Method for recovering styrene monomer from waste polystyrene

The method improves styrene monomer recovery from waste polystyrene by using specific solvents and catalysts to enhance yield and purity, addressing the inefficiencies of existing technologies by minimizing ethylbenzene production and separation costs.

JP7581538B2Active Publication Date: 2024-11-12KOREA RES INST OF CHEM TECH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023562792
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-04
Filing Date
2022-04-15
Publication Date
2024-11-12
Estimated Expiration
2042-04-15

AI Technical Summary

Technical Problem

Existing methods for recovering styrene monomer from waste polystyrene suffer from low yield and purity due to the production of by-products like ethylbenzene, which have similar boiling points to styrene monomer, making separation difficult and economically inefficient.

Method used

A method involving the use of tetrahydrofuran or methyltetrahydrofuran as solvents and potassium carbonate or potassium hydrogen carbonate as catalysts to depolymerize waste polystyrene, followed by distillation and depolymerization, achieving a high yield and purity of styrene monomer by minimizing the production of ethylbenzene and other by-products.

Benefits of technology

The method enhances the yield of styrene monomer to 70% or more, with a weight ratio of styrene to ethylbenzene exceeding 80, while reducing environmental pollution and separation costs by using environmentally friendly solvents and catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581538000002
    Figure 0007581538000002
  • Figure 0007581538000003
    Figure 0007581538000003
  • Figure 0007581538000004
    Figure 0007581538000004
Patent Text Reader

Abstract

The present invention relates to a method for recovering styrene monomer from waste polystyrene, and more specifically, to a method for recovering styrene monomer from waste polystyrene, in which waste polystyrene is depolymerized using an environmentally friendly solvent and a potassium-containing carbonate depolymerization catalyst, thereby suppressing the production of ethylbenzene and the like that are produced as by-products in the styrene monomer recovery step, and enabling the recovery of styrene monomer in a high yield.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering styrene monomer from waste polystyrene, and more particularly, to a method for recovering styrene monomer from waste polystyrene by depolymerizing waste polystyrene in the presence of a catalyst, characterized in that by-products generated by side reactions are suppressed and styrene monomer is recovered in high yield and with high purity. [Background technology]

[0002] As industry develops, large amounts of plastic are being used worldwide. Last year, South Korea produced over 7 million tons of general-purpose plastic products, making it the world's fourth largest plastic producer. However, plastic is discarded in large quantities after use, causing many environmental problems. Waste plastic is currently mainly disposed of by landfilling, but the long biodegradation time in soil and the shortage of landfill sites are causing serious environmental problems. For this reason, there is a lot of interest in developing technology to recycle such waste plastic as a resource.

[0003] Various methods have been proposed for the treatment of waste plastics, but recycling them into added-value fuel oils and raw materials is considered the most environmentally and economically preferable method, rather than simple physical addition or processing.Waste plastic recycling methods are divided into material recycling, which involves recycling the plastic in its original form or after processing, thermal recycling, such as incineration, and chemical recycling, which involves recovering chemical substances such as resin raw materials.

[0004] In the case of physical recycling, polystyrene is mainly recycled to produce recycled resin, lightweight concrete, adhesives, etc., but since this is a physical recycling method, its added value is very low and it cannot be recycled after several physical recyclings, so a large amount of waste polystyrene is generated. In addition, the large amount of contaminated waste polystyrene discharged to agricultural and marine product markets and construction waste sites is not as clean as other waste polystyrene, making it difficult to use for physical recycling.

[0005] Furthermore, since large amounts of contaminated waste polystyrene have a volume more than 50 times that of other waste polystyrene, physical recycling is difficult, and so they are disposed of by landfilling, incineration, etc. However, the incineration method has the problem of causing environmental problems such as the generation of dioxins.

[0006] This has drawn attention to chemical regeneration methods, and the technology to recover the monomer styrene from waste polystyrene was first attempted by Nishizaki et al. in 1997, reporting that it was possible to recover approximately 50% of the monomer from polystyrene by thermal decomposition at 733 K. Based on such technology, many researchers have examined the effects of various catalysts in order to increase the yield of styrene monomer, and many catalysts have been developed.

