Reflection type mask blank for EUV lithography
The reflective mask blank for EUV lithography addresses the issue of resist film wear and protective layer damage by using a ruthenium protective layer, tantalum absorption layer, and chromium-nitrogen-oxygen hard mask layer with controlled film density, enhancing etching selectivity and pattern resolution.
Patent Information
- Application Number
- JP2024116779
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-05-21
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-05-20
AI Technical Summary
Conventional EUV lithography methods face challenges in achieving high-resolution patterns due to the wear of resist films during etching processes, and the use of hard mask layers can lead to damage of protective layers during dry etching with mixed gases, compromising pattern accuracy.
A reflective mask blank for EUV lithography is designed with a specific structure that includes a protective layer of ruthenium, an absorption layer of tantalum, and a hard mask layer of chromium with nitrogen and oxygen, with a film density of 3.00 to 5.40 g/cm³, to enhance etching selectivity and protect the reflective layer during etching processes.
The solution allows for a thin resist film, ensuring high-resolution patterns with minimal damage to the protective layer, thereby improving pattern accuracy and durability during the etching process.
Smart Images

Figure 2024147757000002 
Figure 2024147757000003 
Figure 2024147757000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a reflective mask blank for EUV (Extreme Ultra Violet) lithography (hereinafter, in this specification, sometimes referred to as "EUV mask blank") used in semiconductor manufacturing and the like. [Background technology]
[0002] Conventionally, in the semiconductor industry, photolithography using visible light or ultraviolet light has been used as a transfer technology of fine patterns necessary for forming integrated circuits consisting of fine patterns on Si substrates and the like. However, while the miniaturization of semiconductor devices is accelerating, the limit of conventional photolithography is approaching. In the case of photolithography, the resolution limit of the pattern is about 1 / 2 of the exposure wavelength. Even if the immersion method is used, it is said to be about 1 / 4 of the exposure wavelength, and even if the immersion method using an ArF laser with a wavelength of 193 nm is adopted for exposure, the resolution limit is expected to be about 20 to 30 nm. Therefore, EUV lithography, an exposure technology using EUV light with an even shorter wavelength than ArF laser, is seen as promising as an exposure technology aimed at miniaturization of 20 to 30 nm and below. In this specification, EUV light refers to light rays with a wavelength in the soft X-ray region or vacuum ultraviolet region. Specifically, it refers to light rays with a wavelength of about 10 to 20 nm, especially about 13.5 nm ± 0.3 nm.
[0003] EUV light is easily absorbed by all materials, and the refractive index of materials at this wavelength is close to 1. Therefore, refractive optics, as in conventional photolithography using visible or ultraviolet light, cannot be used. For this reason, EUV lithography uses reflective optics, that is, reflective photomasks and mirrors.
[0004] A mask blank is a pre-patterned laminate used for making photomasks. In the case of an EUV mask blank, a reflective layer that reflects EUV light and an absorbing layer that absorbs EUV light are formed in this order on a substrate such as glass. If necessary, a low-reflective layer against the inspection light of the mask pattern is formed on the absorbing layer. The wavelength range of the inspection light is 190 to 260 nm. The absorption layer is made of a material with a high absorption coefficient for EUV light, specifically a material containing tantalum (Ta), while the low-reflection layer is made of a material with low reflectance characteristics for the pattern inspection wavelength, specifically a material containing Ta and oxygen (O). Hereinafter, in this specification, when a low reflective layer is formed on an absorbing layer, the absorbing layer will be read as a low reflective layer, or a low reflective layer and an absorbing layer.
[0005] A photomask is manufactured from the mask blank having the above structure in the following manner. A resist film is applied to the absorbing layer, which is the top layer of the mask blank. A pattern is formed on the resist film using an electron beam lithography machine. Next, an etching process is carried out using the resist film with the pattern formed as a mask. This transfers the pattern to the absorbing layer. Here, since the resist film is also consumed in the above etching process, the film thickness of the resist film is made sufficiently thick. Although it depends on the type of resist and the etching conditions, the thickness of the resist is usually about 100 nm.
[0006] In recent years, as patterns become finer and denser, higher resolution patterns are required. To obtain higher resolution patterns, it is necessary to reduce the thickness of the resist film. However, when the thickness of the resist is reduced, the resist film is consumed during the etching process, which may result in a decrease in the accuracy of the pattern transferred to the absorber layer.
[0007] In order to solve the above-mentioned problems, it is generally known that the resist can be thinned by providing a layer of a material having resistance to the etching conditions of the absorbing layer, i.e., a hard mask layer (etching mask film), on the absorbing layer (see Patent Document 1). That is, by forming such a hard mask layer, the etching selectivity between the absorbing layer and the hard mask layer under the etching conditions of the absorbing layer, specifically, the ratio between the etching rate of the absorbing layer and the etching rate of the hard mask layer under the etching conditions of the absorbing layer, can be increased, thereby making it possible to thin the resist. Hereinafter, in this specification, the term "etching selectivity under the etching conditions for the absorber layer" means the etching selectivity between the absorber layer and the hard mask layer under the etching conditions for the absorber layer, and the etching selectivity is calculated by the following formula. Etching selectivity = etch rate of absorber layer / etch rate of hard mask layer
[0008] In the reflective mask blank described in Patent Document 1, the absorber layer (absorber film) is made of a material containing tantalum, the etching mask film is made of a material containing chromium, and the oxygen content is 40 at% or more. The etching mask film in Patent Document 1 corresponds to the hard mask layer in this specification. Hereinafter, in this specification, the etching mask film in Patent Document 1 will be referred to as the hard mask layer. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent No. 6343690 Summary of the Invention [Problem to be solved by the invention]
[0010] As described above, by providing a hard mask layer made of a material having a high etching selectivity under the etching conditions for the absorber layer on the absorber layer, the resist can be made thinner. However, when providing a hard mask layer, the following points must be considered. As described with reference to FIG. 2 in Patent Document 1, when a pattern is formed on a mask blank on which a hard mask layer is formed, the following procedure is followed. (1) A resist film is formed on a hard mask layer of a mask blank. (2) A transfer pattern (resist pattern) is formed on a resist film. (3) Using the resist pattern as a mask, dry etching is performed using a mixed gas of a chlorine-based gas and oxygen gas to form a transfer pattern (hard mask pattern) in the hard mask layer. (4) The resist pattern is removed, and dry etching using a fluorine-based gas and then dry etching using a chlorine-based gas not containing oxygen gas are performed using the hard mask pattern as a mask to form a transfer pattern (absorber pattern) in the absorber layer. (5) After the absorber pattern is formed, dry etching is performed using a mixed gas of a chlorine-based gas and an oxygen gas to remove the hard mask pattern.
[0011] On the other hand, when forming a transfer pattern on the absorbing layer by the dry etching process (4) above, a protective layer may be provided between the reflective layer and the absorbing layer in order to protect the reflective layer. Materials containing ruthenium (Ru) are widely used as materials for the protective layer, because the etching rate of the dry etching using a chlorine-based gas that does not contain oxygen gas is slower than that of the absorbing layer, and the material is less susceptible to damage by this dry etching.
[0012] A protective layer made of a material containing Ru is unlikely to be damaged by dry etching using a chlorine-based gas that does not contain oxygen gas. However, as described in paragraph 0032 of JP 11-354407 A, the protective layer is etched by dry etching using a mixed gas of chlorine-based gas and oxygen gas. Therefore, the protective layer is likely to be damaged by dry etching using the mixed gas of chlorine-based gas and oxygen gas used in the above (5). Therefore, if the time required for the above step (5) is long, the protective layer made of a material containing Ru may be damaged by dry etching using a mixed gas of a chlorine-based gas and an oxygen gas.
[0013] In order to solve the above-mentioned problems of the conventional technology, an object of the present invention is to provide an EUV mask blank including a hard mask layer which has a sufficiently high etching selectivity under etching conditions for an absorber layer and which has a sufficient etching rate in a dry etching process using a mixed gas of a chlorine-based gas and an oxygen gas. [Means for solving the problem]
[0014] As a result of intensive research to solve the above problems, the inventors have found that in addition to the material used for the hard mask layer, the film density of the hard mask layer affects the etching rate in a dry etching process using a mixed gas of a chlorine-based gas and an oxygen gas.
