Composite gas adsorbent, method of producing composite gas adsorbent, deodorization filter, and air purifier
A composite gas adsorbent with optimized porous material and supported 2-imidazolidinone and acid enhances adsorption of multiple odorous gases, meeting CADR standards by balancing capacity and rate, addressing inefficiencies in existing technologies.
Patent Information
- Application Number
- JP2024052180
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-03-27
AI Technical Summary
Existing gas adsorbents struggle to efficiently and rapidly remove a variety of odorous gases, including aldehyde-based, basic, and volatile organic compounds, failing to meet the high clean air delivery rate (CADR) standards required for air purifiers, particularly in indoor environments.
A composite gas adsorbent comprising a porous material with a water retention rate of 35% or more, supporting 3% or more of 2-imidazolidinone and an equal or greater amount of inorganic or organic acid, with specific surface area, pore volume, and pore ratio configurations, enhancing chemisorption and physical adsorption capabilities.
The composite gas adsorbent achieves superior adsorption performance for a range of odorous substances, meeting or exceeding CADR standards by balancing adsorption capacity and rate, effectively removing ammonia, toluene, formaldehyde, and other common indoor pollutants.
Smart Images

Figure 2024146872000007 
Figure 2024146872000001 
Figure 2024146872000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite gas adsorbent that adsorbs a composite gas containing a plurality of odorous substances, a method for producing the composite gas adsorbent, a deodorizing filter using the composite gas adsorbent, and an air purifier using the deodorizing filter. [Background technology]
[0002] Odorants present in living and working environments include acidic odorants, neutral odorants, basic odorants, volatile organic compounds, aldehyde odorants, etc. In particular, there is a high demand for the removal and deodorization of aldehyde odorants such as formaldehyde and acetaldehyde, which are believed to be causative agents of sick house syndrome.
[0003] Conventional adsorbents for aldehyde odorants have been made by supporting a compound that reacts with an aldehyde compound on a porous material such as activated carbon or zeolite. For example, Patent Document 1 describes an adsorbent in which a porous carrier supports a cyclic urea compound, such as 2-imidazolidinone or pseudouric acid, as a urea compound having a urea bond in the molecule, and an inorganic acid and / or an organic acid.
[0004] Patent Document 2 describes an adsorbent in which a hydroxyamine compound is supported on activated carbon with an average particle size of 50 to 10,000 μm. Patent Document 3 describes an adsorbent in which a hydroxyamine compound and an amine compound other than the hydroxyamine compound are supported on a porous carrier. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-232189 A [Patent Document 2] JP 2017-094258 A [Patent Document 3] JP 2018-114463 A Summary of the Invention [Problem to be solved by the invention]
[0006] Since a wide variety of odorous gases exist in living environments, particularly indoor environments, there is an increasing demand for gas adsorbents that can remove not only aldehyde-based odorous substances but also each odorous gas in a balanced and rapid manner.
[0007] For gas phase applications, particularly for air purifiers, clean air delivery rate (CADR) performance is required, which is a standard established by the Association of Home Appliance Manufacturers (AHAM) and is an index showing the amount of clean air an air purifier supplies per minute. The market demands performance in terms of how quickly clean air can be delivered, and the adsorbents used are required to have not only adsorption capacity but also adsorption speed.
[0008] The adsorbent described in Patent Document 1 uses, for example, activated carbon as a porous carrier, but if activated carbon with insufficiently developed pores is used, it may be difficult to achieve the required adsorption speed. Furthermore, there is a risk that the pores of the activated carbon may be blocked by the chemical, resulting in insufficient adsorption performance for volatile organic compounds such as toluene and acetic acid.
[0009] The adsorbent described in Patent Document 2 has a specific hydroxylamine compound supported on activated carbon having the above average particle size, and therefore has a high clean air supply rate (CADR) after a load of 50 mg of formaldehyde per sheet (60 m) when a simple formaldehyde test based on the GB standard was conducted. 3 / h or more) and a high clean air supply rate maintenance rate (CADR maintenance rate) (50% or more).
[0010] The adsorbent described in Patent Document 3 contains an amine-supported porous carrier in which a specific hydroxyamine compound is supported in combination with another amine compound, and therefore has high adsorption performance, a high clean air supply rate (CADR) after a load of 50 mg of formaldehyde per sheet, and a high clean air supply rate maintenance rate (CADR maintenance rate).
[0011] Thus, Patent Documents 2 and 3 describe the effect of the supported chemical on aldehydes and the CADR (Clean Air Delivery Rate), which is an index of the adsorption speed. However, the pore characteristics of the adsorbent are within a range (0.30 to 1.40 cc / g) that takes into account the removal of aldehydes and the hardness of the adsorbent, and the relationship with the removal effect and adsorption speed of gases other than aldehydes is unclear.
[0012] The Korean Air Cleaner Association (KACA) standard (SPS-KACA002-132) is a standard for odorant adsorption. According to this standard, the 8m 3 Clean air supply rate (CADR;m 3 / h) is required to have a certain level of initial performance. Therefore, there is an increasing demand for gas adsorbents that can achieve a certain level of adsorption speed while at the same time satisfying a certain level of adsorption capacity for composite gases that include not only aldehydes (aldehyde-based odorants) but also other odorants.
[0013] Therefore, an object of the present invention is to provide a composite gas adsorbent that has a certain level of adsorption capacity for a composite gas containing multiple odorous substances selected from the group consisting of basic odorous substances, volatile organic compounds, and aldehyde-based odorous substances, and that is capable of quickly removing the odorous substances, a manufacturing method for the composite gas adsorbent, a deodorizing filter, and an air purifier. [Means for solving the problem]
[0014] The composite gas adsorbent according to the present invention for achieving the above object has a characteristic configuration in that it has a porous material with a water retention rate of 35 mass% or more, the porous material supports 3 mass% or more of 2-imidazolidinone and 3 mass% or more of inorganic acid or organic acid, the amount of inorganic acid or organic acid supported is equal to or more than the amount of 2-imidazolidinone, and has adsorption performance for a composite gas containing two or more of basic odorous substances, volatile organic compounds, and aldehyde odorous substances.
[0015] As mentioned above, there are many gas adsorbents for aldehydes. However, it has been difficult to rapidly remove basic odorous substances, aldehyde odorous substances, and volatile organic compounds, which can be removed by physical adsorption, using a single gas adsorbent.
