Cutting Tools
The cutting tool with a multilayer coating of alternating zirconium nitride and (Ti 1-x-y Al x Me y )N α layers enhances wear resistance, addressing the wear issues of existing coatings and extending tool life under high thermal and mechanical loads.
Patent Information
- Application Number
- JP2024535575
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-14
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2042-11-21
AI Technical Summary
Existing cutting tools with multilayer coatings, such as those described in Patent Document 1, are prone to wear under high thermal and mechanical loads, leading to reduced tool life.
A cutting tool with a multilayer coating comprising alternating zirconium nitride layers and further nitride layers, where each further nitride layer carries (Ti 1-x-y Al x Me y )N α, with x=0.20~0.90, y=0~0.30, and Me selected from Ta, Si, Cr, W, V, Cr, Hf, Nb, and Mo, and α=0.9 to 1.1, and the zirconium nitride layers are thicker than the further nitride layers, enhancing resistance to adhesive and abrasive wear.
The multilayer coating significantly improves the cutting tool's wear resistance, resulting in extended tool life and improved performance under high loads.
Smart Images

Figure 2024544278000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a cutting tool, comprising a tool body and a multi-layer coating, the multi-layer coating protecting the tool body from wear during cutting, the multi-layer coating comprising a plurality of zirconium nitride layers, the multi-layer coating comprising further nitride layers alternating with the zirconium nitride layers, each of the further nitride layers carrying one zirconium nitride layer, each of the further nitride layers being (Ti 1-x-y Al x Me y )N α where x=0.20 to 0.90, y=0 to 0.30, Me is one or more metal atoms selected from Ta, Si, Cr, W, V, Cr, Hf, Nb, and Mo, and α=0.9 to 1.1, and each of the zirconium nitride layers has a thickness of 35 nm to 750 nm.
[0002] Cutting tools are in frictional contact with the work piece or piece under high loads, which leads to wear of the cutting tool. It is known that applying a suitable coating to the cutting tool can improve tool life. [Background technology]
[0003] Patent Document 1 discloses a multi-layer coated cutting tool. The coating shown in Patent Document 1 is MeN / (Ti 1-x Al x )N / MeN / (Ti 1-x Al x )N / ..., where Me is Zr but may be other metal atoms.
[0004] The multi-layer coating disclosed in the patent application WO 2006 / 023636 is itself subject to wear, especially when a tip is pressed onto it under high thermal and mechanical loads. When the multi-layer coating disclosed in the patent application WO 2006 / 0236366 is worn, it naturally loses its protective effect and the tool life is shortened. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2009 / 105024Al Summary of the Invention [Problem to be solved by the invention]
[0006] It is an object of the present invention to provide a cutting tool having improved wear resistance. [Means for solving the problem]
[0007] This object is achieved by a cutting tool according to claim 1. Advantageous embodiments of the cutting tool are disclosed in the dependent claims, which can be freely combined with one another and with claim 1, the description and the drawings.
[0008] The cutting tool has a tool body and a multilayer coating, the multilayer coating protects the tool body from wear during cutting, the multilayer coating has a plurality of zirconium nitride layers, the multilayer coating has further nitride layers alternated with the zirconium nitride layers, each of the further nitride layers carrying one zirconium nitride layer, each of the further nitride layers carrying a (Ti 1-x-y Al x Me y )N αwhere x=0.20-0.90, y=0-0.30, preferably x=0.40-0.80, y=0-0.30, Me is one or more metal atoms selected from Ta, Si, Cr, W, V, Cr, Hf, Nb and Mo, respectively, α=0.9-1.1, each of the zirconium nitride layers has a thickness of 35 nm-750 nm, and at least one of the zirconium nitride layers is thicker than one of the further nitride layers carrying it. Each zirconium nitride layer improves the resistance to adhesive wear that occurs when a machined tip is pressed onto the multilayer coating. The further nitride layer carrying the thicker zirconium nitride layer makes the thicker zirconium nitride layer harder, thereby improving the resistance of the thicker zirconium nitride layer to adhesive wear and abrasive wear. Atomic composition (Ti 1-x-y Al x Me y )N α It is preferable that the combination of (x, y and α) is one of the following: (x=0.2-0.9, y=0-0.3, α=1.0), (x=0.2-0.9, y=0, α=1.0), (x=0.4-0.8, y=0-0.3, α=1.0), (x=0.4-0.8, y=0, α=1.0).
[0009] The thickness of the thicker zirconium nitride layer is preferably in one of the following ranges: 35 nm to 750 nm, 200 nm to 600 nm, 200 nm to 450 nm and 200 nm to 350 nm. The thickness of the further nitride layers carrying the thicker zirconium nitride layer is preferably in one of the ranges: 30 nm to 300 nm, 50 nm to 150 nm and 60 nm to 100 nm. Preferably, each further nitride layer has a thickness in one of these ranges.
[0010] Preferably, at least two of the further nitride layers, more preferably each of the further nitride layers, have the same atomic composition, such that x, y and α are the same in each of the further nitride layers. The same atomic composition (same x, y and α) means that the values of x, y and α may vary from one further nitride layer to another due to unavoidable variations that occur during the formation of the further nitride layers, e.g. physical vapor deposition. In other words, x, y and α may vary slightly in the further nitride layers, even though they (x, y and α) are intended to be (theoretically) the same.
[0011] According to a further embodiment of the cutting tool, the thicker zirconium nitride layer is 1.2 to 15.0 times, preferably 2.0 to 12.0 times, more preferably 3.0 to 10.0 times thicker than the further nitride layer carrying it. The wear resistance of the thicker zirconium nitride layer is further improved if the thicker zirconium nitride layer is 1.2 to 15.0 times, preferably 2.0 to 12.0 times, more preferably 3.0 to 10.0 times thicker than the further nitride layer.
[0012] The thicker zirconium nitride layer is preferably 1.2 to 15.0 times, 2.0 to 12.0 times, 3.0 to 10.0 times, 3.0 to 5.5 times, or 3.2 to 4.6 times thicker than the further nitride layer.
