METHOD FOR FORMING METAL NITRIDE FILM

The ALD method forms films with varying etch rates on substrate features by using directional plasmas, addressing conformality and thickness control issues, enhancing film properties for semiconductor applications.

JP2024537889AActive Publication Date: 2024-10-16APPLIED MATERIALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024522216
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-18
Filing Date
2022-10-14
Publication Date
2024-10-16
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

Existing film deposition methods, such as CVD and PVD, face challenges in achieving conformality, thickness control, and composition control, leading to device defects and impractical film properties, while selective ALD processes lack practicality due to limited surface chemistry specificity.

Method used

A method involving atomic layer deposition (ALD) is used to form films with varying wet etch rates by treating horizontal and vertical surfaces with directional plasmas, allowing selective removal of films on substrates with features, including top, bottom, and sidewalls, using silicon precursors and nitrogen-containing reactants.

Benefits of technology

The method achieves conformal film deposition with controlled thickness and composition on complex structures, enabling selective removal and utilization of films for applications like gate spacers and barrier layers, improving device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537889000001_ABST
    Figure 2024537889000001_ABST
Patent Text Reader

Abstract

Embodiments of the present disclosure include a method of forming a film that includes conformally depositing a first film on a substrate, treating the first film with a first plasma to form a second film, treating the second film with a second plasma to form a third film, and selectively removing the first film, a portion of the second film, and the third film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001]

[0001] The present disclosure relates generally to methods of depositing films. In particular, the present disclosure relates to processes for selective deposition of ALD films. [Background technology]

[0002] Deposition of films onto substrates is an important process in a variety of industries, including semiconductor processing, diffusion barrier coatings, and dielectrics for magnetic read / write heads. Miniaturization, particularly in the semiconductor industry, requires atomic-level control of film deposition to produce conformal coatings on high aspect ratio structures. One method for controlled and conformal film deposition is atomic layer deposition (ALD), which uses sequential surface reactions to produce layers of the same precise thickness on all parts of a structure. Most ALD processes are based on a binary reaction sequence that deposits a binary compound film. Because the surface reactions are sequential, the two gas-phase reactants do not come into contact, and there are limited gas-phase reactions that can form and deposit particles.

[0003]

[0003] Most film properties cannot meet practical requirements due to lack of continuity, lack of conformality, poor film thickness control, and poor film composition control, such as hydrogen contamination and / or different bonding states of carbon in the film. Traditionally, films formed by chemical vapor deposition (CVD) and physical vapor deposition (PVD) processes are often non-continuous and non-conformal. In addition, CVD processes are generally more difficult to control thickness than ALD processes and may generate gas phase particles, which may result in device defects.

[0004]

[0004] Selective deposition of materials can be achieved in a variety of ways. For example, some processes may have inherent selectivity to surfaces based on their surface chemistry. Such processes are rare and are typically specific to the reactants used, the material formed, and the substrate surface. However, selective deposition processes face the same challenges of meeting practical requirements.

[0005]

[0005] Therefore, there is a need for a process for selectively depositing ALD films. Summary of the Invention

[0006]

[0006] One or more embodiments of the present disclosure are directed to a method of forming a film. The method includes conformally depositing a first film having a horizontal surface and a vertical surface on a substrate. The substrate includes at least one feature having a top surface, a bottom surface, and a sidewall. The horizontal surface of the first film is treated with a first plasma to form a second film on the horizontal surface. The second film has a lower wet etch rate than the first film after being treated with the first plasma. The second film on the horizontal surface is treated with a second plasma to form a third film on the horizontal surface. The third film has a higher wet etch rate than the second film after being treated with the second plasma. The method further includes selectively removing the first film, a portion of the second film, and the third film.

[0007]

[0007] Additional embodiments of the present disclosure are directed to a processing method including exposing a substrate to a deposition environment including at least one deposition cycle. The at least one deposition cycle includes sequentially exposing the substrate to a silicon precursor and a nitrogen-containing reactant to form a first silicon nitride film on the substrate. The substrate has at least one feature including a top surface, a bottom surface, and a sidewall. The first silicon nitride film is treated with a first directional plasma to form a second silicon nitride film. The second silicon nitride film has a lower wet etch rate than the first silicon nitride film after being treated with the first directional plasma. The second silicon nitride film is treated with a second directional plasma to form a third silicon nitride film. The third silicon nitride film has a higher wet etch rate than the second silicon nitride film after being treated with the second directional plasma. The processing method further includes removing the third silicon nitride film, a portion of the second silicon nitride film, and the first silicon nitride film.

