Alkaline degreasing bath and method for preparing same, and method for manufacturing grain-oriented electrical steel sheet with insulating coating

An alkaline degreasing bath with controlled refractive index and silicic acid concentration improves annealing separator adhesion, addressing non-uniformity issues in forsterite coating, resulting in high-quality grain-oriented electrical steel sheets.

JP7582357B2Active Publication Date: 2024-11-13JFE STEEL CORP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2023020318
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-02-16
Filing Date
2023-02-13
Publication Date
2024-11-13
Estimated Expiration
2043-02-13

AI Technical Summary

Technical Problem

Existing methods for producing grain-oriented electrical steel sheets with an insulating coating face issues with non-uniform adhesion of the annealing separator, leading to defects in the forsterite coating, which affects the appearance and performance of the steel sheets.

Method used

The use of an alkaline degreasing bath with specific refractive index and silicic acid concentration, along with additional ions and compounds, to improve the adhesion of the annealing separator before decarburization annealing, ensuring a homogeneous forsterite film formation.

Benefits of technology

The improved adhesion of the annealing separator results in a uniform and aesthetically pleasing forsterite coating, enhancing the quality and performance of the grain-oriented electrical steel sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582357000001
    Figure 0007582357000001
  • Figure 0007582357000002
    Figure 0007582357000002
Patent Text Reader

Abstract

To provide an alkaline degreasing bath suitable for degreasing treatment, which is pretreatment to improve steel sheet adhesion of an annealing separation agent.SOLUTION: An alkaline degreasing bath is used to degrease a cold-rolled sheet of grain-oriented electrical steel and has a bath composition including silicic acid. When the concentration of the silicic acid is defined as A mass% in terms of SiO2, the refractive index, R, of the bath satisfies the following formula (1): 4.6×10-3×A+1.3340≤R (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an alkaline degreasing bath used in the production of grain-oriented electrical steel sheet and a method for preparing the same, and a method for producing grain-oriented electrical steel sheet with an insulating coating using the alkaline degreasing bath. [Background technology]

[0002] Grain-oriented electrical steel sheets are usually made by hot rolling a material containing 4% or less Si, followed by annealing and cold rolling once or twice or more times with intermediate annealing to produce the final thickness. Next, decarburization annealing is performed to decarburize and form an oxide film mainly composed of SiO2. After that, a slurry of an annealing separator mainly composed of MgO is applied using a coating roll or the like, and after drying, the material is wound into a coil and subjected to final annealing, secondary recrystallization, purification, and forsterite film formation. If necessary, insulation coating treatment and heat flattening are performed to produce the final product.

[0003] In the above-mentioned forsterite film formation process, when an annealing separator mainly composed of MgO is applied to a steel sheet, the dispersion state of the particles in the slurry, the degree of hydration, as well as the contact state and adhesion state to the steel sheet surface after drying are important. Usually, the main component MgO is suspended in water using a stirrer together with a small amount of additives, which are mixed as necessary as reaction accelerators, to form a slurry, which is then applied to the steel sheet.

[0004] In order to improve the adhesion of the annealing separator to the steel sheet surface, various techniques for improving the annealing separator have been proposed. For example, Patent Documents 1 to 3 propose techniques for adjusting the activity, specific surface area, and amount of impurities of MgO. Patent Document 4 proposes a technique for adjusting the activity by crushing the annealing separator slurry, and Patent Document 5 proposes a technique for adding metal sulfates, metal chlorides, etc. to the annealing separator. However, in all of these techniques, there was a problem that when the hydration was adjusted to a low side in order to avoid the moisture for hydrating MgO being brought between the steel sheets in the coil and causing coating defects and magnetic deterioration due to the excess moisture, the adhesion of the annealing separator to the steel sheet may not be sufficient.

