Formation method of coating and member with coating formed
By forming a vanadium carbide layer on press molds using a chromium-containing carbon steel material and subsequent nitriding, the method addresses wear and adhesion issues, resulting in a durable film with high hardness and toughness.
Patent Information
- Application Number
- JP2023082471
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional vanadium carbide coatings on press molds fail to provide sufficient wear resistance and adhesion under high surface pressures, leading to peeling and cracking during pressing.
A method involving immersion of a chromium-containing carbon steel material in a molten salt bath to form a vanadium carbide layer, followed by nitriding treatment to create a nitride layer, enhancing hardness and adhesion resistance.
The resulting film exhibits high hardness, excellent adhesion resistance, and toughness, effectively preventing peeling and cracking under high loads, making it suitable for press molds.
Smart Images

Figure 2024165893000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming a coating and a member having a coating formed thereon. [Background technology]
[0002] The molding surface of a die used in press molding (hereinafter referred to as "press die") comes into contact with the workpiece under high load and slides against it when the workpiece is molded, and so wear occurs with repeated use. Therefore, in order to prolong the life of press dies, it is common to form a highly wear-resistant coating on the molding surface.
[0003] An example of a coating formed on the molding surface of a conventional press die is a coating layer made of vanadium carbide formed by immersing a carbon tool steel workpiece in a treatment bath in which vanadium chloride is added and diffused into molten borax (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Unexamined Patent Publication No. 49-118637 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in recent years, with the increasing strength of the workpiece, there is an increasing demand for higher surface pressure during pressing, and the load on the die is becoming even higher. According to the study by the present inventors, in the case of a coating layer made of vanadium carbide as in Patent Document 1, the wear resistance under high surface pressure is insufficient, and when the coating layer and the workpiece slide against each other during pressing, adhesion occurs on the surface of the coating layer, and the surface pressure at the adhesion part becomes even higher, which may cause the coating layer to peel off.
[0006] The present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to provide a method for forming a coating that has high hardness, excellent adhesion resistance, and excellent toughness, and a member formed with such a coating. [Means for solving the problem]
[0007] The method for forming a coating of the present invention is characterized by comprising the following steps (a) and (b). (a) a step of immersing a substrate made of a carbon steel material containing chromium in a molten salt bath containing vanadium to form a carbide layer containing vanadium carbide as a main component and containing at least one of iron and chromium on the substrate; (b) subjecting the carbide layer to a nitriding treatment. The step of carrying out the nitriding treatment is a step of forming a nitride layer on the carbide layer, the nitride layer containing a nitride formed by reaction of at least one of iron, chromium, and vanadium in the carbide layer with nitrogen.
[0008] An example of more detailed features of the coating forming method of the present invention includes the following (1). (1) The chromium-containing carbon steel material contains 75 wt% to 95 wt% of iron and 3 wt% to 20 wt% of chromium.
[0009] The member of the present invention is characterized in that it comprises a substrate made of a carbon steel material containing chromium, a carbide layer mainly composed of vanadium carbide formed on the substrate, and a nitride layer containing at least one nitride of iron, chromium, and vanadium formed on the carbide layer, the nitride layer having a thickness of 10 nm or more and 400 nm or less.
