40%) in addition to the aqueous nickel chloride solution a can be supplied to the sulfurization treatment in the second cementation step S22.
[0067] More specifically, Fig. 3 is a schematic diagram showing an example of the configuration of a copper ion removal apparatus. The copper ion removal apparatus 1 shown in Fig. 3 includes a total of eight reaction tanks (No. 1 to No. 8) connected in series (n=8).
[0068] The copper ion removal device 1 is configured to perform a reduction treatment in which a sulfide raw material A containing nickel sulfide is added to an aqueous nickel chloride solution to reduce copper ions (first cementation step S21) in a total of six tanks, from the first-stage reaction tank (No. 1) located at the most upstream to the sixth-stage reaction tank (No. 6). Also, a sulfide treatment is performed in which a sulfide raw material B containing trinickel disulfide is added to a slurry (first slurry) obtained by the reduction treatment to fix monovalent copper ions as copper sulfide in a total of two tanks, from the seventh-stage reaction tank (No. 7) to the final-stage (eighth-stage) reaction tank (No. 8) located at the most downstream.
[0069] In the copper ion removal apparatus 1, of the total eight reaction tanks, the first-stage reaction tank (No. 1), which is located at the most upstream position, is provided with an initial liquid inlet for supplying an aqueous nickel chloride solution (aqueous nickel chloride solution a) which is an initial liquid for the reduction treatment, and a sulfide raw material A inlet for introducing a sulfide raw material A containing nickel sulfide. The final-stage (eighth-stage) reaction tank (No. 8), which is located at the most downstream position, is provided with a final liquid outlet for discharging a final reaction liquid obtained through the sulfurization treatment, and a sulfide raw material B inlet for introducing a sulfide raw material B containing trinickel disulfide. The seventh-stage reaction tank (No. 7), which is located one stage before the final-stage reaction tank, is also provided with a sulfide raw material B inlet for introducing a sulfide raw material B.
[0070] Furthermore, as described above, in the copper ion removal apparatus 1, the fifth-stage reaction tank (No. 5) is provided with an aqueous solution b inlet for supplying an aqueous nickel chloride solution b. In addition, the fifth-stage reaction tank may be provided with a sulfide raw material B inlet for introducing a sulfide raw material B.
[0071] The reducing power of the sulfide raw material A containing nickel sulfide added in the first cementation step S21 is weaker than that of the sulfide raw material B containing trimickel disulfide added in the second cementation step S22. In other words, the reduction reaction by the sulfide raw material A proceeds relatively slowly, while the sulfurization reaction by the sulfide raw material B proceeds relatively quickly. Therefore, in order to efficiently carry out the reduction treatment by the sulfide raw material A and the sulfurization treatment by the sulfide raw material B, it is advisable to limit the number of reaction tanks in which the sulfurization treatment is carried out to the bare minimum and to use the remaining reaction tanks for the reduction treatment.
[0072] On the other hand, because external factors may force a change in the processing ratio of sulfide raw material A and sulfide raw material B, a sulfide raw material B inlet for charging sulfide raw material B can be provided in the fifth-stage reaction tank to allow for flexible response. In that case, four tanks will be assigned to the first cementation process S21 where reduction treatment is performed, and four tanks will be assigned to the second cementation process S22 where sulfurization treatment is performed.
[0073] In the cementation treatment using the copper ion removal device 1 having the above-mentioned configuration, an aqueous nickel chloride solution a having a ratio of divalent copper ions of 60 to 100% is supplied from a starting solution inlet provided in the first-stage reaction tank (No. 1) and used for reduction treatment. An aqueous nickel chloride solution b having a ratio of divalent copper ions of 0 to 40% is supplied from a solution b inlet provided in the central reaction tank (the fifth-stage reaction tank (n / 2+1st stage when n is an even number)) and used for sulfurization treatment.