[0007] As methods for recovering styrene monomer using the above-mentioned catalysts, there have been proposed a technology for recovering styrene monomer using a metal oxide such as Co3O4, Fe2O3, Cr2O3, or CuO, which has high acidity, as a catalyst (Non-Patent Document 1), a technology for recovering styrene monomer using a sulfate catalyst (Patent Documents 1 and 2), and a two-way catalyst technology in which a metal oxide is used as the main catalyst and a basic catalyst is used as a co-catalyst, each of which is supported on silica and alumina (Patent Document 3).

[0008] However, when a highly acidic metal oxide such as Co3O4, Fe2O3, Cr2O3, or CuO is used as a catalyst as in Non-Patent Document 1, carbocations are generated by the cleavage of the single (CC) bonds of polystyrene, and styrene is separated in a chain reaction to undergo a thermal decomposition reaction. However, since the carbocations are unstable due to a lack of two electrons, they cause side reactions such as attacking the surrounding benzene rings, resulting in a decrease in the yield of styrene monomer.

[0009] On the other hand, when a basic catalyst such as BaO, KO, MgO, ZnO, or CaO, or a sulfate catalyst is used, a stable carbanion without an electron deficiency state is generated by satisfying the octet rule, and styrene is separated in a chain reaction and a thermal decomposition reaction is carried out. However, there is a problem that the by-products ethylbenzene and alpha-methylstyrene are increased, decreasing the selectivity of styrene monomer.

[0010] In particular, ethylbenzene has a similar boiling point to the end product, styrene monomer, which significantly impacts economics by increasing the cost of isolating commercially available high purity (>99.6%) styrene monomer.

[0011] Therefore, a new method is required to recover the monomer styrene from waste polystyrene in high yield and with high purity. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Published Patent No. 2001-294708 (Published date: 2001.10.23) [Patent Document 2] Korean Patent Publication No. 2001-87093 (Publication Date: 2001.09.15) [Patent Document 3] Korean Patent Publication No. 2003-0081717 (Publication date: 2003.10.22) [Non-patent literature]

[0013] [Non-Patent Document 1] Ind.Eng.Res., Vol.34, No.12, 1995, 4519 Summary of the Invention [Problem to be solved by the invention]

[0014] The main object of the present invention is to solve the above-mentioned problems, and to provide a method for recovering styrene monomer in high yield by suppressing the production of ethylbenzene, alpha-methylstyrene, benzene, toluene, etc., which are produced by side reactions in the conventional waste polystyrene recovery process.

[0015] In particular, the aim is to suppress the production of ethylbenzene, which has a boiling point similar to that of styrene monomer and is difficult to separate, and to increase the ease of separation of styrene monomer from the depolymerization product of waste polystyrene. [Means for solving the problem]

[0016] In order to achieve the above object, one embodiment of the present invention provides a method for recovering styrene monomer from waste polystyrene, comprising: (a) adding at least one solvent selected from tetrahydrofuran and methyltetrahydrofuran, and at least one depolymerization catalyst selected from potassium carbonate and potassium hydrogen carbonate to waste polystyrene to obtain a mixture in which polystyrene is dissolved; (b) distilling the mixture in which polystyrene is dissolved to separate and recover the solvent; and (c) depolymerizing the mixture obtained in step (b) from which the solvent is separated and recovered to obtain a styrene monomer-containing product, wherein the product obtained in step (c) has a weight ratio of ethylbenzene (EB) to styrene monomer (SM) (SM / EB) of 80 or more.

[0017] In a preferred embodiment of the present invention, in the step (a), tetrahydrofuran and / or methyltetrahydrofuran is added in an amount of 100 parts by weight to 200 parts by weight based on 100 parts by weight of the waste polystyrene.

[0018] In a preferred embodiment of the present invention, the step (a) is carried out at room temperature and normal pressure.

[0019] In a preferred embodiment of the present invention, the distillation in the step (b) is carried out at a temperature of 80°C to 250°C.

[0020] In a preferred embodiment of the present invention, the depolymerization in the step (c) can be characterized in that it is carried out at 200°C to 600°C.

[0021] In a preferred embodiment of the present invention, in the step (c), potassium carbonate and / or potassium hydrogen carbonate is present in an amount of 1 part by weight to 10 parts by weight based on 100 parts by weight of the waste polystyrene.

