Surface-treated steel sheet and method for manufacturing surface-treated steel sheet
The surface-treated steel sheet with a Ni-containing layer, Ni-W alloy layer, and Fe diffusion alloy layer, along with a W-depleted layer, addresses the cracking and corrosion issues of Ni-W alloy plated steel sheets, enhancing workability and corrosion resistance for square-shaped battery cans.
Patent Information
- Application Number
- JP2024534451
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-07
- Filing Date
- 2024-02-07
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2044-02-07
AI Technical Summary
Ni-W alloy plated steel sheets, while offering better metal elution resistance than Ni-plated steel sheets, suffer from poor workability and are prone to cracking during bending, leading to corrosion of the base metal due to the lack of sacrificial corrosion protection.
A surface-treated steel sheet with a Ni-containing layer and a Ni-W alloy layer, incorporating an Fe diffusion alloy layer and a W-depleted layer within 10 nm from the surface, enhances workability by reducing hardness and preventing crack propagation.
The proposed steel sheet design improves workability and corrosion resistance by suppressing cracks and maintaining metal elution resistance, making it suitable for square-shaped battery cans.
Smart Images

Figure 0007578899000006 
Figure 0007578899000007 
Figure 0007578899000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-treated steel sheet and a method for producing the surface-treated steel sheet. This application claims priority based on Japanese Patent Application No. 2023-016703, filed on February 7, 2023, the contents of which are incorporated herein by reference. [Background technology]
[0002] Ni-plated steel sheets have been used as surface-treated steel sheets for battery cans. Due to the excellent chemical stability of Ni, Ni-plated steel sheets are used for various battery containers, such as battery cans for alkaline manganese dry batteries, lithium ion batteries, and nickel-metal hydride batteries.
[0003] In recent years, Ni-W alloy plated steel sheets containing an alloy of Ni and W as the main components have also begun to be used as materials for battery cans, etc. Examples of Ni-W alloy plated steel sheets are the steel sheets described in Patent Documents 1-4.
[0004] Patent Document 1 discloses a plated steel sheet for battery containers, characterized in that an iron-nickel alloy layer, a nickel layer, and a nickel-tungsten alloy layer are formed, in that order from the bottom, on the side of the steel sheet that will become the inner surface of the battery container.
[0005] Patent Document 2 discloses a Ni-containing surface-treated steel sheet for containers formed by press molding, which includes a steel sheet having a first surface that will become the outside of the container after the press molding, a Ni-containing layer disposed on the first surface of the steel sheet, and a Ni-W alloy plating layer disposed on the Ni-containing layer. The Ni-containing layer has an Fe-Ni diffusion alloy layer, and the amount of Ni contained in the Ni-containing layer is 5 g / m 2 More than 89g / m 2 the thickness of the Ni-W alloy plating layer is 0.02 μm or more and 2 μm or less; and the W concentration in the Ni-W alloy plating layer is, in mass %, 10% or more and 65% or less.
[0006] Patent Document 3 discloses a steel sheet for a non-aqueous electrolyte secondary battery case, comprising: a steel sheet; and a Ni-W-Fe alloy plating layer formed on the surface of the steel sheet, containing a Ni-W-Fe alloy, and serving as the inner surface of the non-aqueous electrolyte secondary battery case.
[0007] Patent Document 4 discloses a steel sheet for use in battery cans of inside-out type alkaline batteries, characterized in that the steel sheet has a plating layer selected from nickel-tungsten (Ni-W) and nickel-cobalt-tungsten (Ni-Co-W) alloys on the surface of one main surface of a base material made of a plate-shaped steel material, and the plating layer has irregularities on the surface formed by dissolution of the tungsten. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2007-51325 A [Patent Document 2] International Publication No. 2012 / 137823 [Patent Document 3] International Publication No. 2017 / 006834 [Patent Document 4] JP 2020-155202 A Summary of the Invention [Problem to be solved by the invention]
[0009] In recent years, there has been an increasing need for prismatic battery cans. Prismatic battery cans are used at neutral potential. Therefore, surface-treated steel sheets for prismatic cans are required to have high resistance to metal elution in electrolytes. Ni-W alloy-plated steel sheets have better resistance to metal elution than Ni-plated steel sheets, which have traditionally been used for battery cans. For this reason, Ni-W alloy-plated steel sheets are considered promising as a material for battery cans.
[0010] However, Ni-W alloy plating is harder than Ni plating and has poor workability. When Ni-W alloy-plated steel sheets are used as materials for rectangular cans, cracks are likely to occur in the Ni-W alloy plating at the bent portions. A crack is a breakage that extends from the surface of the plating layer to the base material. The crack exposes the base material to the outside of the plating, accelerating corrosion of the base material. Since Ni-W alloy plating does not have a sacrificial corrosion protection effect, Ni-W alloy-plated steel sheets are prone to corrosion starting from cracks in the plating.
[0011] For the above reasons, Ni-W alloy plated steel sheets with high formability are desired, but it is very difficult to meet this demand.
[0012] In Patent Document 1, suppression of contact resistance and improvement of discharge characteristics are addressed as issues, but no particular consideration is given to the workability of the plated steel sheet.
[0013] Patent Document 2 aims to improve corrosion resistance after press forming, and proposes a solution to this problem by forming an Fe-Ni diffusion alloy layer at the interface between the steel sheet and the Ni plating layer by heating, and then applying a hard Ni-W alloy plating to the outermost surface. In the plating described in Patent Document 2, a soft Fe-Ni diffusion alloy layer is used to prevent cracks generated in the Ni-W alloy plating layer from propagating to the base steel sheet. However, the plating described in Patent Document 2 has room for improvement in preventing cracks from occurring in the Ni-W alloy plating layer.
[0014] The plated steel sheet disclosed in Patent Document 3 also has a Ni plating layer, which is relatively softer than the Ni-W-Fe alloy plating layer, below the Ni-W-Fe alloy plating layer. However, even in the plating described in Patent Document 3, there is room for improvement in terms of preventing the occurrence of cracks in the Ni-W alloy plating layer.
[0015] Patent Document 4 aims to improve the high-load discharge performance and long-term storage performance of steel sheets, but does not particularly consider the workability of plated steel sheets.
[0016] In view of the above circumstances, an object of the present invention is to provide a surface-treated Ni-W alloy steel sheet having excellent workability and a manufacturing method thereof. [Means for solving the problem]
[0017] The gist of the present invention is as follows.
[0018] (1) A surface-treated steel sheet according to one embodiment of the present invention comprises a base steel sheet, a Ni-containing layer disposed on a surface of the base steel sheet, and a Ni-W alloy layer disposed on the surface of the Ni-containing layer, wherein the Ni-containing layer has an Fe-diffused alloy layer, the Ni-W alloy layer has a thickness of more than 10 nm, and the surface-treated steel sheet has a W-deficient layer within a range from the surface of the Ni-W alloy layer to a depth of 10 nm. (2) Preferably, in the surface-treated steel sheet according to the above-mentioned (1), the surface-treated steel sheet has a W concentration bottom within the range from the surface of the Ni-W alloy layer to a depth of 10 nm, the surface-treated steel sheet has a W concentration peak at a location deeper than the W concentration bottom, and the W concentration W at the W concentration peak is P The W concentration W at the W concentration bottom B The ratio of W B / W P but is less than 0.5. (3) Preferably, in the surface-treated steel sheet according to the above (1) or (2), the Fe-diffused alloy layer is disposed only in the Ni-containing layer, or in the entire Ni-containing layer and only a part of the Ni-W alloy layer, the surface-treated steel sheet has a Ni concentration peak within the range from the surface to a depth of 10 nm in the Ni-W alloy layer, the surface-treated steel sheet has a Ni concentration bottom at a location deeper than the Ni concentration peak in the Ni-W alloy layer, and the Ni concentration at the Ni concentration bottom is B Ni concentration at the Ni concentration peak P Ratio of Ni P / Ni B is 1.1 or greater. (4) Preferably, in the surface-treated steel sheet according to any one of the above (1) to (3), the Ni-containing layer has a thickness of 0.2 to 4.0 μm. (5) In the surface-treated steel sheet according to any one of the above (1) to (4), preferably, the Ni-containing layer and the Ni-W alloy layer each have a coating weight of Ni of 1.8 to 35.6 g / m 2 It is. (6) Preferably, in the surface-treated steel sheet according to any one of the above (1) to (5), the Fe-diffused alloy layer has a thickness of 0.1 to 3.0 μm. (7) In the surface-treated steel sheet according to any one of the above (1) to (6), preferably, the Ni—W alloy layer has an average W concentration of 10 to 45 mass %. (8) Preferably, in the surface-treated steel sheet according to any one of the above (2) to (7), the W concentration W at the W concentration peak P The W concentration W at the W concentration bottom B The ratio W B / W P is greater than or equal to 0.05. (9) Preferably, in the surface-treated steel sheet according to any one of the above (1) to (8), only a part of the Ni-containing layer is the Fe-diffused alloy layer. (10) Preferably, in the surface-treated steel sheet according to any one of (1) to (9) above, the entire Ni-containing layer is the Fe-diffusion alloy layer, and a portion of the Ni-W alloy layer is the Fe-diffusion alloy layer.