[0008]

[0008] In order that the above-mentioned features of the present disclosure may be understood in detail, the present disclosure summarized above will now be more particularly described with reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings merely illustrate exemplary embodiments of the present disclosure, and therefore should not be considered as limiting the scope of the present disclosure, which may admit of other equally effective embodiments. [Brief description of the drawings]

[0009] [Figure 1A-D] FIG. 1 illustrates a substrate according to one or more embodiments of the present disclosure. [Figure 1E] FIG. 1 illustrates a substrate according to one or more embodiments of the present disclosure. [Diagram 2] FIG. 1 is a process flow diagram illustrating a method of forming a film according to one or more embodiments of the present disclosure. [Diagram 3] FIG. 1 is a schematic diagram illustrating a capacitively coupled plasma (CCP) chamber in accordance with one or more embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010]

[0016] Before describing several example embodiments of the present disclosure, it is to be understood that the present disclosure is not limited to the details of structure or process steps set forth in the following description as the present disclosure is capable of other embodiments and of being practiced or carried out in various ways.

[0011]

[0017] The term "substrate" as used herein and in the appended claims refers to a surface, or a portion of a surface, upon which a process acts. Additionally, unless the context clearly indicates otherwise, those skilled in the art will understand that a reference to a substrate may refer to only a portion of a substrate. Additionally, a reference to deposition on a substrate may refer to both a bare substrate and a substrate having one or more films or features deposited or formed thereon.

[0012]

[0018] As used herein, "substrate" refers to any substrate or material surface formed on a substrate on which a film treatment is performed in a manufacturing process. For example, substrate surfaces on which treatment may be performed include materials such as silicon, silicon oxide, strained silicon, silicon-on-insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials, depending on the application. Substrates include, but are not limited to, semiconductor wafers. Substrates may be exposed to pretreatment processes that polish, etch, reduce, oxidize, hydroxylate, anneal, and / or bake the substrate surface. In this disclosure, in addition to film treatments directly on the surface of the substrate itself, any of the disclosed film treatment steps may also be performed on underlying layers formed on the substrate, as disclosed in more detail below, and the term "substrate surface" is intended to include such underlying layers as the context indicates. Thus, for example, when a film / layer or partial film / layer is deposited on a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.

[0013]

[0019] The term "horizontal" as used herein is defined as a plane parallel to the surface of a plane or substrate, regardless of its orientation. In one or more embodiments, the horizontal plane extends from one side of the substrate to the other. As shown in the attached figures, the horizontal plane extends from the left side of the device (page left) to the right side of the device (page right). The term "vertical" refers to a direction perpendicular to the horizontal plane just defined. The vertical plane extends from near the substrate to a point or plane away from the substrate. As shown in the attached figures, the vertical plane extends from the top of the device (top of the page) to the substrate (bottom of the page) such that the vertical plane is parallel to the sidewall of the feature. Terms such as "above", "below", "bottom", "top", "side" (as in "sidewall"), "higher", "lower", "upper", "over", "under" and the like are defined relative to the horizontal plane as shown in the figures. Those skilled in the art will recognize that the directional descriptions are relative to the device orientation and are not limited to any particular substrate orientation.

[0014]

[0020] The term "on" indicates that there is a direct contact between the elements. The term "directly on" indicates that there is a direct contact between the elements, with no intervening elements.

[0015]

[0021] As used herein and in the appended claims, the terms "reactive gas," "precursor," "reactant," and the like are used interchangeably to refer to gases that contain species that react with the substrate surface. For example, a first "reactive gas" may simply adsorb onto the surface of the substrate and be available for further chemical reaction with a second reactive gas.

[0016]

[0022] The term "about" as used herein means approximately or approximately, and in the context of a stated numerical value or range, means a variation of no more than ±15% of the numerical value. For example, values ​​that vary by ±14%, ±10%, ±5%, ±2%, or ±1% would meet the definition of about.

[0017]

[0023] The method described herein uses an atomic layer deposition (ALD) process. As used herein, "atomic layer deposition" or "cyclic deposition" refers to the sequential exposure of a substrate surface to two or more reactive compounds to deposit layers of material. The substrate or a portion of the substrate is separately exposed to two or more reactive compounds that are introduced into a reaction zone of a processing chamber. In a time-domain ALD process, exposure to each reactive compound is separated by a time delay to allow each compound to adhere to and / or react with the substrate surface and then be purged from the processing chamber. These reactive compounds are said to be sequentially exposed to the substrate. In a spatial ALD process, different portions of the substrate surface, or materials on the substrate surface, are exposed to two or more reactive compounds simultaneously, such that any point on the substrate is not substantially exposed to more than one reactive compound at the same time. As used herein and in the appended claims, the term "substantially" as used in this respect means that, as will be understood by those skilled in the art, a small portion of the substrate may be exposed to more than one reactive gas at the same time due to diffusion, and simultaneous exposure is not intended.