[0022] In a preferred embodiment of the present invention, the solvent separated in the step (b), tetrahydrofuran and / or methyltetrahydrofuran, is reused in dissolving the waste polystyrene in the step (a). Effect of the Invention

[0023] The method for recovering styrene monomer from waste polystyrene of the present invention depolymerizes polystyrene using a combination of a specific solvent and a specific catalyst, thereby suppressing the production of ethylbenzene and the like that are produced as by-products in the styrene monomer recovery process, and thereby making it possible to increase the yield of recovered styrene monomer.

[0024] In addition, since the solvent used in the present invention is an environmentally friendly solvent having a low boiling point, it has the effect of preventing environmental pollution caused by the use of existing toxic organic solvents such as toluene, and reducing the recovery cost for reusing the solvent. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 is a schematic process diagram showing a method for recovering styrene monomer from waste polystyrene according to one embodiment of the present invention. [Diagram 2] 1 is a graph showing the yields of products produced in Examples 1 and 2 according to the present invention and Comparative Examples 1 to 5. [Diagram 3] 1 is a graph showing the weight ratio of ethylbenzene to styrene monomer produced in Examples 1 and 2 according to the present invention and Comparative Examples 1 to 5. [Figure 4] 1 is a graph showing the XRD measurement results of K2CO3 obtained after evaporating the solvent from a mixture prepared by dissolving 5 g of pristine K2CO3 and K2CO3 in 100 ml of THF and 100 ml of toluene, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. Generally, the nomenclature used herein is one that is well known and commonly used in the art.

[0027] Throughout this specification, when a part "comprises" a certain element, this means that it may further include other elements, rather than excluding other elements, unless specifically stated to the contrary.

[0028] The term "waste polystyrene" as used in this specification includes waste polystyrene after use in various industrial fields, and can be applied regardless of its shape, use, etc.

[0029] As used herein, "normal temperature" means normal atmospheric temperature, which may be 20±10° C., and "normal pressure" means normal atmospheric pressure.

[0030] As used herein, terms such as "comprise," "include," or "have" refer to the presence of features, values, steps, operations, components, parts, or combinations thereof that are stated in the specification, but do not exclude the possibility that other features, values, steps, operations, components, parts, or combinations thereof that are not mentioned may be present or added.

[0031] The present invention relates to a method for recovering styrene monomer from waste polystyrene, comprising the steps of: (a) adding at least one solvent selected from tetrahydrofuran and methyltetrahydrofuran, and at least one depolymerization catalyst selected from potassium carbonate and potassium hydrogen carbonate to waste polystyrene to obtain a mixture in which polystyrene is dissolved; (b) distilling the mixture in which polystyrene is dissolved to separate and recover the solvent; and (c) depolymerizing the mixture obtained in the step (b) from which the solvent is separated and recovered to obtain a styrene monomer-containing product, wherein the weight ratio (SM / EB) of ethylbenzene (EB) to styrene monomer (SM) in the product obtained in the step (c) is 80 or more. Also, the yield of styrene monomer by the method according to the present invention exceeds 70% by weight.

[0032] More specifically, in the method for recovering styrene monomer according to one embodiment of the present invention, polystyrene is depolymerized using a combination of tetrahydrofuran and / or methyltetrahydrofuran, which are environmentally friendly solvents derived from biomass, and potassium carbonate and / or potassium bicarbonate, which are depolymerization catalysts, thereby suppressing the production of ethylbenzene and the like, which are produced as by-products in the styrene monomer recovery process, and increasing the yield of recovered styrene monomer. In addition, by adding the depolymerization catalyst simultaneously with the solvent when dissolving the waste polystyrene, the depolymerization efficiency of the waste polystyrene can be increased due to the uniform dispersion of the depolymerization catalyst on the solvent.

[0033] BEST MODE FOR CARRYING OUT THE DISCLOSURE Preferred embodiments of the method for recovering styrene monomer from waste polystyrene according to the present invention will be described in detail below with reference to the accompanying drawings.

[0034] FIG. 1 is a schematic process diagram showing a method for recovering styrene monomer from waste polystyrene according to one embodiment of the present invention.

