Inorganic coating composition and method for manufacturing the same

The inorganic coating composition with alkali metal silicate, silica, and metal nitrate hydrate, combined with a specialized milling process, addresses transparency and durability issues in conventional compositions, ensuring high transparency and resistance to interference fringes.

JP2024148102AInactive Publication Date: 2024-10-17WAKO CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023061033
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional inorganic paint compositions using alkali metal silicates as binders suffer from reduced transparency due to non-transparent curing catalysts, which also compromise durability and water resistance, and thick films risk interference fringes.

Method used

An inorganic coating composition comprising alkali metal silicate, silica, metal nitrate hydrate, and a filler, combined with a specific ball milling process using a nylon mill body and zirconia balls, to enhance transparency and prevent interference fringes while maintaining durability and water resistance.

Benefits of technology

The composition achieves high transparency, durability, and water resistance, with no interference fringes, even at thicker film thicknesses, through improved particle size and mixing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148102000001
    Figure 2024148102000001
  • Figure 2024148102000002
    Figure 2024148102000002
  • Figure 2024148102000003
    Figure 2024148102000003
Patent Text Reader

Abstract

To provide an inorganic coating composition which improves transparency of a coating film and achieves sufficient performances, such as durability, weather resistance, and water resistance, and by which it is possible to prevent occurrence of interference fringes of the coating film.SOLUTION: An inorganic coating composition of the invention includes alkali metal silicate, silica, a metal nitrate hydrate, a filler, and water. The metal nitrate hydrate includes either aluminum nitrate, magnesium nitrate, calcium nitrate, barium nitrate, or lithium nitrate. The filler includes either synthesized bentonite, stevensite, or hectorite.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an inorganic coating composition for forming a transparent coating film to be applied to the surfaces of solar panels of a photovoltaic power generation system, mirrors, etc., and a method for preparing the same. [Background technology]

[0002] As conventional inorganic coating compositions, various inorganic coating compositions using alkali metal silicate as a binder have been proposed, such as a mixture of alkali metal silicate, silica, borate, finely divided titanium oxide, and flaky silica. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-15728 A Summary of the Invention [Problem to be solved by the invention]

[0004] Many of the curing catalyst components, such as scaly silica and fine titanium oxide, contained in conventional inorganic coating compositions are not colorless and transparent, and the transparency of the coating is reduced, so it was necessary to limit their amount. If the amount of curing catalyst, scaly silica, fine titanium oxide, etc. added is reduced, the durability and water resistance of the coating film may decrease. In addition, if the thickness of the coating film is reduced to maintain transparency, interference fringes (rainbows) may occur in the coating film.

[0005] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an inorganic coating composition which can improve the transparency of a coating film, sufficiently obtain performance such as durability, weather resistance, and water resistance, and prevent the occurrence of interference fringes in the coating film, and a method for preparing the same. [Means for solving the problem]

[0006] The inorganic coating composition according to claim 1 comprises an alkali metal silicate, silica, a metal nitrate hydrate, a filler, and water.

[0007] According to the above-mentioned configuration, the transparency of the coating film can be improved, and the performance such as durability, weather resistance, water resistance, etc. can be sufficiently obtained. In addition, it is possible to provide an inorganic coating composition that can prevent the occurrence of interference fringes on the coating film while maintaining the transparency of the coating film at a sufficiently high level. Therefore, since the decrease in the transparency of the coating film can be suppressed, the transparency of the coating film can be maintained at a sufficiently high level even if the coating film is formed thick so that the thickness is such that interference fringes are not generated.

[0008] In the method for preparing an inorganic coating composition according to claim 4, a ball mill equipped with a nylon mill body and zirconia balls is used to pulverize and mix an inorganic coating composition comprising an alkali metal silicate, silica, a metal nitrate hydrate, a filler, and water for 8 hours or more. This method for preparing an inorganic coating composition can make the particle size of the coating finer, thereby improving the transparency of the coating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described in detail.

[0010] (Embodiment) The inorganic coating composition according to the embodiment includes an alkali metal silicate, silica, a metal nitrate hydrate, a filler, and water.