[0013] According to a further embodiment of the cutting tool, the cutting tool has a base layer, the base layer being made of (Ti 1-a-b Al a Me * b )N β wherein a=0.20-0.90 and b=0-0.30, preferably a=0.40-0.80 and b=0-0.30, β=0.9-1.1, and Me *are one or more metal atoms selected from Ta, Si, Cr, W, V, Cr, Hf, Nb and Mo, respectively, and the base layer carries the multilayer coating on a portion of the tool body, the base layer being thicker than any of the further nitride layers. The presence of the multilayer coating on the base layer increases the resistance to adhesive and abrasive wear and better protects the tool body against thermal loads. Preferably, the base layer has the same atomic composition as one of the further nitride layers, preferably the further nitride layer closest to the base layer, which is Me * = Me, a = x, b = y, and α = β. The preferred ranges of x, y and α disclosed for the further nitride layer apply analogously to x, y, β. Having the same atomic composition of the base layer and the further nitride layer means that, even though a (theoretical) same atomic composition is intended, a, b and β may vary for said further nitride layer due to unavoidable variations that occur during the formation of the further nitride layer, e.g. physical vapor deposition.
[0014] According to a further embodiment of the cutting tool, the base layer carries one of a number of zirconium nitride layers, whereby the base layer is better protected against adhesive wear, since the tool body carries the following layer sequence: base layer / zirconium nitride layer / further nitride layer / zirconium nitride layer / ...
[0015] According to a further embodiment of the cutting tool, the base layer has a total thickness in the range of 500 nm to 15000 nm, preferably 1000 nm to 10000 nm. When the base layer has a total thickness in said range, the abrasive wear resistance is further improved.
[0016] The total thickness of the base layer is preferably in one of the ranges of 500 nm to 15,000 nm, 1,000 nm to 10,000 nm, 2,000 nm to 4,000 nm, and 2,500 nm to 3,700 nm.
[0017] According to a further embodiment of the cutting tool, the multi-layer coating has a total thickness such that the ratio of the total thickness of the base layer to the total thickness of the multi-layer coating is in the range of from greater than 0 to 3.0, preferably from 0.5 to 1.7. When the ratio of the total thickness of the base layer to the total thickness of the multi-layer coating is in said range, the tool life is further improved.
[0018] The ratio of the total thickness of the base layer to the total thickness of the multilayer coating is preferably one of the ranges of 0 to 3.0, 0.5 to 2.0, 0.5 to 1.7, and 0.75 to 1.7.
[0019] According to a further embodiment of the cutting tool, the tool body is made of a cemented carbide. The cemented carbide has a skeletal structure formed by carbide particles, the cemented carbide has a metal alloy filling the space formed by the skeletal structure, where the metal alloy is softer than the carbide particles. The cemented carbide is a material that provides suitable properties to be used as a tool body under cutting conditions. The carbide particles can be tungsten carbide, titanium carbide and / or titanium carbonitride, whereby carbides of elements of groups IV-VI of the periodic table can additionally be present in smaller amounts. The metal alloy is usually a cobalt-, nickel- or iron-based alloy. A base alloy is understood to mean that the corresponding base element, for example cobalt, forms the main component of the base alloy. The carbide particles are preferably tungsten carbide particles.
[0020] According to a further embodiment of the cutting tool, the cemented carbide has a metal alloy in an amount of 5 weight percent to 20 weight percent in the cemented carbide, where the metal alloy is a cobalt-based alloy and the cemented carbide has carbide particles that are tungsten carbide particles. Under these composition parameters, sufficient hardness and toughness is achieved in a portion of the tool body to cut a workpiece made of a metal alloy, such as a titanium alloy or a steel alloy.
[0021] According to a further embodiment of the cutting tool, the thickness of the thicker zirconium nitride layer and the thickness of the further nitride layer carrying the thicker zirconium nitride layer together result in a bilayer thickness in the range of 65 nm to 1050 nm, preferably 125 nm to 750 nm. If the bilayer thickness is in one of these ranges, the thicker zirconium nitride layer is more resistant to adhesive and abrasive wear.
[0022] The thickness of the bilayer is preferably in one of the ranges of 65 nm to 1050 nm, 125 nm to 750 nm, and 250 nm to 560 nm.
[0023] According to a further embodiment of the cutting tool, the zirconium nitride layers each have the same thickness, which is the thickness of the thicker zirconium nitride layer, and the further nitride layers each have the same thickness, which is the thickness of the further nitride layer carrying the thicker zirconium nitride layer. This results in homogeneous wear properties of the multilayer coating. By "same thickness" is meant a thickness that, even if intended to be the same, may have variations depending on the nature of the process used to form the layers of the multilayer coating. When the layers of the multilayer coating are formed by physical vapor deposition, "same thickness" means that the individual thickness of each layer may vary by ±10%, for example, if the thickness of one of the zirconium nitride layers is 200 nm, the thickness of one of the other zirconium nitride layers is within the range of 180 nm to 220 nm, which is considered to be "same thickness" compared to the thickness of the 200 nm. The thickness variation of ±10% applies equally to the further nitride layers in physical vapor deposition.
[0024] According to a further embodiment of the cutting tool, the individual thickness of the zirconium nitride layer is 1.2 to 15 times, preferably 2.0 to 12.0 times, more preferably 3.0 to 10.0 times, even more preferably 3.0 to 5.5 times, most preferably 3.5 to 4.6 times, greater than the individual thickness of the further nitride layers. According to a further embodiment of the cutting tool, said thicker zirconium nitride layer is the top layer of the multilayer coating exposed for contact with a metal tip. Thus, the cutting tool benefits from the improved wear properties of said thicker zirconium nitride layer during its initial operation.
[0025] According to a further embodiment of the cutting tool, the multi-layer coating has a total thickness in the range of 500 nm to 15000 nm, preferably 1000 nm to 10000 nm. If the total thickness of the multi-layer coating is within said range, a good balance is obtained between saving coating material on the part of the multi-layer coating and a sufficient tool life.
[0026] According to a further embodiment of the cutting tool, the total thickness of the multi-layer coating and the total thickness of the base layer add up to a joint thickness in the range of 1000 nm to 25000 nm, preferably 2000 nm to 15000 nm. When the joint thickness is within said range, a good balance is obtained between material savings in the respective parts of the base coating and the multi-layer coating and a sufficient tool life.
[0027] According to a further embodiment of the cutting tool, each of the zirconium nitride layers and each of the further nitride layers are deposited by physical vapour deposition, which allows for a better control of the thickness of the zirconium nitride layers and the further nitride layers, and if a base layer is present, it is preferably likewise deposited by physical vapour deposition.