[0016] Volatile organic compounds are generally believed to be removed by porous materials through physical adsorption, and porous materials with developed micropores tend to be suitable for this purpose. Basic odorants and aldehyde odorants are generally believed to be removed by porous materials through chemical adsorption. In addition, by using porous materials with developed micropores (<2 nm), more 2-imidazolidinone and inorganic or organic acids, which contribute to chemical adsorption, can be supported on the porous material.
[0017] For substances removed by chemical adsorption, the amount of chemical supported is important. These chemicals are sprayed as an aqueous solution onto the porous material and supported, so in order to support a certain amount of chemical, the porous material needs to be able to absorb a lot of water. If the water retention rate of the porous material is 35% by mass or more, it can support a sufficient amount of chemical necessary to remove odorous substances.
[0018] The amount of 2-imidazolidinone and inorganic or organic acid supported is 3% by mass or more relative to the mass of the porous material having a water retention rate of 35% by mass or more. By setting the amount supported within this range, odorous substances that can be adsorbed by chemical adsorption can be efficiently adsorbed.
[0019] If the amount of inorganic acid or organic acid supported is less than the same amount as that of 2-imidazolidinone, both agents will be inactivated by a neutralization reaction, and sufficient effect against compound gases will not be obtained. However, by making the amount of inorganic acid or organic acid supported equal to or more than the amount of 2-imidazolidinone, the inorganic acid or organic acid that is effective against basic odorous substances will be more easily retained.
[0020] A further characteristic feature of the composite gas adsorbent according to the present invention is that the specific surface area of the porous material calculated by the BET method from the nitrogen adsorption isotherm is 1000 to 2200 m 2 The point is that / g.
[0021] According to this configuration, it is possible to specify the specific surface area of the porous material that is particularly excellent in adsorption performance for the composite gas, satisfies a certain level of adsorption capacity, and also satisfies the adsorption speed.
[0022] A further characteristic feature of the composite gas adsorbent according to the present invention is that the sum of the pore volume of micropores of less than 2 nm calculated from a nitrogen adsorption isotherm by the HK method and the pore volume of mesopores of 2 to 50 nm calculated by the BJH method is 0.35 to 1.50 cm 3 The point is that / g.
[0023] Mesopores (2 to 50 nm) in porous materials do not directly contribute to gas adsorption, but they act as introduction holes during gas mass transfer to micropores that serve as adsorption sites. Using a porous material with a certain proportion of mesopores improves the adsorption rate and makes it possible to adsorb gas more quickly.
[0024] In order to achieve a certain level of adsorption rate while at the same time satisfying a certain level of adsorption capacity for a composite gas, it is necessary to use a porous material in which the pore volume of the micropores and mesopores is present in a certain amount or more and the micropores and mesopores are present in a certain ratio.
[0025] Therefore, the porous material in the composite gas adsorbent of the present invention has a pore volume of micropores less than 2 nm calculated by the HK method and a pore volume of mesopores of 2 to 50 nm calculated by the BJH method of 0.35 to 1.50 cm 3 Use the one that is / g.
[0026] According to Example 2 described later, the sum is 0.35 to 1.50 cm 3 In the composite gas adsorbent of the present invention, the clean air delivery rate (CADR) for a composite gas containing multiple types of odorous substances (basic odorous substances, volatile organic compounds, and aldehyde odorous substances) is recognized to be superior to the CADR for the composite gas in the gas adsorbent of the comparative example, which has a clean air delivery rate (CADR) of 0.01 to 0.01 g / g.
[0027] Therefore, according to the present configuration, a composite gas adsorbent can be provided that has particularly excellent adsorption performance for basic odorous substances, aldehyde odorous substances, and volatile organic compounds, which can be removed by chemical adsorption, and that has a certain level of adsorption capacity and also meets the adsorption speed requirements.
[0028] A further characteristic feature of the composite gas adsorbent according to the present invention is that, in the porous material, the ratio of the pore volume of the micropores to the sum of the pore volumes is 70 to 89%, and the ratio of the pore volume of the mesopores to the sum of the pore volumes is 11 to 30%.
[0029] In Example 2 described later, it is recognized that the composite gas adsorbent of the present invention is preferably one in which the ratio of the pore volume of the micropores to the sum of the pore volumes is 70 to 89%, and the ratio of the pore volume of the mesopores to the sum of the pore volumes is 11 to 30%.
[0030] Therefore, according to the present configuration, a composite gas adsorbent can be provided that has particularly excellent adsorption performance for basic odorous substances, aldehyde odorous substances, and volatile organic compounds, which can be removed by chemical adsorption, and that has a certain level of adsorption capacity and also meets the adsorption speed requirements.
[0031] A further characteristic feature of the composite gas adsorbent according to the present invention is that the basic odorous substance is ammonia, the volatile organic compound is at least one of toluene and acetic acid, and the aldehyde odorous substance is at least one of acetaldehyde and formaldehyde.
[0032] According to the present configuration, it is possible to identify the main odorous substances present in the living environment or working environment, and provide a composite gas adsorbent that has particularly excellent adsorption performance for a composite gas containing the odorous substance, meets a certain level of adsorption capacity, and also meets the adsorption speed.
[0033] A further characteristic feature of the composite gas adsorbent according to the present invention is that the organic acid is represented by the following chemical formula 1:
[0034] [C1] TIFF2024146872000001.tif21169
[0035] According to this configuration, since a readily available carboxylic acid can be used as the organic acid, the composite gas adsorbent of the present invention can be easily provided.
[0036] A further characteristic feature of the composite gas adsorbent according to the present invention is that the inorganic acid is phosphoric acid.
[0037] According to this configuration, phosphoric acid, which is easily available, can be used as the inorganic acid, so that the composite gas adsorbent of the present invention can be easily provided.
[0038] A characteristic feature of the method for producing a composite gas adsorbent according to the present invention is that it includes a preparation step of preparing an aqueous solution by dissolving powdered or particulate 2-imidazolidinone and an inorganic acid or an organic acid in water, and a supporting step of bringing the aqueous solution into contact with a porous material and causing the porous material to support the aqueous solution.
[0039] The preparation step can prepare an aqueous solution in which powdery or particulate 2-imidazolidinone and powdery or particulate inorganic or organic acid are dissolved in water. Alternatively, the preparation step can prepare an aqueous solution in which powdery or particulate 2-imidazolidinone is dissolved in water, and prepare an aqueous solution in which powdery or particulate inorganic or organic acid is dissolved in water separately from the aqueous solution.
[0040] In the supporting step, the aqueous solution and the porous material are brought into contact with each other, whereby 2-imidazolidinone and the inorganic acid or organic acid can be supported evenly throughout the porous material.