[0074] Here, although the sulfide raw material B is charged into the seventh and eighth reaction tanks to perform the second cementation step S22 of sulfurization treatment, the nickel chloride aqueous solution b is supplied to the fifth reaction tank because it is more efficient. In other words, the nickel chloride aqueous solution a, which has a ratio of divalent copper ions of 60 to 100% and is supplied to the first reaction tank, gradually undergoes a reduction reaction, so that by the time it reaches the fifth reaction tank, the ratio of divalent copper ions has decreased to the same level or lower than that of the nickel chloride aqueous solution b, which has a ratio of divalent copper ions of 0 to 40%. Basically, the nickel chloride aqueous solution b also contains divalent copper ions, so that the overall reduction reaction and sulfurization reaction can be most efficiently performed by adding the nickel chloride aqueous solution b to the fifth reaction tank.
[0075] In this way, for example, by performing a cementation treatment using the copper ion removal device 1, the nickel chloride aqueous solutions a and b, which are different in composition, particularly in terms of the divalent copper ion ratio, can be supplied to the reaction at appropriate timing from separate stages. This makes it possible to efficiently reduce the divalent copper ions in the nickel chloride aqueous solution a to monovalent copper ions in the first cementation step S21, and also makes it possible to more effectively remove copper ions from the copper-containing nickel chloride aqueous solution via fixation of the monovalent copper ions as sulfides in the second cementation step S22.
[0076] With regard to the copper ion removal apparatus 1, the cementation treatment is composed of two stages, namely, a reduction treatment (first cementation step S21) and a sulfurization treatment (second cementation step S22), and therefore at least two reaction tanks are required to constitute the apparatus. However, in a copper ion removal apparatus consisting of, for example, two reaction tanks in total, the capacity of the reaction tanks must be increased as the amount of treatment increases and the scale of the reaction increases, which not only results in huge equipment costs but is also undesirable from the viewpoint of maintainability. For this reason, it is preferable to configure the copper ion removal apparatus so that the total number of reaction tanks constituting the apparatus is four or more depending on the scale, and to configure the apparatus so that each of the reduction treatment and the sulfurization treatment is carried out in a plurality of reaction tanks.
[0077] In addition, when a solution is continuously supplied to a reaction tank, the residence time varies to a certain extent. Therefore, in a batch reaction, it is more advantageous to increase the capacity of the reaction tank in terms of cost, etc., but in a continuous reaction, it is overwhelmingly more advantageous to increase the number of reaction tanks rather than increasing the capacity of the reaction tank in terms of reaction stability and uniformity.
[0078] [Regarding ORP control of slurry obtained from the second cementation process] Although not essential, in the method according to the present embodiment, it is preferable to control the oxidation-reduction potential (ORP) (based on a silver / silver chloride electrode) of the second slurry obtained through the second cementation step S22 to be within a specific range. Specifically, it is preferable to control the ORP of the second slurry to be −100 mV or more and less than 0 mV, and it is more preferable to control the ORP to be −50 mV or more and less than 0 mV.
[0079] In this way, by controlling and treating the ORP of the obtained second slurry to be within the above-mentioned specific range, it is possible to efficiently remove not only copper ions but also silver, which is an impurity, from the copper-containing nickel chloride aqueous solution (chlorine leachate), and obtain a solution with an effectively reduced silver concentration. Note that the impurity silver is distributed to the cementation residue and removed together with copper fixed as sulfide through the second cementation step S22.
[0080] The method for controlling the ORP of the second slurry is not particularly limited, and can be carried out, for example, by adjusting the copper concentration of the copper-containing nickel chloride aqueous solution to be subjected to the cementation step S2.
[0081] 2. Method for producing nickel chloride aqueous solution from which copper ions have been removed The above-mentioned method for removing copper ions from the aqueous nickel chloride solution can be applied to the treatment in the cementation step S2 in the MCLE process. Therefore, it can be defined as a method (production method) for obtaining an aqueous nickel chloride solution from a raw material containing nickel, in which copper ions have been removed. In addition, since high-purity electric nickel can be obtained from the produced aqueous nickel chloride solution (aqueous nickel chloride solution from which copper ions have been removed) through electrolysis in the electrolysis step, it can also be defined as a production method for electric nickel.