[0010] More detailed examples of the features of the member of the present invention include the following (2) to (8). (2) The thickness of the carbide layer is not less than 1 μm and not more than 20 μm. (3) The nitride layer contains iron at 5 at % to 30 at %. (4) The nitride layer contains chromium at 5 at % to 30 at %. (5) The nitride layer contains 10 at % to 60 at % of vanadium. (6) The nitride layer has an amount of at least one nitride of iron, chromium, and vanadium that gradually decreases toward the carbide layer. (7) The nitride layer has a gradually increasing amount of vanadium carbide approaching the carbide layer. (8) The member is a press die. Effect of the Invention
[0011] According to the present invention, it is possible to provide a method for forming a coating that has high hardness, excellent adhesion resistance, and excellent toughness, and a member having the coating formed thereon. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic diagram for explaining the formation of a film according to one embodiment of the present invention. [Diagram 2] Fig. 2(a) is a schematic diagram showing an example of the step (a) of forming a carbide layer according to one embodiment of the present invention, and Fig. 2(b) is a schematic diagram showing the process of forming a carbide layer. [Diagram 3] FIG. 3 is a photograph showing a vertical cross section of the coating of the member according to Example 1. [Figure 4] FIG. 4 is a graph showing the results of a component analysis of the surface layer of the member according to Example 1. [Diagram 5] FIG. 5 is a graph showing the dynamic friction coefficients of the surfaces of the members according to Example 1, Comparative Example 1, and Comparative Example 2. [Figure 6] FIG. 6(a) is a photograph showing the coating surface of the member of Example 1 after the friction and wear test, and FIG. 6(b) is a photograph showing the coating surface of the member of Comparative Example 2 after the friction and wear test. [Figure 7] FIG. 7(a) is a photograph showing the surface of the member according to Example 1 after the press test, and FIG. 7(b) is a photograph showing the surface of the member according to Comparative Example 2 after the press test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Method of forming the film] Hereinafter, one embodiment of the method for forming a coating according to the present invention will be described with reference to the drawings. Fig. 1 is a schematic diagram for explaining the formation of a coating according to the following embodiment. Fig. 2(a) is a schematic diagram showing an example of the step (a) of forming a carbide layer, and Fig. 2(b) is a schematic diagram showing the process of forming the carbide layer.
[0014] First, as shown in FIG. 1, in step (a) of the method for forming a coating according to the present embodiment, a carbide layer 3 is formed on a substrate 2 made of a carbon steel material containing chromium by a salt bath method. The salt bath method is a method for forming a coating of metal carbide on a surface of a steel material by immersing the steel material in a molten salt bath containing borax (Na2B4O7) that has been heated to a molten state and then cooling the steel material. Specifically, as shown in FIG. 2(a), a substrate 2 made of a carbon steel material containing chromium is immersed in a molten salt bath 6 containing vanadium in a bath 5 that has been preheated using a heating element 7, and then cooled to form a carbide layer 3 containing vanadium carbide as a main component on the surface of the substrate 2. In this specification, the main component refers to the component having the highest mass ratio among all components. Next, the process of forming vanadium carbide on a substrate 2 made of a carbon steel material containing chromium will be described in more detail with reference to FIG. 2(b). As an example of the molten salt bath 6 in Fig. 2(b), an example will be described in which vanadium pentoxide (VO5) is used as the vanadium compound for forming carbide, metallic aluminum (Al) is added as the reducing agent, and a borax-containing molten salt bath heated to 1000°C is used. In this molten salt bath 6, both vanadium pentoxide and metallic aluminum exist in a molten state, and fine metallic vanadium (V) particles are precipitated in the molten salt bath 6 by the reduction reaction of metallic aluminum, as represented by the following formula (1). 3V2O5+10Al→6V+5Al2O3(1) When the substrate 2 made of carbon steel containing chromium is immersed in the molten salt bath 6 in which such a reaction proceeds, some of the fine metallic vanadium particles generated by the above formula (1) come into physical contact with and adhere to the surface of the substrate 2. Thereafter, the fine metallic vanadium particles adhered to the surface of the substrate 2 preferentially bond with the carbon (C) contained in the carbon steel substrate 2 as shown in the following formula (2), forming vanadium carbide (VC) on the surface of the substrate 2, which covers the surface of the substrate 2 as a coating (also described as a "VC coating"). Metallic V particles in molten salt bath + C in substrate → vanadium carbide (VC) (2) Furthermore, when the base material 2 made of carbon steel containing chromium is treated by the above-mentioned salt bath method, the formed carbide layer 3 contains vanadium carbide as the main component, as well as very small amounts of iron (Fe) and chromium (Cr) originating from the carbon steel. The carbide layer 3 may further contain a small amount of metallic vanadium (V).
