Copper ion removal method from aqueous nickel chloride solution and production method of aqueous nickel chloride solution

The method of adding sulfide raw materials with high nickel and iron content in a two-step cementation process addresses the inefficiency of copper ion removal in nickel chloride solutions, enhancing copper ion conversion to sulfides, improving electrolytic nickel quality and reducing nickel loss in the electrolytic nickel manufacturing process.

JP2024145682APending Publication Date: 2024-10-15SUMITOMO METAL MINING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023058137
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The challenge in the electrolytic nickel manufacturing process is the inefficient removal of copper ions from nickel chloride solutions, leading to impurities in the electrolytic nickel, which affects its quality and increases nickel loss due to insufficient cementation reactions when high copper concentrations are maintained to reduce nickel loss.

Method used

A method involving the addition of sulfide raw materials with high nickel and iron content to nickel chloride solutions, utilizing a two-step cementation process to convert copper ions into sulfides, including a reduction step with nickel sulfide and a sulfurization step with trinickel disulfide, optimizing the addition of these materials across multiple reaction tanks to enhance copper ion removal efficiency.

Benefits of technology

This approach effectively reduces copper ions in nickel chloride solutions, improving the quality of electrolytic nickel and reducing nickel loss by enhancing the chlorine leaching rate without altering raw material ratios, thus stabilizing the nickel hydrometallurgical process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145682000001_ABST
    Figure 2024145682000001_ABST
Patent Text Reader

Abstract

To provide a method for efficiently removing copper ions, from an aqueous nickel chloride solution including copper ions.SOLUTION: There is provided a method for removing copper ions from an aqueous nickel chloride solution including copper ions, comprising: a first cementation step for adding a sulfide raw material A including nickel sulfide to the aqueous nickel chloride solution, for reducing bivalent copper ions in the aqueous nickel chloride solution to monovalent copper ions; and a second cementation step for adding a sulfide raw material B including disulfide nickel to first slurry acquired in the first cementation step, for stabilizing the monovalent copper ion included in the first slurry as a sulfide, in the second cementation step, in addition to the sulfide raw material B, a sulfide raw material C in which a total content of metallic iron and metallic nickel is 60 to 85 mass% is added to first slurry.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a technique for removing copper contained in an aqueous nickel chloride solution. More specifically, the present invention relates to a method for removing copper ions from an aqueous nickel chloride solution in, for example, a cementation step in a nickel hydrometallurgical process, and a method for producing an aqueous nickel chloride solution from which copper ions have been removed. [Background technology]

[0002] In the process of producing electrolytic nickel from raw materials such as nickel sulfide, the step of removing copper ions, which are impurities, from an aqueous solution of nickel chloride is an important step.

[0003] Specifically, in the manufacturing process of electrolytic nickel, nickel raw material such as nickel sulfide is leached with chlorine to obtain a chlorine leachate, from which high-purity electrolytic nickel is electrowinning, but the chlorine leachate obtained by chlorine leaching usually contains copper ions at a ratio of about several tens of g / L. Therefore, a process (rough copper removal) is carried out to remove copper ions from the copper-containing nickel chloride aqueous solution, which is the obtained chlorine leachate, to a concentration range of several tens of mg / L or less, and then a purification process is carried out to remove other remaining impurity elements such as iron and cobalt, thereby further reducing the concentration to a low level, thereby obtaining an electrolyte to be subjected to electrolytic treatment (for example, Patent Document 1).

[0004] One method for removing copper ions from copper-containing nickel chloride aqueous solutions is the cementation reaction, which uses the difference in standard electrode potential between different metal elements to carry out an exchange reaction between compounds and ions, and is widely used in fields such as wastewater treatment and metal refining.

[0005] Here, in the process for producing electrolytic nickel, when a sulfide raw material A containing nickel sulfide and a sulfide raw material B containing nickel disulfide are used as raw materials, if these raw materials are added to a copper-containing nickel chloride aqueous solution obtained by chlorine leaching to remove copper ions, the copper ions can be removed and nickel in the raw materials can be leached simultaneously, which is efficient. This method has been industrialized in nickel hydrometallurgy plants as shown in Patent Document 1.

[0006] The manufacturing process of electrolytic nickel utilizing such a cementation reaction includes a chlorine leaching step in which raw materials such as nickel sulfide are leached with chlorine, and a cementation step in which copper ions are removed from the chlorine leaching solution (copper-containing nickel chloride aqueous solution).

[0007] In the chlorine leaching process, nickel is leached by blowing chlorine gas into the cementation residue, which contains raw materials such as nickel sulfide, copper sulfide fixed in the cementation process, and unreacted sulfide raw materials A and B that did not contribute to the cementation reaction. The reaction in the chlorine leaching process proceeds through the oxidation-reduction reaction of monovalent and divalent Cu ions, in other words, Cu ions function as ion carriers that absorb chlorine gas, so the nickel grade in the chlorine leaching residue decreases as the copper concentration in the chlorine leaching solution increases.

[0008] Therefore, the higher the copper concentration in the chlorine leaching solution obtained through the treatment in the chlorine leaching process and the larger the amount of copper circulated in the form of cementation residue through the cementation process, the higher the chlorine leaching rate can be, and the lower the nickel grade in the chlorine leaching residue, making it possible to reduce nickel loss.

[0009] However, if the copper concentration in the chlorine leaching solution is increased to reduce nickel loss, the reaction (cementation reaction) does not proceed sufficiently in the cementation step, and there is a high risk of copper removal failure. In the manufacturing process of electrolytic nickel, if copper removal failure occurs in the cementation step, copper as an impurity element remains in the electrolyte used for electrowinning of electrolytic nickel, deteriorating the quality of the electrolytic nickel. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2017-155281 A Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been proposed in view of the above circumstances, and an object of the present invention is to provide a method for efficiently removing copper ions from an aqueous nickel chloride solution containing copper ions. [Means for solving the problem]

[0012] The present inventors have conducted extensive research and have found that the above-mentioned problems can be solved by adding a sulfide raw material having a relatively high content of metallic nickel and metallic iron to the nickel chloride aqueous solution in a cementation treatment of the aqueous solution of nickel chloride containing copper ions, thereby immobilizing copper as an impurity as a sulfide, and have thus completed the present invention.

[0013] (1) A first aspect of the present invention is a method for removing copper ions from an aqueous nickel chloride solution containing copper ions, comprising: a first cementation step of adding a sulfide raw material A containing nickel sulfide to the aqueous nickel chloride solution and reducing divalent copper ions in the aqueous nickel chloride solution to monovalent copper ions; and a second cementation step of adding a sulfide raw material B containing nickel disulfide to a first slurry obtained in the first cementation step and immobilizing the monovalent copper ions contained in the first slurry as sulfides. In the second cementation step, a sulfide raw material C having a total content of metallic nickel and metallic iron of 60 to 85 mass% is added to the first slurry together with the sulfide raw material B.