[0011] The alkali metal silicate includes a silicate of an alkali metal. The alkali metal silicate includes, for example, lithium silicate, sodium silicate, or potassium silicate, or a mixture of two or more selected from these. The silica includes, for example, spherical silica (silicon dioxide, SiO2) of 12 to 15 nanometers. This silica has excellent dispersibility and high transparency due to its nanometer size.

[0012] Metal nitrate hydrates are easily soluble in water, have high dispersibility, and are highly transparent. Examples of metal nitrate hydrates include aluminum nitrate, magnesium nitrate, calcium nitrate, barium nitrate, and lithium nitrate, or a mixture of two or more selected from these.

[0013] The filler includes, for example, synthetic bentonite, stevensite, or hectorite, or a mixture of two or more selected from these, which have high dispersibility in water and high transparency.

[0014] Next, the mixing ratio of each component of the inorganic coating composition according to the embodiment will be described with reference to Table 1 below. As shown in Table 1, the mixing ratio of each component relative to 100 parts by weight of alkali metal silicate is set as follows. The mixing ratio of metal nitrate hydrate is set in the range of 0.1 to 10 parts by weight. The mixing ratio of filler is set in the range of 0.1 to 10 parts by weight. The mixing ratio of water is set to be 10 parts by weight. The mixing ratio of silica is set so that the total mixing ratio of silica, metal nitrate hydrate, filler, and water is 100 parts by weight.

[0015] [Table 1]

[0016] The inorganic coating composition according to the embodiment and the coating film formed therefrom have the following effects.

[0017] The inorganic coating composition according to the embodiment has the effect of improving the transparency of the coating, since the metal nitrate hydrate and the filler are added in the mixing ratio shown in Table 1. Furthermore, the inorganic coating composition according to the embodiment has the effect of being able to sufficiently increase the curing power of the coating film, and is able to sufficiently maintain the durability and water resistance of the coating film.

[0018] Next, the results of comparative experiments on coatings made from inorganic coating compositions that were actually created are shown below.

[0019] As the inorganic coating composition according to the embodiment, two types of inorganic coating compositions with different mixing ratios of each component were prepared. Each of these was applied to a plate glass and dried to obtain Example 1 and Example 2. For comparison, two types of inorganic coating compositions with different mixing ratios of each component were prepared as a conventional inorganic coating composition. Each of these was applied to a plate glass and dried to obtain Comparative Example 1 and Comparative Example 2. Table 2 shows the mixing ratios of each component in Example 1 and Example 2. Table 3 shows the mixing ratios of each component in Comparative Example 1 and Comparative Example 2.

[0020] [Table 2]

[0021] [Table 3]

[0022] The inorganic coating compositions according to Examples 1 and 2 were prepared as follows. In the preparation of the inorganic coating compositions according to Examples 1 and 2, the inorganic materials having the respective mixing ratios shown in Table 2 were placed in a cylindrical nylon mill body with zirconia balls inside, and the mill body was attached to a rotating machine. Next, the rotating machine was started, and the inorganic materials in the mill body were pulverized and mixed by rotating the mill body. The time for pulverizing and mixing the inorganic materials can be 8 hours or more. In Examples 1 and 2, the time for pulverizing and mixing the inorganic materials was 8 hours. The inorganic coating compositions according to Examples 1 and 2 were prepared by the above steps. Next, the inorganic coating compositions of Examples 1 and 2 were spray-coated on a plate glass, and dried with hot air at 220 to 250 ° C. for about 50 minutes to obtain a coating film with a thickness of about 10 μm. The coating film thickness of 10 μm is a sufficiently thick film thickness to improve the performance of the coating film, such as durability, weather resistance, and water resistance.

[0023] The inorganic coating compositions according to Comparative Example 1 and Comparative Example 2 were prepared as follows. In preparing the inorganic coating compositions according to Comparative Example 1 and Comparative Example 2, the inorganic materials having the respective mixing ratios shown in Table 3 were placed in a cylindrical magnetic mill body with alumina balls placed inside, and the mill body was attached to a rotating machine. Next, the rotating machine was started, and the inorganic materials in the mill body were pulverized and mixed by rotating the mill body. The time for pulverizing and mixing the inorganic materials was about 30 minutes to 1 hour. In Comparative Example 1 and Comparative Example 2, the time for pulverizing and mixing was set to 1 hour. The inorganic coating compositions according to Comparative Example 1 and Comparative Example 2 were prepared by the above process. Next, the inorganic coating compositions of Comparative Example 1 and Comparative Example 2 were spray-coated on a plate glass, and dried with hot air at 220 to 250 ° C. for about 50 minutes to obtain a coating film having a thickness of about 10 μm.