[0019] (11) A method for producing a surface-treated steel sheet according to another embodiment of the present invention includes the steps of electrolytically Ni-plating a base steel sheet, electrolytically Ni-W alloy-plating the base steel sheet having a Ni-plated layer, and annealing the base steel sheet having the Ni-plated layer and a Ni-W alloy layer disposed thereon, wherein the dew point of the atmosphere in the annealing is -25 to 5°C, the soaking time in the annealing is 10 to 180 seconds, and the maximum temperature in the annealing is 630 to 860°C. (12) In the method for producing a surface-treated steel sheet according to the above (11), preferably, in the Ni electroplating, a Ni coating weight is set to 1.5 to 33 g / m 2Let us assume that. (13) In the method for producing a surface-treated steel sheet according to the above (11) or (12), preferably, in the Ni electric plating and the Ni-W alloy electric plating, a total Ni coating weight is 1.8 to 35.6 g / m 2 Let us assume that. Effect of the Invention
[0020] According to the present invention, it is possible to provide a surface-treated Ni-W alloy steel sheet having excellent workability and a method for producing the same. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a schematic cross-sectional view of an example (partial diffusion) of a surface-treated steel sheet according to the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view of another example (partial diffusion) of the surface-treated steel sheet according to the present embodiment. [Diagram 3] FIG. 2 is a schematic cross-sectional view of another example (total diffusion) of the surface-treated steel sheet according to the present embodiment. [Figure 4] FIG. 2 is a schematic diagram of a W concentration curve of a Ni—W alloy layer in an example of a surface-treated steel sheet according to the present embodiment. [Diagram 5] FIG. 2 is a schematic diagram of a Ni concentration curve of a Ni—W alloy layer in an example of a surface-treated steel sheet according to the present embodiment. [Figure 6] 2 is a flowchart illustrating an example of a method for manufacturing a surface-treated steel sheet according to the present embodiment. [Figure 7] FIG. 2 is a cross-sectional view of a die used in a drawbead test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] (1. Surface-treated steel sheet 1) As shown in FIG. 1 and other figures, the surface-treated steel sheet 1 according to one embodiment of the present invention includes a base steel sheet 11, a Ni-containing layer 12 disposed on the surface of the base steel sheet 11, and a Ni-W alloy layer 13 disposed on the surface of the Ni-containing layer 12, the Ni-containing layer 12 having an Fe-diffused alloy layer 14, the Ni-W alloy layer 13 having a thickness of more than 10 nm, and the surface-treated steel sheet 1 having a W-deficient layer 131 within a range from the surface of the Ni-W alloy layer 13 to a depth of 10 nm. The surface-treated steel sheet 1 according to this embodiment will be described in detail below. Note that the entire plating layer including the Ni-containing layer 12 and the Ni-W alloy layer 13 may be simply referred to as the "plating layer".
[0023] (Base material steel plate 11) The surface-treated steel sheet 1 has a base steel sheet 11. The base steel sheet 11 is a steel sheet that serves as a substrate for the surface-treated steel sheet 1. The components, sheet thickness, metal structure, and the like of the base steel sheet 11 are not particularly limited and can be appropriately selected depending on the application of the surface-treated steel sheet 1.
[0024] (Ni-containing layer 12) The surface-treated steel sheet 1 has a Ni-containing layer 12 disposed on the surface of a base steel sheet 11. The Ni-containing layer 12 is a layer containing Ni that is provided on the surface of the base steel sheet 11. The Ni-containing layer 12 may be provided on only one surface of the base steel sheet 11, or on both surfaces.
[0025] (Ni-W alloy layer 13) The surface-treated steel sheet 1 further has a Ni-W alloy layer 13 disposed on the surface of the Ni-containing layer 12. The Ni-W alloy layer 13 is an alloy plating layer containing Ni as a main component and further containing W. The Ni-W alloy plating is harder than Ni. By analyzing the component distribution of the plating layer using glow discharge optical emission spectrometry, which is an analytical method capable of measuring the distribution of chemical components in the depth direction from the surface of the plating layer, it is possible to distinguish between the Ni-W alloy layer 13 having a high W concentration and the Ni-containing layer 12 having a low W concentration.
[0026] The thickness of the Ni-W alloy layer 13 is at least more than 10 nm. The thickness of the Ni-W alloy layer 13 is more preferably 20 nm or more, 50 nm or more, 80 nm or more, 100 nm or more, or 150 nm or more. The upper limit of the thickness of the Ni-W alloy layer 13 is not particularly limited, but the thickness is, for example, 350 nm or less, 320 nm or less, or 300 nm or less. For example, when the surface-treated steel sheet 1 is a battery can, the thickness of the Ni-W alloy layer on the outer surface of the battery can is preferably within a range of 100 nm to 300 nm. In addition, the thickness of the Ni-W alloy layer on the inner surface of the battery can is preferably within a range of 20 nm to 40 nm.
[0027] The Ni-W alloy layer 13 may be provided on only one surface or both surfaces of the base steel sheet 11. A surface treatment layer such as a coating film may be further provided on the surface of the Ni-W alloy layer 13.
[0028] (Fe diffusion alloy layer 14) At least a portion of the Ni-containing layer 12 is an Fe-diffusion alloy layer 14. That is, the Ni-containing layer 12 has an Fe-diffusion alloy layer 14. The Fe-diffusion alloy layer 14 is an alloy layer formed by diffusing Fe of the base steel sheet 11 into the inside of the plating layer. The Fe-diffusion alloy layer 14 is obtained, for example, by plating the surface of the base steel sheet 11 and then performing an alloying treatment such as annealing.
[0029] In the cross-sectional schematic diagram illustrated in FIG. 1, only a part of the Ni-containing layer 12 is the Fe diffusion alloy layer 14 in contact with the base steel sheet 11. On the other hand, as illustrated in FIG. 2 and FIG. 3, the entire Ni-containing layer 12 may be the Fe diffusion alloy layer 14. Also, as illustrated in FIG. 2 and FIG. 3, the Fe diffusion alloy layer 14 may extend to the Ni-W alloy layer 13. That is, the Ni-W alloy layer 13 may have the Fe diffusion alloy layer 14. As illustrated in FIG. 2, only a part of the Ni-W alloy layer 13 may be the Fe diffusion alloy layer 14, or as illustrated in FIG. 3, the entire Ni-W alloy layer 13 may be the Fe diffusion alloy layer 14. Note that, as illustrated in FIG. 3, a plating layer in which the entire Ni-containing layer 12 and the Ni-W alloy layer 13 are the Fe diffusion alloy layer 14 may be referred to as a full diffusion plating layer. On the other hand, as illustrated in Fig. 1 or 2, a plating layer in which the Ni-containing layer 12 and the Ni-W alloy layer 13 are partly formed as the Fe diffusion alloy layer 14 may be referred to as a partial diffusion plating layer. The Fe diffusion alloy layer 14 formed on the Ni-containing layer 12 may be referred to as a Ni-Fe alloy layer, and the Fe diffusion alloy layer 14 formed on the Ni-W alloy layer 13 may be referred to as a Ni-W-Fe alloy layer. In general, a surface-treated steel sheet in which only a part of the Ni-containing layer 12 is the Fe diffusion alloy layer 14, and a surface-treated steel sheet in which the entire Ni-containing layer 12 is the Fe diffusion alloy layer 14 and only a part of the Ni-W alloy layer 13 is the Fe diffusion alloy layer 14 are referred to as a partial diffusion plated steel sheet. A surface-treated steel sheet in which the entire Ni-containing layer 12 and the Ni-W alloy layer 13 are the Fe diffusion alloy layer 14 are referred to as a full diffusion plated steel sheet.