[0015] Based on the above findings, the present invention provides a reflective mask blank for EUV lithography, comprising a reflective layer that reflects EUV light, a protective layer for the reflective layer, an absorption layer that absorbs EUV light, and a hard mask layer formed in this order on a substrate, The protective layer contains ruthenium (Ru), The absorbing layer contains tantalum (Ta); the hard mask layer contains chromium (Cr) and at least one of nitrogen (N) and oxygen (O); The film density of the hard mask layer is 3.00 to 5.40 g / cm 3 We provide a reflective mask blank for EUV lithography.
[0016] The present invention also provides a reflective mask blank for EUV lithography, comprising a substrate on which a reflective layer that reflects EUV light, a protective layer for the reflective layer, an absorption layer that absorbs EUV light, a low-reflection layer for light having a wavelength of 190 to 260 nm that is used as inspection light for a mask pattern, and a hard mask layer are formed in this order, The protective layer contains ruthenium (Ru), The absorbing layer contains tantalum (Ta); The low reflective layer contains tantalum (Ta) and oxygen (O), the hard mask layer contains chromium (Cr) and at least one of nitrogen (N) and oxygen (O); The film density of the hard mask layer is 3.00 to 5.40 g / cm 3 We provide a reflective mask blank for EUV lithography.
[0017] The hard mask layer may further contain at least one of carbon (C) and boron (B).
[0018] The hard mask layer preferably has a thickness of 2 to 30 nm. Effect of the Invention
[0019] The hard mask layer in the reflective mask blank for EUV lithography of the present invention has a sufficiently high etching selectivity under the etching conditions of the absorber layer, which makes it possible to achieve a thinner resist film, which is required for obtaining a high-resolution pattern. The hard mask layer in the reflective mask blank for EUV lithography of the present invention has a sufficient etching rate in a dry etching process using a mixed gas of a chlorine-based gas and an oxygen gas, so that the Ru-containing protective layer is unlikely to be damaged when the hard mask layer is removed after the absorber layer is patterned. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of a reflective mask blank for EUV lithography of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a procedure for forming a pattern on the reflective mask blank for EUV lithography shown in FIG. 1, in which a resist film is formed on a hard mask layer. [Diagram 3]FIG. 3 is a schematic cross-sectional view showing a procedure subsequent to that shown in FIG. 2, in which a pattern is formed on the resist film. [Figure 4] FIG. 4 is a schematic cross-sectional view showing a step subsequent to that of FIG. 3 in which a hard mask layer has been patterned. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing a procedure subsequent to that shown in FIG. 4, in which the absorbing layer and the low-reflecting layer are patterned. [Figure 6] FIG. 6 is a schematic cross-sectional view showing a step subsequent to that of FIG. 5, in which the hard mask layer has been removed. [Figure 7] FIG. 7 is a graph showing the relationship between the oxygen content in the CrO film and the relative etching rate. [Figure 8] FIG. 8 is a graph showing the relationship between the oxygen content in the hard mask layer and the relative etching rate in the examples and comparative examples. [Figure 9] FIG. 9 is a graph showing the relationship between the film density of the hard mask layer and the relative etching rate in the examples and the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, a reflective mask blank for EUV lithography according to this embodiment will be described with reference to the drawings. Fig. 1 is a schematic cross-sectional view showing one embodiment of an EUV mask blank according to the present embodiment. In the EUV mask blank 1 shown in Fig. 1, a reflective layer 12 that reflects EUV light, a protective layer 13 for the reflective layer 12, an absorbing layer 14 that absorbs EUV light, a low reflective layer 15 against inspection light used to inspect a mask pattern, and a hard mask layer 16 are formed in this order on a substrate 11. However, in the EUV mask blank according to the present embodiment, only the substrate 11, the reflective layer 12, the protective layer 13, the absorbing layer 14, and the hard mask layer 16 are essential components in the configuration shown in Fig. 1, and the low reflective layer 15 is an optional component. The protective layer 13 for the reflective layer 12 is a layer provided for the purpose of protecting the reflective layer 12 when the absorbing layer 14 is patterned. The individual components of the EUV mask blank 1 will now be described.
[0022] (substrate) The substrate 11 satisfies the characteristics required for an EUV mask blank. Therefore, the substrate 11 has a low thermal expansion coefficient and is excellent in smoothness, flatness, and resistance to cleaning solutions used for cleaning the mask blank or the photomask after pattern formation. The thermal expansion coefficient of the substrate 11 at 20° C. is 0±0.05×10 -7 / °C is preferable, and 0±0.03×10 -7 / °C. As the substrate 11, specifically, glass having a low thermal expansion coefficient, such as SiO2-TiO2 glass, is used, but the present invention is not limited thereto, and substrates such as crystallized glass in which a β-quartz solid solution is precipitated, quartz glass, silicon, and metal can also be used. It is preferable that the substrate 11 has a smooth surface with a surface roughness (rms) of 0.15 nm or less and a flatness of 100 nm or less, because this allows high reflectance and transfer accuracy to be obtained in the photomask after pattern formation. The size and thickness of the substrate 11 are appropriately determined based on the design values of the mask, etc. In the embodiment shown later, SiO2-TiO2 glass having an outer shape of 6 inches (152 mm) square and a thickness of 0.25 inches (6.3 mm) was used. It is preferable that there are no defects on the surface of the substrate 11 on which the reflective layer 12 is formed. However, even if defects are present, it is acceptable as long as no phase defects are caused by concave defects and / or convex defects. Specifically, it is preferable that the depth of the concave defects and the height of the convex defects are 2 nm or less, and the half-value width of these concave defects and convex defects is 60 nm or less.
[0023] (reflective layer) The reflective layer 12 is not particularly limited as long as it has the desired characteristics as a reflective layer of an EUV mask blank. A characteristic particularly required for the reflective layer 12 is a high EUV light reflectance. Specifically, when a light beam in the wavelength region of EUV light is irradiated onto the surface of the reflective layer 12 at an incident angle of 6 degrees, the maximum value of the light reflectance at a wavelength of about 13.5 nm is preferably 60% or more, more preferably 65% or more. The higher the maximum value of the reflectance, the more preferable, and the upper limit is not particularly limited, but it is usually 75% or less. Even when a protective layer 13 is provided on the reflective layer 12, the maximum value of the light reflectance at a wavelength of about 13.5 nm is preferably 60% or more, more preferably 65% or more. The higher the maximum value of the reflectance, the more preferable, and the upper limit is not particularly limited, but it is usually 75% or less.
[0024] In order to achieve a high EUV light reflectance, a multilayer reflective film in which high refractive index layers and low refractive index layers are alternately stacked multiple times is usually used as the reflective layer 12. In the multilayer reflective film forming the reflective layer 12, Mo is widely used for the high refractive index layers, and Si is widely used for the low refractive index layers. That is, a Mo / Si multilayer reflective film is the most common. However, the multilayer reflective film is not limited thereto, and for example, a Ru / Si multilayer reflective film, a Mo / Be multilayer reflective film, a Mo compound / Si compound multilayer reflective film, a Si / Mo / Ru multilayer reflective film, a Si / Mo / Ru / Mo multilayer reflective film, and a Si / Ru / Mo / Ru multilayer reflective film can also be used.
[0025] The thickness of each layer constituting the multilayer reflective film constituting the reflective layer 12 and the number of repeat units of the layers can be appropriately selected depending on the film material used and the EUV light reflectance required for the reflective layer. Taking a Mo / Si multilayer reflective film as an example, to obtain a reflective layer 12 with a maximum EUV light reflectance of 60% or more, the multilayer reflective film may be laminated with Mo layers having a thickness of 2.3±0.1 nm and Si layers having a thickness of 4.5±0.1 nm so that the number of repeat units is 30 to 60.