[0018]

[0024] In one aspect of a time-domain ALD process, a first reactive gas (i.e., a first precursor or compound A) is pulsed into the reaction zone following a first time delay. Then, a second precursor or compound B is pulsed into the reaction zone, followed by a second delay. During each time delay, a purge gas, such as argon, is introduced into the process chamber to purge the reaction zone or remove any residual reactive compounds or reaction by-products from the reaction zone. Alternatively, the purge gas can flow continuously throughout the deposition process, with the purge gas only flowing during the time delay between pulses of reactive compounds. The reactive compounds are pulsed alternately until a desired film or film thickness is formed on the substrate surface. In either scenario, the ALD process of pulsing compound A, purge gas, compound B, purge gas is one cycle. The cycle can start with either compound A or compound B and continue in the respective order of the cycle until a film of the desired thickness is obtained.

[0019]

[0025] In an embodiment of a spatial ALD process, a first reactive gas and a second reactive gas (e.g., nitrogen gas) are simultaneously supplied to a reaction zone but separated by an inert gas curtain and / or a vacuum curtain. By moving the substrate relative to the gas supply, any point on the substrate is exposed to the first reactive gas and the second reactive gas.

[0020]

[0026] Some embodiments of the present disclosure are directed to selective deposition methods that allow for different film properties based on deposition location on a 3D structure. For example, films deposited on the top and bottom of a structure can be treated to have different film properties than films deposited on the sidewalls of the structure. Some embodiments of the present disclosure advantageously provide a method of forming a film in which a first film and a third film can be selectively removed by wet etching while leaving other portions (e.g., at least a portion of a second film) intact.

[0021]

[0027] 1A-1E, a substrate 102 is shown at the stage of selective deposition of a film. FIG. 1A shows a substrate 102 including at least one feature 100 having a top surface 110, a bottom surface 130, and a sidewall 120. For illustrative purposes, the substrate 102 is shown with a single feature 100, but one of ordinary skill in the art will appreciate that there may be multiple features. The feature 102 may be any suitable shape, including, but not limited to, a trench, a cylindrical via that transfers current between membranes when filled with, for example, a metal, and an electrode that transfers energy within the same membrane. As used herein, the term "feature" refers to any intentional surface irregularity. The feature may have any suitable aspect ratio (ratio of the depth of the feature to the width of the feature). In some embodiments, the aspect ratio is about 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, or 40:1 or more.

[0022]

[0028] FIG. 1B shows a first film 140 having horizontal and vertical surfaces conformally deposited on a substrate 102. As used herein, the terms “conformal” or “conformally” refer to a film that adheres to and uniformly covers an exposed surface with a thickness that varies less than 1% relative to the average thickness of the film. For example, a 1000 Å thick film would have a thickness variation of less than 10 Å. This thickness and variation includes at least the edges, corners, sides, and bottom of a feature. For example, a conformal film deposited by ALD in various embodiments of the present disclosure will provide coverage over the deposition area of ​​essentially uniform thickness on a complex surface. In one or more embodiments, the conformally deposited first film 140 has a thickness in the range of 20 Å to 100 Å. In one or more embodiments, the conformally deposited first film 140 has a thickness in the range of 30 Å to 80 Å.

[0023]

[0029] Some embodiments of the present disclosure are directed to the wet etch rate of the film, among other film properties. Without intending to be bound by theory, the wet etch rate of the film can be determined based on the particular chemical process and the amount of time the film is in the etching solution. In one or more embodiments, the first film 140 is exposed to air such that a thin layer of native oxide forms on the first film 140. In one or more embodiments, the first film 140 in a dilute HF 100:1 etching solution has a high wet etch rate. In one or more embodiments, the wet etch rate of the first film 140 on the top surface 110 and the bottom surface 130 is at least twice as high as the wet etch rate of the first film 140 on the sidewalls 120. In one or more embodiments, the wet etch rate of the first film 140 on the top surface 110 and the bottom surface 130 in a dilute HF 100:1 etching solution ranges from 5 Å / min to 50 Å / min.

[0024]

[0030] 1C illustrates the treatment of the first film 140 formed in FIG. 1B to form a second film 150. In one or more embodiments, the horizontal surface (or top surface) 152 of the first film 140 is treated with a first plasma 160 having a high ion concentration to form a second film 150 on the top surface 110 and bottom surface 130 of the feature 100. In one or more embodiments, the plasma having a high ion concentration is about 10 10 / cm 3 In one or more embodiments, the plasma having a high ion density has an ion density of about 10 9 / cm 3 , 10 11 / cm 3 , 10 12 / cm 3 , 10 13 / cm 3 , or 10 14 / cm 3 The plasma used in the treatment may be any suitable plasma (e.g., direct or remote) capable of modifying the film properties.

[0025]

[0031] In one or more embodiments, the first plasma 160 is a directional plasma. As used herein and in the appended claims, the term "directional plasma" means that the energetic species (ions and radicals) present in the plasma move in a specific direction. For example, in FIG. 1C, the first plasma 160 is shown moving downward, which allows the energetic species to contact the first film 140 on the top surface 110 and the bottom surface 130, but minimizes contact with the film 140 on the sidewall 120. In other words, the first plasma 160 does not substantially affect the film 140 on the sidewall 120.