[0041] Therefore, according to this configuration, it is possible to produce a composite gas adsorbent that has particularly excellent adsorption performance for a composite gas containing basic odorous substances, volatile organic compounds, and aldehyde-based odorous substances, and that has a certain level of adsorption capacity and also meets the adsorption speed requirements.
[0042] The deodorizing filter for an indoor air cleaner according to the present invention is characterized by the use of the above-mentioned composite gas adsorbent.
[0043] According to this configuration, it is possible to provide a deodorizing filter for indoor air purifiers that has particularly excellent adsorption performance for complex gases containing basic odorous substances, volatile organic compounds, and aldehyde-based odorous substances, meets a certain level of adsorption capacity, and also meets the adsorption speed requirements.
[0044] The air purifier according to the present invention is characterized in that it uses the above-mentioned deodorizing filter.
[0045] According to this configuration, it is possible to provide an air purifier that has particularly excellent adsorption performance for complex gases containing basic odorous substances, volatile organic compounds, and aldehyde-based odorous substances, and that meets a certain level of adsorption capacity and adsorption speed. [Brief description of the drawings]
[0046] [Figure 1] 1 is a flow chart showing a method for producing a composite gas adsorbent according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0047] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The composite gas adsorbent of the present invention has an adsorption performance for a composite gas containing multiple odorous substances present in the environment. The composite gas adsorbent has a porous material with a water retention rate of 35% by mass or more, and the porous material supports 3% by mass or more of 2-imidazolidinone and 3% by mass or more of inorganic acid or organic acid, and the supported amount of inorganic acid or organic acid is equal to or more than the amount of 2-imidazolidinone, and has an adsorption performance for a composite gas containing multiple basic odorous substances, volatile organic compounds, and aldehyde odorous substances.
[0048] (compound gas) The composite gas adsorbent of the present invention has an adsorption performance for a composite gas containing a plurality of basic odorous substances, volatile organic compounds and aldehyde odorous substances, that is, at least two of these substances.
[0049] Examples of basic odorous substances include ammonia, alkylamines (trimethylamine, triethylamine, etc.), aromatic amines (pyridine, etc.), and odorous organic amine compounds other than those mentioned above, but are not limited to these.
[0050] Volatile organic compounds (VOCs) are organic chemical molecules that have a high vapor pressure at room temperature, such as, but not limited to, toluene, acetic acid, formaldehyde, benzene, xylene, ethylbenzene, styrene, propane, hexane, cyclohexane, limonene, pinene, acetaldehyde, hexaldehyde, ethyl acetate, and butanol.
[0051] Examples of aldehyde odorants include, but are not limited to, formaldehyde, acetaldehyde, propionaldehyde, acrolein, n-butyraldehyde, isobutyraldehyde, pentanal, hexanal, heptanal, octanal, nonenal, decanal, 3-methylbutyraldehyde, crotonaldehyde, and 2,4-heptadienal.
[0052] (porous material) A porous material refers to a material having a structure in which many pores are formed. Since many pores are formed in a porous material, the material has a large specific surface area. The size of the pores in a porous material is not particularly limited, but can be, for example, 0.1 to 200,000 nm.
[0053] The porous material in the present invention has a pore volume of micropores less than 2 nm calculated from a nitrogen adsorption isotherm by the HK method and a pore volume of mesopores of 2 to 50 nm calculated by the BJH method of 0.35 to 1.50 cm 3 / g, the ratio of the micropore volume to the sum of the pore volumes is 70 to 89%, and the ratio of the mesopore volume to the sum of the pore volumes is 11 to 30%.
[0054] A nitrogen adsorption isotherm can be obtained by nitrogen adsorption measurement, and the specific surface area can be calculated by analyzing this by the BET (Brunauer-Emmett-Teller) method.
[0055] The pores in porous materials are classified according to their diameter into micropores (<2 nm), mesopores (2-50 nm), and macropores (>50 nm), and the gas adsorption method is generally used to measure micropores and mesopores.
[0056] In the present invention, the HK (Horvath Kawazoe) method is applied as an analytical method used to confirm the proportion of the pore volume of micropores (<2 nm) in a porous material.
[0057] Volatile organic compounds such as toluene and acetic acid are generally believed to be removed by porous materials through physical adsorption, and porous materials with developed micropores tend to be suitable for this purpose. Basic odorants such as ammonia and aldehyde odorants such as formaldehyde and acetaldehyde are generally believed to be removed by porous materials through chemical adsorption. In addition, by using porous materials with developed micropores, it is possible to support more 2-imidazolidinone and inorganic or organic acids, which contribute to chemical adsorption, on the porous material.
[0058] In the present invention, the Barrett-Joyner-Halenda (BJH) method is applied as an analytical method used for confirming the proportion of the pore volume of mesopores (2 to 50 nm) in a porous material.
[0059] Although the mesopores do not directly contribute to gas adsorption, they serve as introduction holes during gas mass transfer to micropores that serve as adsorption sites. By using a porous material in which a certain proportion of mesopores are present, the adsorption rate can be improved and gas can be adsorbed more quickly.
[0060] In order to achieve a certain level of adsorption rate while at the same time satisfying a certain level of adsorption capacity for a composite gas, it is necessary to use a porous material in which the pore volume of these micropores and mesopores is present in a certain number or more and in which the micropores and mesopores are present in a certain ratio.
[0061] From the above viewpoints, the porous material is a material in which the sum of the pore volume of micropores less than 2 nm calculated by the HK method and the pore volume of mesopores of 2 to 50 nm calculated by the BJH method is 0.35 to 1.50 cm 3 The sum of the pore volumes is preferably 0.47 to 1.22, more preferably 0.47 to 0.97, and further preferably 0.67 to 0.86.
[0062] In the present invention, the porous material used has a ratio of the pore volume of micropores to the total pore volume of the porous material of 70 to 89%, preferably 71 to 89%, more preferably 80 to 88%, and further preferably 82 to 86%.
[0063] In the present invention, the porous material used has a ratio of the mesopore volume to the sum of the pore volumes of 11 to 30%, preferably 11 to 29%, more preferably 12 to 20%, and further preferably 14 to 18%.
[0064] From the viewpoint of balancing the adsorption and removal performance and hardness required for an air purifier, the porous material is selected to have a specific surface area of 1000 to 2200 m, calculated by the BET method from the nitrogen adsorption isotherm of the porous material. 2 The specific surface area is preferably 1000 to 2000 m / g. 2 / g, more preferably 1056 to 1996 m 2 / g is preferable.
[0065] The water retention rate is an indicator of the amount of drug that can be supported on a porous material, and can be calculated by impregnating a porous material with water for a certain period of time, then dehydrating it, and measuring the change in mass before and after dehydration.