[0035] Referring to FIG. 1, in a method for recovering styrene monomer from waste polystyrene according to one embodiment of the present invention, first, tetrahydrofuran and / or methyltetrahydrofuran, and potassium carbonate and / or potassium hydrogen carbonate are added to waste polystyrene at room temperature and normal pressure, and the mixture is stirred to obtain a mixture in which polystyrene is dissolved [step (a)].

[0036] In the present invention, the tetrahydrofuran (THF), methyltetrahydrofuran (MTHF) and a mixture thereof are used as a solvent for dissolving waste polystyrene.

[0037] Tetrahydrofuran (THF) and methyltetrahydrofuran (MTHF) have high solubility in polystyrene but low solubility in other synthetic resins such as polypropylene and polyethylene. They are non-flammable and have a high vaporization point. They are produced from biomass and are very environmentally friendly. They can completely dissolve waste polystyrene in a short time even at room temperature and pressure without changing the physical properties of the polystyrene itself, improving the volume reduction efficiency.

[0038] Other than these, toluene, styrene, benzene, xylene, limonene, etc., are solvents capable of dissolving conventional polystyrene. However, they have low solubility in polystyrene, and are highly toxic to the human body, so they may be problematic from an environmental perspective. In addition, they have boiling points almost similar to those of styrene monomer, so the cost required for separating styrene monomer increases as the amount of the styrene monomer increases, which affects the economic efficiency.

[0039] Therefore, in the present invention, waste polystyrene is dissolved using tetrahydrofuran, methyltetrahydrofuran, or a mixture thereof, so that waste polystyrene can be completely dissolved within a short time even under normal temperature and pressure, thereby improving the dissolving efficiency. Also, since the vaporization point is high, it is possible to prevent environmental pollution and solvent loss due to natural evaporation during the solvent collection process, and also to increase the ease of the work process such as solvent recovery described below.

[0040] The tetrahydrofuran and / or methyltetrahydrofuran can be added in an amount of 100 to 200 parts by weight per 100 parts by weight of waste polystyrene. If the amount of the tetrahydrofuran and / or methyltetrahydrofuran is less than 100 parts by weight per 100 parts by weight of waste polystyrene, the volume reduction of polystyrene may be insufficient, and if the amount exceeds 200 parts by weight, the cost of recovering the solvent may increase.

[0041] On the other hand, potassium carbonate (K2CO3) and / or potassium bicarbonate (KHCO3) are thermal decomposition catalysts that promote thermal decomposition reactions and are stable at high temperatures, so they have high catalytic stability and are easy to recover.

[0042] In addition, the potassium carbonate (K2CO3) and / or potassium bicarbonate (KHCO3) are added to polystyrene simultaneously with tetrahydrofuran and / or methyltetrahydrofuran when polystyrene is dissolved, thereby preventing a phenomenon in which a catalyst is aggregated due to the addition of the catalyst in the conventional depolymerization step, and are uniformly dispersed in tetrahydrofuran and / or methyltetrahydrofuran together with polystyrene, thereby improving the depolymerization efficiency of polystyrene.

[0043] In this case, potassium carbonate (K2CO3) and / or potassium bicarbonate (KHCO3) may be present in an amount of 1 to 10 parts by weight based on 100 parts by weight of waste polystyrene. If the potassium carbonate (K2CO3) and / or potassium bicarbonate (KHCO3) is present in an amount of less than 1 part by weight based on 100 parts by weight of waste polystyrene, there is a risk of problems such as a significant decrease in reactivity and a significant increase in the amount of ethylbenzene, and if it exceeds 10 parts by weight, there is a risk of problems such as an increase in costs due to no difference in reactivity.

[0044] The mixture to which tetrahydrofuran and / or methyltetrahydrofuran and potassium carbonate (K2CO3) and / or potassium bicarbonate (KHCO3) are added can be stirred at room temperature and pressure so that the waste polystyrene dissolves. When the waste polystyrene is completely dissolved in the solvent, the mixture can be left to stand temporarily to allow foreign matter other than polystyrene contained in the waste polystyrene, such as flame retardants, binders, coating agents, etc., to settle, and the settled foreign matter can be removed from the mixture by filtration.

[0045] Meanwhile, the method for recovering styrene monomer according to one embodiment of the present invention may further include a step of removing impurities such as vinyl, paper, wood chips, food residue, small stones, etc. adhering to the waste polystyrene by a method such as washing, and pulverizing the waste polystyrene to a size suitable for dissolution, prior to the step (a). In this case, the pulverized waste polystyrene may be pulverized to a size of an average particle size of 1.0 cm to 10 cm, which is a size suitable for dissolution.