[0082] Specifically, the method for producing an aqueous nickel chloride solution includes a chlorine leaching step S1 in which chlorine leaching is performed by blowing chlorine gas into a nickel-containing material slurry to obtain a chlorine leachate and a chlorine leach residue, and a cementation step S2 in which a cementation treatment is performed on the aqueous nickel chloride solution, which is the chlorine leachate, to obtain an aqueous nickel chloride solution from which copper ions have been removed.
[0083] FIG. 4 shows a process diagram for explaining the flow of the MCLE process for producing electrolytic nickel from raw nickel sulfide. As shown in the process flow in FIG. 4, a nickel chloride aqueous solution from which copper ions have been removed can be effectively produced by going through a chlorine leaching process S1 in which the nickel sulfide raw material is chlorine leached, and a cementation process S2 in which the obtained chlorine leachate is subjected to a cementation treatment to fix and remove copper ions. Although FIG. 1 and FIG. 4 are different notations, both are flow diagrams of the electrolytic nickel production process (MCLE process), and all of the "iron removal process", "cobalt solvent extraction process", and "liquid purification process" in FIG. 1 are included in the "liquid purification process S3" in FIG. 4. In addition, the "copper removal electrolysis process" shown in FIG. 1 is omitted in FIG. 4.
[0084] (Chlorine leaching process) In the chlorine leaching step S1, for example, nickel sulfide such as nickel matte produced by a nickel dry smelting method is used as a raw material to leach metals such as nickel with chlorine. Specifically, nickel in the nickel sulfide is leached by, for example, chlorine gas recovered in the electrolysis step S4 together with the cementation residue after the cementation step S2, to generate a copper-containing nickel chloride aqueous solution as a chlorine leachate.
[0085] The nickel sulfide used as the raw material is, for example, repulped and slurried with an aqueous nickel chloride solution (electrolysis waste liquid) obtained in the electrolysis step S4.
[0086] (Cementation process) In the cementation step S2, the nickel chloride aqueous solution containing copper ions (copper-containing nickel chloride aqueous solution), which is the chlorine leaching solution obtained in the chlorine leaching step S1, is subjected to reduction treatment and sulfurization treatment to fix and remove the copper ions in the aqueous solution as sulfides, thereby obtaining a nickel chloride aqueous solution with a reduced copper ion content (cementation end solution).
[0087] The above-mentioned copper ion removal method can be applied to the treatment (cementation treatment) in the cementation step S2.
[0088] Specifically, the cementation step S2 involves a cementation treatment including a first cementation step S21 in which a sulfide raw material A containing nickel sulfide is added to a copper-containing nickel chloride aqueous solution to reduce divalent copper ions in the nickel chloride aqueous solution to monovalent copper ions, and a second cementation step S22 in which a sulfide raw material B containing trinickel disulfide is added to the first slurry obtained in the first cementation step S21 to fix the monovalent copper ions contained in the first slurry as sulfides.
[0089] As the sulfide raw material A added in the first cementation step S21, a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material can be used. As the sulfide raw material B added in the second cementation step S22, nickel matte produced by a nickel pyrometallurgical process can be used.
[0090] In the cementation step S2, the nickel chloride aqueous solution to be subjected to the cementation treatment (to be treated) has a copper ion concentration of 20 to 80 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ +Cu + )) is 60-100%, and "nickel chloride aqueous solution a" has a copper ion concentration of 1-20g / L and the ratio of divalent copper ions (Cu 2+ / (Cu 2+ +Cu + )) is 0 to 40%. Two types of nickel chloride aqueous solutions, "nickel chloride aqueous solution b" and "nickel chloride aqueous solution c" with nickel chloride content of 0 to 40% are added separately to the optimal positions.