[0015] The carbide layer 3 formed in the step (a) contains vanadium carbide as a main component and therefore has high hardness.
[0016] The molten salt bath 6 is not limited to the above-mentioned example, and the components can be changed as appropriate. For example, the reducing agent used in the molten salt bath 6 may be boron carbide (B4C) instead of metallic aluminum.
[0017] The conditions used in the salt bath method can be appropriately set, and for example, the method can be performed under the conditions that the substrate 2 is immersed in a molten salt bath 6 heated to about 1000° C. for 8 hours or more, and then the substrate 2 is taken out and cooled. The type of the heating element 7 used to heat the bath 5 containing the molten salt bath 6 is not particularly limited, and any known type can be used.
[0018] The substrate 2 made of a carbon steel material containing chromium can be a carbon steel material containing any amount of iron and chromium, preferably a carbon steel material containing 75 wt% to 95 wt% iron and 3 wt% to 20 wt% chromium. When the carbide layer 3 is formed by the above method using a carbon steel material satisfying such a composition range, the carbide layer 3 can contain iron and chromium in an amount suitable for forming a nitride layer having a thickness of 10 nm to 400 nm, which will be described later. Examples of the substrate 2 made of a carbon steel material containing chromium include SKD11, SKD61, SKH51, and SUS440.
[0019] Next, as shown in FIG. 1, in step (b), the carbide layer 3 formed on the substrate 2 is subjected to a nitriding treatment to form a nitride layer 4 on the upper part of the carbide layer 3 as a coating containing at least one of iron nitride, chromium nitride, and vanadium nitride. The formation of the nitride layer 4 may utilize iron and chromium contained in the carbide layer 3. In this way, the iron and chromium contained in the carbide layer 3 are consumed by the formation of the nitride layer 4, and as a result, the purity of vanadium carbide in the carbide layer 3 is increased, and the toughness of the carbide layer 3 is improved. Specifically, the nitriding treatment is a treatment in which the substrate 2 having the carbide layer 3 is heated, and then a gas containing nitrogen as a component is brought into contact with the surface of the carbide layer 3 to bond the iron, chromium, and vanadium contained in the carbide layer 3 with the nitrogen to generate nitrides, and thus the nitride layer 4 having a thickness of 10 nm to 400 nm is formed on the carbide layer 3.
[0020] The nitriding treatment in step (b) can be carried out by, for example, ion nitriding, preferably radical nitriding, or gas nitriding, but is not limited thereto.
[0021] Ion nitriding is a nitriding method in which a nitride layer is formed on the surface of a workpiece by using glow discharge in a reduced pressure nitriding atmosphere. In this embodiment, the conditions used in ion nitriding are not particularly limited and can be set appropriately. Radical nitriding is a type of ion nitriding, in which the workpiece is kept at a temperature of 300°C to 650°C, and ammonia (NH3) gas and hydrogen (H2) gas are used to apply a current of 0.001 mA / cm to the surface of the workpiece. 2 ~2.0mA / cm 2 In this embodiment, the conditions used in the radical nitriding are not particularly limited and can be set appropriately.
[0022] Gas nitriding is a method of nitriding a material to be treated by holding the material in a heated state in a nitrogen-based gas atmosphere. In the present embodiment, the conditions used in gas nitriding are not particularly limited and can be set appropriately.
[0023] In this specification, the nitride layer refers to a layer containing a nitride as a main component. The nitride layer 4 contains at least one nitride of iron, chromium, and vanadium, i.e., at least one of iron nitride, chromium nitride, and vanadium nitride, and preferably contains these nitrides as a main component.
[0024] Examples of the iron nitride contained in the nitride layer 4 include commonly known iron nitrides such as diiron mononitride (Fe2N) and tetrairon mononitride (Fe4N).
[0025] Examples of the chromium nitride contained in the nitride layer 4 include commonly known chromium nitrides such as chromium mononitride (CrN) and nichrome nitride (Cr2N).