[0026] Each layer constituting the multilayer reflective film forming the reflective layer 12 may be deposited to a desired thickness using a known deposition method such as magnetron sputtering, ion beam sputtering, etc. A preferred deposition method is, for example, to form a Si / Mo multilayer reflective film using ion beam sputtering, in which a Si target is used as the target, Ar gas is used as the sputtering gas, and a gas pressure of 1.3×10 -2 ~2.7×10 -2 A Si layer is deposited to a thickness of 4.5 nm at an ion acceleration voltage of 300 to 1500 V and a deposition rate of 0.030 to 0.300 nm / sec using a range of 1.3×10 Pa. Next, a Mo target is used as the target, Ar gas is used as the sputtering gas, and a gas pressure of 1.3×10 -2 ~2.7×10 -2 The Mo layer is deposited to a thickness of 2.3 nm at an ion acceleration voltage of 300 to 1500 V and a deposition rate of 0.030 to 0.300 nm / sec using a range of 1000 V and 1000 Pa. This counts as one cycle, and a suitable Si / Mo multilayer reflective film is deposited by laminating Si layers and Mo layers 40 to 50 cycles.
[0027] In order to prevent oxidation of the surface of the reflective layer 12, it is preferable that the top layer of the multilayer reflective film constituting the reflective layer 12 is a layer of a material that is not easily oxidized. The layer of the material that is not easily oxidized functions as a capping layer for the reflective layer 12. A specific example of a layer of a material that is not easily oxidized that functions as a capping layer is a Si layer. When the multilayer reflective film constituting the reflective layer 12 is a Si / Mo multilayer reflective film, the top layer is a Si layer, so that the top layer functions as a capping layer. In this case, the thickness of the capping layer is preferably 11±2 nm.
[0028] (protective layer) The protective layer 13 is provided for the purpose of protecting the reflective layer 12 from damage during an etching process, usually a dry etching process, in which a pattern is formed on the absorbing layer 14. Therefore, a material that is less susceptible to the etching process of the absorbing layer 14 is selected as the material for the protective layer. Specifically, a material is selected that has an etching rate slower than that of the absorbing layer 14 in the above etching process and is less susceptible to damage during the etching process. In the EUV mask blank 1 according to this embodiment, the protective layer 13 is made of a material containing ruthenium (Ru). Specific examples include Ru and Ru compounds, and examples of Ru compounds include RuB, RuSi, RuNb, RuTi, RuY, RuZr, and RuLa. From the viewpoint of dry etching durability, the material containing Ru is preferably a material containing 40.0 at% or more of Ru, more preferably 50.0 at% or more, and even more preferably 55.0 at% or more. The content of Ru in the material is preferably 95 at% or less, and more preferably 90 at% or less. The thickness of the protective layer 13 is preferably from 1 to 20 nm, and more preferably from 1 to 5 nm.
[0029] The protective layer 13 is formed by a known film formation method such as magnetron sputtering or ion beam sputtering. When forming a Ru film by magnetron sputtering, a Ru target is used as the target, and Ar gas is used as the sputtering gas at a gas pressure of 1.0×10 -2 ~1.0×10 0 It is preferable to use a pressure in the range of Pa, and form a film to a thickness of 2 to 5 nm under conditions of an input voltage of 30 to 1500 V and a film formation rate of 0.020 to 1.000 nm / sec.
[0030] (Absorption layer) A characteristic that is particularly required for the absorbing layer 14 is that the EUV light reflectance is extremely low. Specifically, when the surface of the absorbing layer 14 is irradiated with light in the wavelength region of EUV light, the maximum light reflectance at a wavelength of about 13.5 nm is preferably 2% or less, and more preferably 1% or less. The smaller the maximum light reflectance, the more preferable it is. In the EUV mask blank 1 according to this embodiment, even when the surface of the low reflective layer 15 is irradiated with light in the wavelength region of EUV light, the maximum light reflectance at a wavelength of about 13.5 nm is preferably 2% or less, and more preferably 1% or less. The smaller the maximum light reflectance, the more preferable it is.
[0031] In order to achieve the above characteristics, the absorbing layer 14 is made of a material having a high absorption coefficient for EUV light. In the EUV mask blank 1 according to this embodiment, a material containing tantalum (Ta) is used as the material having a high absorption coefficient for EUV light that constitutes the absorbing layer 14.
[0032] From the viewpoint of dry etching characteristics and cleaning resistance, the material containing Ta preferably contains 40.0 at% or more of Ta in the material, more preferably 50.0 at% or more, and even more preferably 55.0 at% or more. The Ta content in the material is preferably 100 at% or less, more preferably 95 at% or less, and even more preferably 90 at% or less. The Ta-containing material used for the absorption layer 14 may be, in addition to Ta, hafnium (Hf), silicon (Si), zirconium (Zr), germanium (Ge), boron (B), palladium (Pd), tin (Sn), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), silver (Ag), cadmium (Cd), indium (In), antimony (Sb), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), platinum (Pt), gold (Au), thallium (Tl), lead (Pb), or the like. (Pb), bismuth (Bi), carbon (C), titanium (Ti), zirconium (Zr), Nb, Mo, ruthenium (Ru), rhodium (Rh), palladium (Pd), calcium (Ca), magnesium (Mg), aluminum (Al), nickel (Ni), copper (Cu), zinc (Zn), gallium (Ga), arsenic (As), selenium (Se), tellurium (Te), hydrogen (H) and nitrogen (N) may be included. Specific examples of materials containing Ta and other elements include TaN, TaNH, TaHf, TaHfN, TaBSi, TaBSiN, TaB, TaBN, TaSi, TaSiN, TaGe, TaGeN, TaZr, TaZrN, TaNb, TaNbN, TaMo, TaMoN, TaPd, TaSn, TaPdN, TaSn, TaCr, TaMn, TaFe, TaCo, TaAg, TaCd, TaIn, TaSb, and TaW. The absorption layer may further contain oxygen, but from the viewpoint of dry etching rate, i.e., patterning, it is preferable that the amount of oxygen is small, and it is preferable that no oxygen is contained.
[0033] The absorbing layer 14 having the above-mentioned configuration can be formed by a known film forming method, for example, magnetron sputtering or ion beam sputtering. For example, when a TaNH film is formed as the absorbing layer 14 by magnetron sputtering, a Ta target is used as the target, and a mixed gas of Ar, N2, and H2 is used as the sputtering gas. For example, the mixed gas has an H2 gas concentration of 1 to 50 vol%, an N2 gas concentration of 1 to 80 vol%, and an Ar gas concentration of 5 to 95 vol%, and a gas pressure of 1.0×10 -1~5.0×10 -1 It is preferable to form the TaNH film to a thickness of 10 to 80 nm under conditions of a pressure in the range of 1 Pa, an input power of 30 to 3000 W, and a film formation rate of 0.5 to 60.0 nm / min. When an inert gas other than Ar is used, the concentration of the inert gas is set to be in the same concentration range as the Ar gas concentration described above. When multiple types of inert gas are used, the total concentration of the inert gas is set to be in the same concentration range as the Ar gas concentration described above.
[0034] The thickness of the absorbing layer 14 is preferably set so that the total thickness together with the low reflective layer 15 is 10 to 90 nm, and the total thickness of both is more preferably 15 nm or more, more preferably 87 nm or less, and further preferably 85 nm or less.
[0035] (Low reflective layer) The low reflection layer 15 is composed of a film that has low reflection with respect to the inspection light used for inspecting the mask pattern. When manufacturing an EUV mask, after a pattern is formed on the absorbing layer, it is inspected whether the pattern is formed as designed. In the inspection of this mask pattern, light with a wavelength of about 190 to 260 nm is usually used as the inspection light. That is, the inspection is performed based on the difference in reflectance of the light with a wavelength of 190 to 260 nm, specifically, the difference in reflectance between the surface of the absorbing layer 14 that is removed and exposed by pattern formation and the surface of the absorbing layer 14 that is not removed by pattern formation and remains. Here, the former surface is the surface of the protective layer 13. Therefore, if the difference in reflectance between the surface of the protective layer 13 and the surface of the absorbing layer 14 with respect to the wavelength of the inspection light is small, the contrast during inspection becomes poor, and accurate inspection cannot be performed.
[0036] The light reflectance of the absorbing layer 14 having the above-mentioned configuration is not necessarily sufficiently low when viewed with respect to the wavelength of the inspection light. As a result, the difference between the reflectance of the surface of the absorbing layer 14 and the reflectance of the surface of the protective layer 13 at the wavelength of the inspection light becomes small, and there is a possibility that sufficient contrast cannot be obtained during inspection. If sufficient contrast cannot be obtained during inspection, defects in the pattern cannot be sufficiently identified during mask inspection, and accurate defect inspection cannot be performed. However, this means that there is room for improvement from the viewpoint of defect inspection, and does not mean that there is a defect as an EUV mask blank.