[0026]

[0032] The directional plasma can be formed in many other ways. In one or more embodiments, the horizontal surface of the first film 140 is exposed to at least one RF frequency. In one or more embodiments, the horizontal surface of the first film 140 is exposed to a first RF frequency in the range of 13.56 MHz to 60 MHz to generate the directional plasma, and a second RF frequency in the range of 350 kHz to 13.56 MHz to adjust the energy and directionality of the first plasma 160. The directional plasma can be formed as a remote plasma, where the plasma species are excited remotely from the substrate surface and flow toward the substrate surface. The substrate may not be part of the electrical path used to generate the plasma. The directional plasma can also be formed as a direct plasma, where the substrate or substrate support serves as an electrode for plasma formation. The remote plasma is generally a diffusion plasma, and can be made directional by applying a bias to the substrate such that ions are attracted to the substrate and move toward the substrate. In one or more embodiments, the directional plasma includes one or more of hydrogen, argon, nitrogen, ammonia, oxygen, and helium. In one or more embodiments, the directional plasma is a capacitively coupled plasma.

[0027]

[0033] The amount of time used for processing can affect the amount of damage caused to the film at the top and bottom of the feature. The plasma species and power can affect the depth of damage caused to the film. Processing processes that cause deeper damage to the film can be repeated less times than processing processes that cause shallower damage to the film. For example, a He / NH3 plasma causes deeper damage than an Ar / NH3 plasma, so a thicker film can be deposited before being treated with a He / NH3 plasma.

[0028]

[0034] In some embodiments, the first film 140 is exposed to the first plasma 160 for a time ranging from 0.5 seconds to 5 seconds as part of a conformal deposition step of an ALD cycle. In other embodiments, the first film 140 is exposed to the first plasma 160 for a time ranging from 1 second to 10 seconds after a predetermined number of ALD cycles. In other embodiments, the first film 140 is exposed to the first plasma 160 for a time ranging from 1 second to 10 seconds after a predetermined thickness of the first film 140 is deposited. In further embodiments, the first film 140 is exposed to the first plasma 160 as part of a post-treatment process. In further embodiments, the post-treatment process includes exposing the first film 140 to the first plasma 160 for a time ranging from 2 seconds to 60 seconds.

[0029]

[0035] In one or more embodiments, the second film 150 is formed on horizontal surfaces on the top surface 110 and on horizontal surfaces on the bottom surface 130. In one or more embodiments, the second film 150 has a lower wet etch rate than the first film 140. In one or more embodiments, the wet etch rate of the second film 150 in a dilute HF 100:1 etching solution ranges from 2 Å / min to 5 Å / min. In one or more embodiments, the wet etch rate of the second film 150 in a dilute HF 100:1 etching solution ranges from 2 Å / min to 3 Å / min.

[0030]

[0036] FIG. 1D illustrates the treatment of the second film 150 formed in FIG. 1C to form a third film 170. In one or more embodiments, the horizontal surface 172 of the second film 150 is treated with a second plasma 165 to form a third film 170 on the top surface 110. In FIG. 1D, the second film 150 is on the bottom surface 130. In one or more embodiments, the first plasma 160 and the second plasma 165 are the same. In FIG. 1D, the second plasma 165 is shown moving downward, which allows energetic species to contact the second film 150 on the top surface 110 and the bottom surface 130, but minimizes contact with the first film 140 on the sidewalls 120. In other words, the second plasma 165 does not substantially affect the film 140 on the sidewalls 120.

[0031]

[0037] In one or more embodiments, the third film 170 has a higher wet etch rate than the second film 150. In some embodiments, the wet etch rate of the third film 170 on the top surface 110 increases at a faster rate than the wet etch rate of the second film 150 on the bottom surface 130 during processing of the second film 150. In one or more embodiments, the third film 170 in a dilute HF 100:1 etching solution has a wet etch rate in the range of 10 Å / min to 15 Å / min or greater.

[0032]

[0038] 1E illustrates selective removal of first film 140 from vertical surfaces and sidewalls 120 of feature 100, portions of second film 150, and third film 170. In one or more embodiments, first film 140 and third film 170 are selectively removed by etching with dilute hydrofluoric acid (HF). In one or more embodiments, second film 150 has a thickness in the range of 20 Å to 60 Å after selective removal of portions of second film 150. The thickness of second film 150 after selective removal is less than the thickness of second film 150 formed in FIG. 1C.

[0033]

[0039] 1E, the remaining portion of the second film 150 may be used for front-end-of-the-line (FEOL) dielectric applications such as gate spacers, etc. In one or more embodiments, the remaining portion of the second film 150 is used as a barrier layer.