[0026] The vanadium nitride contained in the nitride layer 4 may be a commonly known vanadium nitride such as vanadium nitride (VN).
[0027] The nitride layer 4 may contain unavoidable components that are mixed in during the formation process, and may also contain an altered layer (not shown) that contains the unavoidable components to the extent that the performance is not affected. The unavoidable components contained in the altered layer are not particularly limited, and examples thereof include compounds containing oxygen (O) or carbon (C).
[0028] The nitride layer 4 contains a nitride formed by reaction of nitrogen with at least one of iron, chromium, and vanadium, and therefore has the properties of high hardness and low dynamic friction coefficient. In particular, the nitride layer 4 formed by the above method is formed with a very thin film thickness on the carbide layer 3, which can suppress wear when high surface pressure is applied to the coating, and can suppress peeling and lateral cracks of the coating caused by adhesion. Preferably, the film thickness of the nitride layer 4 is 1 / 100 or less of the film thickness of the carbide layer 3.
[0029] The nitride layer 4 has a higher hardness than the carbide layer 3, which in turn has a higher hardness than the substrate 2 made of chromium-containing carbon steel. In this way, a hardness gradient is formed from the substrate 2 toward the nitride layer 4, which makes it possible to improve the durability of the coating and suppress peeling and lateral cracking of the coating.
[0030] The coating consisting of the carbide layer 3 and the nitride layer 4 formed on the substrate 2 by the above steps (a) and (b) has high hardness, excellent adhesion resistance, and excellent toughness. Therefore, the member 1 having the coating formed on the substrate 2 by the method according to this embodiment is suitable as a press die that is subjected to a high load during use.
[0031] [Part] An embodiment of the member 1 having a coating according to the present invention will be described below.
[0032] As shown in FIG. 1, a member 1 according to this embodiment has a substrate 2 made of a chromium-containing carbon steel material, a carbide layer 3 provided on the substrate 2 as a coating containing vanadium carbide as a main component, and a nitride layer 4 provided on the carbide layer 3 as a coating containing at least one nitride of iron, chromium, and vanadium.
[0033] The substrate 2 used in the member 1 can be the same as that described above in the coating formation method.
[0034] The carbide layer 3 of the member 1 can be formed in the same manner as described above in the coating formation method. The thickness of the carbide layer 3 is not particularly limited as long as it is larger than the thickness of the nitride layer 4, and can be appropriately changed to an extent that does not affect the performance of the carbide layer 3, but is preferably 1 μm to 20 μm, and more preferably 3 μm to 15 μm.
[0035] The nitride layer 4 of the member 1 can be formed in the same manner as described above in the method of forming the film. The film thickness of the nitride layer 4 is preferably 10 nm to 400 nm, more preferably 15 nm to 200 nm. From the viewpoint of increasing the hardness of the nitride layer 4 and ensuring the wear resistance and durability, the lower limit is preferably 10 nm. From the viewpoint of ensuring the impact resistance of the nitride layer 4, the upper limit is preferably 400 nm. The nitride layer 4 is not particularly limited as long as it contains nitride as the main component, but preferably contains 5 at% to 30 at% of iron, 5 at% to 30 at% of chromium, or 10 at% to 60 at% of vanadium. When the content of each component contained in the nitride layer 4 satisfies the above range, the hardness of the nitride layer 4 is increased and excellent adhesion resistance is easily obtained. In addition, it is preferable that the amount of at least one nitride of iron, chromium, and vanadium gradually decreases toward the carbide layer 3 in the nitride layer 4. Furthermore, it is preferable that the amount of vanadium carbide in the nitride layer 4 gradually increases toward the carbide layer 3. By gradually increasing the amount of vanadium carbide toward the carbide layer 3, adhesion to the underlying carbide layer 3 is improved, and the hardness gradient between the nitride layer 4 and the carbide layer 3 becomes gentle, making it possible to suppress peeling and lateral cracking of the film consisting of the carbide layer 3 and the nitride layer 4.