[0066] In the present invention, the lower limit of the water retention rate of the porous material is set to a range of 35% by mass or more, preferably 38% by mass or more, and more preferably 41% by mass or more.
[0067] In the present invention, the upper limit of the water retention rate of the porous material is in the range of 80 mass % or less, preferably 78 mass % or less, more preferably 75 mass % or less, and further preferably 61 mass % or less.
[0068] Alkali metals and the like are present on the surface of the porous material, and these metals may undergo a neutralizing reaction with the inorganic or organic acid supported thereon, reducing the reactivity with basic odorous substances such as ammonia and thus reducing the adsorption performance. Therefore, it is preferable to use a porous material with a low content of the above-mentioned metals.
[0069] The ignition residue refers to the amount of metal contained in the porous material, and can be measured by igniting the porous material in an electric furnace and determining the residue. The measurement can be performed, for example, by the method described in JIS K1474 "Ignition residue."
[0070] In the present invention, the ignition residue of the porous material is in the range of 0.1 to 7.0%, preferably 0.1 to 3.0%.
[0071] Bulk density is the value obtained by filling a powder in a container of a certain volume in a certain way and dividing the mass of the powder by the volume, including the voids between the particles. Bulk density varies depending on the pore characteristics of the porous material. If there are few micropores, the mass of the porous material contained per certain volume is heavy, so the bulk density value tends to be high. On the other hand, if there are many mesopores, the mass of the porous material contained per certain volume is light, so the bulk density value tends to be low.
[0072] In addition, if the bulk density is large, when the composite gas adsorbent is packed into a filter in terms of mass, the packed amount of the composite gas adsorbent is small, and the performance may be deteriorated. On the other hand, if the bulk density is small, the packed amount of the composite gas adsorbent is increased, but the pressure loss during the passage of air through the filter may be large. Therefore, it is preferable that the bulk density is within a certain range.
[0073] The bulk density can be measured by a method in which a porous material is packed into a packing density measurement container using a packing density measurement device and the mass per unit volume is determined. The measurement may be performed, for example, by the method described in JIS K1474 "packing density."
[0074] In the present invention, the bulk density of the porous material is in the range of 0.35 to 0.65, preferably 0.40 to 0.55.
[0075] The raw material of the porous material is not particularly limited, and examples thereof include plant-based materials (e.g., plant-derived materials such as wood, sawdust, charcoal, fruit shells such as coconut shells and walnut shells, fruit seeds, pulp manufacturing by-products, lignin, and blackstrap molasses), mineral-based materials (e.g., mineral-derived materials such as peat, lignite, brown coal, bituminous coal, anthracite, coke, coal tar, coal pitch, petroleum distillation residue, and petroleum pitch), synthetic resin-based materials (e.g., synthetic resin-derived materials such as phenol resin, polyvinylidene chloride, and acrylic resin), and natural fiber-based materials (e.g., natural fiber-derived materials such as cellulose and regenerated fiber such as rayon).
[0076] Among these raw materials for the porous material, plant-based materials are preferred because they have many micropores and therefore have excellent adsorption performance. Among the plant-based materials, fruit shells such as coconut shells are preferred as the raw material for the porous material because they can exhibit adsorption performance more efficiently. In this embodiment, a description will be given of the case where coconut shells, which are plant-based materials, are used as the raw material for the porous material.
[0077] The porous material can be obtained by carbonizing or infusible the above-mentioned raw material as necessary, and then activating it. The carbonization method, infusibility method and activation method are not particularly limited, and known methods can be applied. For example, the activation method can be performed by a gas activation method or a chemical activation method. The gas activation method is a method in which the carbon raw material (or its carbonized or infusible product) is heat-treated at about 500 to 1000°C in an activation gas (water vapor, carbon dioxide, etc.). The chemical activation method is a method in which the carbon raw material (or its carbonized or infusible product) is mixed with an activator (phosphoric acid, zinc chloride, potassium hydroxide, sodium hydroxide, etc.) and heat-treated at about 300 to 800°C.
[0078] The shape of the porous material is not particularly limited, and can be, for example, particulate, fibrous (thread, woven cloth, felt), block, powder, etc., and can be appropriately selected according to the specific usage. Taking into consideration high adsorption performance per unit volume and packing into the filter, the shape is preferably particulate. The dimensions of the porous material are not particularly limited, and the particle size, etc. can be appropriately adjusted according to the specific usage.
[0079] The porous material used may be a commercially available product.
[0080] (Amine compounds) It is known that aldehydes form aldehyde-amine bonds such as Schiff bases with amine compounds. Therefore, when an amine compound is supported on a porous material, the aldehyde-based odorous substances, which are the cause of unpleasant odors, can be efficiently adsorbed onto the porous material through chemical bonds as a result of the bonding reaction.
[0081] The amine compound is not particularly limited as long as it has at least one amino group in the molecule, and may be, for example, a primary amine, a secondary amine, or a tertiary amine.
[0082] In the present invention, in consideration of operability and safety, a case in which 2-imidazolidinone (ethylene urea) is used as the amine compound will be described.
[0083] In the present embodiment, the amount of 2-imidazolidinone supported is 3% by mass or more based on the mass of the porous material. By setting the amount supported within this range, odorous substances that can be adsorbed by chemical adsorption can be efficiently adsorbed.
[0084] If the amount supported is less than 3% by mass, the amount supported is too small to exhibit sufficient removal performance against aldehyde-based odorous substances, so the lower limit of the amount supported should be 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more.
[0085] If the supported amount exceeds 30 mass%, the amount is excessively supported, and as a result, pores effective for adsorbing volatile organic compounds are blocked, making it impossible to exhibit sufficient removal performance for complex gases, particularly volatile organic compounds, and therefore the upper limit of the supported amount is preferably 30 mass% or less, more preferably 25 mass% or more and less than 30 mass%, and even more preferably 20 mass% or more and less than 25 mass%.
[0086] (inorganic or organic acid) Inorganic acids or organic acids have excellent adsorption performance for basic odorants such as ammonia. In addition, inorganic acids or organic acids alone do not have the ability to adsorb aldehyde odorants, but by supporting inorganic acids or organic acids together with 2-imidazolidinone on a porous material, the adsorption rate of aldehyde odorants can be improved.
[0087] Examples of inorganic acids that can be used in the present invention include, but are not limited to, phosphoric acid, hydrochloric acid, sulfuric acid, and nitric acid.