[0030] (W-depleted layer 131 in Ni-W alloy layer 13) 4, the surface-treated steel sheet 1 according to this embodiment has a W-deficient layer 131 within a range from the surface of the Ni-W alloy layer 13 to a depth of 10 nm. The surface of the Ni-W alloy layer 13 does not mean the interface between the Ni-W alloy layer 13 and the Ni-containing layer 12, but means the surface of the Ni-W alloy layer 13 on the opposite side to the Ni-containing layer 12. The W concentration in the W-deficient layer 131 is lower than the W concentration in a region of the Ni-W alloy layer 13 that is more than 10 nm deep from the surface of the Ni-W alloy layer 13.
[0031] According to Fick's law, the concentration gradient of an element causes the diffusion of the element. The diffusion rate of an element is proportional to the concentration gradient. Before the alloying treatment, the W concentration of the Ni-W alloy layer 13 is high, while the W concentration of the Ni-containing layer 12 is substantially 0 mass %. When the alloying treatment is performed on the multi-layer plating in which the Ni-containing layer 12 and the Ni-W alloy layer 13 are superposed, it is expected that diffusion of W atoms will occur from the Ni-W alloy layer 13 to the Ni-containing layer 12. Therefore, in the plating layer after the normal alloying treatment, it is expected that W will monotonically decrease from the Ni-W alloy layer 13 toward the Ni-containing layer 12. However, in the surface-treated steel sheet 1 according to this embodiment, a phenomenon contrary to this expectation occurs. The Ni-W alloy layer 13 of the surface-treated steel sheet 1 according to this embodiment has a W-deficient layer 131 in which the W concentration is low near the surface opposite to the Ni-containing layer 12. The W-deficient layer 131 can be formed, for example, by appropriately controlling the dew point of the atmosphere during annealing for the alloying treatment. Furthermore, when the present inventors analyzed various surface-treated steel sheets, they found that there was almost no diffusion of W from the Ni—W alloy layer 13 to the Ni-containing layer 12 .
[0032] (Action and effect) The surface-treated steel sheet 1 according to this embodiment has a Ni-W alloy layer 13. W has the function of increasing the resistance of the Ni plating layer to metal elution in an electrolytic solution. However, W hardens the Ni plating layer, impairing its workability. A plating layer with low workability is prone to cracks during press forming and the like. A crack is a breakage that extends from the surface of the plating layer to the base material. The crack exposes the base material to the outside of the plating, promoting corrosion of the base material. Ni plating and Ni-W alloy plating do not have a sacrificial anticorrosive effect, so Ni-plated steel sheets and Ni-W alloy-plated steel sheets are prone to corrosion starting from cracks in the plating.
[0033] In order to improve the workability of the plating layer, the present inventors provided a Ni-containing layer 12 between the Ni-W alloy layer 13 and the base steel sheet 11. Furthermore, at least a part of the Ni-containing layer 12 was alloyed. The Ni-containing layer 12 and the Fe-diffused alloy layer 14 prevent cracks from progressing to the base steel sheet 11, and thus prevent the base steel sheet 11 from being exposed to a corrosive environment.
[0034] However, although the Ni-containing layer 12 and the Fe-diffused alloy layer 14 mitigate the adverse effects of cracks, they do not suppress the occurrence of cracks on the surface of the plating layer. The present inventors considered the need to suppress the occurrence of cracks in the Ni-W alloy layer 13 and investigated methods for doing so. The present inventors then found that the occurrence of cracks can be suppressed by providing a W-deficient layer 131 in the vicinity of the surface of the Ni-W alloy layer 13.
[0035] In general, the hardness of the Ni-W alloy layer 13 increases in proportion to the W concentration. It is presumed that the hardness of the Ni-W alloy layer 13 is reduced in the W-deficient layer 131. The vicinity of the surface of the Ni-W alloy layer 13 becomes the starting point of cracks during bending of the surface-treated steel sheet 1. The inventors presume that the W-deficient layer 131 reduces the hardness of the vicinity of the surface of the Ni-W alloy layer 13, thereby suppressing the occurrence of cracks.
[0036] As described above, in the surface-treated steel sheet 1 according to this embodiment, the Ni-containing layer 12 and the Fe-diffused alloy layer 14 are used to prevent cracks from progressing to the base steel sheet 11. In addition, in the surface-treated steel sheet 1 according to this embodiment, the W-deficient layer 131 is used to suppress the occurrence of cracks. Therefore, the surface-treated steel sheet 1 according to this embodiment has excellent workability, despite having the Ni-W alloy layer 13 which is hard and prone to cracking.
[0037] According to the results of experiments conducted by the present inventors, the depth at which the W depleted layer 131 is formed is within a range of 10 nm from the surface of the plating layer. If the thickness of the Ni-W alloy layer is 10 nm or less, the W depleted layer 131 is not formed inside the Ni-W alloy layer. Therefore, the thickness of the Ni-W alloy layer needs to be more than 10 nm.
[0038] The above describes the most basic aspect of the surface-treated steel sheet 1 according to this embodiment. Next, a more preferred aspect of the surface-treated steel sheet 1 according to this embodiment will be described.
[0039] (W concentration at W concentration peak W P W concentration at the W concentration bottom B (ratio of As described later, by continuously analyzing the W concentration in the Ni-W alloy layer 13 from the surface of the Ni-W alloy layer 13 along the depth direction using XPS, a W concentration curve as shown in Fig. 4 can be obtained. If the W concentration curve has a bottom of the W concentration in a region from the surface of the Ni-W alloy layer 13 to a depth of 10 nm, it is considered that a W-deficient layer 131 exists. The size of the bottom in the W concentration curve, i.e., the W concentration W at the W concentration bottom, is B is not particularly limited, but may be, for example, more than 0 mass %.
[0040] In addition, the W concentration at the W concentration peak, W P W concentration at the W concentration bottom B The ratio of W B / W P may be used to limit the magnitude of the bottom in the W concentration curve. P is a point where the W concentration is maximum in the W concentration curve of the Ni-W alloy layer 13. P is the W concentration at the W concentration peak. In other words, P is the maximum value of the W concentration in the W concentration curve of the Ni-W alloy layer 13. B This is the location where the W concentration is minimum within a range from the surface to a depth of 10 nm in the W concentration curve of the Ni-W alloy layer 13. B is the W concentration at the W concentration bottom. In other words, B is the minimum value of the W concentration within a range from the surface to a depth of 10 nm in the W concentration curve of the Ni-W alloy layer 13. However, when the W concentration is approximately constant within a range from the surface to a depth of 10 nm, or when the W concentration within the range decreases monotonically from the surface toward the inside of the Ni-W alloy layer 13, the W concentration bottom 13W B is considered not to exist.
[0041] In the surface-treated steel sheet 1 according to this embodiment, the W concentration W at the W concentration peakP W concentration at the W concentration bottom B The ratio of W B / W P is preferably 0.5 or less. This makes it possible to further suppress the occurrence of cracks on the surface of the Ni-W alloy layer 13. B / W P is more preferably 0.4 or less, 0.3 or less, or 0.2 or less.