[0036] Although there is no limitation on the use of the member 1, it is preferable that the member 1 is used as a die, particularly a press die. The member 1 of the present embodiment has excellent wear resistance and adhesion resistance, and is therefore suitable as a press die that is subjected to a high load during use.
[0037] The manufacturing method of the member 1 can be, for example, by applying the above-mentioned coating formation method, in which the carbide layer 3 is first formed on the base material 2 made of a carbon steel material containing chromium, and then the outermost surface of the carbide layer 3 is subjected to a nitriding treatment to form the nitride layer 4. However, the method is not limited to this. EXAMPLES
[0038] Examples and comparative examples to which the present invention is applied will be described below. However, these examples are merely illustrative of the present invention and do not limit the scope of the invention.
[0039] Example 1 SKD11 was prepared as a substrate, and immersed in a molten salt bath of anhydrous borax with vanadium pentoxide and metallic aluminum added and heated to 1000°C for about 8 hours. After that, SKD11 was removed from the molten salt bath and cooled, and a process of forming a carbide layer on the surface of SKD11 was carried out. Next, a radical nitriding process was carried out on the carbide layer of SKD11 at a gas temperature of 490°C, using ammonia gas (NH3) for a treatment time of 6 hours, and a process of forming a nitride layer on the outermost surface of the carbide layer was carried out. The member of Example 1 was produced by these processes.
[0040] Comparative Example 1 SKD11 was prepared as a base material and used as a component.
[0041] Comparative Example 2 A member was produced in the same manner as in Example 1, except that the nitriding treatment was not carried out.
[0042] The produced members were evaluated by the following methods and conditions.
[0043] [Micrograph of longitudinal section] The member of Example 1 was cut so that the longitudinal cross section was visible, and a photograph of the longitudinal cross section of the member of Example 1 was taken using a scanning electron microscope SU8020 (Hitachi High-Technologies Corporation).
[0044] [XPS] The components of the surface layer of the member of Example 1 were analyzed by X-ray photoelectron spectroscopy (XPS) using a Quantera SXM (ULVAC-PHI, Inc.).
[0045] [hardness] The hardness H of the members of Example 1 and Comparative Example 2 was measured using a nanoindenter (Elionix Co., Ltd.) with an indentation load of 50 mN and a load holding time of 5 seconds. IT After measuring the Vickers hardness H V was converted to.
[0046] [Average friction coefficient] Using an abrasion friction tester (Shinto Scientific Co., Ltd.), the average friction coefficients of the surfaces of the members of Example 1 and Comparative Examples 1 and 2 were measured by a ball-on-disk test with a load of 100 gf, a rotation speed of 100 rpm, and a mating material of JSC1180Y.
[0047] [Kinematic friction coefficient] Edge test pieces and flat test pieces simulating dies were prepared, and the workpiece (JSC1180Y) was sandwiched between them, and the pressing force was set to 16 kN or 18 kN and the speed was set to 200 mm / min, and the workpiece was pulled out 100 mm. The dynamic friction coefficients of the surfaces of the members of Example 1 and Comparative Examples 1 and 2 were measured using an autograph (Shimadzu Corporation). In addition, photographs of the coating surfaces of the members of Example 1 and Comparative Example 2 after the test were taken.
[0048] [Toughness] A nanoindenter (Elionix Co., Ltd.) was used to create a load-displacement diagram during the indentation process with an indenter load of 50 mN, and the plastic deformability (toughness) of the coatings of the members of Example 1 and Comparative Example 2 was calculated from the load-displacement diagram.
[0049] [Press Test] Using a digital electric servo press (maximum load 1500 kN) (Amada Press System Co., Ltd.), a press test was performed on the components of Example 1 and Comparative Example 2 with a pressure of 100 kN, and photographs were taken of the coating surfaces of the components of Example 1 and Comparative Example 2 after the press test.