[0005] In addition, various techniques have been proposed for obtaining a homogeneous forsterite coating, such as electrolytic degreasing of cold-rolled sheets before decarburization annealing. For example, Patent Document 6 proposes a technique for adding a chelating agent to an alkaline degreasing bath, Patent Document 7 proposes a technique for controlling the iron concentration in an alkaline degreasing bath, and Patent Document 8 proposes a technique for adding a chelating agent to an alkaline degreasing bath and adjusting the iron ion concentration by adding an organic iron salt. However, even with these techniques, there is a problem in that when the adhesion of the annealing separator to the steel sheet is insufficient, defects in the forsterite coating may occur frequently. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 1-177376 [Patent Document 2] Japanese Patent Application Publication No. 3-75219 [Patent Document 3] JP 2003-27251 A [Patent Document 4] Japanese Patent Application Publication No. 6-212249 [Patent Document 5] Japanese Patent Application Publication No. 11-36018 [Patent Document 6] Japanese Patent Application Publication No. 2-243771 [Patent Document 7] Japanese Patent Application Publication No. 3-240922 [Patent Document 8] Japanese Patent Application Publication No. 6-192898 Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, grain-oriented electrical steel sheet with an insulating coating, a typical example of which is a forsterite coating, can be obtained by decarburization annealing the grain-oriented electrical steel sheet after cold rolling, applying an annealing separator slurry containing MgO as a main component, and then performing finish annealing to form a forsterite coating.

[0008] In this case, if the adhesion of the annealing separator to the electrical steel sheet after decarburization annealing is insufficient, the thickness of the forsterite coating formed will be non-uniform, making the coating more susceptible to defects. This non-uniform forsterite coating may also cause the insulating coating formed thereon to be non-uniform. Since multiple electrical steel sheets are often stacked together and used as iron cores, there is a strong demand for electrical steel sheets to have a uniform, beautiful, and good appearance.

[0009] The present invention has been made in view of the above points, and aims to provide an alkaline degreasing bath suitable for use in a degreasing treatment, which is a pretreatment for improving the adhesion of an annealing separator to a steel sheet, and a method for preparing the same. Another aim of the present invention is to propose a method for producing a grain-oriented electrical steel sheet in which a homogeneous forsterite film is formed by carrying out a degreasing treatment using the alkaline degreasing bath. [Means for solving the problem]

[0010] As a result of intensive research into achieving the above object, the inventors have discovered that degreasing using a specific alkaline degreasing bath before decarburization annealing improves the adhesion of an annealing separator to a cold-rolled sheet after decarburization annealing, and have completed the present invention. That is, the gist of the present invention is as follows.

[0011] 1. An alkaline degreasing bath having a bath composition containing silicic acid, which is used for degreasing cold-rolled sheets of grain-oriented electrical steel, An alkaline degreasing bath, in which, when the silicic acid concentration is A mass % in terms of SiO2, the refractive index R of the bath satisfies the following formula (1). 4.6×10 -3 ×A+1.3340≦R (1)

[0012] 2. The alkaline degreasing bath according to 1 above, wherein the refractive index R is 1.4200 or less.

[0013] 3. The alkaline degreasing bath according to 1 or 2, wherein the silicic acid concentration is 0.2% by mass or more and 10.0% by mass or less, calculated as SiO2.

[0014] 4. An alkaline degreasing bath according to any one of claims 1 to 3, which contains at least one of alkali metal ions, alkaline earth metal ions and ions of Group 16.

[0015] 5. The alkaline degreasing bath according to any one of 1 to 4 above, which contains at least one of a chelating agent, a surfactant, and an organic acid metal salt.

[0016] 6. A method for producing grain-oriented electrical steel sheet with an insulating coating, comprising hot rolling and cold rolling a material for grain-oriented electrical steel to obtain a cold-rolled sheet, degreasing the cold-rolled sheet using an alkaline degreasing bath described in any one of items 1 to 5 above, and then subjecting the cold-rolled sheet to decarburization annealing. After that, an annealing separator is applied to the surface of the decarburization annealed sheet, and then finish annealing is performed.

[0017] 7. The method for producing a grain-oriented electrical steel sheet with an insulating coating according to 6 above, wherein the temperature of the alkaline degreasing bath is 30°C or higher and 95°C or lower, and the degreasing time in the alkaline degreasing bath is 1 second or higher and 40 seconds or lower.