[0037] In the EUV mask blank 1 according to this embodiment, it is preferable to form a low-reflection layer 15 for the inspection light on the absorbing layer 14, since this will result in extremely low light reflectance at the wavelength of the inspection light, resulting in good contrast during inspection.
[0038] In order to achieve the above characteristics, the low reflection layer 15 is made of a material having a lower refractive index at the wavelength of the inspection light than the absorption layer 14 . The reflectance of the low reflection layer 15 to the inspection light is preferably 15% or more lower than the reflectance of the surface of the protective layer 13 to the inspection light, the difference being more preferably 20% or more, and even more preferably 25% or more.
[0039] In order to achieve the above characteristics, in the EUV mask blank 1 according to this embodiment, a material containing Ta and oxygen (O) is used as a constituent material of the low reflective layer 15, whereas the absorption layer 14 is made of a material containing Ta.
[0040] The material containing Ta and O preferably contains Ta and O in a total content of 40.0 at% or more, more preferably 50.0 at% or more, and further preferably 55.0 at% or more. The upper limit of the total content is not particularly limited, and may be 100 at%. An example of a material containing Ta and O is TaO.
[0041] The material containing Ta and O used for the low reflective layer 15 may contain other elements exemplified above (absorption layer) in addition to Ta and O. Specific examples of the material containing the above-mentioned other elements in addition to Ta and O include oxides of the specific examples of the material containing Ta and other elements.
[0042] When the low reflective layer 15 is formed on the absorbing layer 14, the total thickness of the two is preferably 10 to 90 nm, more preferably 15 nm or more, more preferably 87 nm or less, and even more preferably 85 nm or less. If the thickness of the low reflective layer 15 is thicker than the thickness of the absorbing layer 14, the EUV light absorption characteristics of the absorbing layer 14 may be deteriorated. Therefore, it is preferable that the thickness of the low reflective layer 15 is thinner than the thickness of the absorbing layer 14. Therefore, the thickness of the low reflective layer 15 is preferably 1 to 20 nm, more preferably 1 to 15 nm, and even more preferably 1 to 10 nm.
[0043] The low reflection layer 15 having the above-mentioned structure can be formed by a known film formation method, for example, magnetron sputtering or ion beam sputtering. For example, when a TaONH film is formed as the low reflection layer 15 by magnetron sputtering, a Ta target is used as the target, and a mixed gas of Ar, O2, N2, and H2 is used as the sputtering gas. The mixed gas has, for example, an H2 gas concentration of 1 to 50 vol%, an O2 gas concentration of 1 to 80 vol%, an N2 gas concentration of 1 to 80 vol%, and an Ar gas concentration of 5 to 95 vol%, and a gas pressure of 1.0×10 -1 ~5.0×10 0 It is preferable to form a film to a thickness of 3 to 30 nm under conditions of a pressure in the range of 1 Pa, an input power of 30 to 3000 W, and a film formation rate of 0.01 to 60 nm / min. When an inert gas other than Ar is used, the concentration of the inert gas is set in the same concentration range as the above-mentioned Ar gas concentration.
[0044] In the EUV mask blank 1 according to the present embodiment, the reason why the formation of the low reflective layer 15 on the absorbing layer 14 is preferable is because the wavelength of the pattern inspection light is different from the wavelength of the EUV light. Therefore, when EUV light having a wavelength of about 13.5 nm is used as the pattern inspection light, it is considered that it is not necessary to form the low reflective layer 15 on the absorbing layer 14. The wavelength of the inspection light tends to shift to the short wavelength side as the pattern dimensions become smaller, and is considered to shift to 193 nm and further to 13.5 nm in the future. When the wavelength of the inspection light is 13.5 nm, it is considered that it is not necessary to form the low reflective layer 15 on the absorbing layer 14.
[0045] (Hard mask layer) The hard mask layer 16 is required to have a sufficiently high etching selectivity under the etching conditions for the absorber layer 14 and the low reflective layer 15. To achieve this, the hard mask layer 16 needs to have sufficient etching resistance against the etching conditions for the absorber layer 14 and the low reflective layer 15. As described above, when the absorbing layer or the low-reflecting layer is made of a material containing Ta, the etching of the absorbing layer is performed in the order of dry etching using a fluorine-based gas and dry etching using a chlorine-based gas not containing oxygen gas. Therefore, the hard mask layer 16 is required to have high etching resistance against dry etching using a fluorine-based gas and dry etching using a chlorine-based gas not containing oxygen gas. On the other hand, dry etching using a mixed gas of a chlorine-based gas and an oxygen gas is used for etching the hard mask layer 16. Therefore, the hard mask layer 16 is also required to have a sufficient etching rate in the dry etching using a mixed gas of a chlorine-based gas and an oxygen gas.
[0046] Of the two requirements mentioned above, in order to satisfy the former requirement of high etching resistance, the hard mask layer 16 of the EUV mask blank 1 according to this embodiment contains chromium (Cr) and at least one of nitrogen (N) and oxygen (O). Specific examples include a CrN film containing Cr and N, a CrO film containing Cr and O, and a CrON film containing Cr, O, and N.
[0047] Of the two requirements mentioned above, the latter, a sufficient etching rate, was considered to be controllable by the composition ratio of elements contained in the hard mask layer in conventional techniques such as Patent Document 1. For example, in the case of a CrO film, increasing the O content was considered preferable because it increases the etching rate in dry etching using a mixed gas of a chlorine-based gas and an oxygen gas. Therefore, the reflective mask blank of Patent Document 1 is described as having a hard mask layer made of a material containing chromium and having an oxygen content of 40 at% or more. 7 is a graph showing the relationship between the oxygen content in the CrO film that becomes the hard mask layer and the relative etching rate. The relative etching rate in the graph shows the relative rate when the etching rate in Example 1 in the examples described later is set to 1 in dry etching using a mixed gas of a chlorine-based gas and an oxygen gas. As shown in Fig. 7, when the oxygen content in the CrO film is increased in order to obtain a sufficient etching rate in dry etching using a mixture of chlorine-based gas and oxygen gas, the etching rate increases rapidly, making it difficult to control the etching rate. When a CrN film or a CrON film is used as a hard mask layer, a similar phenomenon is predicted for the nitrogen content or the oxygen and nitrogen content in the film.
[0048] On the other hand, as shown in the examples described later, it has been newly discovered that there is a good correlation between the film density of the hard mask layer and the etching rate in dry etching using a mixed gas of a chlorine-based gas and an oxygen gas.
[0049] Based on the above findings, the EUV mask blank 1 according to this embodiment has a film density of the hard mask layer 16 of 3.00 to 5.40 g / cm in order to satisfy the latter of the two requirements described above, namely, a sufficient etching rate. 3 It is. If the film density of the hard mask layer 16 is within the above range, a sufficient etching rate can be obtained in dry etching using a mixed gas of a chlorine-based gas and an oxygen gas. The film density of the hard mask layer 16 is 5.40 g / cm 3 If the etching rate exceeds 100%, a sufficient etching rate cannot be obtained in the dry etching using a mixed gas of a chlorine-based gas and an oxygen gas, and therefore the time required to remove the hard mask pattern by dry etching as described in (5) above becomes long, and the protective layer 12 made of a material containing Ru may be damaged by the dry etching using a mixed gas of a chlorine-based gas and an oxygen gas. The film density of the hard mask layer 16 is 3.00 g / cm 3 If it is less than this, the etching rate in dry etching using a mixed gas of a chlorine-based gas and an oxygen gas becomes too fast, making it difficult to control the etching. In addition, the etching resistance to dry etching using a fluorine-based gas and dry etching using a chlorine-based gas not containing oxygen gas decreases, and the etching selectivity in the etching conditions for the absorption layer 14 and the low reflective layer 15 decreases, resulting in problems such as the like. The film density of the hard mask layer 16 is 3.50 g / cm 3 More than 4.00 g / cm is preferable. 3 More preferably, 4.20 g / cm 3 More preferably, the film density is 5.00 g / cm. 3 Less than 4.80 g / cm is preferred. 3 The following is even more preferred: The film density of the hard mask layer 16 was measured using X-ray reflectivity in the examples described later, but is not limited to this. For example, the density can also be calculated from the ratio of the surface density measured by Rutherford backscattering spectroscopy to the film thickness measured by a transmission electron microscope.