[0091] Specifically, in the first cementation step S21, a "nickel chloride aqueous solution a" is used as the nickel chloride aqueous solution for treatment, and in the second cementation step S22, in addition to the nickel chloride aqueous solution a, a "nickel chloride aqueous solution b" is further added and subjected to treatment.
[0092] According to such a method, the divalent copper ions contained in the copper-containing nickel chloride aqueous solution can be efficiently reduced to monovalent copper ions in the first cementation step S21, and the monovalent copper ions can be fixed as sulfides in the second cementation step S22, thereby effectively removing the copper ions from the nickel chloride aqueous solution.
[0093] Moreover, according to this method, it is possible to effectively remove copper ions without carrying out pretreatment such as reducing the copper ion concentration of the copper-containing nickel chloride aqueous solution to be subjected to the treatment in the cementation step S2. Therefore, in consideration of the circulation cycle of the nickel hydrometallurgical refining process, it is possible to effectively prevent a situation in which the copper ions functioning as ion carriers for chlorine gas absorption become insufficient, resulting in a deterioration in the leaching rate in the chlorine leaching step S1.
[0094] Furthermore, since copper ions can be efficiently removed, the copper concentration of the chlorine leaching solution can be intentionally increased to improve the leaching rate in the chlorine leaching step S1, i.e., the nickel recovery rate.
[0095] Furthermore, an increase in the reduction treatment capacity in the first cementation step S21 means an increase in the treatment capacity of the sulfide raw material A containing nickel sulfide, making it possible to treat a larger amount of raw material.
[0096] Here, the cementation residue containing copper sulfide obtained through the treatment in the cementation step S2 is repeatedly returned to the chlorine leaching step S1 as described above, and is subjected to leaching treatment with chlorine gas together with new nickel sulfide raw material. At this time, if a pretreatment is performed to reduce the copper ion concentration from the chlorine leaching solution prior to the treatment in the cementation step S2 in order to obtain an aqueous nickel chloride solution in which copper ions are effectively reduced in the cementation step S2, the amount of cementation residue obtained is reduced, and the amount of copper circulated to the chlorine leaching step S1 is reduced. In the chlorine leaching treatment, copper ions are an important element that functions as an ion carrier for chlorine gas absorption, so a decrease in the amount of copper circulated means a decrease in the chlorine leaching rate.
[0097] Fig. 5 is a graph showing the relationship between the copper ion concentration in the starting solution in the cementation step S2 (chlorine leachate, which is a copper-containing nickel chloride aqueous solution) and the nickel grade in the chlorine leach residue obtained from the chlorine leach step S1. As the copper ion concentration in the starting solution in the cementation step S2 is lower, the copper ion concentration in the nickel chloride aqueous solution obtained through the treatment in the cementation step S2 is further reduced, but as shown in the graph in Fig. 5, it can be seen that the nickel grade contained in the chlorine leach residue is higher.
[0098] This indicates that the lower the copper ion concentration in the starting solution in the cementation step S2, the less copper there is in the cementation residue, and the less copper circulates to the chlorine leaching step S1, i.e., the less copper functions as an ion carrier for absorbing chlorine gas. As a result, the chlorine leaching rate in the chlorine leaching step S1 decreases, and the nickel that should have been leached is lost as it is contained in the chlorine leaching residue.
[0099] In this respect, the method according to the present embodiment can effectively remove copper ions without carrying out pretreatment such as reducing the copper ion concentration of the aqueous nickel chloride solution to be subjected to the treatment in the cementation step S2, and therefore the amount of copper contained in the cementation residue is secured. Then, by circulating the cementation residue to the treatment in the chlorine leaching step S1 and subjecting it to the chlorine leaching treatment, a sufficient amount of copper comes to function as an ion carrier for absorbing chlorine gas, and the chlorine leaching treatment can be carried out effectively and efficiently. EXAMPLES
[0100] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0101] [Example 1] In the MCLE process, the chlorine leachate (nickel chloride aqueous solution a) obtained through the chlorine leaching process was added to the first cementation step in the cementation process for treatment. In the first cementation step, nickel-cobalt mixed sulfide (MS) containing nickel sulfide was added to the nickel chloride aqueous solution a to perform a reduction treatment to reduce the divalent copper ions in the aqueous solution to monovalent copper ions. The composition of the nickel chloride aqueous solution a used for treatment is shown in Table 2 below.