[0028] Further advantages of the cutting tool are explained below with reference to the drawings and the embodiments shown therein. [Brief description of the drawings]
[0029] [Figure 1] FIG. 1 is a schematic diagram of a portion of a cutting tool according to a first embodiment. [Diagram 2] FIG. 4 is a schematic diagram of a portion of a cutting tool according to a second embodiment. [Diagram 3] 11 is a micrograph of a sample according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] 1 shows a schematic diagram of a cutting tool 1 according to a first embodiment. The cutting tool 1 comprises a tool body 2 and a multilayer coating 3. The multilayer coating 3 coats the tool body 2 and thereby protects it from wear. The multilayer coating 3 comprises zirconium nitride layers 4. The multilayer coating 3 comprises further nitride layers 5 alternately stacked with the zirconium nitride layers 4, each of the further nitride layers 5 carrying one of the zirconium nitride layers 4.
[0031] The further nitride layers 5 are each 1-x-y Al x Me y )N α Here, x=0.2 to 0.9, preferably x=0.4 to 0.8, y=0 to 0.3, Me is one or more metal atoms selected from Ta, Si, Cr, W, V, Cr, Hf, Nb, and Mo, and α=0.9 to 1.1. When y=0, (Ti 1-x-y Al x Me y )N α is (Ti 1-x Al x )N α When α=1.0, (Ti 1-x-y Al x Me y )N α is (Ti 1-x-y Al x Me y )N 1.0 When y=0 and α=1.0, (Ti 1-x-y Al x Me y )N α is (Ti 1-x Al x )N 1.0 It becomes.
[0032] In the embodiment shown in FIG. 1, the further nitride layer 5 has the same atomic composition (Ti 1-x-y Al x Me y )N α That is, in each of the further nitride layers 5, x, y and α are the same. The same atomic composition (same x, y and α) means that the values of x, y and α may vary from one further nitride layer 5 to another further nitride layer 5 due to unavoidable variations that occur during the formation of the further nitride layers 5, similar to the variations in the first embodiment by physical vapor deposition. In other words, if the same alloy target is used for each of the further nitride layers 5, for example in the case of physical vapor deposition, x, y and α will vary slightly even if they are intended to be identical.
[0033] The cutting tool 1 also has a further nitride layer 5 with x, y and α in the above ranges but with a different atomic composition (Ti 1-x-y Al x Me y )N α By different atomic composition is meant that the atomic composition is deliberately intended to vary throughout the further nitride layer, for example by using different alloy targets under physical vapor deposition for the deposition of the further nitride layer 5.
[0034] 1, each zirconium nitride layer 4 is thicker than the further nitride layer 5 carrying said thicker zirconium nitride layer 4, which has been found to improve the tool life of the cutting tool 1. However, the cutting tool 1 can also be used when at least one of the zirconium nitride layers 4 is thicker than one of the further nitride layers 5 carrying said thicker zirconium nitride layer 4.
[0035] Each of the zirconium nitride layers 4 has an individual thickness d4 in the range of 35 nm to 750 nm measured in a cross section perpendicular to the top surface 6 of the multilayer coating 3, as shown in Figure 1. d4 is preferably in one of the ranges of 35 nm to 750 nm, 200 nm to 600 nm, 200 nm to 450 nm, and 200 nm to 350 nm.
[0036] Each of the further nitride layers 5 has an individual thickness d5, measured in the same manner as the individual thickness d4, in the range of 30 nm to 300 nm, preferably 50 nm to 200 nm. d5 is preferably in one of the following ranges: 30 nm to 300 nm, 50 nm to 150 nm and 60 nm to 100 nm.
[0037] The sum of all the individual thicknesses d4 and d5 is the total thickness d3 of the multilayer coating 3. The total thickness d3 of the multilayer coating 3 is in the range of 500 nm to 15000 nm, preferably 1000 nm to 10000 nm. d3 is preferably in one of the ranges of 500 nm to 15000 nm, 1000 nm to 10000 nm, 2000 nm to 4000 nm, and 2500 nm to 3700 nm.
[0038] As can be seen in FIG. 1, each individual thickness d4 is greater than each individual thickness d5. The individual thicknesses d4 may vary or be the same among the zirconium nitride layers 4. The latter is shown in FIG. 1. By "same individual thickness" it is to be understood a thickness that, even if the same thickness is intended, has a variation that depends on the nature of the process used to form the zirconium nitride layers 4. When the zirconium nitride layers 4 are formed by physical vapor deposition, "same thickness" means that the individual thicknesses of the zirconium nitride layers 4 may vary ±10% among one another.
[0039] The individual thicknesses d5 may vary between the further nitride layers 5 or may be the same. The latter is illustrated in Figure 1. "The same individual thickness" should be understood as a thickness that, even if the same thickness is intended, has a variation that depends on the nature of the process used to form the further nitride layers 5. In the case where the further nitride layers 5 are formed by physical vapor deposition, "the same thickness" means that the individual thicknesses of the further nitride layers 5 may vary by ±10% between each other.
[0040] In Fig. 1 the zirconium nitride layers 4 and the further nitride layers 5 are grouped as bilayers 45. Each bilayer 45 thus comprises one of the zirconium nitride layers 4 and one of the further nitride layers 5 carrying the zirconium nitride layer 4 of the bilayer 45. The individual thicknesses d4 and d5 of each bilayer 45 add up to a bilayer thickness d45, which is preferably in one of the ranges 65 nm to 1050 nm, 125 nm to 750 nm and 250 nm to 560 nm.
[0041] The individual thickness d4 of each zirconium nitride layer 4 is related to the individual thickness d5 of the further nitride layer 5 carrying the thicker zirconium nitride layer 4 such that d4 / d5 is greater than 1.0, preferably d4 / d5 is in the range of 1.2 to 15.0. d4 / d5 is preferably in one of the ranges 1.2 to 15.0, 2.0 to 12.0, 3.0 to 10.0, 3.0 to 5.5 and 3.2 to 4.6.
[0042] One of the zirconium nitride layers 4 is the top layer of the multi-layer coating 3 exposed for contact with the metal tip.
[0043] The tool body 2 is made of a cemented carbide. The tool body 2 has a cutting edge and optionally at least one chip flute, and the multi-layer coating 3 is deposited on a portion of the cutting edge and, if chip flutes are present, on at least one chip flute.
[0044] The zirconium nitride layer 4 and the further nitride layer 5 are respectively deposited by physical vapor deposition in the layer sequence further nitride layer 5 / zirconium nitride layer 4 / further nitride layer 5 / zirconium nitride layer 4 etc., ending with the zirconium nitride layer 4. The physical vapor deposition is performed in a nitrogen atmosphere using a zirconium target for the zirconium nitride layer 4 and an alloy target for the further nitride layer 5.