[0050] As described above, members were prepared by the methods of Example 1 and Comparative Examples 1 and 2, and each evaluation test was performed. The following Table 1 is a table summarizing the evaluation results of the Vickers hardness of the members of Example 1 and Comparative Examples 1 and 2, and the average friction coefficient of the members of Example 1 and Comparative Examples 1 and 2. Table 2 is a table summarizing the evaluation results of the toughness of the coating of the members of Example 1 and Comparative Example 2, in which "coating surface" represents the vicinity of the outermost surface of the carbide layer, "coating center" represents the vicinity of the center of the carbide layer, and "coating-substrate interface" represents the vicinity of the interface between the carbide layer and the substrate. FIG. 3 is a photograph showing the longitudinal section of the member of Example 1, and the length of the size bar at the lower right of the photograph is 5 μm. FIG. 4 is a graph showing the results of the component analysis by XPS of the member of Example 1, in which the horizontal axis represents the sputtering depth (nm) (SiO2 equivalent) and the vertical axis represents the atomic concentration (at%). Fig. 5 is a bar graph summarizing the evaluation results of the dynamic friction coefficient of the surfaces of the members of Example 1 and Comparative Examples 1 and 2, with the horizontal axis representing the pressing force (kN) and the vertical axis representing the average dynamic friction coefficient. Fig. 6(a) is a photograph showing the coating surface after the above test was performed on the member of Example 1, and Fig. 6(b) is a photograph showing the coating surface after the above test was performed on the member of Comparative Example 2. Fig. 7(a) is a photograph showing the coating surface after the press test was performed on the member of Example 1, and Fig. 7(b) is a photograph showing the coating surface after the press test was performed on the member of Comparative Example 2.
[0051] [Table 1]
[0052] [Table 2]
[0053] As can be seen from Fig. 3, in the member of Example 1, a coating consisting of a carbide layer 3 and a nitride layer 4 was formed on the substrate 2. It was also confirmed that the thickness of the carbide layer 3 was approximately 7.3 µm. On the other hand, in Comparative Example 1, the substrate 2 was used as is, and therefore neither the carbide layer 3 nor the nitride layer 4 was formed. In Comparative Example 2, a coating consisting only of the carbide layer 3 was formed on the substrate 2.
[0054] As can be seen from FIG. 4, the nitride layer of the member of Example 1 contains 14 at% iron (Fe), 8 at% chromium (Cr), and 33 at% nitrogen (N). It is believed that the iron and chromium are in a state of being combined with nitrogen, and it is estimated that they are contained in the nitride layer as iron nitride and chromium nitride, respectively. Furthermore, the nitride layer of the member of Example 1 contains 34 at% vanadium (V), and it is estimated that a part of the vanadium is contained in the nitride layer as vanadium nitride in which the vanadium is combined with nitrogen. Also, from the result of FIG. 4, it was confirmed that the nitride layer exists from the outermost layer to a depth of 25 nm in the coating of the member of Example 1. In addition, as can be seen from FIG. 4, the carbide layer of the member of Example 1 contains 54 at% vanadium (V) and 42 at% carbon (C). It is believed that this vanadium is in a state of being combined with carbon, and it is estimated that vanadium carbide is contained as the main component.
[0055] As can be seen from Table 1, the surface hardness of the member of Example 1 is greater than the surface hardness of the members of Comparative Example 1 and Comparative Example 2. In addition, the average friction coefficient of the surface of the member of Example 1 is lower than the average friction coefficient of the surface of the members of Comparative Example 1 and Comparative Example 2. From these results, it was confirmed that the member of Example 1 has a higher hardness and better adhesion resistance than the members of Comparative Examples 1 and 2.