[0014] (2) A second aspect of the present invention is a method for removing copper ions from an aqueous nickel chloride solution, wherein an added amount of the sulfide raw material C in the first aspect of the invention is 5 to 30% in terms of nickel amount ratio with respect to a total added amount of the sulfide raw material B and the sulfide raw material C.

[0015] (3) A third invention of the present invention is a method for removing copper ions from an aqueous nickel chloride solution according to the first or second invention, wherein the cementation treatment is carried out using a copper ion removal apparatus having a total of n reaction tanks (n is an integer of 4 or more) connected in series, and in the copper ion removal apparatus, the sulfide raw material A is charged into a first stage reaction tank located at the most upstream position, the sulfide raw material B is charged into a final stage (n stage) reaction tank located at the most downstream position and an (n-1) stage reaction tank located one stage before the final stage reaction tank, and the sulfide raw material C is charged into the (n-1) stage reaction tank.

[0016] (4) The fourth aspect of the present invention is any one of the first to third aspects of the present invention, wherein the nickel chloride aqueous solution to be treated has a copper ion concentration of 20 to 80 g / L and a ratio of divalent copper ions (Cu 2+ / (Cu 2+ +Cu +)) is 60 to 100%, and the copper ion concentration is 1 to 20 g / L and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ +Cu + and a nickel chloride aqueous solution b having a nickel chloride concentration of 0 to 40%. In the first cementation step, the nickel chloride aqueous solution a is used as the nickel chloride aqueous solution for treatment, and in the second cementation step, in addition to the nickel chloride aqueous solution a, the nickel chloride aqueous solution b is further added and used for treatment.

[0017] (5) A fifth aspect of the present invention is a method for removing copper ions from an aqueous nickel chloride solution according to the fourth aspect of the present invention, wherein the cementation treatment is carried out using a copper ion removal apparatus having a total of n reaction tanks (n is an integer of 4 or more) connected in series, and the nickel chloride aqueous solution a is supplied to a first-stage reaction tank located at the most upstream in the copper ion removal apparatus, and the sulfide raw material A is charged therein, the sulfide raw material B is charged to a final-stage (n-th) reaction tank located at the most downstream and an (n-1)-th reaction tank located one stage before the final-stage reaction tank, the sulfide raw material C is charged into the (n-1)-th reaction tank, and the nickel chloride aqueous solution b is supplied to a central reaction tank (however, when n is an even number, the (n / 2+1)-th reaction tank).

[0018] (6) A sixth aspect of the present invention is a method for removing copper ions from an aqueous nickel chloride solution according to any one of the first to fifth aspects of the present invention, wherein the sulfide raw material A is a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material, and the sulfide raw material B and the sulfide raw material C are nickel matte produced by a nickel dry smelting method.

[0019] (7) A seventh aspect of the present invention is a method for obtaining an aqueous nickel chloride solution from a raw material containing nickel, the method comprising: a chlorine leaching step of blowing chlorine gas into a nickel-containing material slurry to perform chlorine leaching to obtain a chlorine leachate and a chlorine leach residue; and a cementation step of performing the cementation treatment for performing the copper ion removal method according to claim 1 on the aqueous nickel chloride solution containing copper ions, which is the chlorine leachate, to obtain the aqueous nickel chloride solution from which the copper ions have been removed. The slurry produced in the cementation step is subjected to solid-liquid separation to obtain a cementation residue, and the slurry of the cementation residue (residue slurry) is transferred to the chlorine leaching step. In the chlorine leaching step, chlorine leaching is performed by blowing chlorine gas into the nickel-containing material slurry containing the residue slurry. This is a method for producing an aqueous nickel chloride solution.

[0020] (8) An eighth aspect of the present invention is a method for producing an aqueous nickel chloride solution, wherein an amount of the sulfide raw material C added is 5 to 30% in terms of nickel amount ratio with respect to a total amount of the sulfide raw material B and the sulfide raw material C added in the seventh aspect.

[0021] (9) A ninth aspect of the present invention is a method for producing an aqueous nickel chloride solution according to the seventh or eighth aspect of the present invention, wherein the cementation treatment is carried out using a copper ion removal apparatus having a total of n reaction tanks (n is an integer of 4 or more) connected in series, and in the copper ion removal apparatus, the sulfide raw material A is charged into a first stage reaction tank located at the most upstream position, the sulfide raw material B is charged into a final stage (nth stage) reaction tank located at the most downstream position and an (n-1)th stage reaction tank located one stage before the final stage reaction tank, and the sulfide raw material C is charged into the (n-1)th stage reaction tank. Effect of the Invention

[0022] According to the present invention, it is possible to provide a method for efficiently removing copper ions from an aqueous nickel chloride solution containing copper ions.

[0023] As a result, when applied to a nickel hydrometallurgical process, it is possible to increase the copper concentration in the nickel chloride aqueous solution (chlorine leachate) without significantly changing the raw material ratio or total processing volume. As a result, it is possible to effectively reduce the nickel loss discharged outside the system by lowering the nickel grade in the chlorine leach residue. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a process diagram showing a schematic flow of a nickel hydrometallurgical process (MCLE process). [Diagram 2] FIG. 2 is a process diagram showing an example of a cementation process flow. [Diagram 3] FIG. 1 is a schematic diagram showing an example of the configuration of a copper ion removal device. [Figure 4] FIG. 1 is a process diagram illustrating the flow of the MCLE process for producing electrolytic nickel from raw nickel sulfide. [Diagram 5] FIG. 1 is a graph showing the test results of Test Example 1, and is a graph showing the relationship between the total added amounts of sulfide raw materials B and C added in the second cementation step and the difference in the addition position of sulfide raw material C. [Figure 6] FIG. 13 is a graph showing the test results of Test Example 2, and is a graph showing the relationship of the copper reduction efficiency in the second cementation step to the amount of sulfide raw material C added. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, a specific embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail with reference to the drawings. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention.

[0026] ≪1. Method for removing copper ions from nickel chloride solution≫ The method for removing copper ions according to the present embodiment is a method for removing copper ions from an aqueous nickel chloride solution containing the copper ions.

[0027] For example, the copper-containing nickel chloride aqueous solution to be treated is a copper-containing nickel chloride aqueous solution (chlorine leachate) obtained by chlorine leaching of raw nickel sulfide in a nickel hydrometallurgy process (MCLE process).The copper ion removal method can be applied to the treatment in the cementation step in the MCLE process.

[0028] 2 is a process diagram showing an example of the flow of cementation treatment for carrying out this method. Specifically, this method includes a first cementation step S21 in which a sulfide raw material A containing nickel sulfide is added to a copper-containing nickel chloride aqueous solution to reduce divalent copper ions in the nickel chloride aqueous solution to monovalent copper ions, and a second cementation step S22 in which a sulfide raw material B containing trinickel disulfide is added to a first slurry obtained in the first cementation step S21 to fix the monovalent copper ions contained in the first slurry as sulfides.

[0029] The treatment in the first cementation step S21 is also called a “reduction treatment,” and the treatment in the second cementation step S22 is also called a “sulfurization treatment.” An overview of each of the first cementation step S21 and the second cementation step S22 will be described below.