[0024] Next, the ultraviolet transmittance, visible light transmittance, and solar radiation transmittance were measured for the glass plates coated with the inorganic coating compositions of Examples 1 and 2, and the inorganic coating compositions of Comparative Examples 1 and 2.

[0025] The conditions for measuring the ultraviolet transmittance are as follows. Test method: The ultraviolet ray transmittance was calculated according to JIS S 3107:2013 Automotive Window Film 6.5 Ultraviolet ray transmittance test 6.5.3 test method. Test equipment: Shimadzu Corporation UV / Vis / NIR spectrophotometer SolidSpec-3700 Wavelength range: 300~380nm

[0026] The conditions for measuring the visible light transmittance are as follows: Test method: Visible light transmittance was determined according to JIS S 3107:2013 Automotive Window Film 6.5 Ultraviolet Ray Transmittance Test 6.5.3 Test Method. Test equipment: Shimadzu Corporation UV / Vis / NIR spectrophotometer SolidSpec-3700 Wavelength range: 380~780nm

[0027] The conditions for measuring the solar transmittance are as follows. Test method: The solar transmittance was calculated according to JIS R 3106:2019 Test methods for transmittance, reflectance, and emissivity of flat glass, and calculation method for solar heat gain coefficient of architectural flat glass No.8 Calculation method for solar transmittance, solar reflectance, and solar absorptance. Test equipment: Shimadzu Corporation UV / Vis / NIR spectrophotometer SolidSpec-3700 Wavelength range: 300~2500nm

[0028] These measurements were carried out at the East Branch of the Japan Paint Inspection Association. The measurement results are shown in Table 4. An unpainted glass plate was used as the reference.

[0029] [Table 4]

[0030] According to Table 4, the plate glasses of Examples 1 and 2 to which the inorganic coating composition according to the embodiment was applied had higher transparency than the plate glasses of Comparative Examples 1 and 2. Furthermore, for the plate glasses of Examples 1 and 2, no interference fringes were observed even when a coating film of the inorganic coating composition was formed to a thickness of 10 μm.

[0031] The inorganic coating composition according to the comparative example comprises an alkali metal silicate, silica, a borate as a curing agent, fine titanium oxide, and scaly silica, and water. In contrast, the inorganic coating composition according to the embodiment comprises an alkali metal silicate, silica, a metal nitrate hydrate, a filler, and water. Thus, the inorganic coating composition according to the embodiment has a different composition from the comparative example, and comprises a metal nitrate hydrate and a filler, so that the transparency of the coating film is improved and sufficient performance such as durability, weather resistance, and water resistance can be obtained. In addition, even if the coating film is formed thick enough to prevent interference fringes from occurring, the transparency of the coating film can be maintained at a sufficiently high level.

[0032] The inorganic coating composition for comparison was ground and mixed using a ball mill that combines alumina balls and a magnetic mill body. When the inorganic coating composition is ground and mixed using this ball mill, it may be slightly colored due to the white color of the alumina balls, and the transparency of the coating film may decrease. Since the coloring increases when the grinding and mixing processing time is set to a long time, the grinding and mixing processing time is limited to about 30 minutes to 1 hour.

[0033] In contrast, the inorganic coating composition according to the embodiment was ground and mixed using a ball mill that combines zirconia balls and a nylon mill body. The zirconia balls are stronger than the alumina balls because they are fired at a higher temperature, and the inorganic coating composition is not colored by the ball mill. In addition, the nylon mill body is less hard than the magnetic mill body, so the zirconia balls are prevented from being scraped by the mill body during the ball milling and mixing. Therefore, the transparency of the inorganic coating composition can be improved by using a ball mill that combines a nylon mill body and zirconia balls.