[0050] When the hard mask layer 16 contains Cr and at least one of N and O, the contents of Cr, N and O in the hard mask layer preferably satisfy the following. Cr: 30.0 to 50.0 at% N: 0.0 to 50.0 at% O: 0.0 to 70.0 at%
[0051] The hard mask layer 16 may further contain at least one of carbon (C) and boron (B) in addition to Cr, N, and O. Since C and B have smaller atomic weights than N and O, the inclusion of these elements can reduce the film density of the hard mask layer 16. Specifically, examples of the hard mask layer 16 include a CrCN film containing Cr, N, and C, a CrCO film containing Cr, O, and C, a CrCON film containing Cr, O, N, and C, a CrBN film containing Cr, N, and B, a CrBO film containing Cr, O, and B, a CrBON film containing Cr, O, N, and B, a CrBCN film containing Cr, N, B, and C, a CrBCO film containing Cr, O, B, and C, and a CrBOCN film containing Cr, O, N, B, and C.
[0052] When the hard mask layer 16 further contains at least one of C and B in addition to Cr, N, and O, the contents of Cr, N, O, C, and B in the hard mask layer preferably satisfy the following. Cr: 30.0 to 50.0 at% N: 0.0 to 50.0 at% O: 0.0 to 70.0 at% C: 0.0 to 30.0 at% B: 0.0 to 50.0 at%
[0053] The hard mask layer 16 may contain elements other than those mentioned above as long as they do not adversely affect the above-mentioned characteristics. For example, the hard mask layer 16 may contain at least one element selected from the group consisting of H, Si, Ge, Ru, and Al in a total content of 20.0 at% or less.
[0054] The film thickness of the hard mask layer 16 is preferably from 2 to 30 nm, more preferably from 2 to 25 nm, and further preferably from 2 to 10 nm.
[0055] The hard mask layer 16 can be formed by a known film forming method, for example, a sputtering method such as magnetron sputtering or ion beam sputtering.
[0056] When forming a CrO film by sputtering, for example, sputtering may be performed using a Cr target in an atmosphere containing an inert gas containing at least one of He, Ar, Ne, Kr, and Xe (hereinafter simply referred to as an inert gas) and O2 gas. When using magnetron sputtering, the film may be formed under the following film formation conditions. The sputtering gas used is a mixed gas of Ar and O2, with the O2 gas concentration being 15 to 100 vol%, preferably 20 to 80 vol%, and the Ar gas concentration being 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0057] When forming a CrN film by sputtering, sputtering may be performed using a Cr target in an atmosphere containing an inert gas and nitrogen (N2). When using magnetron sputtering, the film may be formed under the following film formation conditions. The sputtering gas used is a mixed gas of Ar and N2, with the N2 gas concentration being 15 to 100 vol%, preferably 20 to 80 vol%, and the Ar gas concentration being 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less. In addition, even if O2 is not introduced as a sputtering gas when forming the CrN film, oxygen may be unintentionally mixed into the film due to residual moisture in the chamber or degassing from the components. This also applies to the CrBN and CrBCN films described below.
[0058] When forming a CrON film by sputtering, sputtering may be performed using a Cr target in an atmosphere containing an inert gas, O2, and N2. When using magnetron sputtering, the film may be formed under the following film formation conditions. The sputtering gas used is a mixed gas of Ar, O2, and N2. The N2 gas concentration is 14.9 to 99.9 vol%, preferably 20.0 to 80.0 vol%, the O2 gas concentration is 0.1 to 85.0 vol%, preferably 0.5 to 80.0 vol%, and the Ar gas concentration is 0.0 to 85.0 vol%, preferably 20.0 to 80.0 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0059] When forming a CrCN film by sputtering, sputtering may be performed in an atmosphere containing an inert gas and N2 using a Cr target and a C target, or a target containing Cr and C. When using magnetron sputtering, it may be performed under the following film formation conditions. The sputtering gas used is a mixed gas of Ar and N2, with the N2 gas concentration being 15 to 100 vol%, preferably 20 to 80 vol%, and the Ar gas concentration being 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0060] When forming a CrCO film by sputtering, sputtering may be performed using a Cr target and a C target in an atmosphere containing an inert gas and O2, or using a target containing Cr and C. When using magnetron sputtering, the film may be formed under the following film forming conditions. The sputtering gas used is a mixed gas of Ar and O2, with the O2 gas concentration being 15 to 100 vol%, preferably 20 to 80 vol%, and the Ar gas concentration being 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0061] When forming a CrCON film by sputtering, sputtering may be performed using a Cr target and a C target in an atmosphere containing an inert gas, O2, and N2, or using a target containing Cr and C. When using magnetron sputtering, the film formation conditions are specifically as follows. The sputtering gas used is a mixed gas of Ar, O2, and N2. The N2 gas concentration is 14.9 to 99.9 vol%, preferably 20 to 80 vol%, the O2 gas concentration is 0.1 to 85 vol%, preferably 0.5 to 80 vol%, and the Ar gas concentration is 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0062] When forming a CrBN film by sputtering, sputtering may be performed in an atmosphere containing an inert gas and N2 using a Cr target and a B target, or a target containing Cr and B. When magnetron sputtering is used, it may be performed under the following film formation conditions. The sputtering gas used is a mixed gas of Ar and N2, with the N2 gas concentration being 15 to 100 vol%, preferably 20 to 80 vol%, and the Ar gas concentration being 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0063] When forming a CrBO film by sputtering, sputtering may be performed using a Cr target and a B target in an atmosphere containing an inert gas and O2, or using a target containing Cr and B. When using magnetron sputtering, it may be performed under the following film formation conditions. The sputtering gas used is a mixed gas of Ar and O2, with the O2 gas concentration being 15 to 100 vol%, preferably 20 to 80 vol%, and the Ar gas concentration being 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0064] When forming a CrBON film by sputtering, sputtering may be performed using a Cr target and a B target in an atmosphere containing an inert gas, O2, and N2, or using a target containing Cr and B. When using magnetron sputtering, the film may be formed under the following specific film forming conditions. The sputtering gas used is a mixed gas of Ar, O2, and N2. The N2 gas concentration is 14.9 to 99.9 vol%, preferably 20 to 80 vol%, the O2 gas concentration is 0.1 to 85 vol%, preferably 0.5 to 80 vol%, and the Ar gas concentration is 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0065] When forming a CrBCN film by sputtering, sputtering may be performed in an atmosphere containing an inert gas and N2 using a Cr target, a B target, and a C target, a target containing Cr, one of B and C, and the other target, or a target containing Cr, B, and C. When magnetron sputtering is used, it may be performed under the following film formation conditions. The sputtering gas used is a mixed gas of Ar and N2, with the N2 gas concentration being 15 to 100 vol%, preferably 20 to 80 vol%, and the Ar gas concentration being 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0066] When forming a CrBCO film by sputtering, sputtering may be performed using a Cr target, a B target, and a C target in an atmosphere containing an inert gas and O2, a target containing Cr, one of B and C, and the other target, or a target containing Cr, B, and C. When magnetron sputtering is used, it may be performed under the following film formation conditions. The sputtering gas used is a mixed gas of Ar and O2, with the O2 gas concentration being 15 to 100 vol%, preferably 20 to 80 vol%, and the Ar gas concentration being 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0067] When forming a CrBOCN film by sputtering, sputtering may be performed using a Cr target, a B target, and a C target in an atmosphere containing an inert gas, O2, and N2, a target containing Cr, one of B and C, and the other target, or a target containing Cr, B, and C. When using magnetron sputtering, the following film formation conditions may be used. The sputtering gas used is a mixed gas of Ar, O2, and N2. The N2 gas concentration is 14.9 to 99.9 vol%, preferably 20 to 80 vol%, the O2 gas concentration is 0.1 to 85 vol%, preferably 0.5 to 80 vol%, and the Ar gas concentration is 0 to 85 vol%, preferably 20 to 80 vol%. Gas pressure is 5.0 x 10 -2 ~1.0×10 0 Pa, preferably 1.0×10 -1 Pa or more, preferably 2.0×10 -1 Pa or more, and preferably 8.0×10 -1 Pa or less, more preferably 4.0×10 -1 Pa or less. The input power density per target area is 2.0 to 13.0 W / cm 2 and preferably 3.0 W / cm 2 More preferably, 4.0 W / cm 2 More than 12.0 W / cm 2 Less than or equal to 10.0 W / cm 2 The following is the result. The film formation rate is 0.010 to 0.400 nm / sec, preferably 0.015 nm / sec or more, more preferably 0.020 nm / sec or more, and preferably 0.300 nm / sec or less, more preferably 0.200 nm / sec or less. The distance between the target and the substrate is 50 to 500 mm, preferably 100 mm or more, more preferably 150 mm or more, and is preferably 400 mm or less, more preferably 300 mm or less.