[0030] <1-1. About the cementation process> [First cementation process S21] First, in the first cementation step S21, a sulfide raw material A containing nickel sulfide (NiS) is added to the copper-containing nickel chloride aqueous solution (chlorine leachate) to be treated, thereby reducing the copper ions in the aqueous solution. As the sulfide raw material A, a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material can be used.

[0031] In the first cementation step S21, it is presumed that a reduction reaction of copper ions occurs, for example, as shown in the following formulas [1] and [2]. 4NiS+2Cu 2+ → Ni 2+ +Ni3S4+2Cu + [1] NiS+2Cu + → Ni 2+ +Cu2S [2]

[0032] As shown in formula [1] above, in the reduction treatment in the first cementation step S21, a sulfide raw material A containing nickel sulfide is added to the nickel chloride aqueous solution, and the nickel sulfide reduces the divalent copper ions in the aqueous solution to monovalent copper ions. The copper ions thus reduced are fixed as copper sulfides by the sulfide raw material B added in the next step, the second cementation step S22.

[0033] The temperature conditions for the reduction treatment in the first cementation step S21 are not particularly limited, and may be in the range of about 80 to 110° C., and preferably in the range of 80 to 90° C. By performing the treatment under such temperature conditions, the oxidation-reduction potential (based on a silver / silver chloride electrode) of the first slurry obtained through the treatment can be set to about 350 to 420 mV. In order to increase the reaction temperature, steam or the like can be used for temperature increase operation.

[0034] [Second cementation process S22] (About sulfurization treatment) Next, in the second cementation step S22, a sulfide raw material B containing trinickel disulfide (nickel subsulfide, Ni3S2) is added to the first slurry obtained through the first cementation step S21, and the monovalent copper ions in the slurry are precipitated and removed as copper sulfide. As the sulfide raw material B, nickel matte produced by a nickel dry smelting method can be used. The nickel matte contains trinickel disulfide and nickel metal.

[0035] In the second cementation step S22, for example, sulfurization reactions represented by the following formulas [3] to [5] are presumed to occur. Note that the following reaction formulas are reaction formulas when nickel matte is used as the sulfide raw material B. Ni 0 +Cu 2+ →Ni 2+ +Cu + [3] Ni3S4+6Cu + →3Ni 2+ +S+3Cu2S [4] Ni3S2+6Cu + +S→3Ni 2+ +3Cu2S [5]

[0036] As shown in the above formulas [3] to [5], the trinickel disulfide (Ni3S2) and nickel metal (Ni) contained in the added nickel matte cause a reaction (sulfurization treatment) in which monovalent copper ions are precipitated and removed as solids. As a result, the copper ions contained in the copper-containing nickel chloride aqueous solution are fixed and removed mainly as copper sulfide.

[0037] (Concurrent use of sulfide raw material C) Here, the copper ion removal method according to the present embodiment is characterized in that in the second cementation step S22, the above-mentioned sulfide raw material B is added to the first slurry, and further a sulfide raw material C having a total content of metallic nickel and metallic iron of 60 to 85 mass % is added, and then treatment is performed.

[0038] In this way, by using a sulfide raw material C such as nickel matte having a high content of metallic nickel and metallic iron, it is possible to promote the reduction of divalent copper ions remaining in the first slurry, as shown in the following formulas [6] and [7]. Fe 0 +2Cu 2+ → Fe 2+ +2Cu + [6] Ni 0 +2Cu 2+ → Ni 2+ +2Cu +[7]

[0039] By promoting the reduction of copper ions in this way, the amount of copper ions that undergo the sulfurization reaction with the monovalent copper ions obtained by reduction (reaction equations [4] and [5] above) increases, making it possible to carry out a more sufficient cementation process.

[0040] By subjecting the nickel chloride aqueous solution (final cementation solution) obtained by applying such a removal method to the manufacturing process of electrolytic nickel, the content of copper ions in the aqueous solution is effectively reduced, making it possible to obtain highly pure electrolytic nickel.

[0041] In addition, when the chlorine leachate obtained through the chlorine leaching step S1 in the nickel hydrometallurgy process (MCLE process) is used as the copper-containing nickel chloride aqueous solution to be treated, the copper ions can be effectively removed without taking measures such as reducing the copper ion concentration of the nickel chloride aqueous solution. In other words, the copper concentration in the chlorine leachate can be increased without significantly changing the raw material ratio or the total processing amount, and as a result, it is possible to effectively reduce the nickel loss discharged outside the system by reducing the nickel grade in the chlorine leach residue. In other words, when considering the circulation cycle of the nickel hydrometallurgy process, it is possible to effectively prevent a situation in which the copper ions functioning as ion carriers for chlorine gas absorption are insufficient and the chlorine leach rate in the chlorine leaching step S1 deteriorates.

[0042] Furthermore, since copper ions can be efficiently removed, the copper concentration of the chlorine leaching solution can be intentionally increased to improve the leaching rate in the chlorine leaching step S1, i.e., the nickel recovery rate.

[0043] Regarding sulfide raw material C, if the total content of metallic nickel and metallic iron is less than 60 mass%, the metallic (Ni 0 , Fe 0Since the ratio of nickel and iron present in the form of sulfides (NiS, Ni3S2, FeS, Fe3S2, etc.) increases rather than in the form of sulfides (NiS, Ni3S2, FeS, Fe3S2, etc.) increases, an improvement in the reduction efficiency of copper ions cannot be expected. On the other hand, if the total content of metallic nickel and metallic iron exceeds 85 mass%, although an improvement in the reduction efficiency of copper ions can be expected, for example, in the dry smelting process for producing nickel matte, matte with a high iron quality is obtained, and the removal of iron in the subsequent process requires cost and effort, and there is a possibility that the overall operation efficiency will decrease. In other words, an increase in the total content of metallic nickel and metallic iron is likely to lead to an increase in the input amount of iron as an impurity. Moreover, when the reduction degree is increased in order to increase the total content of metallic nickel and metallic iron in the production of sulfide raw material C, considering the ease of reduction of nickel and iron, only metallic iron will increase, which is not preferable.

[0044] The amount of sulfide raw material C added is not particularly limited, but is preferably 5 to 30 mass % in terms of nickel ratio, and more preferably 10 to 25 mass % in terms of nickel ratio, relative to the total amount of sulfide raw material B and sulfide raw material C. By adding sulfide raw material C in such an amount, the reduction efficiency of copper ions can be more effectively increased.

[0045] As the sulfide raw material C, nickel matte or the like produced by a nickel dry smelting method can be used, similar to the sulfide raw material B. Among the nickel matte or the like, one having a relatively high total content of metallic nickel and metallic iron can be used.

[0046] In the second cementation step S22, a chlorine leaching residue may be added as a sulfur source to more efficiently immobilize the monovalent copper ions as sulfides. The chlorine leaching residue is a residue remaining in the solid phase in the chlorine leaching step S1 in the MCLE process, and its main component is sulfur. By adding this as a sulfur source, the monovalent copper ions can be immobilized as copper sulfide together with the nickel matte.