[0042] On the other hand, W B / W P may be 0.05 or more, 0.07 or more, 0.1 or more, or 0.15 or more. B / W P By increasing the temperature, the resistance to metal elution of the surface-treated steel sheet 1 is further improved. For example, when the surface-treated steel sheet 1 is used as a material for a battery can, the W B / W P By making the ratio 0.05 or more, the electrolyte resistance of the battery can is further improved.
[0043] (Ni concentration peak 13Ni P ) As described above, the plating layer of the surface-treated steel sheet 1 according to this embodiment may be a partial diffusion plating layer as exemplified in Figures 1 and 2, or a full diffusion plating layer as exemplified in Figure 3. When the plating layer of the surface-treated steel sheet 1 is a partial diffusion plating layer, the inventors have found that, as shown in Figure 5, P It has been found that it is possible to dispose the above in the vicinity of the surface of the Ni-W alloy layer 13.
[0044] That is, in the surface-treated steel sheet 1 according to the present embodiment, when the Fe-diffused alloy layer 14 is disposed only in the Ni-containing layer 12 as shown in FIG. 1, or when the Fe-diffused alloy layer 14 is disposed in the entire Ni-containing layer 12 and only a part of the Ni-W alloy layer 13 as shown in FIG. 2, the surface-treated steel sheet 1 has a Ni concentration peak 13 within a range from the surface of the Ni-W alloy layer 13 to a depth of 10 nm. P The surface-treated steel sheet 1 has a Ni concentration peak 13Ni PAt a deeper location, Ni concentration is at bottom 13Ni B The Ni concentration at the bottom is Ni B Ni concentration at the Ni concentration peak P Ratio of Ni P / Ni B is preferably 1.1 or more.
[0045] Ni concentration peak 13Ni P This is the location where the Ni concentration is maximum within a range from the surface to a depth of 10 nm in the Ni concentration curve of the Ni-W alloy layer 13. P is the Ni concentration at the Ni concentration peak. In other words, P is the maximum value of the Ni concentration within a range from the surface to a depth of 10 nm in the Ni concentration curve of the Ni-W alloy layer 13. However, when the Ni concentration is approximately constant within a range from the surface to a depth of 10 nm, or when the Ni concentration within the range increases monotonically from the surface toward the inside of the Ni-W alloy layer 13, the Ni concentration peak 13 P is considered not to exist. Ni concentration bottom 13Ni B This is the location where the Ni concentration is minimum in the Ni concentration curve of the Ni-W alloy layer 13. B is the Ni concentration at the Ni concentration bottom. In other words, B This is the minimum value of the Ni concentration in the Ni concentration curve of the Ni—W alloy layer 13 .
[0046] Considering the diffusion law, the Ni concentration peak 13Ni is the same as the W depletion zone 131. Pis also a unique phenomenon. Before the alloying treatment, the Ni concentration of the Ni-W alloy layer 13 is smaller than the Ni concentration of the Ni-containing layer 12. When the alloying treatment is performed on the multi-layer plating in which the Ni-containing layer 12 and the Ni-W alloy layer 13 are superposed, diffusion of Ni atoms occurs from the Ni-containing layer 12 to the Ni-W alloy layer 13. Therefore, in the plating layer after the normal alloying treatment, it is expected that Ni monotonically decreases from the Ni-containing layer 12 toward the Ni-W alloy layer 13. However, in the surface-treated steel sheet 1 according to the present embodiment, a phenomenon contrary to this expectation may occur. The Ni-W alloy layer 13 of the surface-treated steel sheet 1 according to the present embodiment may have a Ni concentration peak where the Ni concentration is high in the vicinity of the surface opposite to the Ni-containing layer 12. According to the findings of the present inventors, the Ni concentration peak can be formed, for example, by appropriately controlling the dew point of the atmosphere during annealing for the alloying treatment and making the plating layer a partial diffusion layer.
[0047] In the surface-treated steel sheet 1 according to this embodiment, the Ni concentration at the Ni concentration bottom is B Ni concentration at the Ni concentration peak P Ratio of Ni P / Ni B is preferably 1.1 or more. The higher the Ni concentration, the lower the hardness of the Ni-W alloy layer 13. P / Ni B By making the ratio of Ni to W alloy layer 13 equal to or greater than 1.1, the occurrence of cracks on the surface of the Ni-W alloy layer 13 can be further suppressed. P / Ni B More preferably, Ni is 1.15 or more, or 1.2 or more. P / Ni B The larger is the better, and there is no need to limit the upper limit. P / Ni B may be 1.4 or less, 1.35 or less, or 1.3 or less.
[0048] (Thickness of Ni-containing layer 12) The thickness of the Ni-containing layer 12 is not particularly limited. Even if the Ni-containing layer 12 is only slightly thick, it has the effect of suppressing the progress of cracks. On the other hand, from the viewpoint of further improving the workability of the surface-treated steel sheet 1, it is advantageous for the Ni-containing layer 12 to be thicker. Therefore, the thickness of the Ni-containing layer 12 may be, for example, 0.2 μm or more. This further improves the workability of the surface-treated steel sheet 1. The thickness of the Ni-containing layer 12 may be 0.7 μm or more, 1.0 μm or more, or 1.5 μm or more. The upper limit of the thickness of the Ni-containing layer 12 is not particularly specified. For example, the Ni-containing layer 12 may be 4.0 μm or less, 3.0 μm or less, or 2.0 μm or less.
[0049] (Ni deposition amount) The amount of Ni contained in the plating layer (i.e., the Ni-containing layer 12 and the Ni-W alloy layer 13) is not particularly limited, but is, for example, 1.8 to 35.6 g / m 2 The Ni coating weight may be within the range of 1.8 g / m 2 Setting the Ni coating weight at 35.6 g / m or more further improves the corrosion resistance of the surface-treated steel sheet 1 after processing. 2 By setting the Ni coating amount to 4.5 g / m or less, the manufacturing cost of the surface-treated steel sheet 1 can be reduced. 2 More than 6.2g / m 2 or more than 8.9 g / m 2 The Ni coating weight may be 26.7 g / m or more. 2 Below, 17.8g / m 2 or less than 13.4 g / m 2 It may be the following.
[0050] The thickness of the plating layer (i.e., the total thickness of the Ni-containing layer 12 and the Ni-W alloy layer 13) is not particularly limited. For example, the thickness of the plating layer may be within a range of 0.2 μm to 5.0 μm. The thickness of the plating layer may be 4.0 μm or less.
[0051] (Thickness of Fe-diffused alloy layer 14) The thickness of the Fe diffusion alloy layer 14 is not particularly limited. Even if the thickness is small, the Fe diffusion alloy layer 14 can suppress the progress of cracks, improve the workability of the surface-treated steel sheet 1, and improve the corrosion resistance of the processed part. On the other hand, the thickness of the Fe diffusion alloy layer 14 may be, for example, 0.1 μm or more. This can further improve the workability of the surface-treated steel sheet 1. The thickness of the Fe diffusion alloy layer 14 may be 0.5 μm or more, 0.6 μm or more, or 0.7 μm or more. The upper limit of the thickness of the Fe diffusion alloy layer 14 is not particularly specified. For example, the entire plating layer may be the Fe diffusion alloy layer 14. On the other hand, the Fe diffusion alloy layer 14 may be 3.0 μm or less, 2.0 μm or less, 1.5 μm or less, or 1.0 μm or less.
[0052] (Average W concentration in Ni-W alloy layer 13) The Ni-W alloy layer 13 contains Ni as a main component and further contains W. "Contains Ni as a main component" means that the Ni concentration is 50 mass % or more. The average W concentration in the Ni-W alloy layer 13 is not particularly limited, but may be within a range of 10 to 45 mass %, for example.
[0053] W increases the metal elution resistance of the Ni-W alloy layer 13. By setting the average W concentration within the above range, the metal elution resistance of the Ni-W alloy layer 13 can be further increased. The average W concentration in the Ni-W alloy layer 13 may be 15 mass% or more, 20 mass% or more, or 30 mass% or more. In addition, by reducing the W concentration in the Ni-W alloy layer 13, the workability of the Ni-W alloy layer 13 can be further improved. Therefore, the average W concentration in the Ni-W alloy layer 13 may be 40 mass% or less, 37 mass% or less, or 35 mass% or less. For example, the Ni-W alloy layer 13 may contain Cr, Mo, etc.