[0046] Thereafter, the mixture obtained by adding the tetrahydrofuran and / or methyltetrahydrofuran and potassium carbonate (K2CO3) and / or potassium hydrogen carbonate (KHCO3) and dissolving polystyrene is distilled to separate and recover the solvent tetrahydrofuran and / or methyltetrahydrofuran, since the mixture may be decomposed at the reaction temperature or inhibit the catalytic reaction [step (b)].

[0047] The distillation can be carried out using a conventional distiller under normal pressure at 80° C. to 250° C. If the distillation is carried out at a temperature lower than 80° C., tetrahydrofuran and / or methyltetrahydrofuran cannot be adequately separated and recovered from the mixture in which polystyrene is dissolved, and if the distillation is carried out at a temperature higher than 250° C., problems may occur in solvent recovery due to thermal decomposition of the solvent.

[0048] The tetrahydrofuran and / or methyltetrahydrofuran thus separated and recovered can be reused in dissolving the waste polystyrene in step (a).

[0049] Thereafter, the mixture in which the tetrahydrofuran and / or methyltetrahydrofuran has been separated and in which the polystyrene has been dissolved is subjected to a depolymerization reaction in the presence of potassium carbonate (K2CO3) and / or potassium bicarbonate (KHCO3) to obtain a product containing a styrene monomer [step (c)].

[0050] The depolymerization can be carried out at 200°C to 600°C for 0.5 to 5 hours. If the depolymerization temperature is less than 200°C, the reactivity may be significantly reduced because depolymerization does not occur, and if the depolymerization temperature exceeds 600°C, the amount of benzene and toluene may be significantly increased due to a cracking reaction, resulting in a significantly reduced amount of styrene monomer produced, and there is a risk of a problem that dimers and trimers with high boiling points may be mixed into the product. In addition, if the depolymerization time is less than 0.5 hours, the reaction time is insufficient, resulting in a small amount of styrene monomer recovered, and if the depolymerization time exceeds 5 hours, the amount of ethylbenzene may be significantly increased, resulting in a problem of reduced productivity due to increased energy consumption.

[0051] Thereafter, the product obtained by the depolymerization reaction can be collected and cooled. In this case, the cooling can be performed by any cooling method used in the art, such as an indirect cooling method in which a refrigerant is compressed and evaporated, and the collected product is cooled using the heat of evaporation of the refrigerant, or a direct cooling method, without any limitation.

[0052] The products obtained from the depolymerization reaction include not only the final target component styrene monomer (SM), but also high boiling point substances such as ethylbenzene (EB), toluene, cumene, and alpha methylstyrene, and depolymerization reaction residues, which not only hinder the depolymerization reaction but also reduce the yield of styrene monomer. Conventionally, the yield of styrene monomer has decreased during long-term operation.

[0053] Therefore, in the method for recovering styrene monomer according to the present invention, the waste polystyrene is dissolved and depolymerized using a potassium-containing carbonate catalyst together with an environmentally friendly solvent, and thus the final target component, styrene monomer, can be recovered at a yield of 70% or more, and ethylbenzene (EB), toluene, cumene, and alphamethylstyrene can be recovered at a yield of 3.5% or less, respectively. In particular, in the method for recovering styrene monomer according to the present invention, the weight ratio (SM / EB) of styrene monomer (SM) to ethylbenzene (EB) can be recovered at 80 or more, preferably 84 or more.

[0054] That is, the method for recovering styrene monomer according to the present invention can facilitate the separation process for recovering the final styrene monomer by suppressing the production of ethylbenzene, alpha-methylstyrene, toluene, especially ethylbenzene, which are produced by side reactions in the conventional styrene monomer recovery process. EXAMPLES

[0055] The present invention will be described in more detail with reference to the following specific examples. The following examples are merely illustrative to aid in understanding the present invention, and the scope of the present invention is not limited thereto.