[0088] The organic acids used in the present invention include, for example, carboxylic acids, sulfonic acids, sulfinic acids, phenols, enols, thiophenols, imides, oximes, aromatic sulfonamides, primary and secondary nitro compounds, etc., but are not limited to these.
[0089] The organic acid used in the present invention is preferably a compound represented by the following chemical formula 1.
[0090] [C1] TIFF2024146872000002.tif21169
[0091] Specific examples of the compound represented by the above chemical formula 1 include carboxylic acids, sulfonic acids, and sulfinic acids.
[0092] These inorganic acids or organic acids may be commercially available products.
[0093] Of these inorganic or organic acids, it is preferable to use hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, carboxylic acid, sulfonic acid, or sulfinic acid. In this embodiment, a case where phosphoric acid is used as the inorganic acid will be described.
[0094] In this embodiment, the amount of inorganic acid or organic acid supported is 3% by mass or more based on the mass of the porous material. By setting the amount supported within this range, odorous substances that can be adsorbed by chemical adsorption, particularly basic odorous substances, can be efficiently adsorbed.
[0095] If the amount supported is less than 3% by mass, the amount supported is too small to exhibit sufficient removal performance against basic odorous substances, so the lower limit of the amount supported should be 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more.
[0096] If the supported amount exceeds 30 mass%, the amount is excessively supported, and as a result, pores effective for adsorbing volatile organic compounds are blocked, making it impossible to exhibit sufficient removal performance for complex gases, particularly volatile organic compounds, and therefore the upper limit of the supported amount is preferably 30 mass% or less, more preferably 25 mass% or more and less than 30 mass%, and even more preferably 20 mass% or more and less than 25 mass%.
[0097] Furthermore, the present application has found that a certain level of effectiveness against basic odorous substances (ammonia) can be obtained by supporting an inorganic acid or an organic acid in an amount equal to or greater than the amount of 2-imidazolidinone. Therefore, the amount of inorganic acid or organic acid supported is preferably equal to or greater than the amount of 2-imidazolidinone, specifically 1 to 5 times, preferably 1.0 to 3 times, and more preferably 1.1 to 3 times.
[0098] As described above, the composite gas adsorbent of the present invention is configured to have a porous material with a water retention rate of 35% by mass or more, to support 3% by mass or more of 2-imidazolidinone and 3% by mass or more of inorganic acid or organic acid, and to support the inorganic acid or organic acid in an amount equal to or more than that of 2-imidazolidinone. As a result, the composite gas adsorbent of the present invention is particularly excellent in adsorption performance for basic odorous substances (ammonia, etc.) that can be removed by chemical adsorption, aldehyde odorous substances (acetaldehyde, formaldehyde, etc.), and volatile organic compounds (toluene, acetic acid, etc.) that can be removed by physical adsorption, and can satisfy a certain level of adsorption capacity and adsorption speed.
[0099] (Method of manufacturing composite gas adsorbent) The method for producing the composite gas adsorbent of the present invention includes a preparation step A of preparing an aqueous solution by dissolving powdered or particulate 2-imidazolidinone and an inorganic or organic acid in water, and a support step B of bringing the aqueous solution into contact with a porous material to support the aqueous solution on the porous material (FIG. 1). After the support step B, a drying treatment or the like may be performed by a known method.
[0100] In the preparation step A, an aqueous solution is prepared by dissolving powdery or particulate 2-imidazolidinone and powdery or particulate inorganic or organic acid in water. Alternatively, in the preparation step A, an aqueous solution is prepared by dissolving powdery or particulate 2-imidazolidinone in water, and an aqueous solution is prepared by dissolving powdery or particulate inorganic or organic acid in water separately from the aqueous solution.
[0101] The contact in the supporting step B is not particularly limited as long as the aqueous solution and the porous material can be brought into contact with each other, and can be, for example, a case in which the aqueous solution is sprayed onto the porous material, a case in which the aqueous solution is sprinkled onto the porous material, or a case in which the porous material is immersed in the aqueous solution.
[0102] In this case, the following methods can be used to contact the porous material with 2-imidazolidinone and an inorganic acid or an organic acid.
[0103] (a) An aqueous solution containing 2-imidazolidinone and an inorganic or organic acid is sprayed and / or sprinkled onto a porous material. (b) Immersing the porous material in an aqueous solution containing 2-imidazolidinone and an inorganic acid or an organic acid. (c) A 2-imidazolidinone-treated product obtained by spraying and / or scattering an aqueous solution containing 2-imidazolidinone onto a porous material, or by immersing a porous material in an aqueous solution containing 2-imidazolidinone, is mixed with an inorganic acid- or organic acid-treated product obtained by spraying and / or scattering an aqueous solution containing an inorganic acid or an organic acid onto a porous material, or by immersing a porous material in an aqueous solution containing an inorganic acid or an organic acid.
[0104] By the above-mentioned supporting step B, 2-imidazolidinone and an inorganic acid or an organic acid can be supported evenly over the entire porous material.
[0105] The temperature of the aqueous solution containing 2-imidazolidinone is preferably 15 to 30° C., and the temperature of the aqueous solution containing an inorganic acid or an organic acid is preferably 15 to 30° C. The supporting time is not particularly limited, but is preferably within 1 hour.
[0106] According to the manufacturing method of the composite gas adsorbent of the present invention, it is possible to prepare a composite gas adsorbent that has particularly excellent adsorption performance for a composite gas containing basic odorous substances, volatile organic compounds and aldehyde-based odorous substances, and that satisfies a certain level of adsorption capacity and also satisfies the adsorption speed.
[0107] (Application to industrial products) The composite gas adsorbent of the present invention can be incorporated into industrial products for use.
[0108] The industrial products in question refer to industrial products and raw materials that have been widely known in the past, including, but not limited to, paints, adhesives, inks, sealants, paper products, binders, resin emulsions, pulp, wood materials, wood products, plastic products, films, wallpapers, building materials (plasterboard, interior materials, ceiling materials, floor materials, etc.), textile products, and filters (especially deodorizing filters for indoor air purifiers and cabin air filters, etc.).
[0109] When a filter (particularly a deodorizing filter) is used as an industrial product, a known structure can be adopted as the structure.
[0110] In addition, composite materials of these are also included in industrial products. Examples of composite materials include, but are not limited to, composite materials of wood materials and plastics.
[0111] By contacting industrial products such as the above-mentioned deodorizing filters for indoor air purifiers containing the composite gas adsorbent of the present invention with, for example, multiple types of odorous substances (basic odorous substances, volatile organic compounds, and aldehyde-based odorous substances) contained in an indoor environment, the composite gas adsorbent comes into contact with the odorous substances, and the odorous substances can be efficiently adsorbed and removed. EXAMPLES
[0112] The method for producing the composite gas adsorbent of the present invention will be described below.