[0068] When an inert gas other than Ar is used, the concentration of the inert gas is set to be in the same concentration range as the Ar gas concentration described above. When multiple types of inert gas are used, the total concentration of the inert gas is set to be in the same concentration range as the Ar gas concentration described above.
[0069] The film density of the hard mask layer in this embodiment can be controlled not only by the component ratio of the composition used in the hard mask layer, but also by film formation conditions such as the gas pressure of the sputtering gas, the input power density per target area, and the distance between the target and the substrate. Specifically, in order to obtain a low-density film with the same film composition, it is possible to implement at least one condition selected from the group consisting of increasing the gas pressure, decreasing the input power density per target area, and increasing the distance between the target and the substrate. Conversely, in order to obtain a high-density film with the same composition, it is possible to implement at least one condition selected from the group consisting of decreasing the gas pressure, increasing the input power density per target area, and decreasing the distance between the target and the substrate.
[0070] The EUV mask blank 1 according to this embodiment may have a functional film known in the field of EUV mask blanks, in addition to the reflective layer 12, protective layer 13, absorbing layer 14, and hard mask layer 16, as well as the low reflective layer 15 and other protective layers formed as necessary. A specific example of such a functional film is a high dielectric coating applied to the back side of the substrate to promote electrostatic chucking of the substrate, as described in JP 2003-501823 A. Here, the back side of the substrate refers to the surface of the substrate 11 in FIG. 1 opposite to the side on which the reflective layer 12 is formed. The high dielectric coating applied to the back side of the substrate for such a purpose is selected so that the electrical conductivity and thickness of the constituent material are such that the sheet resistance is 100Ω / □ or less. The constituent material of the high dielectric coating can be widely selected from those described in known documents. For example, a high dielectric constant coating described in JP 2003-501823 A, specifically, a coating made of silicon, TiN, molybdenum, chromium, and TaSi can be applied. The thickness of the high dielectric coating can be, for example, 10 to 1000 nm. The high dielectric coating can be formed by using a known film formation method, for example, a sputtering method such as magnetron sputtering or ion beam sputtering, a CVD (chemical vapor deposition) method, a vacuum deposition method, or an electrolytic plating method.
[0071] Next, a procedure for forming a pattern on the EUV mask blank according to this embodiment will be described with reference to FIGS. 2 to 6. When forming a pattern on the EUV mask blank, as shown in FIG. 2, a resist film 20 is formed on the hard mask layer 16 of the EUV mask blank 1, and a pattern is formed on the resist film 20 using an electron beam lithography machine as shown in FIG. 3. Next, as shown in FIG. 4, a pattern is formed on the hard mask layer 16 using the patterned resist film as a mask. Note that FIG. 4 shows a state in which the resist film 20 has been removed after the patterning of the hard mask layer 16. To form a pattern on the hard mask layer 16, dry etching using a mixed gas of a chlorine-based gas and an oxygen gas may be performed. Next, as shown in FIG. 5, a pattern is formed on the absorption layer 14 and the low reflective layer 15 using the patterned hard mask layer 16 as a mask. To form a pattern on the absorption layer 14 and the low reflective layer 15, dry etching may be performed using a fluorine-based gas and then using a chlorine-based gas that does not contain oxygen gas. Next, as shown in FIG. 6, the hard mask layer 16 is removed. The hard mask layer 16 may be removed by dry etching using a mixed gas of a chlorine-based gas and an oxygen gas. EXAMPLES
[0072] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. Among Examples 1 to 10, Examples 1 to 3, 5, and 7 are Comparative Examples, and Examples 4, 6, and 8 to 10 are Examples.
[0073] [Example 1] In Example 1, an EUV mask blank 1 having the configuration shown in FIG. 1 was produced. A SiO2-TiO2-based glass substrate (6-inch (152 mm) square, 6.3 mm thick) was used as the substrate 11 for film formation. The thermal expansion coefficient of this glass substrate at 20°C is 0.2×10 -7 / ℃, Young's modulus is 67GPa, Poisson's ratio is 0.17, and specific rigidity is 3.07×10 7 m 2 / s 2The glass substrate was polished to a smooth surface with a surface roughness (rms) of 0.15 nm or less and a flatness of 100 nm or less.
[0074] On the back surface of the substrate 11, a 100 nm-thick Cr film was formed by magnetron sputtering, thereby providing a high dielectric coating with a sheet resistance of 100 Ω / □. The substrate 11 (6-inch (152 mm) square outer shape, 6.3 mm thick) was fixed to a conventional flat electrostatic chuck via the Cr film, and a Si layer (4.5 nm thick) and a Mo layer (2.3 nm thick) were alternately formed on the surface of the substrate 11 by ion beam sputtering for 40 cycles, thereby forming a Si / Mo multilayer reflective film (reflective layer 12) with a total thickness of 272 nm (=(4.5 nm+2.3 nm)×40). Furthermore, a Ru film (thickness: 2.5 nm) was formed on the Si / Mo multilayer reflective film (reflective layer 12) by ion beam sputtering, thereby forming a protective layer 13.
[0075] The deposition conditions for the Si layer, Mo layer and Ru film are as follows. (Si layer deposition conditions) Target: Si target (boron doped) Sputtering gas: Ar gas (gas pressure 2.0 × 10 -2 Pa) Voltage: 700V Deposition rate: 0.077nm / sec Film thickness: 4.5 nm (Mo layer deposition conditions) Target: Mo target Sputtering gas: Ar gas (gas pressure 2.0 × 10 -2 Pa) Voltage: 700V Deposition rate: 0.064nm / sec Film thickness: 2.3 nm (Ru film formation conditions) Target: Ru target Sputtering gas: Ar gas (gas pressure 2.0 × 10 -2 Pa) Voltage: 500V Deposition rate: 0.023nm / sec Film thickness: 2.5 nm
[0076] Next, an absorption layer 14 (TaNH film) containing Ta, N and H was formed on the protective layer 13 by magnetron sputtering. The film formation conditions for the absorption layer 14 are as follows. (Film formation conditions for the absorption layer 14 (TaNH film)) Target: Ta target Sputtering gas: mixed gas of Ar, N2 and H2 (Ar: 89 vol%, N2: 8.3 vol%, H2: 2.7 vol%, gas pressure: 4.6 × 10 -1 Pa) Input power: 300W Deposition speed: 1.5nm / min Film thickness: 70nm
[0077] Next, a low reflective layer 15 (TaONH film) containing Ta, O, N and H was formed on the absorption layer 14 (TaNH film). The film formation conditions for the low reflective layer 15 (TaONH film) were as follows. (Deposition conditions of low reflection layer 15 (TaONH film)) Target: Ta target Sputtering gas: mixed gas of Ar, O2, N2 and H2 (Ar: 48 vol%, O2: 36 vol%, N2: 14 vol%, H2: 2 vol%, gas pressure: 3.0 × 10 -1 Pa) Input power: 450W Deposition speed: 1.5nm / min Film thickness: 10 nm
[0078] Next, a hard mask layer 16 (CrO film) containing Cr and O was formed on the low reflective layer 15 by magnetron sputtering, thereby obtaining an EUV mask blank 1 in which the reflective layer 12, the protective layer 13, the absorption layer 14, the low reflective layer 15 and the hard mask layer 16 were formed in this order on the substrate 11. The film formation conditions for the hard mask layer 16 are as follows. (Deposition conditions of hard mask layer 16 (CrO film)) Target:Cr target Sputtering gas: Ar and O2 mixed gas (Ar: 35 vol%, O2: 65 vol%, gas pressure: 1.5 × 10 -1 Pa) Input power density per target area: 4.1W / cm 2 Deposition speed: 0.250nm / sec Distance between target and board: 300mm Film thickness: 10 nm
[0079] The hard mask layer 16 (CrO film) of the EUV mask blank 1 obtained by the above procedure was subjected to the following evaluations (1) to (4). (1) Film composition The composition of the hard mask layer 16 (CrO film) was measured using an X-ray Photoelectron Spectrometer (manufactured by PERKIN ELEMER-PHI), a Secondary Ion Mass Spectrometer (manufactured by PHI-ATOMIKA), and a Rutherford Back Scattering Spectroscopy (manufactured by Kobe Steel, Ltd.) The composition ratio (at%) of the hard mask layer 16 (CrO film) was Cr:O=75.8:24.2, that is, the Cr content was 75.8 at% and the O content was 24.2 at%.