[0018] 8. The method for producing a grain-oriented electrical steel sheet with an insulation coating according to 6 or 7 above, further comprising electrolytically degreasing the cold-rolled sheet.

[0019] 9. A method for preparing an alkaline degreasing bath having a bath composition containing silicic acid for use in degreasing a cold-rolled sheet of grain-oriented electrical steel, comprising: A method for adjusting an alkaline degreasing bath, comprising adjusting a refractive index R of the bath to satisfy the following formula (1) when the silicic acid concentration is A mass % in terms of SiO2. 4.6×10 -3 ×A+1.3340≦R (1)

[0020] 10. The method for preparing an alkaline degreasing bath according to 9 above, wherein the refractive index R is 1.4200 or less.

[0021] 11. The method for preparing an alkaline degreasing bath according to claim 9 or 10, wherein the silicic acid concentration is 0.2% by mass or more and 10.0% by mass or less, calculated as SiO2.

[0022] 12. The method for preparing an alkaline degreasing bath according to any one of items 9 to 11 above, further comprising adding to the alkaline degreasing bath at least one of alkali metal ions, alkaline earth metal ions and ions of Group 16.

[0023] 13. The method for preparing an alkaline degreasing bath according to any one of items 9 to 12, further comprising adding to the alkaline degreasing bath at least one of a chelating agent, a surfactant, and an organic acid metal salt. Effect of the Invention

[0024] Use of the alkaline degreasing bath of the present invention makes it possible to manufacture grain-oriented electrical steel sheet having a forsterite coating which exhibits excellent adhesion of the annealing separator to the steel sheet and which also exhibits excellent appearance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] <How the present invention was arrived at> The present inventors conducted various investigations to find factors that affect the adhesion of an annealing separator to a steel sheet, and have now discovered that a grain-oriented electrical steel sheet that has been degreased in an alkaline degreasing bath before decarburization annealing has extremely good adhesion of an annealing separator to its surface.

[0026] Therefore, the present inventors have investigated the conditions for degreasing before decarburization annealing. Specifically, various ions, compounds, and solvents were further added to the silicate aqueous solution used for alkaline degreasing, and the amounts of these added were adjusted. Then, the inventors have found that when the silicate aqueous solution with the adjusted amounts was used as an alkaline degreasing bath to degrease a cold-rolled sheet, decarburization annealing was performed, and then an annealing separator slurry was applied, the inventors found that adhesion to the steel sheet surface could be improved in some cases.

[0027] The present invention, which was made based on these findings, will be described in more detail below. <Alkaline degreasing bath> First, the alkaline degreasing bath of the present invention will be described. Note that the following description also includes a description of degreasing using the alkaline degreasing bath of the present invention. As described above, the grain-oriented electrical steel sheet after cold rolling is subjected to decarburization annealing, and then a slurry of an annealing separator mainly composed of MgO is applied thereto, followed by finish annealing to form a forsterite coating, thereby obtaining an electrical steel sheet with a forsterite coating.

[0028] In the present invention, before the decarburization annealing, degreasing is carried out using the alkaline degreasing bath of the present invention. When the silicic acid concentration (SiO2 equivalent) of the alkaline degreasing bath of the present invention is A (unit: mass %), it is essential that the refractive index R of the alkaline degreasing bath of the present invention satisfies the following formula (1). 4.6×10 -3 ×A+1.3340≦R (1)

[0029] By degreasing using the above-mentioned alkaline degreasing bath, the decarburization-annealed sheet that is then subjected to decarburization annealing has excellent adhesion of the annealing separator. Thereafter, a slurry of an annealing separator mainly composed of MgO is applied and then finish annealing is performed to obtain an electrical steel sheet with a homogeneous forsterite coating.

[0030] Here, the reason why the adhesion of the annealing separator can be controlled by controlling the refractive index R of the above-mentioned alkaline degreasing bath is not clear, but it is thought that when the refractive index R satisfies the above formula (1), the adsorption state of the annealing separator is stabilized, and as a result, the adhesion of the annealing separator to the steel sheet can be controlled.