[0113] [Example 1] [Examples 1-1 to 1-5 and Comparative Examples 1-1 to 1-6] The porous material was made from coconut shells (known coconut shells collected around Southeast Asia were purchased) as a raw material. The raw material was carbonized by a standard method and then activated. The activation was performed by a gas activation method. In the gas activation method, the raw material was heat-treated at 900°C in an activation gas (steam).
[0114] The heat treatment (steam activation treatment) time was 30 minutes in Examples 1-1 and 1-3 and Comparative Examples 1-1 to 1-4, and 150 minutes in Examples 1-2, 1-4, and 1-5 and Comparative Examples 1-5 to 1-6.
[0115] The porous material has a water retention rate of 35% by mass or more (38 to 51% by mass), and the porous material is supported with 3% by mass or more (5% by mass) of 2-imidazolidinone and 3% by mass or more of inorganic acid or organic acid (5 to 25% by mass phosphoric acid), and the inorganic acid or organic acid and 2-imidazolidinone are supported so that the amount of the inorganic acid or organic acid supported is equal to or more than the amount of 2-imidazolidinone (1 to 5 times). Furthermore, in order to support a drug in the pores inside the porous material, Examples 1-1 to 1-5 were prepared so that the ratio of the amount of supported drug to the water retention rate was 0.2 or more (0.3 to 0.6). The ratio of the amount of supported drug to the water retention rate is 0.1 or more, preferably 0.2 or more, more preferably 0.1 to 0.8, and further preferably 0.2 to 0.6.
[0116] An aqueous solution was prepared (preparation step A) by dissolving powdered 2-imidazolidinone and liquid phosphoric acid (concentration 85%: an example of an inorganic acid) in water to obtain the loading amounts shown in Table 1. While maintaining the temperature of the aqueous solution at room temperature, the aqueous solution was contacted with 100 g of the porous material that had been subjected to the above treatment for 15 minutes (loading step B).
[0117] The amounts of 2-imidazolidinone and inorganic acid or organic acid supported, the ratio of the amount of supported drug to the water retention rate, and the ratio of the amount of 2-imidazolidinone supported to the amount of inorganic acid or organic acid supported were adjusted for each of the Examples and Comparative Examples so as to obtain the values shown in Table 1.
[0118] <Measurement of water retention rate> The water retention rate before the supporting step B was measured as follows. Use a constant temperature shaker (with an amplitude of 40 mm, adjustable to 120 - 130 oscillations per minute, and 50 °C), weigh 50 g of the porous material dried at 115 ± 5 °C for 3 hours to the nearest 10 mg, and denote it as W0 (g). Put the weighed porous material into a 500 mL Erlenmeyer flask, add 200 mL of distilled water, shake it in a constant temperature shaker at 50 °C for 20 minutes, and then dehydrate the porous material in a centrifuge for 1 minute. Weigh the dehydrated sample to the nearest 10 mg, denote it as We (g), and calculate the water retention rate according to the following formula.
[0119] <Water Retention Rate Calculation Method> Water Retention Rate (%) = (We - W0) ÷ We × 100
[0120] <CADR Measurement Method> Set 6.0 g of the composite gas adsorbent of the present invention on a 9 cm × 9 cm filter, set it on top of the exhaust fan in the laboratory (1 m 3 ), then inject gas into the laboratory so that the concentrations of ammonia, toluene, acetic acid, formaldehyde, and acetaldehyde in the laboratory reach 10 ppm each, and operate the exhaust fan. Use an FT-IR gas analyzer (MATRIX MG5: manufactured by Bruker Japan Co., Ltd.) to measure the concentration of each gas in the laboratory every 2 minutes for 60 minutes. From the relationship between the elapsed time and the gas concentration in the air, calculate the clean air delivery rate (CADR) (m 3 / h) of each gas by the following method.
[0121] CADR Calculation Method 1) Calculate the logarithm Ln(Ct / C0) from the initial concentration (C0) and the concentration (Ct) at each time. 2) Calculate the slope K from the logarithm Ln(Ct / C0) and time. 3) Multiply the slope K by the test space (30 m 3 ) to calculate the CADR (m 3 / H). Regarding the calculation method of the slope K, it is distinguished and performed by the following two methods according to the value of C / C0. · When C / C0 < 0.1, calculate at the point until it falls below 0.1 · When C / C0 ≥ 0.1, calculate at all points up to 60 minutes
[0122] The results are shown in Table 1.
[0123] [Table 1]
[0124] In Examples 1-1 to 1-5, when the amount of 2-imidazolidinone supported is 3% by mass or more and the amount of phosphoric acid supported is 3% by mass or more, the ratio of the amount of phosphoric acid supported to the amount of 2-imidazolidinone is equal to or more, and the ratio of the amount of drug supported to the water retention rate is 0.6 or less, the total CADR value is 942 to 1354 m 3 / h.
[0125] The CADR performance ratio indicates the ratio (%) of each odorous substance (basic odorous substances (ammonia), volatile organic compounds (VOCs: toluene, acetic acid), and aldehyde odorous substances (formaldehyde, acetaldehyde)) to the total CADR value.
[0126] On the other hand, in the case of Comparative Examples 1-1 and 1-2, in which the amount of phosphoric acid supported is less than 3 mass% and the ratio of the amount of phosphoric acid supported to 2-imidazolidinone is less than the same, the total CADR value is 741,763 m 3 / h, which is lower than the total CADR value of the above examples, and the CADR performance ratios of basic odorous substances were 3.3% and 2.7%, which are lower than the CADR performance ratios (basic odorous substances) of the above examples. From this, it was recognized that the CADR performance ratios of basic odorous substances in Comparative Examples 1-1 and 1-2 were inferior.
[0127] In addition, as in Comparative Examples 1-3 and 1-4, when the amount of 2-imidazolidinone supported is less than 3 mass% or the ratio of the amount of phosphoric acid supported to the amount of 2-imidazolidinone is equal to or more than the same amount, the total CADR value is 991 to 1005 m 3 / h, which is comparable to Examples 1-1 and 1-3, but the CADR performance ratios of aldehyde odorous substances in Comparative Examples 1-3 and 1-4 were 9.0 and 12.0%, respectively, which were lower than the CADR performance ratios (aldehyde odorous substances) of the above Examples. From this, it was recognized that the CADR performance ratios of aldehyde odorous substances in Comparative Examples 1-3 and 1-4 were inferior.