[0047] [Solid-liquid separation step S23] The second slurry obtained through the sulfurization treatment in the second cementation step S22 is composed of a cementation residue containing sulfide of sulfurized copper and a final cementation liquid which is an aqueous nickel chloride solution from which copper has been removed. Therefore, by subjecting the second slurry to a solid-liquid separation treatment (solid-liquid separation step S23), the final cementation liquid and the cementation residue can be separated and recovered.

[0048] <1-2. Nickel chloride aqueous solution used as the starting solution for treatment> The copper concentration of the copper-containing nickel chloride aqueous solution, which is the reaction starting liquid in the cementation step S2, is preferably adjusted according to the addition ratios of the sulfide raw materials A, B, and C. For example, the sulfide raw material A, which is mainly composed of nickel sulfide (NiS), has a lower copper ion reducing power than the sulfide raw materials B and C. Therefore, for example, under the condition of the same nickel processing amount, when the addition ratio of the sulfide raw material A is increased, it is necessary to reduce the copper ions with less of the sulfide raw materials B and C in the second cementation step S22, and therefore it is necessary to lower the copper concentration of the nickel chloride aqueous solution, which is the reaction starting liquid. In addition, the strength of the reducing power depends on the sulfide raw material C (Fe 0 , Ni 0 ) > sulfide raw material B (Ni3S2) > sulfide raw material A (NiS), it is more efficient to have sulfide raw material A mainly responsible for the reduction of divalent copper ions, and sulfide raw materials B and C mainly responsible for the reduction of monovalent copper ions.

[0049] Therefore, in the method according to the present embodiment, preferably, two types of nickel chloride aqueous solutions having different ratios of divalent copper ions in the copper ions are used separately.

[0050] That is, the nickel chloride aqueous solution to be subjected to the cementation treatment (to be treated) has a copper ion concentration of 20 to 80 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ +Cu +)) is 60-100%, and "nickel chloride aqueous solution a" has a copper ion concentration of 1-20g / L and the ratio of divalent copper ions (Cu 2+ / (Cu 2+ +Cu + It is preferable to add two types of nickel chloride aqueous solutions, "aqueous nickel chloride solution b" having an average nickel chloride concentration of 0 to 40% and "aqueous nickel chloride solution b" having an average nickel chloride concentration of 0 to 40% respectively, separately at optimal positions.

[0051] Specifically, in the first cementation step S21, a "nickel chloride aqueous solution a" is used as the nickel chloride aqueous solution for treatment, and in the second cementation step S22, in addition to the nickel chloride aqueous solution a, a "nickel chloride aqueous solution b" is further added and then subjected to treatment.

[0052] The "aqueous nickel chloride solution a" is not particularly limited, but for example, a chlorine leachate obtained through the chlorine leach step S1 in a nickel hydrometallurgical process (MCLE process) can be used.

[0053] The method according to the present embodiment may further include a copper removal electrolysis step in which copper powder is recovered by electrowinning using a part of the first slurry obtained through the first cementation step S21 as a starting solution, and an electrolysis waste liquid is obtained. In this case, the electrolysis waste liquid (copper removal electrolysis waste liquid) obtained from the copper removal electrolysis step may be used as the "nickel chloride aqueous solution b".

[0054] Table 1 below shows an example of the liquid composition of the "chlorine leaching solution" used as the "nickel chloride aqueous solution a" and the "decopper electrolysis waste liquid" used as the "nickel chloride aqueous solution b".

[0055] [Table 1]

[0056] As shown in the composition example in Table 1, the chlorine leaching solution (nickel chloride aqueous solution a) has high nickel and copper concentrations, and is also at a relatively high temperature. In addition, due to its high oxidation-reduction potential (ORP), almost all of the copper ions in the solution exist in the form of divalent copper ions. On the other hand, the copper removal electrolysis waste solution (nickel chloride aqueous solution b) has low nickel and copper concentrations, and is also at a relatively low temperature. In addition, due to its low ORP, almost all of the copper ions in the solution exist in the form of monovalent copper ions.

[0057] Therefore, even if the decoppering electrolysis waste liquid (nickel chloride aqueous solution b) is subjected to treatment in the first cementation step S21, it hardly reacts with the sulfide raw material A. When performing treatment in the first cementation step S21, if the nickel chloride aqueous solution to be treated contains an aqueous solution with a high ratio of monovalent copper ions, such as nickel chloride aqueous solution b, the divalent copper ions in the chlorine leachate (nickel chloride aqueous solution a) are diluted with the monovalent copper ions, decreasing the ratio of divalent copper ions, and the efficiency of reduction of divalent copper ions to monovalent copper ions by the sulfide raw material A decreases.

[0058] Therefore, as described above, in the first cementation step S21, "nickel chloride aqueous solution a" is used as the nickel chloride aqueous solution for treatment, and in the second cementation step S22, in addition to the nickel chloride aqueous solution a, "nickel chloride aqueous solution b" is further added to the first slurry for treatment. By carrying out treatment in this manner, it is possible to efficiently reduce the divalent copper ions contained in the nickel chloride aqueous solution to be treated (nickel chloride aqueous solution a) to monovalent copper ions in the first cementation step S21, and to more effectively remove the copper ions from the nickel chloride aqueous solution through fixation of the monovalent copper ions as sulfides in the second cementation step S22.

[0059] Moreover, the most effective means for reducing as many divalent copper ions as possible to monovalent copper ions in the first cementation step S21 is to extend the reaction time, i.e., the residence time in the reaction tank. Therefore, by not subjecting the copper removal electrolytic waste liquid (nickel chloride aqueous solution b) to treatment in the first cementation step S21 or adding it further downstream of the first cementation step S21, the treatment flow rate in the first cementation step S21 is reduced, and the residence time of the nickel chloride aqueous solution (nickel chloride aqueous solution a) is extended accordingly. This allows the divalent copper ions contained in the nickel chloride aqueous solution (nickel chloride aqueous solution a) to be treated in the first cementation step S21 to be efficiently reduced to monovalent copper ions.

[0060] (About nickel chloride solution a) The nickel chloride aqueous solution a is the starting solution for the cementation treatment. As described above, the nickel chloride aqueous solution a has a copper ion concentration of 20 to 80 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ +Cu + )) is 60 to 100%. The temperature is not particularly limited, and a temperature of about 70 to 100° C. can be used.

[0061] As such an aqueous nickel chloride solution a, a chlorine leachate obtained through the chlorine leach step S1 in a nickel hydrometallurgical process (MCLE process) can be used.

[0062] The chlorine leaching step S1 in the MCLE process is briefly described below. In the chlorine leaching step S1, nickel sulfide such as nickel matte produced by a nickel dry smelting method is used as a raw material, and metals such as nickel are leached with chlorine gas together with the cementation residue after the cementation step to generate a copper-containing nickel chloride aqueous solution as a chlorine leachate.