[0031] The refractive index R of the alkaline degreasing bath of the present invention preferably satisfies the following formula (2), and more preferably satisfies the following formula (3), which improves the adhesion of the annealing separator to the decarburized annealed steel sheet and enables the formation of a homogeneous forsterite coating. 4.6×10 -3 ×A+1.3350≦R (2) 4.6×10 -3 ×A+1.3360≦R (3)

[0032] Furthermore, the alkaline degreasing bath of the present invention preferably contains a silicate. That is, sodium orthosilicate (Na4SiO4), sodium metasilicate (Na2SiO3), or a liquid mixture of various sodium silicates, so-called water glass, etc. are suitable. It is also possible to use an alkali metal silicate, such as potassium or lithium, instead of sodium. The refractive index R of a pure silicate aqueous solution satisfies the following formula (X) when the silicic acid concentration (SiO2 equivalent) is A (unit: mass %). R = 4.6 × 10 -4 ×A+1.330···(X)

[0033] On the other hand, if the refractive index R of the alkaline degreasing bath is too high, the concentration of silicic acid becomes too high, increasing the viscosity of the alkaline degreasing bath, reducing the degreasing efficiency, or leaving an excess of silicic acid on the steel sheet surface. In this case, compounds that are not originally formed on the surface of the decarburized annealed sheet may be formed, and the adhesion of the annealing separator to the decarburized annealed sheet is likely to be insufficient. For this reason, the refractive index R of the alkaline degreasing bath of the present invention is preferably 1.4200 or less, more preferably 1.4150 or less, because the annealing separator has excellent adhesion to the decarburized annealed sheet.

[0034] Here, the refractive index R of the alkaline degreasing bath is measured using a digital refractometer RX-5000i manufactured by Atago Co., Ltd. under the condition of a liquid temperature of 20°C.

[0035] The silicic acid concentration A (SiO2 equivalent) of the alkaline degreasing bath of the present invention is preferably 0.2 mass% or more, more preferably 0.5 mass% or more. On the other hand, if the silicic acid concentration is too high, the refractive index R increases, but the effect of improving the steel sheet adhesion of the annealing separator may be difficult to obtain. For this reason, the silicic acid concentration (SiO2 equivalent) of the alkaline degreasing bath of the present invention is preferably 10.0 mass% or less, more preferably 8.0 mass% or less.

[0036] Here, the silicic acid concentration A (unit: mass %) in terms of SiO2 in the alkaline degreasing bath is measured and calculated, for example, by an inductively coupled plasma (ICP) emission spectrometer.

[0037] The alkaline degreasing bath of the present invention contains, in addition to silicic acid and Na, ions of alkali metals such as K; ions of alkaline earth metals such as Mg, Ca, and Sr; cations such as Fe, Al, Mn, Cu, Ti, Ni, Sn, Se, and Cr; 2- , Se 2- It is preferable that the annealing separator contains anions such as the above anions, and ions such as the above ions. This improves the adhesion between the annealing separator and the decarburized annealed sheet. The reason for this is not clear, but it is believed that these ions have the effect of further stabilizing the control of the surface properties of the decarburized annealed sheet.

[0038] The content of the above-mentioned ions in the alkaline degreasing bath of the present invention is appropriately adjusted according to the desired refractive index R. That is, the value of the refractive index R is controlled by adjusting the content of these ions.

[0039] Furthermore, the alkaline degreasing bath of the present invention may contain water-soluble organic compounds such as chelating agents, surfactants, and organic acid metal salts. The chelating agents may include oxycarboxylic acid-type substances such as sodium citrate and sodium gluconate, aminocarboxylic acid-type substances such as ethylenediaminetetraacetic acid and sodium diethylenetriaminepentaacetate, and phosphonic acid-type substances such as etidronic acid. The surfactants may include ionic surfactants such as linear alkylbenzenesulfonates and alkyl sulfates, and nonionic surfactants such as polyoxyethylene alkyl ethers and polyhydric alcohols.

[0040] The content of the water-soluble organic compounds in the alkaline degreasing bath of the present invention is appropriately adjusted according to the desired refractive index R. In other words, the value of the refractive index R can also be controlled by adjusting the content of these water-soluble organic compounds.