[0128] Furthermore, in Comparative Examples 1-5 and 1-6, when the ratio of the amount of inorganic acid or organic acid and 2-imidazolidinone supported to the water retention rate was 0.8, the total CADR value was 1345,768 m 3 / h, but the CADR value for volatile organic compounds is 513,459 m 3 / h, which was a lower result than the CADR value of the volatile organic compounds in each Example. This confirmed that the pores were clogged by supporting an excessive amount of the drug, resulting in a decrease in the adsorption performance of the volatile organic compounds.
[0129] [Example 2] [Examples 2-1 to 2-7 and Comparative Example 2-1] The same porous material as in Example 1 was used, and the same carbonization and activation treatments were carried out.
[0130] The time of the heat treatment (steam activation treatment) was adjusted for each of Examples 2-1 to 2-7 and Comparative Example 2-1 so that the specific surface area of each of them was the value shown in Table 2. The time was as follows: Example 2-1: 30 minutes, Example 2-2: 60 minutes, Example 2-3: 90 minutes, Example 2-4: 120 minutes, Example 2-5: 150 minutes, Example 2-6: 180 minutes, Example 2-7: 210 minutes, and Comparative Example 2-1: 0 minutes.
[0131] An aqueous solution was prepared by dissolving 5.1 g of powdered 2-imidazolidinone and 7.8 g of liquid phosphoric acid (concentration 85%: an example of an inorganic acid) in 22.7 mL of water (Preparation step A). The aqueous solution was kept at room temperature and contacted with 100 g of the porous material that had been subjected to the above treatment for 15 minutes (Supporting step B).
[0132] The composite gas adsorbents (Examples 2-1 to 2-7) and the adsorbent of Comparative Example 2-1 were produced as described above. The loading amount of 2-imidazolidinone in the produced porous materials (Examples 2-1 to 2-7 and Comparative Example 2-1) was 5.1% by mass, and the loading amount of phosphoric acid was 7.8% by mass.
[0133] Each physical property value of the porous materials (Examples 2-1 to 2-7, Comparative Example 2-1) produced in Example 2 was measured by the method shown below.
[0134] <Measurement of Nitrogen Adsorption Isotherm> Using a high-precision gas / vapor adsorption amount measuring device BELSORP-max (manufactured by MicrotracBEL Corporation), the porous material was heated at 250 °C for 3 hours under vacuum, and then the nitrogen adsorption isotherm of the porous material at 77 K was measured. The specific surface area (m 2 / g) was calculated by the BET method from the nitrogen adsorption isotherm.
[0135] <Measurement of Pore Volume of Micropores by HK Method> The HK method was applied to the nitrogen adsorption isotherm obtained above, and the pore volume (I) (cm 3 / g) of micropores less than 2 nm was calculated. In the analysis by the HK method, the reference curve "NGCB-BEL.t" provided by MicrotracBEL Corporation was used.
[0136] <Measurement of Pore Volume of Mesopores by BJH Method> The BJH method was applied to the nitrogen adsorption isotherm obtained above, and the pore volume (II) (cm 3 / g) of mesopores of 2 to 50 nm was calculated. In the analysis by the BJH method, the reference curve "NGCB-BEL.t" provided by MicrotracBEL Corporation was used.
[0137] The water retention rate and CADR performance of the porous materials (Examples 2-1 to 2-7, Comparative Example 2-1) produced in Example 2 were measured in the same manner as in Example 1 by the method described above.
[0138] The results are shown in Table 2.
[0139] [Table 2]
[0140] In Examples 2-1 to 2-7, the total CADR value for the composite gas containing multiple types of odorous substances was 918 to 1228. On the other hand, in Comparative Example 2-1, the total CADR value for the composite gas was 281. From this, it was recognized that the composite gas adsorbent of the present invention has a CADR superior to that of the gas adsorbent of the comparative example. In particular, it was recognized that in Examples 2-1 to 2-7, the volatile organic compounds (CADR: 503 to 673) and the aldehyde-based odorous substances (CADR: 186 to 244) had a CADR superior to that of the comparative example (volatile organic compounds CADR: 93, aldehyde-based odorous substances CADR: 30). Therefore, it was found that the composite gas adsorbent of the present invention can meet a certain level of adsorption capacity for the composite gas containing basic odorous substances (ammonia), volatile organic compounds (toluene, acetic acid), and aldehyde-based odorous substances (formaldehyde, acetaldehyde) as odorous substances, and can rapidly remove them.
[0141] Furthermore, in Examples 2-1 to 2-7, the CADR performance ratios (19.5 to 21.0%) of aldehyde odorous substances were recognized to be particularly superior to the CADR performance ratio (10.6%) of aldehyde odorous substances in Comparative Example 2-1.
[0142] The specific surface area in Examples 2-1 to 2-7 is 1056 to 2139 m 2 On the other hand, the specific surface area in Comparative Example 2-1 was 672 m 2 Therefore, the composite gas adsorbent of the present invention has a specific surface area of 1000 to 2200 m, calculated by the BET method from the nitrogen adsorption isotherm of the porous material. 2 / g is considered to be a good choice.
[0143] Thus, when the specific surface area is 1000m 2When the adsorbent has a CADR of less than 1.0 / g, the total CADR value for the composite gas and the CADR performance ratio for each gas (especially aldehyde odorants) are not excellent, and therefore it was found to be undesirable.
[0144] Specific surface area is 2200m 2 Similarly, when the CADR was greater than 100 / g, the total CADR value and the CADR performance ratio for each gas were not excellent, and this was also considered to be undesirable (results not shown).
[0145] In Examples 2-1 to 2-7, the water retention of the porous material was 38 to 61 mass%. On the other hand, the water retention of the comparative example 2-1 was 25%. Therefore, it was found that the composite gas adsorbent of the present invention is preferably one in which the water retention of the porous material is 35% or more in Example 2 as well.
[0146] In Examples 2-1 to 2-7, the sum of the pore volume (I) of micropores less than 2 nm calculated by the HK method and the pore volume (II) of mesopores of 2 to 50 nm calculated by the BJH method was 0.47 to 1.22 cm 3 On the other hand, the sum of the pore volumes in Comparative Example 2-1 was 0.29 cm 3 / g. Therefore, the composite gas adsorbent of the present invention has a pore volume of 0.35 to 1.50 cm3. 3 / g is considered to be a good choice.
[0147] The sum of the pore volumes is 0.35 cm 3 / g or less than 1.50cm 3 / g is not preferred because the total CADR for the composite gas in the composite gas adsorbent is not excellent.