[0063] In the chlorine leaching step S1, for example, reactions shown in the following formulas [6] to [8] occur. Cl2+2Cu+ → 2Cl - +2Cu 2+ [6] NiS+2Cu 2+ → Ni 2+ +S 0 +2Cu + [7] Cu2S+2Cu 2+ → 4Cu + +S 0 [8]

[0064] That is, in the chlorine leaching step S1, when the raw nickel sulfide is delivered, the metal components contained in the nickel sulfide, such as nickel sulfide (NiS) and copper sulfide (Cu2S), are oxidized and leached by the "divalent copper ions" oxidized by chlorine gas. This produces a chlorine leaching solution, a nickel chloride aqueous solution containing copper ions (copper-containing nickel chloride aqueous solution). As shown in formula [6], it is estimated that oxidative leaching using divalent copper ions as electron carriers is carried out in the chlorine leaching step S1. In addition, NiS in formula [7] represents the main component of MS, and Cu2S in formula [8] represents the main component of cementation residue.

[0065] (About nickel chloride aqueous solution b) The nickel chloride aqueous solution b is the starting solution for the cementation treatment, similar to the nickel chloride aqueous solution a. As described above, the nickel chloride aqueous solution b has a copper ion concentration of 1 to 20 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ +Cu + )) is 0 to 40%. That is, the nickel chloride aqueous solution b is an aqueous solution having a smaller content of divalent copper ions than the nickel chloride aqueous solution a, in other words, a larger content of monovalent copper ions.

[0066] The temperature of the aqueous nickel chloride solution b is not particularly limited, and may be about 40 to 60°C.

[0067] As such an aqueous nickel chloride solution b, a copper removal electrolysis waste solution obtained through a copper removal electrolysis step in a nickel hydrometallurgical refining process (MCLE process) can be used.

[0068] The copper removal electrolysis process in the MCLE process is briefly described below. In the MCLE process, which produces electrolytic nickel from nickel chloride solution, copper derived from the raw material (nickel sulfide) is circulated in the process system while maintaining a certain concentration. Copper plays an important role as a leaching agent for efficiently and stably leaching nickel in the raw material during the chlorine leaching process (chlorine leaching process S1). In the MCLE process, the copper contained in the raw material is stored in the process system, and a large amount of copper is circulated as the chlorine leaching solution and cementation residue. On the other hand, in order to maintain an appropriate amount of copper circulating in the system, it is necessary to extract an amount of copper from the system that corresponds to the amount of copper newly supplied from the raw material. Therefore, in the MCLE process, a process (copper removal electrolysis process) is performed to remove part of the copper circulating in the system by electrowinning.

[0069] In the copper removal electrolytic treatment, a part of the first slurry obtained through the first cementation step S21 in the cementation step S2 is used as a starting solution, and copper powder is recovered by electrowinning and an electrolytic waste solution is obtained. As the electrolytic feed solution, a solution obtained by removing solids from the first slurry through solid-liquid separation (final reaction solution of the treatment in the first cementation step S21) is preferably used. Specifically, in the copper removal electrolytic treatment, the electrolytic feed solution is supplied to an electrolytic cell equipped with an electrode pair consisting of a positive electrode and a negative electrode, and electrolytic treatment is performed. As a result of this electrolytic treatment, dendritic copper powder is precipitated on the surface of the negative electrode, and chlorine gas is generated at the positive electrode.

[0070] On the other hand, after the copper removal electrolytic treatment, a solution from which copper has been separated, recovered and removed (copper removal electrolytic waste liquid) is obtained. As described above, this copper removal electrolytic waste liquid is the end-of-reaction solution from the treatment (reduction treatment) in the first cementation step S21, that is, the solution after electrolysis to recover copper powder from a solution containing a large amount of monovalent copper ions. Therefore, the copper removal electrolytic waste liquid is a solution with a relatively low copper ion concentration and a small ratio of divalent copper ions.

[0071] <1-3. Copper ion removal equipment> Now, the cementation process consisting of the first cementation process S21 and the second cementation process S22 can be carried out using a copper ion removal apparatus equipped with a total of n reaction tanks (n is an integer of 4 or more) connected in series.

[0072] In such a cementation process using a copper ion removal apparatus in which n reaction tanks are connected in series, a first cementation process S21 (reduction process) is carried out in the first reaction tank located most upstream to the n-2th reaction tank located two tanks before the final reaction tank, and a second cementation process S22 (sulfurization process) is carried out in the final (nth) reaction tank located most downstream from the n-1th reaction tank located one tank before the final reaction tank.

[0073] In the method according to the present embodiment, the copper-containing nickel chloride aqueous solution to be treated is supplied to the first-stage reaction tank located at the most upstream position, and a sulfide raw material A containing nickel sulfide is also charged therein. A sulfide raw material B containing trinickel disulfide is charged into the final-stage (n-th) reaction tank located at the most downstream position, and the n-1-th reaction tank located one stage before the final-stage reaction tank. Then, the above-mentioned sulfide raw material C, i.e., a sulfide raw material C having a total content of metallic nickel and metallic iron of 60 to 85 mass %, is charged and treated in the n-1-th reaction tank located one stage before the final-stage reaction tank.

[0074] In this way, by charging the sulfide raw material C to the (n-1)th stage reaction tank and treating it, the sulfide raw material C can be made to contribute sufficiently to the reduction reaction with copper ions, and the reduction efficiency can be improved more effectively. Note that, for example, if the sulfide raw material C is charged to the final stage (nth stage) reaction tank, the reaction time between the sulfide raw material C and the copper ions will be short, and there is a possibility that the sulfide raw material C will not contribute sufficiently to the reduction reaction.

[0075] In the cementation treatment using this copper ion removal device, when two types of nickel chloride aqueous solutions a and b having different ratios of divalent copper ions in the copper ions as described above are used separately as the nickel chloride aqueous solution to be treated, the nickel chloride aqueous solutions are supplied as follows: That is, the nickel chloride aqueous solution a is supplied to the first stage reaction tank located at the most upstream position, and the nickel chloride aqueous solution b is supplied to the central reaction tank (however, when n is an even number, the n / 2+1 stage reaction tank).

[0076] In this manner, the supply inlets of the aqueous nickel chloride solutions a and b having different compositions are changed so that the aqueous nickel chloride solution a (having a ratio of divalent copper ions of 60 to 100%) can be supplied to the reduction treatment in the first cementation step S21, and the aqueous nickel chloride solution b (having a ratio of divalent copper ions of 0 to 40%) can be supplied to the sulfurization treatment in the second cementation step S22 in addition to the aqueous nickel chloride solution a.

[0077] More specifically, Fig. 3 is a schematic diagram showing an example of the configuration of a copper ion removal apparatus. The copper ion removal apparatus 1 shown in Fig. 3 includes a total of eight reaction tanks (No. 1 to No. 8) connected in series (n=8).