[0045] 2 shows a schematic diagram of a cutting tool 10 according to a second embodiment. The cutting tool 10 comprises a tool body 2 of the cutting tool 1, a multi-layer coating 30 which protects the tool body 2 against wear, and a base layer 7 carrying the multi-layer coating 30.
[0046] The only difference between the multi-layer coatings 3 and 30 is that the further nitride layer 5 of the multi-layer coating 3 closest to the tool body 2 is replaced by a base layer 7, and the zirconium nitride layer 4 closest to the tool body 2 is supported by the base layer 7, as shown in FIG. 2.
[0047] It is therefore also true for the multi-layer coating 30 that each zirconium nitride layer 4 is thicker than the further nitride layer 5 carrying said thicker zirconium nitride layer 4. Similarly, the cutting tool 10 can also be used when at least one of the zirconium nitride layers 4 is thicker than one of the further nitride layers 5 carrying said thicker zirconium nitride layer 4. The individual thicknesses d4 and d5 in the multi-layer coating 30 and the thickness relationship d4 / d5 are the same as described for the multi-layer coating 3.
[0048] The individual thicknesses d4 and d5 of the multi-layer coating 30 add up to a total thickness d30 of the multi-layer coating 30. The total thickness d30 is within the ranges described for the total thickness d3.
[0049] The base layer 7 has a total thickness d7, measured in the same manner as the thicknesses d4 and d5, which is preferably in one of the ranges of 500 nm to 15000 nm, 1000 nm to 10000 nm, 2000 nm to 4000 nm, and 2500 nm to 3700 nm.
[0050] The thickness d7 of the base layer 7 is related to the total thickness d30 of the multilayer coating 30, with d7 / d30 being in the range from greater than 0 to 3.0. d7 / d30 is preferably in one of the ranges from greater than 0 to 3.0, 0.5-2.0, 0.5-1.7, and 0.75-1.7.
[0051] As can be seen from FIG. 2, the thickness d7 is greater than any of the individual thicknesses d5 of the further nitride layers 5.
[0052] The thicknesses d7 and d30 add up to a junction thickness d730 in the range of 1000 nm to 25000 nm, preferably 2000 nm to 15000 nm.
[0053] The base layer 7 is (Ti 1-a-b Al a Me * )N β Here, a=0.20 to 0.90 and b=0 to 0.30, preferably a=0.40 to 0.80 and b=0 to 0.30, and β=0.9 to 1.1. When b=0, (Ti 1-a-b Al a Me * b )N β The atomic structure of (Ti 1-a Al a )N β When β=1.0, (Ti 1-a-b Al a Me * b )N β is (Ti 1-a-b Al a Me * b )N 1.0 When b = 0 and β = 1.0, (Ti 1-a-b Al a Me * b )N β (Ti 1-a Al a )N 1.0In the embodiment shown in FIG. 2, the base layer 7 has an atomic composition (Ti 1-a-b Al a Me * b )N β and has the same atomic composition in the sense of "same atomic composition" described above for the further nitride layer 5, i.e. x=a, y=b, α=β and Me=Me * and are within the range of fluctuations that occur during physical vapor deposition or, if another process for the formation of the base layer 7 is used, within the range of fluctuations of that process. * If this is intended, the same target can be used to deposit the base layer 7 and the further nitride layer 5 under physical vapour deposition.
[0054] The cutting tool 10 may also be used when targets of intentionally different composition are used to deposit the base layer 7 and the further nitride layer 5 if the base layer 7 has an atomic composition that is set to be different from the atomic composition of the further nitride layer 5, for example under physical vapor deposition.
[0055] The base layer 7 is deposited by physical vapour deposition, as is the further nitride layer 5 closest to the tool body 2 in FIG. EXAMPLES
[0056] Table 1 shows samples A to N (including sample E1) which are coated cemented carbide end mill bodies having the same design and dimensions. Sample A has a base layer according to the second embodiment shown in Figure 2 and no multilayer coating on top. Sample B has a multilayer coating according to the first embodiment shown in Figure 1. Samples C to N (including sample E1) each have a base layer and a multilayer coating according to the second embodiment shown in Figure 2.
[0057] The specific atomic composition and coating structure of samples A-N (including sample E1) are given in the column "Coating (BL = base layer, ML = multilayer)" in Table 1. ML means that the corresponding coating has a multilayer coating with a zirconium nitride layer and a further nitride layer alternating with the zirconium nitride, as shown in multilayer coatings 3 and 30 in Figures 1 and 2, respectively. The atomic composition of the further nitride layer is given in the column "Coating (BL = base layer, ML = multilayer)" in Table 1. BL means that the coating of the sample has a base layer, if present, which carries a multilayer coating, if present, as shown for base layer 7 in Figure 2. The composition of the base layer is expressed in the same way as the composition of the further nitride layer.
[0058] The total thickness of each substrate, if present, is given in Table 1, column "d(BL)", which corresponds to substrate thickness d7 in FIG. 2. The total thickness of each multi-layer coating, if present, is given in Table 1, column "d(ML)". The ratio of total substrate thickness to total multi-layer coating thickness, if present, is given in Table 1, column "d(BL) / d(ML)", which corresponds to the d7 / d30 ratio disclosed in FIG. 2. The total coating thickness is given in Table 1, column "d(Total)" and is the sum of total multi-layer coating thickness, if present, and total substrate thickness, if present. The individual thicknesses of the zirconium nitride layers, if present, are given in Table 1, column "d(Zirconium Nitride)". The individual thicknesses of the further nitride layers, if present, are given in Table 1, column "d(Ti 1-x-y Al x Me y )N α The thickness of the bilayer represented by d45 in Figures 1 and 2, if any, is given in the column "d(zirconium nitride) + d((Ti 1-x-y Al x Me y )N α The respective ratios of the individual thicknesses of the zirconium nitride layers to the individual thicknesses of the further nitride layers, if present, are shown in Table 1, column “d(zirconium nitride) / d(Ti 1-x-y Al x Me y )N α " is given to The milling distance for each sample used is shown in Table 1 under the column "Milling distance."
[0059] The coatings shown in the column "Coating (BL=base layer, ML=multilayer)" of Table 1 were each deposited by physical vapor deposition in a nitrogen atmosphere in the following manner.
[0060] For Sample A, an alloy target of 33.0 atomic percent titanium and 67.0 atomic percent aluminum (hereinafter abbreviated as "TiAl 33 / 67 target") was used to deposit a base layer onto the tool body of Sample A until the base layer reached the thickness shown in Table 1.