[0054] (Components of Ni-containing layer 12) The Ni-containing layer 12 is a layer mainly composed of Ni and Fe diffused from the base steel sheet 11. For example, the total content of Ni and Fe in the Ni-containing layer 12 may be 98.0 mass% or more, 98.5 mass% or more, or 99.0 mass% or more. The total content of Ni and Fe in the Ni-containing layer 12 may be 100 mass% or less, 99.5 mass% or less, or 99.0 mass% or less. The ratio of Ni and Fe in the Ni-containing layer 12 is not uniform in the thickness direction of the Ni-containing layer 12 (thickness direction of the surface-treated steel sheet 1). This is because, as described above, a part or the whole of the Ni-containing layer 12 is made into the Fe diffusion alloy layer 14, and the amount of Fe diffused from the base steel sheet 11 in the Fe diffusion alloy layer 14 differs in the thickness direction of the Fe diffusion alloy layer 14. In the Fe diffusion alloy layer 14, the Fe content increases closer to the base steel sheet 11. The thickness of the Fe diffusion alloy layer 14 can be appropriately selected.
[0055] The Ni-containing layer 12 may contain elements other than Ni and Fe. For example, the Ni-containing layer 12 may contain Cr and Mo. For example, the Ni-containing layer 12 may contain one or both of Cr and Mo, and the total content thereof may be more than 0 mass% and 0.1 mass% or less. In addition, various alloy elements contained in the base steel plate 11 may diffuse into the Ni-containing layer 12 during the alloying treatment. Therefore, the Ni-containing layer 12 may contain various impurity elements. In addition, W may diffuse into the Ni-containing layer 12 from the Ni-W alloy layer 13. However, the W content of the Ni-containing layer 12 is usually less than 1.0%.
[0056] (Components of Ni-W alloy layer 13) As described above, the Ni-W alloy layer 13 contains Ni as a main component and further contains W. As illustrated in FIG. 2, when a part or all of the Ni-W alloy layer 13 is the Fe diffusion alloy layer 14, the Ni-W alloy layer 13 may further contain Fe. When the Ni-W alloy layer 13 does not have the Fe diffusion alloy layer 14, the total content of Ni and W in the Ni-W alloy layer 13 may be 95.0 mass% or more, 96.0 mass% or more, or 97.0 mass% or more. When the Ni-W alloy layer 13 does not have the Fe diffusion alloy layer 14, the total content of Ni and W in the Ni-W alloy layer 13 may be 100 mass% or less, 99.0 mass% or less, or 98.0 mass% or less. When the Ni-W alloy layer 13 has the Fe diffusion alloy layer 14, the total content of Ni, W, and Fe in the Ni-W alloy layer 13 may be 95.0 mass% or more, 96.0 mass% or more, or 97.0 mass% or more. When the Ni--W alloy layer 13 has the Fe-diffused alloy layer 14, the total content of Ni, W, and Fe in the Ni--W alloy layer 13 may be 100 mass % or less, 99.0 mass % or less, or 98.0 mass % or less.
[0057] Like the Ni-containing layer 12, the Ni-W alloy layer 13 may contain elements other than Ni, W, and Fe. As described above, the Ni-W alloy layer 13 may contain, for example, Cr and Mo. For example, the Ni-W alloy layer 13 may contain one or both of Cr and Mo, and the total content thereof may be more than 0 mass% and 5 mass% or less. The Ni-W alloy layer 13 may also contain various impurity elements.
[0058] (11 types of base steel plate, etc.) The components and metal structure of the base steel sheet 11 are not particularly limited. The components and metal structure of the base steel sheet 11 can be appropriately selected depending on the application of the surface-treated steel sheet 1. For example, the chemical components of the base steel sheet 11 may contain, in unit mass%, C: 0.0001 to 0.08, Si: 0.001 to 0.03, Mn: 0.01 to 0.4, P: 0.001 to 0.03, S: 0.000 to 0.03, and the balance may contain iron and impurities. The base steel sheet 11 may contain elements other than C, Si, Mn, P, and S.
[0059] When the surface-treated steel sheet 1 is used as a material for a battery container, for example, the base steel sheet 11 is preferably low carbon aluminum-killed steel, IF steel (Interstitial Free Steel / ultra-low carbon steel), etc. Specific examples of the chemical composition (unit: mass%) of the base steel sheet 11 are as follows: (Example 1) Low carbon aluminum killed steel C: 0.057, Si: 0.004, Mn: 0.29, P: 0.014, S: 0.007, Al: 0.050, Cu: 0.034, Ni: 0.021, balance: Fe and impurities (Example 2) IF steel C: 0.004, Si: 0.01, Mn: 0.16, P: 0.013, S: 0.006, Al: 0.029, Cu: 0.027, Ni: 0.022, Ti: 0.013, balance: iron and impurities (Example 3) IF steel C: 0.0012, Si: less than 0.01, Mn: 0.16, P: 0.013, S: 0.006, Al: 0.029, Cu: 0.027, Ni: 0.022, Ti: 0.020, balance: iron and impurities
[0060] There is also no particular limitation on the thickness of the base steel sheet 11. When the surface-treated steel sheet 1 is used, for example, as a material for a battery container, the thickness of the base steel sheet 11 is preferably, for example, 0.15 to 2.00 mm.
[0061] (Measurement method) The presence or absence of the W depletion layer 131 is determined by using XPS (X-ray Photoelectron Spectroscopy). By measuring the distribution of the W concentration in the Ni-W alloy layer 13 in the depth direction from the surface of the Ni-W alloy layer 13 using XPS, a W concentration curve of the Ni-W alloy layer 13 can be obtained as shown in the schematic diagram of Fig. 4. If this W concentration curve has a bottom within a range of 10 nm deep from the surface of the Ni-W alloy layer 13, it is determined that the W depletion layer 131 exists.
[0062] W concentration at W concentration peak P W concentration at the W concentration bottom BThe ratio of W B / W P The W concentration bottom 13W is also measured based on the W concentration curve of the Ni-W alloy layer 13 obtained by the above-mentioned procedure. B and W concentration peak 13W P The position of the W atom and the W concentration at that position can be easily identified.
[0063] Ni concentration at bottomNi concentration B Ni concentration at the Ni concentration peak P Ratio of Ni P / Ni B The Ni concentration of the Ni-W alloy layer 13 is also measured by XPS. By measuring the distribution of the Ni concentration of the Ni-W alloy layer 13 in the depth direction from the surface of the Ni-W alloy layer 13 by XPS, a Ni concentration curve of the Ni-W alloy layer 13 can be obtained as shown in the schematic diagram of FIG. 5. Based on the shape of the Ni concentration curve of the Ni-W alloy layer 13, the Ni concentration bottom 13 B and Ni concentration peak 13Ni P The position of the Ni-containing gas, as well as the Ni concentration at that position, can be easily identified.
[0064] The XPS measurement conditions were as follows: An ULVAC-PHI (PHI5600) was used, and the X-ray source was MgKα. The analysis area was 800 μmφ. Measurement elements: In addition to W, Ni, and Fe, O and C were also measured simultaneously. Argon was used for sputtering to perform depth direction analysis.
[0065] The amount of Ni attached is measured by inductively coupled plasma optical emission spectroscopy (ICP-OES). First, a specified area of the plating layer is dissolved in acid. Next, the total amount of Ni contained in the solution is quantitatively analyzed by ICP-OES. The total amount of Ni quantified by ICP-OES is divided by the specified area mentioned above to obtain the amount of Ni attached per unit area.
[0066] The thickness of the Ni-containing layer 12, the Ni-W alloy layer 13, and the Fe-diffused alloy layer 14 are measured by GDS (Glow Discharge Optical Emission Spectrometry). By using GDS to measure the distribution of element concentrations in the Ni-containing layer 12 and the Ni-W alloy layer 13 in the depth direction from the plating layer surface, element concentration curves can be obtained.