[0148] In Examples 2-1 to 2-7, the ratio of the pore volume of the micropores to the sum of the pore volumes [(I) / ((I)+(II))] was 71 to 89%. On the other hand, the ratio in Comparative Example 2-1 was 89%. Therefore, it was found that the composite gas adsorbent of the present invention is preferably one having the ratio of 70 to 89%.
[0149] In addition, when the ratio is less than 70% or more than 89%, it is recognized that it is not preferable because the total CADR value for the composite gas in the composite gas adsorbent is not excellent.
[0150] In Examples 2-1 to 2-7, the ratio of the mesopore volume to the sum of the pore volumes [(II) / ((I)+(II))] was 11 to 29%. On the other hand, the ratio in Comparative Example 2-1 was 11%. Therefore, it was found that the composite gas adsorbent of the present invention should preferably have the ratio of 11 to 30%.
[0151] In addition, when the ratio is less than 11% or more than 30%, it is recognized that it is not preferable because the total CADR value for the composite gas in the composite gas adsorbent is not excellent.
[0152] Therefore, it was found that the composite gas adsorbent of the present invention should preferably have a 2-imidazolidinone loading amount of 3 mass% or more and a phosphoric acid loading amount of 3 mass% or more, and the ratio of the amount of phosphoric acid loaded to the amount of 2-imidazolidinone is equal to or greater than the amount loaded.
[0153] [Example 3] [Examples 3-1 to 3-3] The same porous material as in Example 1 was used, and the same carbonization and activation treatments were carried out.
[0154] The amounts of 2-imidazolidinone and inorganic acid or organic acid supported, the ratio of the amount of supported drug to the water retention rate, and the ratio of the amount of 2-imidazolidinone supported to the amount of inorganic acid or organic acid supported were adjusted for each Example in accordance with the method of Example 1 so as to obtain the values shown in Table 3.
[0155] That is, the porous material has a water retention rate of 35% by mass or more (61% by mass), and the porous material is supported with 3% by mass or more (15-35% by mass) of 2-imidazolidinone and 3% by mass or more of inorganic acid or organic acid (16.5-38.5% by mass phosphoric acid), and the inorganic acid or organic acid and 2-imidazolidinone are supported so that the amount of the inorganic acid or organic acid supported is equal to or more than the amount of 2-imidazolidinone (1.1 times). Furthermore, Examples 3-1 to 3-3 were prepared so that the ratio of the amount of supported drug to the water retention rate was 0.5 to 1.2.
[0156] [Table 3]
[0157] In Examples 3-1 to 3-3, when the amount of 2-imidazolidinone supported is 3% by mass or more, the amount of phosphoric acid supported is 3% by mass, the ratio of the amount of phosphoric acid supported to the amount of 2-imidazolidinone is equal to or more, and the ratio of the amount of drug supported to the water retention rate is 1.2 or less, the total CADR value is 1064 to 1481 m 3 / h.
[0158] On the other hand, in the case of Comparative Examples 1-1 and 1-2, in which the amount of phosphoric acid supported is less than 3 mass% and the ratio of the amount of phosphoric acid supported to 2-imidazolidinone is less than the same, the total CADR value is 741,763 m 3 / h, which is lower than the total CADR value of the above examples, and the CADR performance ratios of basic odorous substances were 3.3% and 2.7%, which are lower than the CADR performance ratios (basic odorous substances) of the above examples. From this, it was recognized that the CADR performance ratios of basic odorous substances in Comparative Examples 1-1 and 1-2 were inferior. [Industrial Applicability]
[0159] INDUSTRIAL APPLICABILITY The present invention can be utilized in a composite gas adsorbent that adsorbs a composite gas containing a plurality of odorous substances, a method for producing the composite gas adsorbent, a deodorizing filter using the composite gas adsorbent, and an air purifier using the deodorizing filter. [Explanation of symbols]
[0160] A Preparation process B. Supporting process
Claims
1. a porous material having a water retention rate of 35% by mass or more, 3% by mass or more of 2-imidazolidinone and 3% by mass or more of an inorganic acid or an organic acid being supported on the porous material, and the amount of the inorganic acid or the organic acid supported is equal to or more than the amount of 2-imidazolidinone; A composite gas adsorbent having adsorption performance for a composite gas containing a plurality of basic odorous substances, volatile organic compounds, and aldehyde odorous substances.
2. The specific surface area of the porous material calculated by the BET method from the nitrogen adsorption isotherm is 1000 to 2200 m 2 2. The composite gas adsorbent according to claim 1, wherein the molecular weight of the composite gas adsorbent is 1 / g.
3. The porous material has a pore volume of micropores less than 2 nm calculated from a nitrogen adsorption isotherm by the HK method and a pore volume of mesopores from 2 to 50 nm calculated by the BJH method of 0.35 to 1.50 cm 3 2. The composite gas adsorbent according to claim 1, wherein the molecular weight of the composite gas adsorbent is 1 / g.
4. 4. The composite gas adsorbent according to claim 3, wherein the ratio of the pore volume of the micropores to the sum of the pore volumes of the porous material is 70 to 89%, and the ratio of the pore volume of the mesopores to the sum of the pore volumes is 11 to 30%.
5. The composite gas adsorbent according to any one of claims 1 to 4, wherein the basic odorant is ammonia, the volatile organic compound is at least one of toluene and acetic acid, and the aldehyde odorant is at least one of acetaldehyde and formaldehyde.
6. The composite gas adsorbent according to any one of claims 1 to 4, wherein the organic acid is represented by the following chemical formula 1: [Case 1]
7. The composite gas adsorbent according to any one of claims 1 to 4, wherein the inorganic acid is phosphoric acid.
8. A method for producing a composite gas adsorbent, comprising: a preparation step of preparing an aqueous solution by dissolving powdered or particulate 2-imidazolidinone and an inorganic acid or an organic acid in water; and a supporting step of contacting the aqueous solution with a porous material to cause the porous material to support the aqueous solution.
9. A deodorizing filter for an indoor air purifier, comprising the composite gas adsorbent according to any one of claims 1 to 4.
10. An air purifier using the deodorizing filter according to claim 9.
Citation Information
Patent Citations
Porous adsorbent and filter
JP2001232189A
Activated carbon for removing mercury or mercury compound
JP2005349364A
Method of producing chemical-carrying active carbon, chemical-carrying active carbon and filter using the carbon
JP2014047087A
Porous adsorbent and filter
KR1020030016069A
Composite gas adsorbent member, adsorbent filter in which same is used, and method for manufacturing composite gas adsorbent member
WO2017086177A1