[0034]

[0040] 1B-1E show selectively deposited ALD films. In one or more embodiments, the first film 140, the second film 150, and the third film 170 independently comprise one or more of a metal nitride, silicon nitride (SiN), silicon oxynitride (SiON), and silicon oxycarbonitride (SiOCN).

[0035]

[0041] Formation of each of the first film 140, second film 150, and third film 170 may be performed by any suitable method, including, but not limited to, atomic layer deposition (ALD), plasma enhanced atomic layer deposition (PEALD), chemical vapor deposition (CVD), and plasma enhanced chemical vapor deposition (PECVD). In some embodiments, each of the first film 140, second film 150, and third film 170 is formed by an ALD process in which the substrate 102 is sequentially exposed to a metal-containing precursor and a nitrogen reactant. In one or more embodiments, the first film 140, second film 150, and third film 170 each comprise silicon nitride (SiN). In some embodiments, a silicon-containing precursor and a nitrogen reactant are used to form a film comprising silicon nitride (SiN). As used in this regard, a "silicon precursor" reacts with the surface of the substrate, thereby leaving silicon molecules on the substrate 102. As used in this regard, a "nitrogen reactant" reacts with silicon molecules on the substrate 102.

[0036]

[0042] Although the following embodiments of the present disclosure are described with respect to the deposition of silicon nitride (SiN) films, those skilled in the art will understand that the present disclosure is not so limited. Other films, such as films including metal nitrides, silicon oxynitride (SiON), and silicon oxycarbonitride (SiOCN), can be deposited, treated, and etched.

[0037]

[0043] In some embodiments, silicon nitride (SiN) films are formed on the substrate 102 with exposure to a nitrogen precursor between exposure to the silicon precursor and exposure to the nitrogen reactant. A "nitrogen precursor" as used in this regard is one that reacts with the substrate surface and only minimally reacts with silicon species already present on the substrate 102. Stated differently, the nitrogen precursor includes species that do not react with silicon precursor molecules on the substrate 102. The exposure to the nitrogen precursor can occur before, during, or after exposure to the silicon precursor, since both the nitrogen precursor species and the silicon precursor species are reactive with the substrate 102 and only minimally reactive with each other.

[0038]

[0044] Suitable silicon precursors include, but are not limited to, silane, disilane, dichlorosilane (DCS), bis(diethylamino)silane (BDEAS), tetrakis(dimethylamino)silane (TDMAS), and / or bis(t-butylamino)silane (BTBAS). In some embodiments, the silicon precursor comprises dichlorosilane. In one or more embodiments, the silicon precursor consists essentially of dichlorosilane, meaning that there is less than 1% of silicon species other than dichlorosilane on an atomic basis.

[0039]

[0045] Suitable nitrogen precursors include, but are not limited to, molecular nitrogen and ammonia. The process conditions employed during the exposure of the nitrogen precursor can affect the reactivity of the nitrogen species with the silicon species on the surface. In some embodiments, the process conditions are configured such that the nitrogen precursor reacts substantially only with the substrate surface. As used in this respect, the term "substantially only with" means that the nitrogen precursor reacts with less than about 10% of the silicon species on the surface.

[0040]

[0046] The nitrogen reactant is a species that forms a metal nitride film on the substrate 102. In some embodiments, the nitrogen reactant provides nitrogen atoms for the formation of a metal nitride film (e.g., SiN). In one or more embodiments, the nitrogen reactant does not include a nitrogen-containing species and forms a nitride film by promoting a reaction between surface species. Suitable nitrogen reactants include, but are not limited to, nitrogen plasma, ammonia plasma, plasma including a mixture of two or more of hydrogen, nitrogen, ammonia, helium, argon, or oxygen. In some embodiments, the nitrogen reactant includes an argon and ammonia plasma, an argon and nitrogen plasma, an argon and oxygen plasma, or a helium and ammonia plasma. In some embodiments, the nitrogen reactant includes a nitrogen-free plasma that reacts with nitrogen species on the surface. In some embodiments, the nitrogen reactant includes a hydrogen and argon plasma, or a hydrogen and nitrogen plasma, or a hydrogen and helium plasma, or a hydrogen and ammonia plasma, or a hydrogen and oxygen plasma.

[0041]

[0047] In some embodiments, forming a silicon nitride (SiN) film includes sequentially exposing a substrate surface to a silicon precursor comprising dichlorosilane, a nitrogen precursor comprising ammonia, and a nitrogen reactant comprising a N2 / Ar plasma or a H2 / Ar plasma.

[0042]

[0048] FIG. 2 is a process flow diagram illustrating a method of forming a film. FIG. 2 illustrates a method of forming any of the embodiments of the film shown in FIG. 1A-FIG. 1E. In some embodiments, the method includes two processes: film deposition and plasma treatment. The method described herein can be repeated to form a film of a desired thickness. Each step of the film formation process can be repeated in sequence to form a film for treatment. The conformally deposited film can then be treated and the process repeated.