[0056] As can be seen from FIG. 5, the average dynamic friction coefficient when the pressing force is 16 kN is the lowest in the member of Example 1, and is comparable in the members of Comparative Examples 1 and 2. In addition, the average dynamic friction coefficient when the pressing force is 18 kN is the lowest in the member of Example 1, followed by the member of Comparative Example 2, and the highest in the member of Comparative Example 1. Thus, the low dynamic friction coefficient on the surface of the member of Example 1 is considered to be due to the presence of a nitride layer with a very thin film thickness. The lower the dynamic friction coefficient, the less adhesion of the mating material can be caused when a high surface pressure is applied to the member, making it suitable as a coating for press dies. In fact, as can be seen from FIG. 6(a), almost no adhesion is observed in the coating after the above test in the member of Example 1. On the other hand, as can be seen from FIG. 6(b), many adhesions are observed in the coating after the above test in the member of Comparative Example 2. From the above results, it was confirmed that the member of Example 1 has a lower dynamic friction coefficient on the surface than the members of Comparative Examples 1 and 2, and has good adhesion resistance.
[0057] As can be seen from Table 2, the toughness of the coating of Example 1 is higher than that of the coating of Comparative Example 2. In particular, it was confirmed that the coating of Example 1 has good toughness at all depth positions ("coating surface", "coating center", and "coating-substrate interface"). Also, FIG. 7(a) shows a photograph of the coating of Example 1 after 500 press tests, and almost no noticeable damage such as scratches is observed. On the other hand, FIG. 7(b) shows a photograph of the coating of Comparative Example 2 after 200 press tests, and it was confirmed that the coating peeled off and many transverse cracks occurred at the 100th to 200th press tests. From these results, it was confirmed that the coating of Example 1 has good toughness compared to the coating of Comparative Example 2.
[0058] From the above results, it was confirmed that a coating having high hardness, excellent adhesion resistance, and excellent toughness can be formed on a substrate made of a chromium-containing carbon steel material by the method of Example 1. It was also confirmed that the method of Example 1 can provide a member having a coating made of a carbide layer and a nitride layer on a substrate made of a chromium-containing carbon steel material. [Industrial Applicability]
[0059] INDUSTRIAL APPLICABILITY The present invention can provide a method for forming a coating that has high hardness, excellent adhesion resistance, and excellent toughness, and a member formed with the coating, and thus can be widely used in industrial fields such as automobiles. [Explanation of symbols]
[0060] 1. Materials 2 Base material 3 Carbide layer 4. Nitride layer 5. Bathtub 6 Molten Salt Bath 7 Heating element
Claims
1. A process for forming a carbide layer containing vanadium carbide as a main component and containing at least one of iron and chromium on a substrate made of a carbon steel material containing chromium by immersing the substrate in a molten salt bath containing vanadium; and subjecting the carbide layer to a nitriding treatment. The step of performing the nitriding treatment is a step of forming a nitride layer on the carbide layer, the nitride layer containing a nitride formed by a reaction between at least one of iron, chromium, and vanadium in the carbide layer and nitrogen. A method for forming a coating.
2. 2. The method for forming a coating according to claim 1, wherein the chromium-containing carbon steel material contains 75 wt % to 95 wt % of iron and 3 wt % to 20 wt % of chromium.
3. A substrate made of a carbon steel material containing chromium; a carbide layer mainly composed of vanadium carbide formed on the substrate; a nitride layer formed on the carbide layer, the nitride layer including at least one nitride of iron, chromium, and vanadium; The nitride layer has a thickness of 10 nm or more and 400 nm or less.
4. 4. The member according to claim 3, wherein the carbide layer has a thickness of 1 μm or more and 20 μm or less.
5. 4. The member of claim 3, wherein the nitride layer contains 5 at% to 30 at% iron.
6. 4. The member of claim 3, wherein the nitride layer contains 5 at% to 30 at% chromium.
7. 4. The member of claim 3, wherein the nitride layer contains 10 at% to 60 at% vanadium.
8. 4. The member of claim 3, wherein said nitride layer has an amount of nitride of at least one of iron, chromium, and vanadium that tapers toward said carbide layer.
9. 4. The member of claim 3, wherein said nitride layer has a gradually increasing amount of vanadium carbide approaching said carbide layer.
10. The member according to any one of claims 3 to 9, wherein the member is a press die.
Citation Information
Patent Citations
JP1974118637A