[0080] (2) Film density The film density was evaluated by the following method, instead of using the EUV mask blank 1 produced by the above procedure. A hard mask layer 16 (CrO film) was formed as a sample on a 4-inch quartz substrate serving as a sample stage under the same conditions as described above. The film density of the above samples was measured using X-ray reflectometry (XRR).
[0081] (3) Etching characteristics (1) The etching characteristics (1) were evaluated by the following method, instead of using the EUV mask blank 1 prepared by the above procedure. A Si chip (10 mm x 30 mm) on which a hard mask layer 16 (CrO film) was formed under the same conditions as above was placed on the sample stage of an ICP (inductively coupled plasma) etching device as a sample. The above sample was subjected to ICP plasma etching under the conditions shown below to determine the etching rate, which was shown as a relative rate when the etching rate in Example 1 was taken as 1. ICP antenna bias: 200W Substrate bias: 40W Etching time: 30 sec Trigger pressure: 3.0×10 0 Pa Etching pressure: 3.0×10 -1 Pa Etching gas: Cl2 / O2 Gas flow rate (Cl2 / O2): 10 / 10sccm
[0082] (4) Etching characteristics (2) The etching characteristics (2) were evaluated by the following method, instead of using the EUV mask blank 1 prepared by the above procedure. A Si chip (10 mm x 30 mm) on which an absorption layer 14 (TaNH film) and a hard mask layer 16 (CrO film) were formed under the same conditions as above was placed as a sample. The above sample was ICP plasma etched using the chlorine-based gas process not containing oxygen gas shown below. Note that the absorption layer 14 (TaNH film) was ICP plasma etched using the chlorine-based gas process not containing oxygen gas shown below after the surface native oxide film was removed using the fluorine-based gas process shown below. (Fluorine gas process) ICP antenna bias: 100W Substrate bias: 40W Etching time: 15 sec Trigger pressure: 3.0×10 0 Pa Etching pressure: 3.0×10 -1 Pa Etching gas: CF4 / He Gas flow rate (Cl2 / He): 4 / 16sccm (Chlorine gas process that does not contain oxygen gas) ICP antenna bias: 100W Substrate bias: 40W Etching time: 30 sec Trigger pressure: 3.0×10 0 Pa Etching pressure: 3.0×10 -1 Pa Etching gas: CF4 / He Gas flow rate (CF4 / He): 12 / 12sccm The etching rates of the TaNH film and the CrO film were determined, and the etching selectivity under the etching conditions for the absorption layer was calculated based on the following formula. Etching selectivity = Etching rate of TaNH film / Etching rate of CrO From the obtained results, the etching selectivity under the etching conditions of the absorption layer was evaluated according to the following criteria: A is very good, B is good, and C is poor. A: Etching rate of TaNH film / etching rate of CrO>7 / 1 B: Etching rate of TaNH film / etching rate of CrO=7 / 1~3 / 1 C: Etching rate of TaNH film / etching rate of CrO<3 / 1
[0083] (5) Durability of Ru protective layer For EUV mask blanks, it is necessary to reduce damage to a protective layer made of a material containing Ru (hereinafter, sometimes referred to as a Ru protective layer) caused by dry etching using a mixed gas of chlorine-based gas and oxygen gas, which is performed for the purpose of removing a hard mask pattern. As a result of intensive research into the application conditions of the process for various hard mask layers, it was found that damage to the Ru protective layer can be reduced when the relative rate described in the above etching characteristic (1) is 1.65 to 3.5. Therefore, when the relative rate described in the above etching characteristic (1) is 1.65 to 3.5, the durability of the Ru protective layer is very good, and is indicated as A in the table, and when it is less than 1.65 or exceeds 3.5, the durability of the Ru protective layer is poor, and is indicated as C in the table.
[0084] [Example 2] In Example 2, an EUV mask blank was produced in the same manner as in Example 1, except that a CrON film was formed as the hard mask layer 16 under the following conditions. (Deposition conditions of hard mask layer 16 (CrON film)) Target:Cr target Sputtering gas: mixed gas of Ar, O2 and N2 (Ar: 27 vol%, O2: 55 vol%, N2: 18 vol%, gas pressure: 2.6 × 10 -1 Pa) Input power density per target area: 4.1W / cm 2 Deposition speed: 0.270nm / sec Distance between target and board: 300mm Film thickness: 10 nm The composition ratio (at %) of the hard mask layer 16 (CrON film) was Cr:O:N=45.8:44.2:10.0, that is, the Cr content was 45.8 at %, the O content was 44.2 at %, and the N content was 10.0 at %.
[0085] [Example 3] In Example 3, an EUV mask blank was produced in the same manner as in Example 1, except that a CrON film was formed as the hard mask layer 16 under the following conditions. (Deposition conditions of hard mask layer 16 (CrON film)) Target:Cr target Sputtering gas: mixed gas of Ar, O2 and N2 (Ar: 16 vol%, O2: 67 vol%, N2: 17 vol%, gas pressure: 2.6 × 10 -1 Pa) Input power density per target area: 4.1W / cm 2 Deposition rate: 0.040nm / sec Distance between target and board: 300mm Film thickness: 10 nm The composition ratio (at %) of the hard mask layer 16 (CrON film) was Cr:O:N=34.9:64.7:0.4, that is, the Cr content was 34.9 at %, the O content was 64.7 at %, and the N content was 0.4 at %.
[0086] [Example 4] In Example 4, an EUV mask blank was produced in the same manner as in Example 1, except that a CrON film was formed as the hard mask layer 16 under the following conditions. (Deposition conditions of hard mask layer 16 (CrON film)) Target:Cr target Sputtering gas: mixed gas of Ar, O2 and N2 (Ar: 33 vol%, O2: 45 vol%, N2: 22 vol%, gas pressure: 2.6 × 10 -1 Pa) Input power density per target area: 4.1W / cm 2 Deposition rate: 0.027nm / sec Distance between target and board: 300mm Film thickness: 10 nm The composition ratio (at %) of the hard mask layer 16 (CrON film) was Cr:O:N=36.5:62.3:1.2, that is, the Cr content was 36.5 at %, the O content was 62.3 at %, and the N content was 1.2 at %.
[0087] [Example 5] In Example 5, an EUV mask blank was produced in the same manner as in Example 1, except that a CrN film was formed as the hard mask layer 16 under the following conditions. (Deposition conditions of hard mask layer 16 (CrN film)) Target:Cr target Sputtering gas: N2 gas (Ar: 50 vol%, N2: 50 vol%, gas pressure: 2.6 × 10 -1 Pa) Input power density per target area: 9.9W / cm 2 Deposition rate: 0.053nm / sec Distance between target and board: 150mm Film thickness: 10 nm The composition ratio (at %) of the hard mask layer 16 (CrN film) was Cr:O:N=49.4:3.0:47.6, that is, the Cr content was 49.4 at %, the O content was 3.0 at %, and the N content was 47.6 at %. The hard mask layer 16 (CrN film) contains O, and it is believed that oxygen was mixed in due to residual moisture in the chamber or degassing from the components during the deposition of the CrN film.