[0043]

[0049] Some embodiments of the present disclosure are advantageously carried out in a single processing chamber. In some embodiments, the selective deposition includes two processes in a single processing chamber: film deposition and plasma treatment. These two processes constitute a single ALD cycle. The metal precursor and nitrogen reactant form a conformally deposited metal nitride film, and the plasma treatment modifies the film on the top and bottom of the feature. The plasma treatment process forms N-H or metal-oxide bonds on the film surface and may penetrate the film to a depth based on the treatment time and plasma power. This has been found to result in higher wet etch rates at the top surface 110 and bottom surface 130 of the feature 100. The deposition film thickness and plasma treatment level can be adjusted to increase the wet etch rate selectivity. The selective deposition in some embodiments is carried out at a substrate temperature ranging from about 200° C. to about 550° C.

[0044]

[0050] 2, the method 200 includes, at step 210, conformally depositing a first film on a substrate. The substrate comprises at least one feature having a top surface, a bottom surface, and a sidewall. The first film has a horizontal surface and a vertical surface. In one or more embodiments, conformally depositing the first film includes exposing the substrate to a metal-containing precursor and a nitrogen reactant. In one or more embodiments, conformally depositing the first film includes exposing the substrate to a silicon-containing precursor and a nitrogen reactant.

[0045]

[0051] In step 220, the method 200 includes treating a horizontal surface of the first film with a first plasma to form a second film on the horizontal surface. In one or more embodiments, treating the horizontal surface of the first film includes exposing the film to at least one RF frequency. In one or more embodiments, treating the first film includes exposing the film to a first RF frequency in a range from 13.56 MHz to 60 MHz to generate a directional plasma and exposing the film to a second RF frequency in a range from 350 kHz to 13.56 MHz to adjust the energy and directionality of the directional plasma.

[0046]

[0052] In some embodiments, the first film is exposed to the first plasma for a time ranging from 0.5 seconds to 5 seconds as part of the conformal deposition step of a single ALD cycle. In other embodiments, the first film is exposed to the first plasma for a time ranging from 1 second to 10 seconds after performing a predetermined number of ALD cycles. In other embodiments, the first film is exposed to the first plasma for a time ranging from 1 second to 10 seconds after a predetermined thickness of the first film is deposited. In further embodiments, the first film is exposed to the first plasma as part of a post-treatment process. In further embodiments, the post-treatment process includes exposing the first film 140 to the first plasma 160 for a time ranging from 2 seconds to 60 seconds.

[0047]

[0053] In step 230, the method 200 includes treating the second film on the horizontal surface with a second plasma to form a third film on the horizontal surface. In one or more embodiments, the third film has a higher wet etch rate than the second film. In step 240, the method 200 includes selectively removing the first film, a portion of the second film, and the third film. In one or more embodiments, removing the third film and the first film includes etching with dilute hydrofluoric acid (HF). In one or more embodiments, the second film has a thickness in the range of 20 Å to 60 Å after selective removal.

[0048]

[0054] An embodiment of the present disclosure provides a processing method for forming a silicon nitride film. The processing method may be used to form any of the embodiments of the film shown in Figures 1A-1E. The processing method may be carried out under the same or similar process conditions as the method described above with reference to Figure 2, unless otherwise indicated. In one or more embodiments, the processing method includes exposing a substrate to a deposition environment including at least one deposition cycle. In one or more embodiments, the deposition cycle includes sequentially exposing the substrate to a silicon precursor and a nitrogen-containing reactant to form a first silicon nitride film on the substrate. The substrate has at least one feature including a top surface, a bottom surface, and a sidewall. The processing method includes treating the first silicon nitride film with a first directional plasma to form a second silicon nitride film, and treating the second silicon nitride film with a second directional plasma to form a third silicon nitride film. The processing method further includes removing the third silicon nitride film, a portion of the second silicon nitride film, and the first silicon nitride film. An embodiment of the present disclosure provides for repeating the deposition cycle to form a first silicon nitride film having a thickness in the range of 20 Å to 100 Å.

[0049]

[0055] FIG. 3 is a schematic diagram illustrating a capacitively coupled plasma (CCP) chamber 300. The CCP chamber 300 can be used as a component of a processing chamber. The CCP chamber 300 can function to generate a plasma in the processing chamber. In one or more embodiments, the CCP chamber 300 includes a top electrode 310 and a bottom electrode 320. In one or more embodiments, the RF plasma 350 can be generated by and delivered through one or more of a first RF power source 360 ​​and a second RF power source 370. In one or more embodiments, the top electrode 310 is a showerhead. In one or more embodiments, the bottom electrode 320 is a pedestal. In one or more embodiments, a wafer 330 is provided on the bottom electrode 320. As used herein and in the appended claims, the term "provided" as used in this aspect means that the wafer 330 is placed or positioned in an environment for processing. In one or more embodiments, one or more of the films of the embodiments illustrated in FIGS. 1A-1E are deposited on the wafer 330.