[0056] <Example 1> 60g of crushed waste polystyrene was placed in a reactor that could be opened and closed at room temperature, and 100g of tetrahydrofuran and 3g of potassium carbonate (K2CO3) (Sigma-Aldrich, ACS reagent>99%) as a catalyst were added thereto, and the mixture was stirred at room temperature and pressure for 10 minutes to dissolve the waste polystyrene and disperse the catalyst. The mixture in which the waste polystyrene was dissolved was distilled at 200°C for 30 minutes to separate tetrahydrofuran. The temperature was then raised to 375°C, and a depolymerization reaction was carried out at this temperature for 1 hour. The product decomposed by the depolymerization reaction was obtained by liquefying it in a condenser. The obtained product was measured using a GC / FID (Yongling Instruments) equipped with a capillary column (capillary column, HP-5, 30m x 0.32mm x 1.0μm, cross-linked 5% PH ME Siloxane), and the results are shown in Table 1, Figure 1, and Figure 2.

[0057] <Example 2> The waste polystyrene was depolymerized in the same manner as in Example 1 to obtain a product, but 3 g of potassium bicarbonate (KHCO3) (Sigma-Aldrich, ACS reagent>99.7%) was used as a catalyst instead of potassium carbonate (K2CO3) to perform depolymerization. The product was measured in the same manner as in Example 1, and the results are shown in Table 1, Figure 1, and Figure 2.

[0058] <Comparative Example 1> The waste polystyrene was depolymerized in the same manner as in Example 1 to obtain a product, but the depolymerization was carried out without adding a catalyst. The product was measured in the same manner as in Example 1, and the results are shown in Table 1, Figure 1, and Figure 2.

[0059] <Comparative Example 2> The waste polystyrene was depolymerized in the same manner as in Example 1 to obtain a product, but 3 g of barium oxide (BaO) (Sigma-Aldrich, CS reagent>97%) was used as a catalyst instead of potassium carbonate (K2CO3) to perform depolymerization. The product was measured in the same manner as in Example 1, and the results are shown in Table 1, Figure 1, and Figure 2.

[0060] <Comparative Example 3> The waste polystyrene was depolymerized in the same manner as in Example 1 to obtain a product, but 3 g of calcium oxide (CaO) was used as a catalyst instead of potassium carbonate (K2CO3). The product was measured in the same manner as in Example 1, and the results are shown in Table 1, Figure 1, and Figure 2.

[0061] <Comparative Example 4> The waste polystyrene was depolymerized in the same manner as in Example 1 to obtain a product, but 3 g of strontium oxide (SrO) was used as a catalyst instead of potassium carbonate (K2CO3). The product was measured in the same manner as in Example 1, and the results are shown in Table 1, Figure 1, and Figure 2.

[0062] <Comparative Example 5> The waste polystyrene was depolymerized in the same manner as in Example 1 to obtain a product, but 3 g of KNO3 was used as a catalyst instead of potassium carbonate (K2CO3). The product was measured in the same manner as in Example 1, and the results are shown in Table 1, Figure 1, and Figure 2.

[0063] <Comparative Example 6> The waste polystyrene was depolymerized in the same manner as in Example 1 to obtain a generated product, but the depolymerization was performed using toluene instead of tetrahydrofuran as a solvent. The obtained product was measured in the same manner as in Example 1, and the results are shown in Table 1, Figure 1, and Figure 2.

[0064] [Table 1]

[0065] As shown in Table 1, Figures 1 and 2, in the cases of Examples 1 and 2, the yield of styrene monomer (SM) was higher than in Comparative Examples 1 to 6, but the yields of the by-products ethylbenzene (EB), toluene, cumene, and alphamethylstyrene (a-MS) were lower than in the cases of Comparative Examples 1 to 6. In particular, in the cases of Examples 1 and 2, the yield of styrene monomer (SM) was 70% by weight or more, and the weight ratio of styrene monomer (SM) to ethylbenzene (EB) was 84 or more.

[0066] Comparing Examples 1 and 2 with Comparative Examples 1 to 5, it was found that the presence or absence of a catalyst or the type of catalyst also had a significant relationship with the yield of styrene monomer (SM) and the amount of by-products generated. In particular, even when the same potassium salt was used, there was a large difference in activity depending on the type of anion. 2- ) or bicarbonate (HCO3 - ) had a high yield of styrene monomer (SM) and low yields of by-products such as ethylbenzene (EB).