[0088] [Example 6] In Example 6, an EUV mask blank was produced in the same manner as in Example 1, except that a CrN film was formed as the hard mask layer 16 under the following conditions. (Deposition conditions of hard mask layer 16 (CrN film)) Target:Cr target Sputtering gas: N2 gas (N2: 100 vol%, gas pressure: 8.7 x 10 -1 Pa) Input power density per target area: 9.9W / cm 2 Deposition speed: 0.045nm / sec Distance between target and board: 150mm Film thickness: 10 nm The composition ratio (at %) of the hard mask layer 16 (CrN film) was Cr:O:N=49.6:9.6:40.8, that is, the Cr content was 49.6 at %, the O content was 9.6 at %, and the N content was 40.8 at %. The hard mask layer 16 (CrN film) contains O, and it is believed that oxygen was mixed in due to residual moisture in the chamber or degassing from the components during the deposition of the CrN film.
[0089] [Example 7] In Example 7, an EUV mask blank was produced in the same manner as in Example 1, except that a CrCN film was formed as the hard mask layer 16 under the following conditions. (Deposition conditions of hard mask layer 16 (CrCN film)) Target: Two-target sputtering with Cr and C targets Sputtering gas: Ar and N2 mixed gas (Ar: 78.5 vol%, N2: 21.5 vol%, gas pressure: 2.6 × 10 -1 Pa) Input power density per Cr target area: 9.9W / cm 2 C Power density per target area: 12.3 W / cm 2 Deposition speed: 0.130nm / sec Distance between target and board: 150mm Film thickness: 10 nm The composition ratio (at%) of the hard mask layer 16 (CrCN film) was Cr:C:O:N=50.2:19.1:3.6:27.1, that is, the Cr content was 50.2 at%, the C content was 19.1 at%, the O content was 3.6 at%, and the N content was 27.1 at%. The hard mask layer 16 (CrCN film) contains O, and it is believed that oxygen was mixed in due to residual moisture in the chamber or degassing from the components during the deposition of the CrN film.
[0090] [Example 8] In Example 8, an EUV mask blank was produced in the same manner as in Example 1, except that a CrCN film was formed as the hard mask layer 16 under the following conditions. (Deposition conditions of hard mask layer 16 (CrCN film)) Target: Two-target sputtering with Cr and C targets Sputtering gas: N2 gas (N2: 100 vol%, gas pressure: 2.6 × 10-1 Pa) Input power density per Cr target area: 9.9W / cm 2 Input power density per target area: 2.0W / cm 2 Deposition rate: 0.110nm / sec Distance between target and board: 150mm Film thickness: 10 nm The composition ratio (at%) of the hard mask layer 16 (CrCN film) was Cr:C:O:N=36.9:25.2:0.2:37.7, that is, the Cr content was 36.9 at%, the C content was 25.2 at%, the O content was 0.2 at%, and the N content was 37.7 at%. The hard mask layer 16 (CrCN film) contains O, and it is believed that oxygen was mixed in due to residual moisture in the chamber or degassing from the components during the deposition of the CrN film.
[0091] [Example 9] In Example 9, an EUV mask blank was produced in the same manner as in Example 1, except that a CrCON film was formed as the hard mask layer 16 under the following conditions. (Deposition conditions of hard mask layer 16 (CrCON film)) Target: Two-target sputtering with Cr and C targets Sputtering gas: mixed gas of Ar, O2 and N2 (Ar: 59 vol%, O2: 1 vol%, N2: 40 vol%, gas pressure: 2.6 × 10 -1 Pa) Input power density per Cr target area: 9.9W / cm 2 C Power density per target area: 4.9W / cm 2 Deposition speed: 0.130nm / sec Distance between target and board: 150mm Film thickness: 10 nm The composition ratio (at%) of the hard mask layer 16 (CrCON film) was Cr:C:O:N=40.9:9.5:15.9:33.7, that is, the Cr content was 40.9 at%, the C content was 9.5 at%, the O content was 15.9 at%, and the N content was 33.7 at%.
[0092] [Example 10] In Example 10, an EUV mask blank was produced in the same manner as in Example 1, except that a CrO film was formed as the hard mask layer 16 under the following conditions. (Deposition conditions of hard mask layer 16 (CrO film)) Target:Cr target Sputtering gas: Ar and O2 mixed gas (Ar: 10 vol%, O2: 90 vol%, gas pressure: 2.6 × 10 -1 Pa) Input power density per target area: 6.5W / cm 2 Deposition rate: 0.038nm / sec Distance between target and board: 300mm Film thickness: 10 nm The composition ratio (at %) of the hard mask layer 16 (CrO film) was Cr:O=33.5:66.5, that is, the Cr content was 33.5 at % and the O content was 66.5 at %.
[0093] [Table 1]
[0094] Fig. 8 shows the relationship between the oxygen content in the film composition of the hard mask layer and the relative etching rate for Examples 1 to 10. In Fig. 8, Examples 4, 6, and 8 to 10 are indicated as Examples by △, and Examples 1 to 3, 5, and 7 are indicated as Comparative Examples by □. As is clear from the figure, no significant correlation was found between the oxygen content in the film composition of the hard mask layer and the relative etching rate.
[0095] Fig. 9 shows the relationship between the film density of the hard mask layer and the relative etching rate for Examples 1 to 10. In Fig. 9, Examples 4, 6, and 8 to 10 are indicated as Examples by △, and Examples 1 to 3, 5, and 7 are indicated as Comparative Examples by □. As is clear from the figure, a good correlation was observed between the film density of the hard mask layer and the relative etching rate.
[0096] As can be seen from Table 1, the film density of the hard mask layer is 3.00 to 5.40 g / cm 3 In Examples 4, 6, and 8 to 10, the durability of the Ru protective layer was very good, being A, and the selectivity with respect to the absorption layer, i.e., the etching selectivity, was also very good or good, being A or B. 3 In Examples 1, 2, 5, and 7, the durability of the Ru protective layer was poor, being C. 3 In Example 3, in which the thickness was less than C, the durability of the Ru protective layer was poor, and the etching selectivity was also poor, being C.
[0097] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2019-095189) filed on May 21, 2019, the contents of which are incorporated herein by reference. [Explanation of symbols]
[0098] 1: EUV mask blank 11: Substrate 12: Reflective layer (multilayer reflective film) 13:Protective layer 14: Absorption layer 15:Low reflective layer 16: Hard mask layer 20: Resist film
Claims
1. A reflective mask blank for EUV lithography, comprising: a reflective layer that reflects EUV light; a protective layer for the reflective layer; an absorbing layer that absorbs EUV light; and a hard mask layer, which are formed in this order on a substrate, The protective layer contains ruthenium (Ru), the absorbing layer contains tantalum (Ta); the hard mask layer contains chromium (Cr) and at least one of nitrogen (N) and oxygen (O); The film density of the hard mask layer is 3.00 to 5.40 g / cm 3 A reflective mask blank for EUV lithography.
2. A reflective mask blank for EUV lithography, comprising: a reflective layer that reflects EUV light; a protective layer for the reflective layer; an absorption layer that absorbs EUV light; a low-reflection layer for light having a wavelength of 190 to 260 nm that is an inspection light for a mask pattern; and a hard mask layer, which are formed in this order on a substrate; The protective layer contains ruthenium (Ru), the absorbing layer comprises tantalum (Ta); the low reflective layer contains tantalum (Ta) and oxygen (O); the hard mask layer contains chromium (Cr) and at least one of nitrogen (N) and oxygen (O); The film density of the hard mask layer is 3.00 to 5.40 g / cm 3 A reflective mask blank for EUV lithography.
3. 3. The reflective mask blank for EUV lithography according to claim 1, wherein the hard mask layer further contains at least one of carbon (C) and boron (B).
4. 4. The reflective mask blank for EUV lithography according to claim 1, wherein the hard mask layer has a thickness of 2 to 30 nm.
Citation Information
Patent Citations
Method of manufacturing amorphous carbon film used in semiconductor device and method of manufacturing the semiconductor device
JP2012212706A
Reflective mask blank, reflective mask and reflective mask manufacturing method
JP2013084910A
Metal doping of amorphous carbon and silicon film used as hard mask by substrate processing system
JP2016166405A
Reflective mask blank, reflective mask and method for manufacturing reflective mask
JP2017062521A
Development of high etch selectivity hard mask material by ion implantation into amorphous carbon film
JP2017507477A
Cited By
Blankmask and photomask for extreme ultraviolet lithography including hard mask film containing chromium and niobium
JP2026082626A