[0050]

[0056] In one or more embodiments, an RF plasma 350 is formed between the first electrode 310 and the bottom electrode 320. In one or more embodiments, a sheath 340 represents the direction of electric field flow. In the embodiment shown in Figure 3, the sheath 340 represents the electric field flowing downward toward the bottom electrode 320. In one or more embodiments, the electric field flows upward toward the top electrode 310 (not shown).

[0051]

[0057] According to one or more embodiments, the substrate is subjected to processing before and / or after forming the film. This processing can be performed in a single processing chamber or in one or more separate processing chambers. In some embodiments, the substrate is transferred from the first chamber to a separate second chamber for further processing. The substrate can be transferred directly from the first chamber to the separate processing chamber, or the substrate can be transferred from the first chamber to one or more transfer chambers and then to the separate processing chamber. Thus, the processing apparatus can include multiple chambers coupled to a transfer station. This type of apparatus can be referred to as a "cluster tool" or a "cluster system", or the like.

[0052]

[0058] Generally, a cluster tool is a modular system that includes multiple chambers that perform various functions, including centering and orienting, annealing, deposition, and / or etching of the substrate. According to one or more embodiments, the cluster tool includes at least a first chamber and a central transfer chamber. The central transfer chamber may house a robot that can shuttle the substrate between the processing chambers and the load lock chambers, and between the processing chambers and the load lock chambers. The transfer chamber is typically maintained under vacuum and provides an intermediate stage for shuttle the substrate from one chamber to another and / or to the load lock chambers positioned at the front end of the cluster tool. Two well-known cluster tools that can be adapted for the present disclosure are the Centura® and Endura®, both available from Applied Materials, Inc., Santa Clara, Calif. However, the exact arrangement and combination of chambers may be varied for purposes of performing the specific steps of the processes described herein. Other processing chambers that can be used include, but are not limited to, cyclic layer deposition (CLD), atomic layer deposition (ALD), chemical vapor deposition (CVD), physical vapor deposition (PVD), etching, pre-cleaning, chemical cleaning, thermal treatments such as RTP, plasma nitridation, annealing, orientation, hydroxylation, and other substrate processes. Performing processes in chambers on a cluster tool can avoid contamination of the substrate surface with atmospheric impurities without oxidation prior to depositing a subsequent film.

[0053]

[0059] According to one or more embodiments, the substrate is continuously under vacuum or "load-lock" conditions and is not exposed to ambient air when being transferred from one chamber to the next. The transfer chamber is therefore under vacuum and is "pumped down" under vacuum pressure. An inert gas may be present in the processing chamber or the transfer chamber. In some embodiments, an inert gas is used as a purge gas to remove some or all of the reactants. According to one or more embodiments, a purge gas is injected at the exit of the deposition chamber to prevent the transfer of reactants from the deposition chamber to the transfer chamber and / or additional processing chambers. Thus, the flow of inert gas forms a curtain at the exit of the chamber.

[0054]

[0060] Substrates can be processed in a single substrate deposition chamber, where a single substrate is loaded, processed, and unloaded before another substrate is processed. Substrates can also be processed in a continuous manner, similar to a conveyor system, where multiple substrates are individually loaded into a first portion of the chamber, moved through the chamber, and unloaded from a second portion of the chamber. The geometry of the chamber and associated conveyor system can form a linear or curved path. Additionally, the processing chamber can be a carousel, where multiple substrates move about a central axis and are exposed to processes such as deposition, etching, annealing, cleaning, etc. throughout the carousel path.

[0055]

[0061] During processing, the substrate may be heated or cooled. Such heating or cooling may be accomplished by any suitable means, including, but not limited to, varying the temperature of the substrate support and flowing a heated or cooled gas over the substrate surface. In some embodiments, the substrate support includes a heater / cooler that is controllable to conductively vary the substrate temperature. In one or more embodiments, the gas employed (either reactive or inert) is heated or cooled to locally vary the substrate temperature. In some embodiments, a heater / cooler is positioned within the chamber adjacent to the substrate surface to convectively vary the substrate temperature.

[0056]

[0062] The substrate may be stationary or may be rotated during processing. The rotating substrate may be rotated continuously or in small steps. For example, the substrate may be rotated throughout the entire process or the substrate may be rotated only a small amount between exposures to different reactive or purge gases. Rotating the substrate during processing (continuously or stepwise) may result in more uniform deposition or etching, for example by minimizing the effects of local variations in gas flow profiles.