[0067] In addition, comparing the results of Example 1 and Comparative Example 6, it was found that even if the type of catalyst was the same, the type of solvent used to dissolve waste styrene was also related to the final styrene monomer yield and the amount of by-reaction products generated. Comparative Example 6 used toluene, which has been widely used as a solvent for reducing the volume of waste styrene, as the solvent, while Example 1 used THF as the solvent. When toluene was used as the solvent, the yield of styrene monomer was 62.3 wt%, which was only about 88% of the yield when THF was used as the solvent, and the yield of ethylbenzene was high.

[0068] To confirm the cause of this difference in activity, pristine K2CO3 and K2CO3 (5 g) were dissolved in 100 ml of THF and 100 ml of toluene, respectively, and the mixtures were stirred for 24 hours. The solvent was then evaporated at 120°C for 12 hours, and the resulting K2CO3 was analyzed by XRD (Rigaku Ultima IV). The results are shown in Figure 4.

[0069] Referring to FIG. 4, K2CO3 after dissolving in THF and toluene shows a general change in crystallity compared to pristine K2CO3. In particular, in the case of toluene, the peak at 2theta=32.5° increases significantly and the peak at 2theta=31.6° decreases. This indicates that K2CO3 shows greater stability in THF than in toluene and has less tendency to undergo phase transformation. It was confirmed that the K2CO3 structure is more stable in THF solution than in toluene.

[0070] Therefore, in the case of depolymerizing waste polystyrene using a combination of a solvent and a catalyst, in which at least one of THF and MTHF is selected as a solvent and at least one of K2CO3 and KHCO3 is selected as a depolymerization catalyst as in the present invention, styrene monomer can be recovered in high yield by depolymerization, and the production of ethylbenzene, which has a boiling point similar to that of styrene monomer, can be suppressed, thereby reducing the cost of the product separation process, and therefore it has been found that the efficiency of the depolymerization process of waste polystyrene can be greatly improved in a new industrial aspect.

[0071] Although the preferred embodiment of the present invention has been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the claims, the detailed description of the invention, and the accompanying drawings, which of course also fall within the scope of the present invention.

Claims

1. (a) adding at least one solvent selected from tetrahydrofuran and methyltetrahydrofuran, and at least one depolymerization catalyst selected from potassium carbonate and potassium hydrogen carbonate to waste polystyrene to obtain a mixture in which polystyrene is dissolved; (b) distilling the mixture in which the polystyrene is dissolved to separate and recover the solvent; (c) depolymerizing the mixture obtained in step (b) by separating and recovering the solvent to obtain a styrene monomer-containing product; A method for recovering styrene monomer from waste polystyrene, wherein the product obtained in step (c) has a weight ratio of styrene monomer (SM) to ethylbenzene (EB) (SM / EB) of 80 or more.

2. The method for recovering styrene monomer from waste polystyrene according to claim 1, characterized in that in the step (a), tetrahydrofuran and / or methyltetrahydrofuran is added in an amount of 100 parts by weight to 200 parts by weight based on 100 parts by weight of the waste polystyrene.

3. 2. The method for recovering styrene monomer from waste polystyrene according to claim 1, wherein the step (a) is carried out at room temperature and normal pressure.

4. The method for recovering styrene monomer from waste polystyrene according to claim 1, wherein the distillation in step (b) is carried out at 80°C to 250°C.

5. The method for recovering styrene monomer from waste polystyrene according to claim 1, wherein the depolymerization in step (c) is carried out at a temperature of 200°C to 600°C.

6. The method for recovering styrene monomer from waste polystyrene according to claim 1, wherein the potassium carbonate and / or potassium hydrogen carbonate in step (c) is present in an amount of 1 part by weight to 10 parts by weight per 100 parts by weight of the waste polystyrene.

7. 2. The method for recovering styrene monomer from waste polystyrene according to claim 1, wherein the solvent separated in step (b) is reused for dissolving the waste polystyrene in step (a).

Citation Information

Patent Citations

  • Method for recovering styrene from polystyrene

    JP1996073647A

  • Method for pyrolyzing styrene resin

    JP1996283745A

  • Method for recycling monomer from plastic waste

    JP2000327831A

  • Recovery of polystyrene from flame retardant polystyrene

    JP2001019794A

  • Method for decomposing waste plastic

    JP2001139723A