[0061] For sample B, a TiAl 33 / 67 target was used to deposit the first further nitride layer, which is shown in column “d((Ti 1-x-y Al x Me y )N α " on the tool body of Sample B, then a first layer of zirconium nitride was deposited on the first further nitride layer using a zirconium target until the first zirconium nitride layer reached its individual thickness shown in Table 1, after which a second further nitride layer was deposited on the first zirconium nitride layer in a manner similar to the first further nitride layer. The last two deposition steps were repeated to achieve the multilayer coating of Sample A having a total multilayer coating thickness shown in Table 1, column "d(ML)", where the zirconium nitride layer is the top layer. The thickness of the zirconium nitride layer is intended to be the same in the multilayer coating of Sample B, subject to a thickness variation of ±10% between the zirconium nitride layers. The thickness of the further nitride layers is intended to be the same in the multilayer coating of Sample B, subject to a thickness variation of ±10% between the further nitride layers.
[0062] For each of Samples C through G (including Sample E1), a base layer of the composition shown in Table 1 was deposited in the same manner as for Sample A, and then a multilayer coating was deposited on each base layer in the same manner as for Sample B.
[0063] For sample H, a base layer was deposited on the tool body of sample H in the same manner as sample A using an alloy target having a composition of 49.5 atomic percent titanium, 49.5 atomic percent aluminum, and 1.0 atomic percent tantalum (hereinafter abbreviated as "TiAlTa 49.5 / 49.5 / 1 target"), and then a multilayer coating was deposited on the base layer of sample H in the same manner as sample B, except that the TiAlTa 49.5 / 49.5 / 1 target was used instead of the TiAl 33 / 67 target.
[0064] For Sample I, a base layer was deposited on the tool body of Sample I in the same manner as Sample A using an alloy target with a composition of 42.5 atomic percent titanium, 42.5 atomic percent aluminum, and 15.0 atomic percent tantalum (hereinafter abbreviated as "TiAlTa 42.5 / 42.5 / 15 target"), and then a multilayer coating was deposited on the base layer of Sample I in the same manner as Sample B, except that the TiAlTa 42.5 / 42.5 / 15 target was used instead of the TiAl 33 / 67 target.
[0065] For sample J, an alloy target having a composition of 28.5 atomic percent titanium, 66.5 atomic percent aluminum, and 5.0 atomic percent chromium (hereinafter abbreviated as "TiAlCr 28.5 / 66.5 / 5 target") was used to deposit a base layer on the tool body of sample J in the same manner as sample A, and then a multilayer coating was deposited on the base layer of sample J in the same manner as sample B, except that the TiAlCr 28.5 / 66.5 / 5 target was used instead of the TiAl 33 / 67 target.
[0066] For sample K, a base layer was deposited on the tool body of sample K in the same manner as sample A using an alloy target having a composition of 34.4 atomic percent titanium, 63.5 atomic percent aluminum, and 2.1 atomic percent vanadium (hereinafter abbreviated as "TiAlV 34.4 / 63.5 / 2.1 target"). Then, a multilayer coating was deposited on the base layer of sample K in the same manner as sample B, except that the TiAlV 34.4 / 63.5 / 2.1 target was used instead of the TiAl 33 / 67 target.
[0067] For sample L, an alloy target having a composition of 29.8 atomic percent titanium, 66.0 atomic percent aluminum, and 4.2 atomic percent silicon (hereinafter abbreviated as "TiAlSi 29.8 / 66 / 4.2 target") was used to deposit a base layer on the tool body of sample L in the same manner as sample A, and then a multilayer coating was deposited on the base layer of sample L in the same manner as sample B, except that the TiAlSi 29.8 / 66 / 4.2 target was used instead of the TiAl 33 / 67 target.
[0068] For sample M, an alloy target having a composition of 31.0 atomic percent titanium, 65.5 atomic percent aluminum, and 3.5 atomic percent tungsten (hereinafter abbreviated as "TiAlW 31 / 65.5 / 3.5 target") was used to deposit a base layer on the tool body of sample M in the same manner as sample A, and then a multilayer coating was deposited on the base layer of sample M in the same manner as sample B, except that a TiAlW 31 / 65.5 / 3.5 target was used instead of the TiAl 33 / 67 target.
[0069] For sample N, a base layer was deposited on the tool body of sample N in the same manner as sample A using an alloy target with a composition of 32.0 atomic percent titanium, 65.5 atomic percent aluminum, and 2.5 atomic percent molybdenum (hereinafter abbreviated as "TiAlMo 32 / 65.5 / 2.5 target"), and then a multilayer coating was deposited on the base layer of sample N in the same manner as sample B, except that a TiAlMo 32 / 65.5 / 2.5 target was used instead of the TiAl 33 / 67 target.
[0070] The composition given for each coating in Table 1, column “Coating (BL = base layer, ML = multilayer)” is the composition measured for each sample A-N (including sample E1) using energy dispersive X-ray spectroscopy with a scanning electron microscope dedicated to the detection of light chemical elements such as nitrogen (N).
[0071] In each column of Table 1, the thicknesses given for each coating are “d(BL)”, “d(ML)”, “d(total thickness)”, “d(zirconium nitride)” and “d(Ti 1-x-y Al x Me y )N α ) was measured on a cross section in the same manner as in Figures 1 and 2 using a scanning electron microscope, and the measured d(zirconium nitride) and d((Ti 1-x-y Al x Me y )N α ) are the average thicknesses across the corresponding zirconium nitride layers and further nitride layers, respectively, in the corresponding multi-layer coating.
[0072] The milling distances shown in the corresponding columns of Table 1 were obtained in the following manner. Samples A-N (including sample E1) were used to mill a titanium-based alloy with a composition of 90 weight percent titanium, 6 weight percent aluminum, and 4 weight percent vanadium under identical milling conditions. The milling conditions were a milling speed of 80 m / min, a feed rate of 0.05 mm, a milling depth of 4 mm, and a milling width of 10 mm. The tool life criterion was to stop milling when significant wear and chipping of the cutting edge were observed. The milling distance was recorded when the tool life criterion was reached.
[0073] A comparison of the milling distances shown in Table 1 indicates that the multilayer coatings of samples B to N (including sample E1) provide longer tool life compared to when only a base layer is used for wear protection, as in sample A.