[0041] The solvent for the alkaline degreasing bath of the present invention is preferably water, but is not limited to this.Other solvents such as ethanol, acetonitrile, and ethylenediamine may also be used.

[0042] The contents of these solvents in the alkaline degreasing bath of the present invention are appropriately adjusted according to the desired refractive index R. In other words, the value of the refractive index R can also be controlled by adjusting the contents of these solvents.

[0043] In order to obtain a sufficient effect from the degreasing, the degreasing temperature (temperature of the alkaline degreasing bath) is preferably 30° C. or higher, and more preferably 40° C. or higher. On the other hand, if the degreasing temperature is too high, precipitation may occur due to a change in the pH of the liquid caused by the evaporation of the solvent, making it difficult to control the refractive index R, which is uneconomical. For this reason, the temperature of the alkaline degreasing bath is preferably 95° C. or less, and more preferably 90° C. or less.

[0044] Similarly, in order to obtain a sufficient effect from the degreasing, the degreasing time is preferably 1 second or more, and more preferably 2 seconds or more. On the other hand, if the treatment time is too long, the apparatus used for the treatment may become long and bulky, which is uneconomical. Therefore, the degreasing treatment time is preferably 50 seconds or less, and more preferably 40 seconds or less.

[0045] In addition, the degreasing treatment is preferably an electrolytic degreasing treatment. The electrolytic degreasing method is not particularly limited as long as the cold-rolled sheet can be brought into contact with the alkaline degreasing bath of the present invention and an electric current can be applied. For example, a method in which a cold-rolled sheet of a grain-oriented electrical steel sheet is immersed in the alkaline degreasing bath of the present invention and an electric current is applied indirectly can be mentioned. In this case, it is preferable to satisfy the above-mentioned degreasing temperature and degreasing time.

[0046] <Composition of steel> First, the chemical composition of a preferred steel will be described. In the following, unless otherwise specified, the unit "%" for the content of each element means "mass %".

[0047] (C: 0.001~0.10%) C is useful for generating Goss orientation crystal grains. To effectively exert this effect, the C content is preferably 0.001% or more. On the other hand, if the C content is too high, decarburization may be insufficient even by decarburization annealing, so the C content is preferably 0.10% or less.

[0048] (Si: 1.0~5.0%) Silicon increases electrical resistance and reduces iron loss, and also stabilizes the BCC structure of iron, making high-temperature heat treatment possible, so the Si content is preferably 1.0% or more, and more preferably 2.0% or more. On the other hand, if the Si content is too high, cold rolling becomes difficult, so the Si content is preferably 5.0% or less.

[0049] (Mn: 0.01 to 1.0%) Mn effectively contributes to improving the hot brittleness of steel. Furthermore, when S or Se is mixed, Mn forms precipitates such as MnS and MnSe, and functions as an inhibitor of grain growth. For this reason, the Mn content is preferably 0.01% or more. On the other hand, if the Mn content is too high, the grain size of precipitates such as MnSe becomes coarse and the inhibitor function may be lost, so that the Mn content is preferably 1.0% or less.

[0050] (sol.Al:0.003~0.050%) Al forms AlN in steel, which becomes a dispersed second phase and functions as an inhibitor, so the Al content is preferably 0.003% or more as sol.Al. On the other hand, if the Al content is too high, AlN precipitates coarsely and may lose its inhibitory function, so the Al content is preferably 0.050% or less as sol.Al.

[0051] (N:0.001~0.020%) Like Al, N forms AlN, so the N content is preferably 0.001% or more. On the other hand, if the N content is too high, swelling may occur during heating of the slab, and therefore the N content is preferably 0.020% or less.

[0052] (At least one of S and Se: 0.001-0.05%) S and Se combine with Mn and Cu to form MnSe, MnS, Cu2-xSe, and Cu2-xS, which become dispersed second phases in the steel and function as inhibitors. Therefore, the total content of at least one of S and Se is preferably 0.001% or more. On the other hand, if the content of S and Se is too high, not only will the solid solution be incomplete when the slab is heated, but defects may also occur on the product surface. Therefore, the total content of at least one of S and Se is preferably 0.05% or less.