[0034] In addition, in a ball mill using a combination of a nylon mill body and zirconia balls, the inorganic coating composition is not colored, so the grinding and mixing time can be set long. With the inorganic coating composition according to the embodiment, the grinding and mixing process can be performed for 8 hours or more. This makes it possible to create an inorganic coating composition with a smaller particle size, so that the transparency of the coating film can be further improved. Furthermore, even if the coating film is formed to a thickness of 10 μm so that interference fringes are not generated, the transparency of the coating film can be maintained at a sufficiently high level.

[0035] In addition, in the method for preparing an inorganic coating composition according to the embodiment, grinding and mixing are carried out using a ball mill that combines a mill body made of nylon, which has a low specific gravity, with zirconia balls, which have a high specific gravity, so that the efficiency of grinding and mixing can be improved.

[0036] Next, the measurement results of the average particle size and transparency of the inorganic coating composition will be described. Table 5 shows the transmittance (R) and transmittance (B) of the plate glass of Example 2 and the plate glass of Comparative Example 2, and the average particle size of the inorganic coating composition. The transmittance (R) is the transmittance of red light having a wavelength of about 640 to 770 nm. The transmittance (B) is the transmittance of blue light having a wavelength of about 430 to 490 nm.

[0037] [Table 5]

[0038] According to Table 5, it is shown that the transparency of the plate glass of Example 2 is higher than that of the plate glass of Comparative Example 2. It is also shown that the average particle size of the inorganic coating composition of Example 2 is smaller than that of the inorganic coating composition of Comparative Example 2. Therefore, it is shown that the particle size of the inorganic coating composition can be made finer according to the method for preparing the inorganic coating composition of the embodiment. It is also shown that the transparency of the coating film can be improved by making the particle size of the inorganic coating composition finer.

[0039] Further, a durability test was conducted on the plate glasses of Examples 1 and 2. The durability test was conducted by a boiling test. The plate glasses of Examples 1 and 2 were immersed in boiling water and kept boiling for 2 hours while being heated. After 2 hours, the plate glasses were taken out and the water was removed, and changes in the coating state such as discoloration, stains, corrosion, surface deterioration, peeling of the coating were observed. As a result of the boiling test, no changes in the coating state were observed on the plate glasses of Examples 1 and 2. This test showed that the coating films of Examples 1 and 2 had sufficient performance such as durability, weather resistance, and water resistance.

[0040] As described above, according to the inorganic coating composition and the method for preparing the inorganic coating composition according to the embodiment, it is possible to provide an inorganic coating composition that can improve the transparency of the coating film and retains properties such as durability, weather resistance, and water resistance.

[0041] Although a preferred embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the spirit of the present invention, and it goes without saying that these modifications are also included within the scope of the present invention.

Claims

1. An alkali metal silicate; Silica and a metal nitrate hydrate; A filler; Water, The inorganic coating composition comprises:

2. 2. The inorganic coating composition according to claim 1, wherein the metal nitrate hydrate comprises any one of aluminum nitrate, magnesium nitrate, calcium nitrate, barium nitrate, and lithium nitrate.

3. 2. The inorganic coating composition of claim 1, wherein the filler comprises one of synthetic bentonite, stevensite, or hectorite.

4. The inorganic coating composition according to claim 1, wherein the alkali metal silicate is 100 parts by weight, the metal nitrate hydrate is 0.1 to 10 parts by weight, the filler is 0.1 to 10 parts by weight, and the water is 10 parts by weight, and the mixing ratio of the silica is set so that the total mixing ratio of the silica, the metal nitrate hydrate, the filler, and the water is 100 parts by weight.

5. A method for preparing an inorganic coating composition, comprising treating an inorganic coating composition comprising an alkali metal silicate, silica, a metal nitrate hydrate, a filler, and water for 8 hours or more using a ball mill equipped with a nylon mill body and zirconia balls.

Citation Information

Patent Citations

  • JP1975054621A

  • Stabilizing silica and method of manufacturing same

    JP1987502257A

  • Inorganic coating composition

    JP1994329949A

  • Inorganic coating composition

    JP1994329950A

  • Refractory composition

    JP1998081557A