[0067] The measurement is performed using a high-frequency glow discharge optical emission surface analyzer (manufactured by Horiba, Ltd., model number: GD-Profiler2). The GDS measurement conditions are as follows: Anode diameter: φ4mm Gas: Ar Gas pressure: 600Pa Output: 35W
[0068] In the surface-treated steel sheet 1 according to this embodiment, a region in the plating layer containing an Fe concentration of 5.0 mass % or more is regarded as an Fe-diffused alloy layer 14. When a component analysis is performed continuously from the surface of the plating layer in the depth direction, the Fe concentration increases closer to the base steel sheet 11. A location with an Fe concentration of 5.0 mass %, identified by a component analysis performed continuously from the surface of the plating layer in the depth direction, is regarded as an interface between the Fe-diffused alloy layer 14 and a plating layer that is not the Fe-diffused alloy layer 14.
[0069] Moreover, in the surface-treated steel sheet 1 according to this embodiment, the region where the Ni concentration is 1.0 mass % or more is regarded as the plating layer, and the other region is regarded as the base steel sheet 11. In the plating layer of the surface-treated steel sheet 1 manufactured by alloying treatment, the Ni concentration decreases toward the base steel sheet 11. A location where the Ni concentration is 1.0 mass %, which is identified by continuously performing component analysis from the surface of the plating layer in the depth direction, is regarded as the interface between the plating layer and the base steel sheet 11 (i.e., the interface between the Fe-diffused alloy layer 14 and the base steel sheet 11).
[0070] The distance between these interfaces is regarded as the thickness of the Fe-diffused alloy layer 14 in the sample obtained by the above-mentioned procedure. This measurement is performed on five samples, and the average value is calculated. This average value is regarded as the thickness of the Fe-diffused alloy layer 14 of the surface-treated steel sheet 1.
[0071] Furthermore, in the surface-treated steel sheet 1 according to this embodiment, a region in the plating layer where the W concentration is 1.0 mass% or more is regarded as the Ni-W alloy layer 13, and a region where the W concentration is less than 1.0 mass% is regarded as the Ni-containing layer 12. A location where the W concentration is 1.0 mass%, which is identified by continuously performing a component analysis from the surface of the plating layer in the depth direction, is regarded as the interface between the Ni-W alloy layer 13 and the Ni-containing layer 12.
[0072] The distance from the interface between the Ni-W alloy layer 13 and the Ni-containing layer 12 to the interface between the plating layer and the base steel sheet 11 is regarded as the thickness of the Ni-containing layer 12 in the sample obtained by the above-mentioned procedure. This measurement is performed on five samples, and the average value is calculated. This average value is regarded as the thickness of the Ni-containing layer 12 of the surface-treated steel sheet 1. In addition, the distance from the surface of the plating layer to the interface between the Ni-W alloy layer 13 and the Ni-containing layer 12 is regarded as the thickness of the Ni-W alloy layer 13 in the sample obtained by the above-mentioned procedure. This measurement is performed on five samples, and the average value is calculated. This average value is regarded as the thickness of the Ni-W alloy layer 13 of the surface-treated steel sheet 1.
[0073] The method for measuring the average W concentration in the Ni-W alloy layer 13 is as follows. Measurement is performed using XPS (X-ray Photoelectron Spectroscopy). First, the surface of the surface-treated steel sheet 1 is sputtered using argon and / or xenon. Next, the components of the Ni-W alloy layer 13 of the surface-treated steel sheet 1 are measured from the surface toward the inside. After the measurement is completed, the cycle of sputtering again and then measuring is repeated. The analysis results of the W concentration along the depth direction are plotted on a graph in which the horizontal axis represents the depth from the surface of the Ni-W alloy layer 13 and the vertical axis represents the W concentration. The value obtained by integrating the graph of the W concentration is divided by the width of the interval (i.e., the thickness of the Ni-W alloy layer 13) and is regarded as the average W concentration. The above-mentioned calculation performed on the W concentration is also applied to the Ni and Fe analysis results, so that the average Ni concentration and the average Fe concentration in the Ni-W alloy layer 13 can be obtained. The component measurement of the plating layer using XPS is performed using a Mg radiation source. In the analysis using the Mg radiation source, there were no Auger peaks overlapping with the photoelectron peaks of Ni, W, or Fe. Peaks of 2p orbitals of Fe, 2p orbitals of Ni, and 4f orbitals of W were observed.
[0074] (2. Method for producing surface-treated steel sheet 1) Next, a description will be given of a method for producing the surface-treated steel sheet 1 according to this embodiment. For example, the production method according to this embodiment can suitably produce the surface-treated steel sheet 1 having the above-mentioned components.
[0075] As illustrated in FIG. 6, a method for producing a surface-treated steel sheet 1 according to another embodiment of the present invention includes the steps of: (S1) a step of electrolytically plating a base steel sheet 11 with Ni; (S2) A process of electroplating the base steel sheet 11 with a Ni-W alloy; (S3) a step of annealing the base steel sheet 11 having the Ni plating layer and the Ni-W alloy layer 13 disposed thereon; The dew point of the atmosphere in the annealing is -25 to 5°C, the soaking time in the annealing is 10 to 180 seconds, and the maximum temperature in the annealing is 630 to 860°C.
[0076] (S1 Electroplating) First, a base steel sheet 11 is electroplated with Ni. The plating base material is the same as the base steel sheet 11 of the surface-treated steel sheet 1 according to the present embodiment described above. As a result, a Ni-containing layer 12 is provided on the surface of the base steel sheet 11, as shown in Fig. 6. The plated steel sheet obtained by electroplating with Ni is hereinafter referred to as a Ni-plated steel sheet.
[0077] (S2 Electric Ni-W alloy plating) Next, the Ni-plated steel sheet is subjected to electric Ni-W alloy plating. As a result, a Ni-W alloy layer 13 is provided on the surface of the Ni-plated steel sheet as shown in Fig. 6. The plated steel sheet obtained by electric Ni-W alloy plating is hereinafter referred to as a multi-layer plated steel sheet.
[0078] (S3 annealing) Next, the multi-layer plated steel sheet (i.e., the base steel sheet 11 having the Ni plating layer and the Ni-W alloy layer 13 disposed thereon) is annealed. As a result, as shown in Fig. 6, Fe of the base steel sheet 11 is diffused into a part of the plating layer to form an Fe diffused alloy layer 14. In this way, a surface-treated steel sheet 1 can be obtained which includes the base steel sheet 11, the Ni-containing layer 12 disposed on the surface of the base steel sheet 11, and the Ni-W alloy layer 13 disposed on the surface of the Ni-containing layer 12, and in which the Ni-containing layer 12 has the Fe diffused alloy layer 14.
[0079] In the annealing, the dew point of the atmosphere is set to −25 to 5° C. This allows the W-deficient layer 131 to be provided in the Ni—W alloy layer 13.
[0080] The inventors presume that the reason why annealing with a dew point within the above range forms the W-deficient layer 131 in the Ni-W alloy layer 13 is as follows. Ni is an element that is less likely to oxidize than W. Under the above conditions, the oxygen concentration is higher than in a conventional alloying treatment atmosphere, and oxidation is more likely to proceed. It is presumed that W, which is located in the outermost layer before the alloying treatment, is oxidized while diffusing throughout the inside of the plating layer due to the alloying treatment in a high dew point atmosphere, and thus the W-deficient layer 131 is formed.
[0081] In addition, when the inventors investigated various surface-treated steel sheets, they found that the diffusion of W from the Ni-W alloy layer to the Ni-containing layer was slight. The thickness of the Ni-W alloy layer determined from the W concentration distribution in the depth direction from the surface of the plating layer was substantially the same as the thickness of the Ni-W alloy layer before the alloying treatment.