[0074] By comparing samples B, C, and D, d(zirconium nitride) / d(Ti 1-x-y Al x Me y )N αThe effect of different d(BL) / d(ML) ratios is shown when is kept (almost) constant (3.4-3.5) in the range of 3.0-10.0, i.e. the milling distance is larger when d(BL) / d(ML) is within the preferred range of 0.5-1.7 (sample C has d(BL) / d(ML)=0.7 and a milling distance of 54 m) and smaller when d(BL) / d(ML) is outside the preferred range of 0.5-1.7 (sample B has d(BL) / d(ML)=0 (no base layer) and a milling distance of 42 m, and sample D has d(BL) / d(ML)=2.0 and a milling distance of 40 m).
[0075] Comparison of samples E, E1 and F shows that when d(BL) / d(ML) is kept (almost) constant (1.3-1.4) within the preferred range of 0.5-1.7, different d(zirconium nitride) / d(Ti 1-x-y Al x Me y )N α The effect of the ratio d(zirconium nitride) / d(Ti 1-x-y Al x Me y )N α is in the preferred range of 3.0 to 10.0, d(zirconium nitride) / d(Ti 1-x-y Al x Me y )N α is outside the preferred range of 3.0 to 10.0 (sample E1 has a d(zirconium nitride) / d(Ti 1-x-y Al x Me y )N α = 5.2, the milling distance was 51 m, and sample E had a d(zirconium nitride) / d(Ti 1-x-y Al x Me y )N α = 1.1, the milling distance was 41 m, and sample F had a d(zirconium nitride) / d(Ti 1-x-y Al x Me y )N α = 11.2 and has a milling distance of 40 m), it is smaller.
[0076] Comparison of samples F and G shows that d(BL) / d(ML) is kept constant (1.4) within the preferred range of 0.5 to 1.7, and d(zirconium nitride) / d(Ti 1-x-y Al x Me y )N α When the ratio is kept nearly constant (11.0-11.2) within the preferred range of 2.0-12.0, the effect of various d thicknesses is shown: the milling distance is greater when d decreases within the range of 35 nm-750 nm (sample F has d=730 nm and milling distance of 40 m, sample G has a smaller d=561 nm and a larger milling distance of 49 m).
[0077] Samples H and I are Me = Ta (Me * =Ta) and has a larger y in the range of 0 to 0.30. Sample J is Me = Cr (Me * =Cr) and has a larger y in the range of 0 to 0.30. For sample K, Me = V(Me * = V) and y in the range of 0 to 0.30. Sample L is Me=Si(Me * =Si) and has a larger y in the range of 0 to 0.30. Sample J is Me = Cr (Me * =Cr) and has a larger y in the range of 0 to 0.30. For sample K, Me = V(Me * = V) and y in the range of 0 to 0.30. Sample L is Me=Si(Me * =Si) and has a larger y in the range of 0 to 0.30. The sample M is Me = W (Me * =W) and has a larger y in the range of 0 to 0.30. Sample N is Me = Mo (Me* =Mo) and has a larger y in the range of 0 to 0.30.
[0078] The following further samples C1-C6 were fabricated, each having a base layer and a multilayer coating carried by the base layer, where each of the multilayer coatings of the further samples has a zirconium nitride layer and a further nitride layer stacked in a manner similar to the second embodiment of Figure 2, with the thicknesses of the base layer, the further nitride layer and the zirconium nitride layer being close to the respective thicknesses of sample C in Table 1 (±10% thickness difference relative to the corresponding layer thicknesses of sample C).
[0079] Sample C1: BL((Ti 0.21 Al 0.79 )N 1.0 ) + ML (zirconium nitride / (Ti 0.21 Al 0.79 )N 1.0 ) Sample C2: BL((Ti 0.30 Al 0.70 )N 1.0 ) + ML (zirconium nitride / (Ti 0.30 Al 0.70 )N 1.0 ) Sample C3: BL((Ti 0.31 Al 0.69 )N 1.0 ) + ML (zirconium nitride / (Ti 0.31 Al 0.69 )N 1.0 ) Sample C4: BL((Ti 0.39 Al 0.61 )N 1.0 ) + ML (zirconium nitride / (Ti 0.39 Al 0.61 )N 1.0 ) Sample C5: BL((Ti 0.51 Al 0.49 )N 1.0 ) + ML (zirconium nitride / (Ti 0.51 Al 0.49 )N 1.0 ) Sample C6:BL((Ti 0.60 Al 0.40 )N 1.0) + ML (zirconium nitride / (Ti 0.60 Al 0.40 )N 1.0 )
[0080] Each of samples C1 to C6, having x=0.4 to 0.8 and y=0, had a milling distance close to the milling distance of sample C shown in Table 1.
[0081] Additional samples were prepared having milling distances close to those of Sample C shown in Table 1, and coating compositions and structures close to those of Sample C (α(α=β)=1.1 and α(α=β)=0.9).
[0082] The following further samples H1 and H2 were made, each having a base layer and a multilayer coating carried by the base layer, where each of the multilayer coatings of the further samples has a zirconium nitride layer and a further nitride layer stacked in a manner similar to the second embodiment of Figure 2, with the thicknesses of the base layer, the further nitride layer and the zirconium nitride layer being close to the respective thicknesses of sample H in Table 1 (±10% thickness difference with respect to the corresponding layer thicknesses of sample H).
[0083] Sample H1: BL((Ti 0.34 Al 0.61 Ta 0.05 )N 1.0 ) + ML (zirconium nitride / (Ti 0.34 Al 0.61 Ta 0.05 )N 1.0 ) Sample H2: BL((Ti 0.30 Al 0.59 Ta 0.11 )N 1.0 ) + ML (zirconium nitride / (Ti 0.30 Al 0.59 Ta 0.11 )N 1.0 )
[0084] Samples H1 and H2, which had x=0.4 to 0.8 and y greater than 0 and smaller than 0.3, had milling distances close to the milling distance of sample H shown in Table 1.
[0085] Further samples J1 and J2 were produced, each having a base layer and a multilayer coating carried by the base layer, where each of the multilayer coatings of the further samples has a zirconium nitride layer and a further nitride layer stacked in a manner similar to the second embodiment of Figure 2, with the thicknesses of the base layer, the further nitride layer and the zirconium nitride layer being close to the respective thicknesses of sample J in Table 1 (±10% thickness difference relative to the corresponding layer thicknesses of sample J).