[0057]

[0063] As used throughout this specification, the terms "one embodiment," "particular embodiment," "one or more embodiments," or "embodiments" mean that a particular feature, structure, material, or characteristic described in connection with that embodiment is included in at least one embodiment of the present disclosure. Thus, the appearances of phrases such as "in one or more embodiments," "in a particular embodiment," "in one embodiment," or "in an embodiment" in various places throughout this specification do not necessarily refer to the same embodiment of the present disclosure. Furthermore, the particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0058]

[0064] Although the present disclosure has been described with reference to particular embodiments, it is to be understood that these embodiments are merely illustrative of the principles and applications of the present disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the disclosed method and apparatus without departing from the spirit and scope of the present disclosure. Thus, the present disclosure is intended to cover modifications and variations that come within the scope of the appended claims and their equivalents.

Claims

1. A method for forming a film, comprising the steps of: Conformally depositing a first film on a substrate, the substrate including at least one feature having a top surface, a bottom surface, and a sidewall, the first film having a horizontal surface and a vertical surface; treating the horizontal surface of the first film with a first plasma to form a second film on the horizontal surface, the second film having a lower wet etch rate than the first film; treating the second film on the horizontal surface with a second plasma to form a third film on the horizontal surface having a higher wet etch rate than the second film; Selectively removing the first film, a portion of the second film, and the third film; The method includes:

2. The method of claim 1 further comprising repeating the method.

3. 2. The method of claim 1 , wherein the first film, the second film, and the third film independently comprise one or more of a metal nitride, silicon nitride (SiN), silicon oxynitride (SiON), and silicon oxycarbonitride (SiOCN).

4. 10. The method of claim 1, wherein conformally depositing the first film comprises exposing the substrate to a silicon-containing precursor and a nitrogen reactant.

5. The method of claim 1 , wherein conformally depositing the first film comprises exposing the substrate to a metal-containing precursor and a nitrogen reactant.

6. 2. The method of claim 1, wherein the wet etch rate of the third film is in the range of 10 Å / min to 15 Å / min or more compared to the wet etch rate of the second film in the range of 2 Å / min to 5 Å / min.

7. The method of claim 1 , wherein the first film has a thickness in the range of 20 Å to 100 Å.

8. 10. The method of claim 1, wherein treating the first film comprises exposing the film to a first RF frequency in a range from 13.56 MHz to 60 MHz to generate a directional plasma, and exposing the film to a second RF frequency in a range from 350 kHz to 13.56 MHz to adjust the energy and directionality of the directional plasma.

9. The method of claim 8 , wherein the directional plasma comprises one or more of hydrogen, argon, nitrogen, ammonia, oxygen, and helium.

10. The method of claim 8 , wherein the directional plasma is a capacitively coupled plasma.

11. The method of claim 8 , wherein the first film is exposed to the directional plasma for a time ranging from 0.5 seconds to 60 seconds.

12. The method of claim 1 , wherein the first plasma and the second plasma are the same.

13. 2. The method of claim 1, wherein a wet etch rate of the third film on the top surface increases at a faster rate than a wet etch rate of the second film on the bottom surface during processing of the second film.

14. 10. The method of claim 1, wherein removing the third film and the first film comprises etching with dilute hydrofluoric acid (HF).

15. A processing method comprising the steps of: exposing a substrate to a deposition environment comprising at least one deposition cycle, the deposition cycle comprising sequentially exposing the substrate to a silicon precursor and a nitrogen-containing reactant to form a first silicon nitride film on the substrate, the substrate having at least one feature comprising a top surface, a bottom surface, and a sidewall; treating the first silicon nitride film with a first directional plasma to form a second silicon nitride film having a lower wet etch rate than the first silicon nitride film; treating the second silicon nitride film with a second directional plasma to form a third silicon nitride film having a higher wet etch rate than the second silicon nitride film; removing the third silicon nitride film, a portion of the second silicon nitride film, and the first silicon nitride film; The method includes:

16. 16. The method of claim 15, further comprising repeating the deposition cycle to form a first silicon nitride film having a thickness in the range of 20 Å to 100 Å.

17. 16. The method of claim 15, wherein the first directional plasma and the second directional plasma independently comprise one or more of hydrogen, argon, nitrogen, ammonia, oxygen, and helium.

18. The method of claim 17 , wherein the first directional plasma and the second directional plasma are capacitively coupled plasmas.

19. 16. The method of claim 15, wherein the first silicon nitride film is exposed to the first directional plasma for a time ranging from 0.5 seconds to 60 seconds.

20. The method of claim 15, wherein the removing comprises etching with dilute hydrofluoric acid (HF).

Citation Information

Patent Citations

  • High electron mobility transistor structure and method

    JP2013118360A

  • Method for laminating nitride film of group xiii metal or semimetal

    JP2017025412A

  • Method for selectively forming silicon nitride film on side wall or flat surface of trench

    JP2017147444A

  • Selective deposition of silicon nitride films for spacers

    JP2019511118A

  • Etching stop layer

    JP2022527468A