[0053] (Other elements) The above-mentioned composition may further contain at least one element (for convenience, referred to as "element A") selected from the group consisting of Cu: 0.01-0.2%, Ni: 0.01-0.5%, Cr: 0.01-0.5%, Sb: 0.01-0.1%, Sn: 0.01-0.5%, Mo: 0.01-0.5%, and Bi: 0.001-0.1%. The magnetic properties can be further improved by adding an element that functions as a supplementary inhibitor, such as element A, which tends to segregate to the crystal grain size or surface. Useful effects can be obtained by making the content of element A equal to or more than the lower limit of the above range. In addition, since secondary recrystallization defects may easily occur if the content of element A is too large, the content of element A is preferably equal to or less than the upper limit of the above range.

[0054] The above-mentioned composition may further contain at least one element selected from the group consisting of B: 0.001-0.01%, Ge: 0.001-0.1%, As: 0.005-0.1%, P: 0.005-0.1%, Te: 0.005-0.1%, Nb: 0.005-0.1%, Ti: 0.005-0.1%, and V: 0.005-0.1%. This further strengthens the ability to suppress the growth of crystal grains, making it possible to stably obtain a higher magnetic flux density.

[0055] (remainder) The balance of the above-mentioned composition is composed of Fe and unavoidable impurities.

[0056] 《Manufacturing method》 Next, an example of a method for producing a cold-rolled sheet of electrical steel will be described. First, for example, steel having the above-mentioned composition is melted by a conventionally known refining process, and a steel slab is obtained by a continuous casting method or an ingot casting-blooming rolling method. The resulting steel slab is then hot rolled to produce a hot rolled sheet, which is then annealed as necessary. The steel slab is then cold rolled once or twice or more with intermediate annealing to produce a cold rolled sheet of the final thickness. The forsterite-coated electrical steel sheet is then manufactured according to the procedure described below.

[0057] <Manufacturing method of forsterite-coated electrical steel sheet> The cold-rolled sheet of electrical steel is degreased using the alkaline degreasing bath of the present invention. Next, primary recrystallization annealing and decarburization annealing are performed, and then an annealing separator containing MgO is applied, followed by final annealing. In this way, an electrical steel sheet having a coating containing forsterite (forsterite coating) formed on the surface is obtained. Compounds are added to the annealing separator as necessary. Examples of compounds to be added include oxides, hydroxides, sulfides, sulfates, chlorides, oxychlorides, borates, etc. of Sb, Mn, Sn, Zr, Ti, Al, alkali metals, alkaline earth metals, etc.

[0058] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the examples described below. EXAMPLES

[0059] A steel slab made from a steel having a chemical composition within the above-mentioned preferred range was subjected to hot rolling and cold rolling to produce a cold-rolled sheet having a thickness of 0.20 mm. The grain-oriented cold-rolled electrical steel sheet was then immersed in the steel for degreasing under the degreasing conditions (degreasing temperature and degreasing time) shown in Table 1, and then decarburization annealing was performed. An annealing separator mainly composed of MgO (MgO: 100 mass% and TiO2: 6 mass%) was then applied to the steel sheet in such a manner that the adhesion amount after drying was 13.0 g / m2 in total on both sides of the steel sheet. 2 An insulating coating (forsterite coating) was formed by applying the coating using a roll coater so that the coating became as shown in Table 1, and then performing high-temperature finish annealing. To perform this treatment, an alkaline degreasing bath shown in Table 1 was prepared. Specifically, an appropriate amount of sodium orthosilicate was added to the solvents (water, acetonitrile) shown in Table 1, and, if necessary, sodium metasilicate or lithium silicate shown in Table 1, compounds such as sodium citrate, ethylenediaminetetraacetic acid, and sodium diethylenetriaminepentaacetate as chelating agents, and compounds such as Fomezarin (product name) manufactured by Kao Corporation as a surfactant, and other metal ions were added to adjust the silicic acid concentration A and refractive index R.