[0078] In the copper ion removal device 1, a total of six tanks, from the first-stage reaction tank (No. 1) located at the most upstream to the sixth-stage reaction tank (No. 6), are configured to perform a reduction treatment in which a sulfide raw material A containing nickel sulfide is added to an aqueous nickel chloride solution to reduce copper ions (first cementation step S21). Also, in a total of two tanks, from the seventh-stage reaction tank (No. 7) to the final-stage (eighth-stage) reaction tank (No. 8) located at the most downstream, a sulfide raw material B containing trinickel disulfide and a sulfide raw material C are added to the slurry obtained by the reduction treatment (first slurry), and a sulfurization treatment is performed to fix monovalent copper ions as copper sulfide.

[0079] In the copper ion removal apparatus 1, of the total eight reaction tanks, the first-stage reaction tank (No. 1) located at the most upstream position is provided with an initial liquid inlet for supplying an aqueous nickel chloride solution (aqueous nickel chloride solution a) which is an initial liquid for the reduction treatment, and a sulfide raw material A inlet for introducing a sulfide raw material A containing nickel sulfide. The final-stage (eighth-stage) reaction tank (No. 8) located at the most downstream position is provided with a final liquid outlet for discharging a final reaction liquid obtained through the sulfurization treatment, and a sulfide raw material B inlet for introducing a sulfide raw material B containing trinickel disulfide. The seventh-stage reaction tank (No. 7) located one stage before the final-stage reaction tank is provided with a sulfide raw material B inlet for introducing a sulfide raw material B, and a sulfide raw material C inlet for introducing a sulfide raw material C.

[0080] Furthermore, as described above, in the copper ion removal apparatus 1, the fifth-stage reaction tank (No. 5) is provided with an aqueous solution b inlet for supplying an aqueous nickel chloride solution b. In addition, the fifth-stage reaction tank may be provided with a sulfide raw material B inlet for introducing a sulfide raw material B.

[0081] The reducing power of the sulfide raw material A containing nickel sulfide added in the first cementation step S21 is weaker than that of the sulfide raw material B containing trimickel disulfide added in the second cementation step S22. In other words, the reduction reaction by the sulfide raw material A proceeds relatively slowly, while the sulfurization reaction by the sulfide raw material B proceeds relatively quickly. Therefore, in order to efficiently carry out the reduction treatment by the sulfide raw material A and the sulfurization treatment by the sulfide raw material B, it is advisable to limit the number of reaction tanks in which the sulfurization treatment is carried out to the bare minimum and to use the remaining reaction tanks for the reduction treatment.

[0082] On the other hand, because external factors may force a change in the processing ratio of sulfide raw material A and sulfide raw material B, a sulfide raw material B inlet for charging sulfide raw material B can be provided in the fifth-stage reaction tank to allow for flexible response. In that case, four tanks will be assigned to the first cementation process S21 where reduction treatment is performed, and four tanks will be assigned to the second cementation process S22 where sulfurization treatment is performed.

[0083] In the cementation treatment using the copper ion removal device 1 having the above-mentioned configuration, an aqueous nickel chloride solution a having a ratio of divalent copper ions of 60 to 100% is supplied from a starting solution inlet provided in the first-stage reaction tank (No. 1) and used for reduction treatment. An aqueous nickel chloride solution b having a ratio of divalent copper ions of 0 to 40% is supplied from a solution b inlet provided in the central reaction tank (the fifth-stage reaction tank (n / 2+1st stage when n is an even number)) and used for sulfurization treatment.

[0084] In this way, by performing the cementation treatment using the copper ion removal device 1, it is possible to optimize the timing of addition of the sulfide raw material C in the second cementation step S22, and to allow the sulfide raw material C to fully contribute to the reduction reaction of the copper ions. Furthermore, by performing the cementation treatment using the copper ion removal device 1, it is particularly preferable that the nickel chloride aqueous solutions a and b, which have different compositions in terms of the divalent copper ion ratio, can be supplied at appropriate timing from separate stages and subjected to the reaction.

[0085] This makes it possible to efficiently reduce the divalent copper ions in the aqueous nickel chloride solution a to monovalent copper ions in the first cementation step S21, and also makes it possible to more effectively remove copper ions from the aqueous copper-containing nickel chloride solution via fixation of the monovalent copper ions as sulfides in the second cementation step S22.

[0086] With regard to the copper ion removal apparatus 1, the cementation treatment is composed of two stages, namely, a reduction treatment (first cementation step S21) and a sulfurization treatment (second cementation step S22), and therefore at least two reaction tanks are required to constitute the apparatus. However, in a copper ion removal apparatus consisting of, for example, two reaction tanks in total, the capacity of the reaction tanks must be increased as the amount of treatment increases and the scale of the reaction increases, which not only results in huge equipment costs but is also undesirable from the viewpoint of maintainability. For this reason, it is preferable to configure the copper ion removal apparatus so that the total number of reaction tanks constituting the apparatus is four or more depending on the scale, and to configure the apparatus so that each of the reduction treatment and the sulfurization treatment is carried out in a plurality of reaction tanks.

[0087] In addition, when a solution is continuously supplied to a reaction tank, the residence time varies to a certain extent. Therefore, in a batch reaction, it is more advantageous to increase the capacity of the reaction tank in terms of cost, etc., but in a continuous reaction, it is overwhelmingly more advantageous to increase the number of reaction tanks rather than increasing the capacity of the reaction tank in terms of reaction stability and uniformity.

[0088] [Regarding ORP control of slurry obtained from the second cementation process] Although not essential, in the method according to the present embodiment, it is preferable to control the oxidation-reduction potential (ORP) (based on a silver / silver chloride electrode) of the second slurry obtained through the second cementation step S22 to be within a specific range. Specifically, it is preferable to control the ORP of the second slurry to be −100 mV or more and less than 0 mV, and it is more preferable to control the ORP to be −50 mV or more and less than 0 mV.

[0089] In this way, by controlling and treating the ORP of the obtained second slurry to be within the above-mentioned specific range, it is possible to efficiently remove not only copper ions but also silver, which is an impurity, from the copper-containing nickel chloride aqueous solution (chlorine leachate), and obtain a solution with an effectively reduced silver concentration. Note that the impurity silver is distributed to the cementation residue and removed together with copper fixed as sulfide through the second cementation step S22.

[0090] The method for controlling the ORP of the second slurry is not particularly limited. For example, it can be performed by adjusting the copper concentration of the copper-containing nickel chloride aqueous solution to be subjected to the cementation step S2. In addition, the ORP can be measured by continuously monitoring it by providing an oxidation-reduction potentiometer in the reaction tank.

[0091] 2. Method for producing nickel chloride aqueous solution from which copper ions have been removed The above-mentioned method for removing copper ions from the aqueous nickel chloride solution can be applied to the treatment in the cementation step S2 in the MCLE process. Therefore, it can be defined as a method (production method) for obtaining an aqueous nickel chloride solution from a raw material containing nickel, in which copper ions have been removed. In addition, since high-purity electric nickel can be obtained from the produced aqueous nickel chloride solution (aqueous nickel chloride solution from which copper ions have been removed) through electrolysis in the electrolysis step, it can also be defined as a production method for electric nickel.