[0102] In the cementation step, as the second cementation step, nickel matte containing trinickel disulfide was added to the first slurry obtained through the first cementation step, and a sulfurization treatment was carried out to fix the monovalent copper ions contained in the first slurry as sulfides. In this case, in Example 1, the electrolytic waste liquid (nickel chloride aqueous solution b) obtained through the copper removal electrolysis step was added to the latter stage of the reduction treatment, and then subjected to the sulfurization treatment. The composition of the nickel chloride aqueous solution b used in the treatment is shown in Table 2 below.
[0103] [Table 2]
[0104] In this way, by adding the copper removal electrolysis waste liquid (nickel chloride aqueous solution b) at the latter stage of the reduction treatment, i.e., just before the treatment in the second cementation process, the oxidation-reduction potential (ORP) (based on a silver / silver chloride electrode) just before the reaction in the second cementation process became 355 mV.
[0105] Generally, it is known that copper ions become almost entirely monovalent copper ions at 380 mV or less. This means that the sulfide reduction treatment by MS in the first cementation step reduced almost all of the copper ions (divalent copper ions) contained in the nickel chloride aqueous solution a to monovalent copper ions.
[0106] As a result of this treatment in the cementation process, the copper ion concentration in the final cementation solution was 0.009g / L, which fully achieved the target copper ion concentration. The copper concentration in the chlorine leachate was 48g / L.
[0107] In addition, the cementation residue obtained through the cementation process was recycled and transferred to the chlorine leaching process, and treatment was carried out in the chlorine leaching process as per normal operations. As a result, the nickel content of the chlorine leaching residue was 2.4 mass%, which was a good result.
[0108] [Comparative Example 1] In Comparative Example 1, the chlorine leaching solution (nickel chloride aqueous solution a) and the copper removal electrolytic waste liquid (nickel chloride aqueous solution b) were added together to the first cementation step for treatment. In other words, unlike Example 1, the copper removal electrolytic waste liquid (nickel chloride aqueous solution b) was not added immediately before the treatment in the second cementation step.
[0109] As a result of this treatment, the ORP just before the reaction in the second cementation process only dropped to 409 mV. This indicates that some of the copper ions contained in the aqueous solution used in the cementation treatment were not reduced and remained as divalent copper ions.
[0110] In order to avoid problems occurring in the second cementation process, there was no choice but to reduce the copper concentration of the cementation starting solution. The copper concentration of the chlorine leaching solution was 42 g / L, and the nickel content of the chlorine leaching residue obtained after the chlorine leaching process was 4.8 mass%.
[0111] The results of the treatment in Example 1 and Comparative Example 1 are summarized in Table 3 below. The values in the table are the average values of the test results obtained by performing the treatment multiple times under the same conditions. The graph in Figure 6 is a graph of the results of the treatment in Example 1 and Comparative Example 1.
[0112] [Table 3]
Claims
1. A method for removing copper ions from a nickel chloride aqueous solution containing copper ions, comprising the steps of: a first cementation step of adding a sulfide raw material A containing nickel sulfide to the nickel chloride aqueous solution and reducing divalent copper ions in the nickel chloride aqueous solution to monovalent copper ions; a second cementation step of adding a sulfide raw material B containing trinickel disulfide to the first slurry obtained in the first cementation step, and immobilizing the monovalent copper ions contained in the first slurry as sulfides; The nickel chloride aqueous solution to be treated has a copper ion concentration of 20 to 80 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ + Cu + )) is 60 to 100%, and the copper ion concentration is 1 to 20 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ + Cu + )) is 0 to 40%. In the first cementation step, the nickel chloride aqueous solution a is used as the nickel chloride aqueous solution for treatment, In the second cementation step, the nickel chloride aqueous solution b is further added to the nickel chloride aqueous solution a and subjected to treatment. A method for removing copper ions from an aqueous nickel chloride solution.