[0086] Sample J1: BL((Ti 0.13 Al 0.60 Cr 0.27 )N 1.0 ) + ML (zirconium nitride / (Ti 0.13 Al 0.60 Cr 0.27 )N 1.0 ) Sample J2: BL((Ti 0.26 Al 0.61 Cr 0.13 )N 1.0 ) + ML (zirconium nitride / (Ti 0.26 Al 0.61 Cr 0.13 )N 1.0 )
[0087] Samples J1 and J2, which had x=0.4 to 0.8 and y greater than 0 and smaller than 0.3, had milling distances close to the milling distance of sample J shown in Table 1.
[0088] Further samples K1 and K2 were produced, each having a base layer and a multilayer coating carried by the base layer, where each of the multilayer coatings of the further samples has a zirconium nitride layer and a further nitride layer stacked in the same manner as in the second embodiment of Figure 2, with the thicknesses of the base layer, the further nitride layer and the zirconium nitride layer being close to the respective thicknesses of sample K in Table 1 (±10% thickness difference with respect to the corresponding layer thicknesses of sample K).
[0089] Sample K1: BL((Ti 0.19 Al 0.59 V 0.22 )N 1.0 ) + ML (zirconium nitride / (Ti 0.19 Al 0.59 V0.22 )N 1.0 ) Sample K2: BL((Ti 0.26 Al 0.59 V 0.15 )N 1.0 ) + ML (zirconium nitride / (Ti 0.26 Al 0.59 V 0.15 )N 1.0 )
[0090] Samples K1 and K2, which had x=0.4 to 0.8 and y greater than 0 and smaller than 0.3, had milling distances close to the milling distance of sample K shown in Table 1.
[0091] Further samples L1 and L2 were produced, each having a base layer and a multilayer coating carried by the base layer, where each of the multilayer coatings of the further samples has a zirconium nitride layer and a further nitride layer stacked in the same manner as the second embodiment of Figure 2, with the thicknesses of the base layer, the further nitride layer and the zirconium nitride layer being close to the respective thicknesses of sample L in Table 1 (±10% thickness difference with respect to the corresponding layer thicknesses of sample L).
[0092] Sample L1: BL((Ti 0.18 Al 0.59 S 0.23 )N 1.0 ) + ML (zirconium nitride / (Ti 0.18 Al 0.59 S 0.23 )N 1.0 ) Sample L2:BL((Ti 0.27 Al 0.61 S 0.12 )N 1.0 ) + ML (zirconium nitride / (Ti 0.27 Al 0.61 S 0.12 )N 1.0 )
[0093] Each of samples L1 and L2, in which x=0.4 to 0.8 and y was greater than 0 and less than 0.3, had a milling distance close to the milling distance of sample L shown in Table 1.
[0094] Further samples M1 and M2 were produced, each having a base layer and a multilayer coating carried by the base layer, where each of the multilayer coatings of the further samples has a zirconium nitride layer and a further nitride layer stacked in the same manner as the second embodiment of Figure 2, with the thicknesses of the base layer, the further nitride layer and the zirconium nitride layer being close to the respective thicknesses of sample M in Table 1 (±10% thickness difference with respect to the corresponding layer thicknesses of sample M).
[0095] Sample M1: BL((Ti 0.12 Al 0.60 W 0.28 )N 1.0 ) + ML (zirconium nitride / (Ti 0.12 Al 0.60 W 0.28 )N 1.0 ) Sample M2:BL((Ti 0.24 Al 0.59 W 0.17 )N 1.0 ) + ML (zirconium nitride / (Ti 0.24 Al 0.59 S 0.17 )N 1.0 )
[0096] Each of samples M1 and M2, in which x=0.4 to 0.8 and y was greater than 0 and less than 0.3, had a milling distance close to the milling distance of sample M shown in Table 1.
[0097] Further samples N1 and N2 were produced, each having a base layer and a multilayer coating carried by the base layer, where each of the multilayer coatings of the further samples has a zirconium nitride layer and a further nitride layer stacked in the same manner as the second embodiment of Figure 2, with the thicknesses of the base layer, the further nitride layer and the zirconium nitride layer being close to the respective thicknesses of sample N in Table 1 (±10% thickness difference with respect to the corresponding layer thicknesses of sample N).
[0098] Sample N1: BL((Ti 0.32 Al 0.59 Mo 0.09 )N 1.0 ) + ML (zirconium nitride / (Ti 0.32 Al0.59 Mo 0.09 )N 1.0 ) Sample N2: BL((Ti 0.18 Al 0.61 Mo 0.21 )N 1.0 ) + ML (zirconium nitride / (Ti 0.18 Al 0.61 Mo 0.21 )N 1.0 )
[0099] Each of samples N1 and N2, in which x=0.4 to 0.8 and y was greater than 0 and less than 0.3, had a milling distance close to the milling distance of sample N shown in Table 1.
[0100] Further samples O1-O3 were produced, each having a base layer and a multilayer coating carried by the base layer, where each of the multilayer coatings of the further samples has a zirconium nitride layer and a further nitride layer stacked in a manner similar to the second embodiment of Figure 2, with the thicknesses of the base layer, the further nitride layer and the zirconium nitride layer being close to the respective thicknesses of sample N in Table 1 (±10% thickness difference relative to the corresponding layer thicknesses of sample N).
[0101] Sample O1: BL((Ti 0.35 Al 0.60 Nb 0.05 )N 1.0 ) + ML (zirconium nitride / (Ti 0.35 Al 0.60 Nb 0.05 )N 1.0 ) Sample O2: BL((Ti 0.30 Al 0.59 Nb 0.11 )N 1.0 ) + ML (zirconium nitride / (Ti 0.30 Al 0.59 Nb 0.11 )N 1.0 ) Sample O3: BL((Ti 0.21 Al 0.59 Nb 0.20 )N 1.0 ) + ML (zirconium nitride / (Ti 0.21 Al 0.59 Nb0.20 )N 1.0 )
[0102] Each of samples O1 to O3, in which x=0.4 to 0.8 and y was greater than 0 and less than 0.3, had a milling distance close to the milling distance of sample N shown in Table 1.
[0103] Further samples P1-P3 were produced, each having a base layer and a multilayer coating carried by the base layer, where each of the multilayer coatings of the further samples has a zirconium nitride layer and a further nitride layer stacked in a manner similar to the second embodiment of Figure 2, with the thicknesses of the base layer, the further nitride layer and the zirconium nitride layer being close to the respective thicknesses of sample N in Table 1 (±10% thickness difference relative to the corresponding layer thicknesses of sample N).