[0092] Specifically, the method for producing an aqueous nickel chloride solution includes a chlorine leaching step S1 in which chlorine leaching is performed by blowing chlorine gas into a nickel-containing material slurry to obtain a chlorine leachate and a chlorine leach residue, and a cementation step S2 in which a cementation treatment is performed on the aqueous nickel chloride solution, which is the chlorine leachate, to obtain an aqueous nickel chloride solution from which copper ions have been removed.

[0093] FIG. 4 shows a process diagram for explaining the flow of the MCLE process for producing electrolytic nickel from raw nickel sulfide. As shown in the process flow in FIG. 4, a nickel chloride aqueous solution from which copper ions have been removed can be effectively produced by going through a chlorine leaching process S1 in which the nickel sulfide raw material is chlorine leached, and a cementation process S2 in which the obtained chlorine leachate is subjected to a cementation treatment to fix and remove copper ions. Although FIG. 1 and FIG. 4 are different notations, both are flow diagrams of the electrolytic nickel production process (MCLE process), and all of the "iron removal process", "cobalt solvent extraction process", and "liquid purification process" in FIG. 1 are included in the "liquid purification process S3" in FIG. 4. In addition, the "copper removal electrolysis process" shown in FIG. 1 is omitted in FIG. 4.

[0094] (Chlorine leaching process) In the chlorine leaching step S1, for example, nickel sulfide such as nickel matte produced by a nickel dry smelting method is used as a raw material to leach metals such as nickel with chlorine. Specifically, nickel in the nickel sulfide is leached by, for example, chlorine gas recovered in the electrolysis step S4 together with the cementation residue after the cementation step S2, to generate a copper-containing nickel chloride aqueous solution as a chlorine leachate.

[0095] The nickel sulfide used as the raw material is, for example, repulped and slurried with an aqueous nickel chloride solution (electrolysis waste liquid) obtained in the electrolysis step S4.

[0096] (Cementation process) In the cementation step S2, the nickel chloride aqueous solution containing copper ions (copper-containing nickel chloride aqueous solution), which is the chlorine leaching solution obtained in the chlorine leaching step S1, is subjected to reduction treatment and sulfurization treatment to fix and remove the copper ions in the aqueous solution as sulfides, thereby obtaining a nickel chloride aqueous solution with a reduced copper ion content (cementation end solution).

[0097] The above-mentioned copper ion removal method can be applied to the treatment (cementation treatment) in the cementation step S2.

[0098] Specifically, the cementation step S2 involves a cementation treatment including a first cementation step S21 in which a sulfide raw material A containing nickel sulfide is added to a copper-containing nickel chloride aqueous solution to reduce divalent copper ions in the nickel chloride aqueous solution to monovalent copper ions, and a second cementation step S22 in which a sulfide raw material B containing trinickel disulfide is added to the first slurry obtained in the first cementation step S21 to fix the monovalent copper ions contained in the first slurry as sulfides.

[0099] Then, in the second cementation step S22, the sulfide raw material C having a total content of metallic nickel and metallic iron of 60 to 85 mass % is further added to the first slurry together with the sulfide raw material B, and then treated.

[0100] According to such a method, the divalent copper ions contained in the copper-containing nickel chloride aqueous solution can be reduced to monovalent copper ions more efficiently and effectively, and the copper ions can be effectively removed from the copper-containing nickel chloride aqueous solution via fixation of the monovalent copper ions as sulfides in the second cementation step S22.

[0101] Moreover, according to this method, it is possible to effectively remove copper ions without carrying out pretreatment such as reducing the copper ion concentration of the copper-containing nickel chloride aqueous solution to be subjected to the treatment in the cementation step S2. Therefore, in consideration of the circulation cycle of the nickel hydrometallurgical refining process, it is possible to effectively prevent a situation in which the copper ions functioning as ion carriers for absorbing chlorine gas are insufficient, resulting in a deterioration in the chlorine leaching rate in the chlorine leaching step S1.

[0102] As the sulfide raw material A added in the first cementation step S21, a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material can be used. As the sulfide raw material B and sulfide raw material C added in the second cementation step S22, nickel matte produced by a nickel dry smelting method can be used.

[0103] In addition, in the cementation step S2, preferably, the nickel chloride aqueous solution to be subjected to the cementation treatment (to be treated) has a copper ion concentration of 20 to 80 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ +Cu + )) is 60-100%, and "nickel chloride aqueous solution a" has a copper ion concentration of 1-20g / L and the ratio of divalent copper ions (Cu 2+ / (Cu 2+ +Cu + Two types of nickel chloride aqueous solutions, "nickel chloride aqueous solution b" having a nickel chloride content of 0 to 40% and "nickel chloride aqueous solution b" having a nickel chloride content of 0 to 40%, are added separately at optimal positions. Specifically, in the first cementation step S21, "nickel chloride aqueous solution a" is used as the nickel chloride aqueous solution for treatment, and in the second cementation step S22, in addition to the nickel chloride aqueous solution a, "nickel chloride aqueous solution b" is further added and used for treatment. EXAMPLES

[0104] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0105] [Test Example 1] 8 reactors (each 60m 3The cementation step in the MCLE process was carried out using a copper ion removal device in which a copper ion removal apparatus and a copper ion removal device were connected in series. Specifically, the cementation step included a first cementation step in which a sulfide raw material A containing nickel sulfide was added to the chlorine leachate (aqueous nickel chloride solution containing copper ions) to be treated, and the divalent copper ions in the aqueous solution were reduced to monovalent copper ions, and a second cementation step in which a sulfide raw material B containing nickel disulfide was added to the resulting first slurry, and the monovalent copper ions were fixed as sulfides. In the second cementation step, a sulfide raw material C having a total content of metallic nickel and metallic iron of 60 to 85 mass% was added to the first slurry together with the sulfide raw material B, and treated.

[0106] In Test Example 1, a chlorine leachate with a copper concentration of 42 to 61 g / L was used, and tests were carried out in a copper ion removal apparatus having eight connected reaction tanks, with the sulfide raw material C added to the sixth, seventh, and eighth reaction tanks counting from the first reaction tank, which is the most upstream reaction tank, to confirm the reduction efficiency of divalent copper ions in the second cementation step. For comparison, a test was also carried out in the case where the sulfide raw material C was not added.

[0107] The amount of sulfide raw material C added was the same in each test. Also, the oxidation-reduction potential (ORP, silver / silver chloride electrode standard) of the slurry obtained from the outlet of the seventh reactor was 220 mV, and the ORP of the slurry obtained from the outlet of the eighth reactor was -30 mV, that is, the reduction conditions were the same in each test.

[0108] Fig. 5 is a graph showing the test results of Test Example 1, and is a graph showing the relationship between the total amount of sulfide raw material B and sulfide raw material C added in the second cementation step and the difference in the addition position of sulfide raw material C. As can be seen from Fig. 5, when sulfide raw material C was added to the seventh reaction tank, that is, the reaction tank located one stage before the final (eighth) reaction tank, the total amount of sulfide raw material B and sulfide raw material C added was the smallest.