2. The cementation treatment is carried out using a copper ion removal apparatus having a total of n reaction tanks (n is an integer of 4 or more) connected in series; In the copper ion removal apparatus, The nickel chloride aqueous solution a is supplied to a first-stage reaction tank located at the most upstream position, and the sulfide raw material A is also charged therein; The sulfide raw material B is charged into a final stage (nth stage) reaction tank located at the most downstream and an (n-1)th stage reaction tank located one stage before the final stage reaction tank, The nickel chloride aqueous solution b is supplied to a reaction tank located in the center (however, when n is an even number, the reaction tank in the n / 2+1 stage). The method for removing copper ions from an aqueous nickel chloride solution according to claim 1.
3. The sulfide raw material A is a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material, The sulfide raw material B is nickel matte produced by a nickel dry smelting method.
3. The method for removing copper ions from an aqueous nickel chloride solution according to claim 1 or 2.
4. a copper removal electrolysis step of recovering copper powder and obtaining electrolytic waste liquid by electrowinning using a part of the first slurry obtained through the first cementation step as an initial liquid, In the cementation treatment, the electrolytic waste liquid obtained from the copper removal electrolysis step is used as the nickel chloride aqueous solution b. The method for removing copper ions from an aqueous nickel chloride solution according to claim 2.
5. A method for obtaining an aqueous nickel chloride solution by removing copper ions from a raw material containing nickel, comprising the steps of: a chlorine leaching step of blowing chlorine gas into the nickel-containing slurry to perform chlorine leaching to obtain a chlorine leaching solution and a chlorine leaching residue; a cementation step of performing the cementation treatment for carrying out the copper ion removal method according to claim 1 on the nickel chloride aqueous solution containing copper ions, which is the chlorine leachate, to obtain a nickel chloride aqueous solution from which copper ions have been removed, The slurry produced in the cementation step is subjected to solid-liquid separation to obtain a cementation residue, and the slurry of the cementation residue (residue slurry) is transferred to the chlorine leaching step; In the chlorine leaching step, chlorine leaching is performed by blowing chlorine gas into the nickel-containing material slurry containing the residue slurry. Method for producing nickel chloride aqueous solution.
6. The method further includes a copper removal electrolysis step of recovering copper powder and obtaining electrolytic waste liquid by electrowinning using a part of the first slurry obtained through the first cementation step in the cementation step as an initial liquid, The nickel chloride aqueous solution to be subjected to the cementation step includes: The nickel chloride aqueous solution a is the chlorine leaching solution obtained from the chlorine leaching step, The nickel chloride aqueous solution b is the electrolytic waste liquid obtained from the copper removal electrolysis step. The method for producing the nickel chloride aqueous solution according to claim 5.
7. By adjusting the copper concentration of the chlorine leachate to be subjected to the cementation step, the oxidation-reduction potential (based on a silver / silver chloride electrode) of the second slurry obtained through the second cementation step is controlled to be −100 mV or more and less than 0 mV. The method for producing an aqueous nickel chloride solution according to claim 5 or 6.
Citation Information
Patent Citations
Chlorination refining method for high-iron low-nickel sulphonium
CN107385233A
Copper removing electorlysis method for copper- containing nickel chloride solution
JP2001115288A
Method for removing copper ion of aqueous nickel chloride solution and apparatus for removal treatment of copper ion
JP2017155281A
Copper removal method, method for producing electrolytically refined nickel
JP2018199858A
Copper removal electrolytic treatment method, copper removal electrolytic treatment device
JP2019178353A