[0104] Sample P1: BL((Ti 0.32 Al 0.61 Hf 0.07 )N 1.0 ) + ML (zirconium nitride / (Ti 0.32 Al 0.61 Hf 0.07 )N 1.0 Sample P2: BL((Ti 0.24 Al 0.61 Hf 0.15 )N 1.0 ) + ML (zirconium nitride / (Ti 0.24 Al 0.61 Hf 0.15 )N 1.0 ) Sample P3: BL((Ti 0.15 Al 0.59 Hf 0.26 )N 1.0 ) + ML (zirconium nitride / (Ti 0.15 Al 0.59 Hf 0.26 )N 1.0 )
[0105] Each of samples P1 to P3, in which x=0.4 to 0.8 and y was greater than 0 and less than 0.3, had a milling distance close to the milling distance of sample N shown in Table 1.
[0106] FIG. 3 shows a scanning electron micrograph obtained from backscattered electrons of sample E1 in the cross section of FIG. FIG. 3 shows, from bottom to top, a portion of the tool body of sample E1 (the bright white, thin bottom slab), the base layer of sample E1 (the larger dark gray slab) and the multilayer coating of sample E1 (the thinner gray slab is the additional nitride layer and the thicker light gray slab is the zirconium nitride layer).
[0107] The micrograph in Figure 3 shows seven zirconium layers and six additional nitride layers. The two outermost layers (the dark, light "top layers") are from the sample preparation and are not part of the coating of sample E1. The micrograph in Figure 3 shows that the zirconium nitride layer closest to the tool body is supported by the base layer, and the zirconium nitride layers further away from the tool body are each supported by one of the additional nitride layers, with each zirconium nitride layer being thicker than the additional nitride layer that supports it.
[0108] [Experimental Results] [Table 1]
Claims
1. A cutting tool (1, 10) having a tool body (2) and a multilayer coating (3, 30), the multilayer coating (3, 30) protecting the tool body (2) from wear during cutting, the multilayer coating (3, 30) having a plurality of zirconium nitride layers (4), the multilayer coating (3, 30) having a plurality of further nitride layers (5) alternately stacked with the plurality of zirconium nitride layers (4), each of the plurality of further nitride layers (5) carrying one of the plurality of zirconium nitride layers (4), the plurality of further nitride layers (5) each being of a composition selected from the group consisting of (Ti 1-x-y A x Me y ) N α wherein x=0.2-0.9 and y=0-0.3, and wherein Me is one or more metal atoms selected from Ta, Si, Cr, W, V, Cr, Hf, Nb and Mo, and α=0.9-1.1, each of the zirconium nitride layers (4) having a thickness (d4) in the range of 35 nm to 750 nm and each of the further nitride layers (5) having a thickness (d5) in the range of 30 nm to 300 nm, and at least one of the zirconium nitride layers (4) is thicker than one of the further nitride layers (5) carrying it.
2. 2. The cutting tool (1, 10) according to claim 1, wherein said thicker zirconium nitride layer (4) is 1.2 to 15.0 times thicker than the further nitride layer (5) carrying it.
3. The cutting tool (1, 10) has a base layer (7), the base layer (7) being made of (Ti 1-a-b A a Me * b ) N β The atomic composition of the compound is represented by the formula: a=0.20-0.90 and b=0-0.30; * are one or more metal atoms selected from Ta, Si, Cr, W, V, Cr, Hf, Nb and Mo, respectively, and the base layer (7) carries the multilayer coating (3, 30) on a portion of the tool body (2), the base layer (7) being thicker than any of the plurality of further nitride layers (5).
4. 4. The cutting tool (1, 10) according to claim 3, wherein said base layer (7) carries one of said zirconium nitride layers (4).
5. The cutting tool (1, 10) according to claim 3 or 4, wherein the base layer (7) has a total thickness (d7) in the range of 500 nm to 15000 nm.
6. The cutting tool (1, 10) according to any one of claims 3 to 5, wherein the base layer (7) has a total thickness (d7), the multilayer coating (3, 30) has a total thickness (d3, d30), and the ratio of the total thickness (d7) of the base layer (7) to the total thickness (d3, d30) of the multilayer coating (3, 30) is in the range of greater than 0 to 3.
0.
7. The cutting tool (1, 10) according to any one of the preceding claims, wherein the tool body (2) is made from a cemented carbide.
8. 8. The cutting tool (1, 10) of claim 7, wherein the cemented carbide has a metal alloy in an amount of 5 weight percent to 20 weight percent in the cemented carbide, the metal alloy being a cobalt-based alloy, and the cemented carbide has carbide particles that are tungsten carbide particles.
9. 9. The cutting tool (1, 10) according to any one of claims 1 to 8, wherein the sum of the thickness (d4) of the thicker zirconium nitride layer (4) and the thickness (d5) of the further nitride layer (5) carrying the thicker zirconium nitride layer (4) results in a bilayer thickness (d45) in the range of 65 nm to 1050 nm.
10. 10. A cutting tool (1, 10) according to any one of claims 1 to 9, wherein the zirconium nitride layers (4) have the same individual thickness (d4), which is the thickness (d4) of the thicker zirconium nitride layer (4), and the further nitride layers (5) have the same individual thickness (d5), which is the thickness (d4) of the further nitride layer (4) carrying the thicker zirconium nitride layer (5).
11. Cutting tool (1, 10) according to claim 10, wherein the individual thickness (d4) of the zirconium nitride layers (4) is 1.2 to 15 times greater than the individual thickness (d5) of the further nitride layers (5).
12. Cutting tool (1, 10) according to any one of the preceding claims, wherein said thicker zirconium nitride layer (4) is the top layer (4) of a multi-layer coating (3, 30) exposed for metal tip contact.
13. A cutting tool (1, 10) according to any one of the preceding claims, wherein the multilayer coating (3, 30) has a total thickness (d3, d30) in the range of 500 nm to 15000 nm.
14. A cutting tool (1, 10) according to claims 13 and 5, wherein the total thickness (d3, d30) of the multilayer coating (3, 30) and the total thickness (d7) of the base layer (7) add up to a joint thickness (d730) in the range of 1000 nm to 25000 nm.
15. Cutting tool (1, 10) according to any one of the preceding claims, wherein each of the plurality of zirconium nitride layers (4) and each of the plurality of further nitride layers (5) are deposited by physical vapour deposition.
Citation Information
Patent Citations
Composite high hardness material
JP2001181825A
Hard film and hard film coated member
JP2016211052A
Multilayered coated cutting tool
US20110111197A1
Multilayered coated cutting tool
WO2009105024A1