[0109] This means that in the second cementation process, the reduction efficiency of copper ions can be maximized by using sulfide raw material C in combination with sulfide raw material B and adding the sulfide raw material C to a reaction tank located one stage before the final (eighth) reaction tank.

[0110] [Test Example 2] In Test Example 2, the sulfide raw material C was added to the seventh-stage reaction tank, and the amount of the sulfide raw material C added was changed. The other conditions were the same as in Test Example 1.

[0111] Fig. 6 is a graph showing the test results of Test Example 2. From the results shown in Fig. 6, it was found that as the added amount of sulfide raw material C increases, the efficiency of copper reduction in the second cementation step increases.

[0112] The reduction efficiency of copper was calculated as follows. Copper reduction efficiency = (Cu concentration of nickel chloride aqueous solution) × ((flow rate of nickel chloride aqueous solution)) / ((Ni content of sulfide raw material B) × (amount of sulfide raw material B added) + (Ni content of sulfide raw material C) × (amount of sulfide raw material C added))

[0113] [Test Example 3 (Examples 1 and 2, Comparative Example 1)] In Test Example 3, similarly to Test Examples 1 and 2, a copper ion removal apparatus having eight reaction tanks connected in series was used to treat the cementation step in the MCLE process. As shown in Table 2 below, the addition composition ratio of sulfide raw materials A, B, and C, and the ORP of the slurry at the outlet of the eighth-stage reaction tank were set, and treatment was performed. Note that Comparative Examples 1 and 2, in which no sulfide raw material C was added, were also performed as conventional examples.

[0114] [Table 2]

[0115] In Examples 1 and 2, by using sulfide raw material C in the second cementation step, the reduction efficiency of copper ions could be increased, and the copper removal process could be effectively carried out even when the Cu concentration in the chlorine leachate was 45 g / L or more.

Claims

1. A method for removing copper ions from a nickel chloride aqueous solution containing copper ions, comprising the steps of: a first cementation step of adding a sulfide raw material A containing nickel sulfide to the nickel chloride aqueous solution and reducing divalent copper ions in the nickel chloride aqueous solution to monovalent copper ions; a second cementation step of adding a sulfide raw material B containing trinickel disulfide to the first slurry obtained in the first cementation step, and immobilizing the monovalent copper ions contained in the first slurry as sulfides; In the second cementation step, a sulfide raw material C having a total content of metallic nickel and metallic iron of 60 to 85 mass% is added to the first slurry together with the sulfide raw material B. A method for removing copper ions from an aqueous nickel chloride solution.

2. The amount of the sulfide raw material C added is 5 to 30% in terms of nickel ratio with respect to the total amount of the sulfide raw material B and the sulfide raw material C added. The method for removing copper ions from an aqueous nickel chloride solution according to claim 1.

3. The cementation treatment is carried out using a copper ion removal apparatus having a total of n reaction tanks (n is an integer of 4 or more) connected in series; In the copper ion removal apparatus, The sulfide raw material A is charged into a first stage reaction tank located at the most upstream, The sulfide raw material B is charged into a final stage (nth stage) reaction tank located at the most downstream and an (n-1)th stage reaction tank located one stage before the final stage reaction tank, The sulfide raw material C is charged into the n-1th stage reaction tank.

3. The method for removing copper ions from an aqueous nickel chloride solution according to claim 1 or 2.

4. The nickel chloride aqueous solution to be treated has a copper ion concentration of 20 to 80 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ + Cu + )) is 60 to 100%, and the copper ion concentration is 1 to 20 g / L, and the ratio of divalent copper ions in the copper ions (Cu 2+ / (Cu 2+ + Cu + )) is 0 to 40%. In the first cementation step, the nickel chloride aqueous solution a is used as the nickel chloride aqueous solution for treatment, In the second cementation step, the nickel chloride aqueous solution b is further added to the nickel chloride aqueous solution a and subjected to treatment. The method for removing copper ions from an aqueous nickel chloride solution according to claim 1.

5. The cementation treatment is carried out using a copper ion removal apparatus having a total of n reaction tanks (n is an integer of 4 or more) connected in series; In the copper ion removal apparatus, The nickel chloride aqueous solution a is supplied to a first-stage reaction tank located at the most upstream position, and the sulfide raw material A is also charged therein; The sulfide raw material B is charged into a final stage (nth stage) reaction tank located at the most downstream and an (n-1)th stage reaction tank located one stage before the final stage reaction tank, The sulfide raw material C is charged into the n-1th stage reaction tank, The nickel chloride aqueous solution b is supplied to a reaction tank located in the center (however, when n is an even number, the reaction tank in the n / 2+1 stage). The method for removing copper ions from an aqueous nickel chloride solution according to claim 4.

6. The sulfide raw material A is a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material, The sulfide raw material B and the sulfide raw material C are nickel matte produced by a nickel dry smelting method.

6. The method for removing copper ions from an aqueous nickel chloride solution according to claim 1, 2, 4 or 5.

7. A method for obtaining an aqueous nickel chloride solution by removing copper ions from a raw material containing nickel, comprising the steps of: a chlorine leaching step of blowing chlorine gas into the nickel-containing slurry to perform chlorine leaching to obtain a chlorine leaching solution and a chlorine leaching residue; a cementation step of performing the cementation treatment for carrying out the copper ion removal method according to claim 1 on the nickel chloride aqueous solution containing copper ions, which is the chlorine leachate, to obtain a nickel chloride aqueous solution from which copper ions have been removed, The slurry produced in the cementation step is subjected to solid-liquid separation to obtain a cementation residue, and the slurry of the cementation residue (residue slurry) is transferred to the chlorine leaching step; In the chlorine leaching step, chlorine leaching is performed by blowing chlorine gas into the nickel-containing material slurry containing the residue slurry. Method for producing nickel chloride aqueous solution.

8. The amount of the sulfide raw material C added is 5 to 30% in terms of nickel ratio with respect to the total amount of the sulfide raw material B and the sulfide raw material C added. The method for producing the nickel chloride aqueous solution according to claim 7.

9. The cementation treatment is carried out using a copper ion removal apparatus having a total of n reaction tanks (n is an integer of 4 or more) connected in series; In the copper ion removal apparatus, The sulfide raw material A is charged into a first stage reaction tank located at the most upstream, The sulfide raw material B is charged into a final stage (nth stage) reaction tank located at the most downstream and an (n-1)th stage reaction tank located one stage before the final stage reaction tank, The sulfide raw material C is charged into the n-1th stage reaction tank. The method for producing an aqueous nickel chloride solution according to claim 7 or 8.

Citation Information

Patent Citations

  • Method for recovering copper and nickel from precious antimony by adopting wet replacement method

    CN112226618A

  • Treatment method of nickel sulfide raw material

    JP2016044355A

  • Method for refining nickel, and chlorine leaching method

    JP2017095782A

  • Method for removing copper ion of aqueous nickel chloride solution and apparatus for removal treatment of copper ion

    JP2017155281A

  • Copper removal method, method for producing electrolytically refined nickel

    JP2018199858A