[0082] (Annealing time and temperature) Furthermore, in the manufacturing method of the surface-treated steel sheet 1 according to the present embodiment, the annealing time is set to 10 to 180 seconds, and the annealing temperature is set to 630 to 860°C. The longer the annealing time, the more the alloying progresses, and the thicker the Fe-diffused alloy layer 14 becomes. Also, the higher the annealing temperature, the more the alloying progresses, and the thicker the Fe-diffused alloy layer 14 becomes. Furthermore, according to the findings of the present inventors, by setting the annealing time and the annealing temperature within the above-mentioned ranges, it is possible to provide a W-deficient layer 131 in the Ni-W alloy layer 13. It is presumed that if the annealing time and the annealing temperature are insufficient and the diffusion of the elements contained in the plating is insufficient, the movement of W becomes insufficient, and the W-deficient layer is not formed. On the other hand, a too long annealing time and the annealing time are disadvantageous in terms of productivity and manufacturing costs.
[0083] The above describes the most basic aspect of the method for producing the surface-treated steel sheet 1 according to this embodiment. Next, a more preferred aspect of the method for producing the surface-treated steel sheet 1 according to this embodiment will be described.
[0084] Within a range of 10 nm from the surface of the Ni-W alloy layer 13, a Ni concentration peak 13Ni P In order to provide the above, it is preferable to form the plating layer as a partial diffusion plating in which only a part of the plating layer is alloyed. That is, it is preferable to set the annealing time and the annealing temperature so that the Fe diffusion alloy layer 14 is disposed only on the Ni-containing layer 12, or on the entire Ni-containing layer 12 and only a part of the Ni-W alloy layer 13. For example, partial diffusion plating can be obtained by setting the Ni-containing layer to 2 μm, setting the annealing soaking time in the annealing to 10 seconds, and setting the annealing temperature in the annealing to 750° C.
[0085] By setting the dew point within the above range and making the plating layer a partial diffusion layer, the Ni concentration peak is 13Ni P The reason for this is presumably because Ni is less oxidizable than W, and the easily oxidizable W is internally oxidized, while the less oxidizable Ni is externally oxidized.
[0086] As described above, the thickness of the Fe-diffused alloy layer 14 is preferably 0.1 to 3.0 μm. In order to obtain such an Fe-diffused alloy layer 14, it is preferable that the soaking time in the annealing is 20 seconds and the annealing temperature in the annealing is 810° C., for example.
[0087] (Bath ingredients) The Ni plating bath used in the electric Ni plating contains Ni as a main component. For example, the proportion of Ni element contained in the plating bath to all metal elements contained in the plating bath may be 95 mass% or more, 96 mass% or more, or 97 mass% or more. In addition to Ni, the Ni plating bath may contain Cr, Mo, etc.
[0088] The Ni-W plating bath used in the electric Ni-W alloy plating contains Ni and W as main components. For example, the ratio of the W element contained in the plating bath to all metal elements contained in the plating bath may be within the range of 10 to 60 mass%. Also, for example, the ratio of the total of the Ni element and the W element contained in the plating bath to all metal elements contained in the plating bath may be 95 mass% or more, 96 mass% or more, or 97 mass% or more. In addition to Ni and W, the Ni-W plating bath may contain Cr, Mo, etc.
[0089] (Ni coating weight in electroplating) In the electroplating of Ni, the Ni coating weight is not particularly limited, but is, for example, 1.5 to 33 g / m 2 This allows the Ni-containing layer 12 to have a Ni deposition amount of 1.5 to 33 g / m 2A more preferable Ni coating weight in the electric Ni plating may be the same as the more preferable Ni coating weight in the Ni-containing layer 12 of the surface-treated steel sheet 1 according to the present embodiment described above. The Ni coating weight can be controlled via the components of the Ni plating bath and the amount of current.
[0090] (Total Ni deposition amount in Ni electroplating and Ni-W alloy electroplating) The total Ni coating weight in the Ni electroplating and Ni-W alloy electroplating is not particularly limited, but may be, for example, 1.8 to 35.6 g / m 2 As a result, the total amount of Ni contained in the Ni-containing layer 12 and the Ni-W alloy layer 13 is set to 1.8 to 35.6 g / m 2 A more preferable total Ni coating amount contained in the Ni-containing layer 12 and the Ni-W alloy layer 13 may be the same as the more preferable total Ni coating amount in the Ni-containing layer 12 and the Ni-W alloy layer 13 of the surface-treated steel sheet 1 according to this embodiment described above. The total Ni coating amount can be controlled via the components of the Ni plating bath and the Ni-W plating bath and the amount of current flow.
[0091] Additionally, the various aspects described with respect to the surface-treated steel sheet 1 according to the present embodiment can be applied to the manufacturing method of the surface-treated steel sheet according to the present embodiment. For example, it goes without saying that the preferred aspects of the base steel sheet 11 in the surface-treated steel sheet 1 according to the present embodiment can be applied to the manufacturing method of the surface-treated steel sheet according to the present embodiment. EXAMPLES
[0092] The effects of one embodiment of the present invention will be explained more specifically with reference to an example. However, the conditions in the example are merely an example of conditions adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to this example of conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0093] Various surface-treated steel sheets were produced by electroplating Ni, electroplating Ni-W alloy, and annealing the base steel sheet. The components of the base steel sheet are shown in Table 1. The components of the plating bath used in the electric Ni-W alloy plating are shown in Table 2. The manufacturing conditions of the surface-treated steel sheets are shown in Table 3. The evaluation results of the surface-treated steel sheets are shown in Tables 4 and 5. Note that conditions not listed in the tables were the same in all examples, and their details are as follows:
[0094] The components of the plating bath for electroplating were NiSO4·6H2O: 240g / L, NiCl2·6H2O: 70g / L, and H3BO3: 45g / L. The pH of the plating bath for electroplating was 4, and the temperature was 50°C. The current density for electroplating was 30A / dm 2 The plating weight in the Ni electroplating was controlled by adjusting the current flow time.
[0095] The Ni ion source for electric Ni-W alloy plating was NiSO4·6H2O, and the W ion source was Na2WO4·2H2O. The composition (W content) of the Ni-W alloy plating was adjusted by changing the ratio of Ni ion concentration and W ion concentration. In addition, 0.5 mol / L of citric acid was added to the plating bath for electric Ni-W alloy plating to stabilize the W ions in the bath. The pH of the plating bath for electric Ni-W alloy plating was 6, and the temperature was 50°C. The current density for electric Ni-W alloy plating was 20 A / dm 2 The plating weight in the electric Ni-W alloy plating was controlled by adjusting the current flow time.
[0096] The thickness of the Fe-diffused alloy layer and the thickness of the Ni-containing layer were measured by the method using GDS described above. The measurement results are shown in Table 4. The thickness of the Ni-W alloy layer was also measured by the method using GDS described above, and it was confirmed that the thickness of the Ni-W alloy layer was more than 10 nm in all examples. Therefore, the thickness of the Ni-W alloy layer is not shown in Table 5.
[0097] Determination of the presence or absence of W depletion zone, W concentration at W concentration peak P W concentration at the W concentration bottomB The ratio of W B / W P Measurement of Ni concentration at bottom B Ni concentration at the Ni concentration peak P Ratio of Ni P / Ni B The measurement was carried out according to the above-mentioned method using XPS. The measurement results are shown in Table 4.
[0098] The average W concentration in the Ni-W alloy layer was measured by the above-mentioned method using XPS. The measurement results are shown in Table 4.
[0099] The workability of the plating was evaluated by a drawbead test. The mold 2 for testing was a concave-convex mold 2 shown in FIG. 7. The material of the mold 2 was SKD11. The lubricant was noxrust550HN. The thickness of the steel plate was 0.4 mm and the width was 30 mm. The drawing speed was 200 mm / min, the sliding distance was 100 mm, and the pressing load was 600 kgf. After the drawbead, the surface-treated steel plate 1 was degreased with alkali to remove the lubricant. Then, a corrosion resistance evaluation test piece of 20 mm x 50 mm was cut out from the surface-treated steel plate 1 that had been subjected to the drawbead. The surface that had been slid against the convex side of the mold 2 was used as the corrosion resistance evaluation surface. The test piece was subjected to a constant temperature and humidity test (60°C, 85% RH). After the constant temperature and humidity test, the area ratio of red rust that had occurred on the corrosion resistance evaluation surface was measured and listed in Table 5. Since corrosion resistance correlates with the state of cracks in the coating layer, workability can be evaluated using the red rust occurrence area ratio. Samples with a red rust occurrence area ratio of 10% or less were judged to be surface-treated steel sheets 1 with excellent workability, and were recorded as "Pass" in Table 5. Samples with a red rust occurrence area ratio of more than 10% were recorded as "Fail" in Table 5.