[0060] For the grain-oriented electrical steel sheets with an insulation coating thus obtained, the adhesion of the annealing separator to the steel sheet and the appearance uniformity of the insulation coating in the decarburized annealed sheet after application of the annealing separator are shown in Table 1. The adhesion of the annealing separator to the steel sheet and the appearance uniformity of the insulation coating were evaluated as follows.

[0061] <Evaluation of adhesion of annealing separator to steel sheet> The adhesion of the annealing separator to the steel sheet was evaluated based on the peeling rate determined by the procedure described below, and when the peeling rate was 20% or less, the adhesion of the annealing separator to the steel sheet was evaluated as good.

[0062] (a) A test piece of 300 mm in the rolling direction (L direction) × 100 mm in the direction perpendicular to the rolling direction (C direction) is taken from a 0.20 mm-thick degreased cold-rolled sheet, and the weight of the test piece is measured. (b) On one side of the test piece in (a), the annealing separator slurry was applied with a weight of 13.0±0.5g / m2 after drying. 2 Apply the mixture so that it becomes even. (c) The weight of the test piece after drying is measured, and the amount of the annealing separator applied is calculated. (d) The test piece (c) is placed on the bottom of a plastic container with the annealing separator-coated surface facing up, and 300 g of Tosoh Corporation's zirconia balls (average particle size: 2 mm) are placed to one side of the test piece. (e) The container is tilted 45 degrees over a period of 5 seconds, and the zirconia ball is slid over the surface of the test piece. After 15 reciprocating movements, the weight of the test piece is measured and the amount of weight loss is calculated. The peeling rate (%) is calculated by dividing the weight loss in (f)(e) by the amount of annealing separator applied in (c).

[0063] <Evaluation of the appearance uniformity of the insulation coating> The homogeneity of the appearance of the insulating coating is evaluated as "X" if it exhibits an uneven appearance, such as uneven coloring on the outer periphery or edges, thin parts of the coating, the metal surface showing through, or defects, and is evaluated as "O" if it forms a uniform coating other than the above.

[0064] [Table 1]

[0065] <Summary of evaluation results> As shown in Table 1 above, the examples of the invention in which pretreatment was performed using an alkaline degreasing bath satisfying formula (1) had excellent adhesion of the annealing separator to the steel sheet and good forsterite coating appearance, compared to the comparative examples which did not satisfy formula (1). Furthermore, when comparing the examples of the invention which satisfied formula (1), the examples of the invention having a refractive index R of 1.4200 or less had better adhesion to the steel sheet than the examples which did not satisfy formula (1). In particular, the adhesion of the annealing separator to the steel sheet was excellent when the silicic acid concentration A was 0.5 to 8 mass%, the degreasing bath temperature was 35°C to 90°C, and the degreasing time was 40 seconds or less. EXAMPLES

[0066] A steel slab made from a steel having a composition within the above-mentioned preferred range was hot-rolled and cold-rolled to produce a cold-rolled sheet having a thickness of 0.20 mm. The grain-oriented electrical steel cold-rolled sheet was then electrolytically degreased under the conditions (electrolytic degreasing temperature and electrolytic degreasing time) shown in Table 2 at a charge density of 12 C / dm 2 Then, the steel sheet was electrolytically degreased with 0.1% NaCl, and then decarburized and annealed. The steel sheet was then coated with an annealing separator mainly composed of MgO (MgO: 100% by mass, TiO2: 6% by mass, and sodium borate: 0.5% by mass) so that the total amount of the coating after drying was 13.0 g / m2 on both sides of the steel sheet. 2 A forsterite coating was formed by applying the solution using a roll coater so that the solution was coated on the substrate and then high-temperature finish annealing was performed. To carry out this treatment, an alkaline degreasing bath shown in Table 2 was prepared. Specifically, an appropriate amount of sodium orthosilicate was added to 10 L of solvent, and the silicic acid concentration A and refractive index R were adjusted by adding lithium silicate shown in Table 2 as necessary, citric acid, etidronic acid, sodium diethylenetriaminepentaacetate as a chelating agent, poly(oxyethylene) alkyl ether, Fomezarin (product name) manufactured by Kao Corporation as a surfactant, and other metal ions.