[0100] The electrolytic solution resistance of the plating was evaluated by electrochemical measurement in an atmosphere-unexposed environment in a glove box. The temperature of the measurement environment was 25°C, the dew point was -80°C or less, and the oxygen concentration was 0.7 ppm or less. In the electrolytic solution, the volume ratio of EC (ethylene carbonate) and EMC (ethyl methyl carbonate) was 1:3 (v / v%). In addition, 2 mass% of VC (vinylene carbonate) and 1 mol / L of LiPF6 were added to the electrolytic solution. The reference electrode and the counter electrode were 1 mmφ Li thin wires. In the electrochemical measurement, first, OCV (open circuit voltage) was performed for 5 minutes. Then, LSV (linear sweep voltammetry) was performed up to 4.5 V vs. Li. The sweep rate in LSV was 20 mV / s. The anode current at 3.8 V vs. Li was recorded and listed in Table 5. The smaller the anode current, the higher the electrolytic solution resistance. The evaluation criteria were as follows (unit: × 10 -6 A / cm 2 ). S: Anode current 0.50 or less A: Anode current: over 0.50 and 1.00 or less B: Anode current over 1.00 and 10.00 or less C: Anode current over 10.00
[0101] The above-mentioned evaluation method and evaluation criteria are stricter than those required for ordinary battery cans. Therefore, even if a sample is classified as "C" in the above-mentioned evaluation criteria, it may be usable as an inner surface material of a battery can. Samples classified as B or higher in the above-mentioned evaluation criteria are considered to be extremely excellent as an inner surface material of a battery can.
[0102] [Table 1]
[0103] [Table 2]
[0104] [Table 3]
[0105] [Table 4]
[0106] [Table 5]
[0107] The test pieces of Examples 23, 24, and 28 did not have a W-deficient layer within a range of 10 nm deep from the surface of the Ni-W alloy layer. The area ratio of red rust generation in these test pieces far exceeded the pass / fail criterion of 10%, and they were judged to have poor workability. In the production of Example 23, the dew point of the annealing atmosphere was below the appropriate range. In the production of Example 24, the maximum temperature during annealing was below the appropriate range. In the production of Example 28, the soaking time was below the appropriate range. It is presumed that the W-deficient layer was not obtained in Examples 23, 24, and 28 due to inappropriate production conditions.
[0108] On the other hand, the test pieces obtained by the appropriate manufacturing method had a W-depleted layer within a range of 10 nm deep from the surface of the Ni-W alloy layer. The area ratio of red rust in these test pieces was 10% or less, and they were judged to have good workability.
[0109] In addition, the W concentration at the W concentration peak, W P W concentration at the W concentration bottom B The ratio of W B / W P It was confirmed that when the temperature was high, the electrolyte resistance of the surface-treated steel sheet was further improved. B / W P The value was 0, and the electrolyte resistance was rated C. B / W P The electrolyte resistance of the examples in which W was 0.05 or more was even better than that of Example 37. B / W PThe higher the value, the higher the electrolyte resistance. [Explanation of symbols]
[0110] 1. Surface-treated steel sheets 11 Base steel plate 12 Ni-containing layer 13 Ni-W alloy layer 131 W Deficiency Zone 13W B Double concentration bottom 13W P W concentration peak 13Ni B Ni concentration bottom 13Ni P Ni concentration peak 14 Fe diffusion alloy layer 2. Mold W P W concentration at W concentration peak W B W concentration at the W concentration bottom Ni P Ni concentration at the Ni concentration peak Ni B Ni concentration at bottom
Claims
1. A base steel plate; A Ni-containing layer disposed on a surface of the base steel sheet; A Ni-W alloy layer disposed on a surface of the Ni-containing layer; A surface-treated steel sheet comprising: The Ni-containing layer has an Fe diffusion alloy layer, The thickness of the Ni—W alloy layer is more than 10 nm, The surface-treated steel sheet has a W-depleted layer within a range of 10 nm deep from the surface of the Ni-W alloy layer. Surface treated steel sheet.
2. the surface-treated steel sheet has a W concentration bottom within the range from the surface of the Ni—W alloy layer to a depth of 10 nm, The surface-treated steel sheet has a W concentration peak at a location deeper than the W concentration bottom, The W concentration W at the W concentration peak P The W concentration W at the W concentration bottom B The ratio W B / W P is less than or equal to 0.5 The surface-treated steel sheet according to claim 1 .
3. The Fe-diffused alloy layer is disposed only on the Ni-containing layer, or on the entire Ni-containing layer and only a portion of the Ni-W alloy layer; the surface-treated steel sheet has a Ni concentration peak within the range from the surface to a depth of 10 nm of the Ni—W alloy layer, The surface-treated steel sheet has a Ni concentration bottom at a location deeper than the Ni concentration peak in the Ni-W alloy layer, Ni concentration at bottom Ni concentration B Ni concentration at the Ni concentration peak P Ratio of Ni P / Ni B is 1.1 or more The surface-treated steel sheet according to claim 1 or 2.
4. The thickness of the Ni-containing layer is 0.2 to 4.0 μm. The surface-treated steel sheet according to claim 1 or 2.
5. The amount of Ni contained in the Ni-containing layer and the Ni-W alloy layer is 1.8 to 35.6 g / m 2 is The surface-treated steel sheet according to claim 1 or 2.
6. The thickness of the Fe diffusion alloy layer is 0.1 to 3.0 μm. The surface-treated steel sheet according to claim 1 or 2.
7. The average W concentration in the Ni--W alloy layer is 10 to 45 mass %. The surface-treated steel sheet according to claim 1 or 2.
8. The W concentration W at the W concentration peak P The W concentration W at the W concentration bottom B The ratio W B / W P is 0.05 or more The surface-treated steel sheet according to claim 2 .
9. Only a portion of the Ni-containing layer is the Fe diffusion alloy layer. The surface-treated steel sheet according to claim 1 or 2.
10. The entire Ni-containing layer is the Fe diffusion alloy layer, and a part of the Ni-W alloy layer is the Fe diffusion alloy layer. The surface-treated steel sheet according to claim 1 or 2.
11. A step of electrolytically plating the base steel sheet with Ni; A step of electrically plating the base steel sheet having a Ni plating layer with a Ni-W alloy; Annealing the base steel sheet having the Ni-plated layer and the Ni-W alloy layer disposed thereon; Equipped with The dew point of the atmosphere in the annealing is set to −25 to 5° C., The soaking time in the annealing is 10 to 180 seconds, The maximum temperature in the annealing is 630 to 860°C. The method for producing a surface-treated steel sheet is characterized by the above.
12. In the electric Ni plating, the Ni deposition amount is 1.5 to 33 g / m 2 Let's say The method for producing a coated steel sheet according to claim 11 .
13. In the Ni electric plating and the Ni-W electric alloy plating, the total Ni coating weight is 1.8 to 35.6 g / m 2 Let's say The method for producing a surface-treated steel sheet according to claim 11 or 12.
Citation Information
Patent Citations
Steel sheet for alkaline battery can, battery can for alkaline battery, alkaline battery, and method for producing steel sheet for alkaline battery can
JP2020155202A
Ni-containing surface-treated steel sheet for containers, and method for producing same
WO2012137823A1
Steel plate for case of non-aqueous-electrolyte secondary cell, and case of non-aqueous-electrolyte secondary cell
WO2017006834A1
Plated steel plate for battery case, battery case using the steel plate for battery case and battery using the battery case
JP2007051325A
WO2022/515634A1