[0067] [Table 2]

[0068] <Summary of evaluation results> As shown in Table 2 above, the examples of the invention in which electrolytic degreasing pretreatment was performed using an alkaline degreasing bath satisfying formula (1) had excellent adhesion of the annealing separator to the steel sheet and a good forsterite coating appearance. The peeling rate of the annealing separator was reduced compared to the case of immersion degreasing. In addition, when comparing the examples of the invention satisfying formula (1), the examples of the invention having a refractive index R of 1.4200 or less had better adhesion to the steel sheet than the examples of the invention that did not satisfy this.

Claims

1. An alkaline degreasing bath having a bath composition containing silicic acid, which is used for degreasing a cold-rolled sheet of grain-oriented electrical steel, The silicic acid concentration is SiO 2 The refractive index R of the bath when converted into A mass % satisfies the following formula (1). 4.6×10 -3 ×A+1.3340≦R≦1.4209 ・・・(1)

2. 2. The alkaline degreasing bath according to claim 1, wherein the refractive index R is less than or equal to 1.4200.

3. The silicic acid concentration is SiO 2 The alkaline degreasing bath according to claim 1 or 2, wherein the alkali content is 0.2 mass % or more and 10.0 mass % or less in terms of alkali content.

4. 3. An alkaline degreasing bath according to claim 1, which contains at least one of alkali metal ions, alkaline earth metal ions and ions of group 16.

5. 3. The alkaline degreasing bath according to claim 1, further comprising at least one of a chelating agent, a surfactant and an organic acid metal salt.

6. A method for producing grain-oriented electrical steel sheet with an insulating coating, comprising the steps of hot rolling and cold rolling a grain-oriented electrical steel material to obtain a cold-rolled sheet, degreasing the cold-rolled sheet using the alkaline degreasing bath according to claim 1 or 2, and then subjecting the cold-rolled sheet to decarburization annealing. Thereafter, an annealing separator is applied to the surface of the decarburization annealed sheet, followed by finish annealing.

7. 7. The method for producing a grain-oriented electrical steel sheet with an insulation coating according to claim 6, wherein the temperature of the alkaline degreasing bath is from 30° C. to 95° C., and the degreasing time in the alkaline degreasing bath is from 1 second to 40 seconds.

8. The method for producing a grain-oriented electrical steel sheet with an insulation coating according to claim 6, wherein the cold-rolled sheet is subjected to electrolytic degreasing.

9. A method for preparing an alkaline degreasing bath having a bath composition containing silicic acid, which is used for degreasing a cold-rolled sheet of grain-oriented electrical steel, comprising the steps of: The silicic acid concentration is SiO 2 A method for adjusting an alkaline degreasing bath, comprising adjusting a refractive index R of the bath to satisfy the following formula (1) when converted into A mass %. 4.6×10 -3 ×A+1.3340≦R≦1.4209 ・・・(1)

10. 10. The method for preparing an alkaline degreasing bath according to claim 9, wherein the refractive index R is 1.4200 or less.

11. The silicic acid concentration is SiO 2 The method for adjusting an alkaline degreasing bath according to claim 9 or 10, wherein the alkali content is 0.2 mass% or more and 10.0 mass% or less in terms of alkali content.

12. 11. The method for preparing an alkaline degreasing bath according to claim 9 or 10, further comprising adding to the alkaline degreasing bath at least one of an alkali metal ion, an alkaline earth metal ion, and an ion of Group 16.

13. 11. The method for preparing an alkaline degreasing bath according to claim 9 or 10, further comprising adding to the alkaline degreasing bath at least one of a chelating agent, a surfactant, and an organic acid metal salt.

Citation Information

Patent Citations

  • Concentrated liquid degreasing agent for silicon steel continuous annealing production line and preparation method thereof

    CN104962938A

  • Environment-friendly processing equipment and method for oriented silicon steel

    CN109136490A

  • Formation of forsterite insulating film on directional silicon steel plate

    JP1983093877A

  • Annealing separating agent for grain-oriented magnetic steel sheet for obtaining uniform glass coating film and excellent magnetic characteristic

    JP1989177376A

  • Production of grain-oriented silicon steel sheet having uniform forsterite coating film